A TiO2-based inorganic composite material and its preparation method and application
Through the low-temperature sintering method of TiO2-based inorganic composite materials, the safety hazards of liquid electrolytes in lithium-ion batteries and the high energy consumption of solid-phase sintering methods are solved, the preparation temperature of lithium-ion batteries is reduced, and the performance and production of LATP solid electrolytes are improved. efficiency.
Patent Information
- Application Number
- CN202210589648.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-27
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-05-27
AI Technical Summary
Liquid electrolytes in traditional lithium-ion batteries have potential safety hazards, and the high sintering temperature when preparing lithium aluminum titanium phosphate (LATP) solid electrolyte using the solid-phase sintering method results in lithium salt volatilization, high energy consumption, and high costs.
Using TiO2-based inorganic composite materials through solid-phase sintering method, the sintering temperature is reduced to 500℃-700℃, and the material is used to prepare LATP solid electrolyte, the sintering temperature is lowered to below 1000℃, and the intergranular bonding strength and ionic conductivity are improved.
Low-temperature sintering is achieved to save energy consumption, reduce costs, maintain the pure phase structure of LATP, and improve the performance and production efficiency of solid electrolytes.
Smart Images

Figure CN115036562B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium battery materials, and in particular to a TiO2-based inorganic composite material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are currently the most mature lithium-series secondary batteries and have broad application prospects in mobile communications, electric vehicles, national defense science and technology and other fields.
[0003] Electrolyte is an important component of lithium-ion batteries. Traditional lithium-ion batteries use liquid electrolytes, which have disadvantages such as high volatility, easy leakage, poor impact resistance, and potential safety hazards. The development of all-solid-state lithium-ion batteries based on solid electrolytes can solve the safety hazards caused by liquid electrolytes. Inorganic solid electrolytes have attracted much attention due to their advantages such as safety and easy preparation, high mechanical strength, high room temperature grain conductivity, high lithium ion mobility, and excellent electrochemical stability.
[0004] Among inorganic solid electrolytes, lithium aluminum titanate phosphate Li 1+x Al x Ti 2-x (PO4)3(LATP) room temperature ionic conductivity up to 10 -3 S / cm, which is close to the level of commercial electrolytes and is particularly noteworthy.
[0005] Currently, the common methods for synthesizing lithium aluminum titanium phosphate mainly include solid-phase sintering, liquid-phase precipitation and sol-gel methods. Among these preparation methods, the solid-phase sintering and liquid-phase precipitation processes are simple and more suitable for industrial mass production. However, when the solid-phase sintering process is used to prepare LATP solid electrolyte, the required sintering temperature is above 1050°C, which causes the loss of lithium in the sintering product due to high-temperature volatilization of lithium salts, resulting in impure products. In addition, the energy consumption of the preparation is relatively large and the cost is high. Summary of the invention
[0006] The embodiment of the present invention provides a TiO2-based inorganic composite material and a preparation method and application thereof. The TiO2-based inorganic composite material is pre-prepared by a solid-phase sintering method, and the sintering temperature is between 500°C and 700°C. The low-temperature sintering saves energy consumption, and the process is simple, which can be applied to mass production, and the performance is stable and easy to preserve. The TiO2-based inorganic composite material is used to prepare a LATP solid-state electrolyte material, which can effectively reduce the sintering temperature when the LATP solid-state electrolyte material is prepared by a solid-phase method, so that the sintering temperature is reduced to below 1000°C, which reduces energy consumption and saves costs. At the same time, due to the low-temperature sintering process, the LATP maintains a pure phase structure, thereby improving the intercrystalline bonding strength and ionic conductivity of the LATP solid-state electrolyte material.
[0007] In a first aspect, an embodiment of the present invention provides a TiO2-based inorganic composite material, wherein the general chemical formula of the TiO2-based inorganic composite material is: Li 1+x Al y Ti 2y-1 O 3z+4 (PO4) z , where 0.1 <x<1,0<y<2,0<z<1;
[0008] The X-ray diffraction pattern of the TiO2-based inorganic composite material contains characteristic diffraction peaks in the range of 10°-60°, wherein the positions of the main peaks are located at 2θ angles of 18.8°, 21.6°, 22.6°, 25.2°, 27.3°, 37.8°, 48.1°53.9° and 55.1°; the peak intensity ratio of the secondary peak to the highest peak in the X-ray diffraction pattern of the TiO2-based inorganic composite material is I=0.51;
[0009] The crystal structure of the TiO2-based inorganic composite material is an anatase crystal structure.
[0010] Preferably, the pH value of the TiO2-based inorganic composite material is 7-8.
[0011] Preferably, the particle size of the TiO2-based inorganic composite material is between 10 μm and 20 μm.
[0012] In a second aspect, an embodiment of the present invention provides a method for preparing the TiO2-based inorganic composite material described in the first aspect, the preparation method comprising:
[0013] Weigh titanium dioxide, lithium source material, aluminum source material and phosphorus source material in proportion, put them into a mixer and mix them evenly to obtain a mixed material;
[0014] Placing the mixed material in a reaction furnace for sintering, setting the sintering temperature between 500° C. and 700° C., and the heat preservation time between 3 hours and 15 hours, to obtain a sintered product;
[0015] The sintered product is crushed to obtain a TiO2-based inorganic composite material;
[0016] The general chemical formula of the TiO2-based inorganic composite material is: Li 1+x Al y Ti 2y-1 O 3z+4 (PO4) z , where 0.1 <x<1,0<y<2,0<z<1;
[0017] The X-ray diffraction pattern of the TiO2-based inorganic composite material contains characteristic diffraction peaks in the range of 10°-60°, wherein the positions of the main peaks are located at 2θ angles of 18.8°, 21.6°, 22.6°, 25.2°, 27.3°, 37.8°, 48.1°53.9° and 55.1°; the peak intensity ratio of the secondary peak to the highest peak in the X-ray diffraction pattern of the TiO2-based inorganic composite material is I=0.51;
[0018] The crystal structure of the TiO2-based inorganic composite material is an anatase crystal structure.
[0019] Preferably, the pH value of the TiO2-based inorganic composite material is 7-8;
[0020] The particle size of the TiO2-based inorganic composite material is between 10 μm and 20 μm.
[0021] Preferably, the lithium source material includes: one or more of lithium carbonate, lithium hydroxide, lithium nitrate or lithium acetate;
[0022] The phosphorus source material includes: one or more of red phosphorus, white phosphorus, black phosphorus, phosphorus pentoxide, phosphorus trioxide, phosphoric acid, diammonium dihydrogen phosphate or diammonium hydrogen phosphate;
[0023] The aluminum source material includes: one or more of aluminum oxide, aluminum hydroxide, aluminum acetate, aluminum nitrate or aluminum chloride.
[0024] Further preferably, the phosphorus source material is phosphoric acid, the lithium source material is lithium carbonate, and the aluminum source material is aluminum oxide.
[0025] Preferably, the reaction furnace comprises: a rotary furnace, a tubular furnace, a bell furnace or a fluidized bed;
[0026] The sintering temperature is 500° C. and the heat preservation time is 10 hours.
[0027] Preferably, the crushing process is specifically as follows: the sintered product is primarily crushed using a ball mill or a roller mill to obtain precursor particles; the precursor particles are then crushed by a jet mill to obtain a TiO2-based inorganic composite material.
[0028] In a third aspect, an application of the TiO2-based inorganic composite material described in the first aspect is provided, wherein the TiO2-based inorganic composite material is used to prepare a LATP solid electrolyte material; and the sintering temperature for preparing the LATP solid electrolyte material is between 850°C and 900°C.
[0029] The embodiment of the present invention provides a TiO2-based inorganic composite material and a preparation method and application thereof. The TiO2-based inorganic composite material is pre-prepared by a solid-phase sintering method, and the sintering temperature is between 500°C and 700°C. The low-temperature sintering saves energy consumption, and the process is simple, which can be applied to mass production, and the performance is stable and easy to preserve. The TiO2-based inorganic composite material is used to prepare a LATP solid-state electrolyte material, which can effectively reduce the sintering temperature when the LATP solid-state electrolyte material is prepared by a solid-phase method, so that the sintering temperature is reduced to below 1000°C, which reduces energy consumption and saves costs. At the same time, due to the low-temperature sintering process, the LATP maintains a pure phase structure, thereby improving the intercrystalline bonding strength and ionic conductivity of the LATP solid-state electrolyte material. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The technical solution of the embodiment of the present invention is further described in detail below through the drawings and examples.
[0031] Figure 1 is a flow chart of a method for preparing a TiO2-based inorganic composite material provided by an embodiment of the present invention;
[0032] Figure 2 is the X-ray diffraction pattern (XRD) of the TiO2-based inorganic composite material prepared in Example 1 of the present invention;
[0033] Figure 3 is the XRD pattern of the TiO2-based inorganic composite material prepared in Example 2 of the present invention;
[0034] Figure 4 is the XRD pattern of the TiO2-based inorganic composite material prepared in Example 3 of the present invention;
[0035] Figure 5 1 is the XRD diagram of LATP prepared in Example 4 and Example 5 of the present invention. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below through the accompanying drawings and specific embodiments, but it should be understood that these embodiments are only used for more detailed description and should not be understood as limiting the present invention in any form, that is, they are not intended to limit the protection scope of the present invention.
[0037] The embodiment of the present invention provides a TiO2-based inorganic composite material, the general chemical formula of the TiO2-based inorganic composite material is: Li 1+x Al y Ti 2y-1 O 3z+4 (PO4) z , where 0.1 <x<1,0<y<2,0<z<1。
[0038] The X-ray diffraction pattern of the TiO2-based inorganic composite material contains characteristic diffraction peaks in the range of 10°-60°, among which the main peaks are located at 2θ angles of 18.8°, 21.6°, 22.6°, 25.2°, 27.3°, 37.8°, 48.1°53.9° and 55.1°; the peak intensity ratio of the second highest peak to the highest peak in the X-ray diffraction pattern of the TiO2-based inorganic composite material is I=0.51; the crystal structure of the TiO2-based inorganic composite material is anatase crystal structure, and the pH value is 7-8.
[0039] The particle size of the TiO2-based inorganic composite material is between 10 μm and 20 μm. Smaller particles can effectively increase the reaction activity of the TiO2-based inorganic composite material, shorten the reaction time, and improve the efficiency of preparing LATP.
[0040] The present invention provides a method for preparing the above-mentioned TiO2-based inorganic composite material, such as Figure 1 As shown, the preparation method comprises:
[0041] 110, weigh titanium dioxide, lithium source material, aluminum source material and phosphorus source material according to molar ratio, put them into a mixer and mix them evenly to obtain a mixed material;
[0042] Wherein, the lithium source material includes: one or more of lithium carbonate, lithium hydroxide, lithium nitrate or lithium acetate;
[0043] The phosphorus source material includes one or more of red phosphorus, white phosphorus, black phosphorus, phosphorus pentoxide, phosphorus trioxide, phosphoric acid, diammonium dihydrogen phosphate or diammonium hydrogen phosphate;
[0044] The aluminum source material includes one or more of aluminum oxide, aluminum hydroxide, aluminum acetate, aluminum nitrate or aluminum chloride.
[0045] In a preferred embodiment, the phosphorus source material is phosphoric acid, the lithium source material is lithium carbonate, and the aluminum source material is aluminum oxide.
[0046] 120, placing the mixed material in a reaction furnace for sintering, setting the sintering temperature between 500° C. and 700° C., and the heat preservation time between 3 hours and 15 hours, to obtain a sintered product;
[0047] The reaction furnace includes: a rotary furnace, a tubular furnace, a bell furnace or a fluidized bed;
[0048] In a preferred embodiment, the sintering temperature is 500° C. and the holding time is 10 hours.
[0049] 130, crushing the sintered product to obtain a TiO2-based inorganic composite material;
[0050] The crushing process is as follows: the sintered product is primarily crushed by a ball mill or a roller mill to obtain precursor particles; the precursor particles are crushed by a jet mill to obtain a TiO2-based inorganic composite material;
[0051] Among them, the chemical formula of TiO2-based inorganic composite materials is: Li 1+x Al y Ti 2y-1 O 3z+4 (PO4) z , where 0.1 <x<1,0<y<2,0<z<1。
[0052] The X-ray diffraction pattern of the TiO2-based inorganic composite material contains characteristic diffraction peaks in the range of 10°-60°, wherein the positions of the main peaks are located at 2θ angles of 18.8°, 21.6°, 22.6°, 25.2°, 27.3°, 37.8°, 48.1°53.9° and 55.1°; the peak intensity ratio of the second highest peak to the highest peak in the X-ray diffraction pattern of the TiO2-based inorganic composite material is I=0.51; the crystal structure of the TiO2-based inorganic composite material is anatase crystal structure;
[0053] The pH value of the TiO2-based inorganic composite material is 7-8, and the particle size is between 10 μm and 20 μm.
[0054] The embodiment of the present invention provides an application of the above-mentioned TiO2-based inorganic composite material. The TiO2-based inorganic composite material can be used to prepare LATP solid electrolyte material. The preparation method specifically includes:
[0055] The TiO2-based inorganic composite material is pulverized;
[0056] The crushed TiO2-based inorganic composite material is placed in a reaction furnace, heated to 850°C-900°C in an argon protective atmosphere, and kept warm for 5-15 hours to obtain a LATP solid electrolyte material;
[0057] The reaction furnace includes: a rotary furnace, a tubular furnace, a bell furnace or a fluidized bed.
[0058] The use of TiO2-based inorganic composite materials to prepare LATP solid electrolyte materials can effectively reduce the sintering temperature when preparing LATP solid electrolyte materials using the solid phase method, reduce the sintering temperature to below 1000°C, and improve the intercrystalline bonding strength and ionic conductivity of the LATP solid electrolyte materials.
[0059] In order to better understand the technical solution provided by the present invention, the preparation process and characteristics of the TiO2-based inorganic composite material of the present invention are respectively described below with multiple specific examples.
[0060] Example 1
[0061] This embodiment provides a method for preparing a TiO2-based inorganic composite material, and the specific steps are as follows:
[0062] 1) 79.87 g of titanium dioxide, 78.2 g of phosphoric acid, 11.65 g of lithium carbonate and 7.12 g of aluminum oxide were weighed in molar ratio, put into a mixer and stirred for 1 hour to obtain a mixed material.
[0063] 2) The mixed material is placed in a sagger and put into a tube furnace for sintering. In an argon atmosphere, the temperature is raised to 500° C. and kept warm for 10 hours to obtain a sintered product.
[0064] 3) The sintered product is subjected to ball milling to obtain a TiO2-based inorganic composite material having the chemical formula: Li 1.5 Al 1.2 Ti 1.4 O 4.9 (PO4) 0.3 .
[0065] The TiO2-based inorganic composite material prepared in this example was characterized and tested:
[0066] The pH value of the TiO2-based inorganic composite material prepared in this example was tested to be 7.2;
[0067] The XRD pattern of the TiO2-based inorganic composite material prepared in this embodiment is as follows: Figure 2 As shown, it contains characteristic diffraction peaks in the range of 10°-60°, and the main peak positions are located at 2θ angles of 18.8°, 21.6°, 22.6°, 25.2°, 27.3°, 37.8°, 48.1°53.9° and 55.1°.
[0068] Example 2
[0069] This embodiment provides a method for preparing a TiO2-based inorganic composite material, and the specific steps are as follows:
[0070] 1) 79.87 g of titanium dioxide, 90.67 g of ammonium dihydrogen phosphate, 9.32 g of lithium hydroxide and 26.78 g of aluminum acetate were weighed in molar ratio, put into a mixer and stirred for 1 hour to obtain a mixed material.
[0071] 2) The mixed material is placed in a sagger and put into a tube furnace for sintering. In an argon atmosphere, the temperature is raised to 700° C. and kept at this temperature for 15 hours to obtain a sintered product.
[0072] 3) The sintered product is subjected to ball milling to obtain a TiO2-based inorganic composite material having the chemical formula: Li 1.9 AlTiO 4.3 (PO4)0.1 .
[0073] The TiO2-based inorganic composite material prepared in this example was characterized and tested:
[0074] The pH value of the TiO2-based inorganic composite material prepared in this example was tested to be 7.8;
[0075] The XRD pattern of the TiO2-based inorganic composite material prepared in this embodiment is as follows: Figure 3 As shown, it contains characteristic diffraction peaks in the range of 10°-60°, and the main peak positions are located at 2θ angles of 18.8°, 21.6°, 22.6°, 25.2°, 27.3°, 37.8°, 48.1°53.9° and 55.1°.
[0076] Example 3
[0077] This embodiment provides a method for preparing a TiO2-based inorganic composite material, and the specific steps are as follows:
[0078] 1) 79.87 g of titanium dioxide, 56.29 g of phosphorus pentoxide, 26.18 g of lithium nitrate and 21.59 g of aluminum nitrate were weighed in molar ratio, put into a mixer and stirred for 1 hour to obtain a mixed material.
[0079] 2) The mixed material is placed in a sagger and put into a rotary furnace for sintering. In an argon atmosphere, the temperature is raised to 500° C. and kept at this temperature for 3 hours to obtain a sintered product.
[0080] 3) The sintered product is subjected to ball milling to obtain a TiO2-based inorganic composite material having the chemical formula: Li 1.7 Al 1.1 Ti 1.2 O 4.6 (PO4) 0.2 .
[0081] The TiO2-based inorganic composite material prepared in this example was characterized and tested:
[0082] The pH value of the TiO2-based inorganic composite material prepared in this example was tested to be 7.5;
[0083] The XRD pattern of the TiO2-based inorganic composite material prepared in this embodiment is as follows: Figure 4 As shown, it contains characteristic diffraction peaks in the range of 10°-60°, and the main peak positions are located at 2θ angles of 18.8°, 21.6°, 22.6°, 25.2°, 27.3°, 37.8°, 48.1°53.9° and 55.1°.
[0084] Example 4
[0085] This embodiment provides a method for preparing a LATP solid electrolyte material using the TiO2-based inorganic composite material prepared in Example 1, and the specific steps are as follows:
[0086] 1) crushing the TiO2-based inorganic composite material prepared in Example 1;
[0087] 2) The crushed TiO2-based inorganic composite material is placed in a tubular furnace, heated to 900° C. in an argon protective atmosphere, and kept warm for 5 hours to obtain a LATP solid electrolyte material.
[0088] The LATP solid electrolyte material prepared in this example was characterized by XRD for its crystal structure. Figure 5 As shown, the crystal form of the LATP solid electrolyte material conforms to the standard card JCPDS NO.82-0297, indicating that the LATP material is successfully prepared by the TiO2-based inorganic composite material of Example 1, and the prepared LATP solid electrolyte material has high crystallinity and purity.
[0089] Example 5
[0090] This embodiment provides a method for preparing a LATP solid electrolyte material using the TiO2-based inorganic composite material prepared in Example 2, and the specific steps are as follows:
[0091] 1) crushing the TiO2-based inorganic composite material prepared in Example 1;
[0092] 2) The crushed TiO2-based inorganic composite material is placed in a tubular furnace, heated to 850°C in an argon protective atmosphere, and kept warm for 15 hours to obtain a LATP solid electrolyte material.
[0093] The LATP solid electrolyte material prepared in this example was characterized by XRD for its crystal structure. Figure 5 As shown, the crystal form of the LATP solid electrolyte material conforms to the standard card JCPDS NO.82-0297, indicating that the LATP solid electrolyte material is successfully prepared by the TiO2-based inorganic composite material of Example 1, and the prepared LATP solid electrolyte material has high crystallinity and purity.
[0094] The embodiment of the present invention provides a TiO2-based inorganic composite material and a preparation method and application thereof. The TiO2-based inorganic composite material is pre-prepared by a solid-phase sintering method, and the sintering temperature is between 500°C and 700°C. The low-temperature sintering saves energy consumption, and the process is simple, which can be applied to mass production, and the performance is stable and easy to preserve. The TiO2-based inorganic composite material is used to prepare a LATP solid-state electrolyte material, which can effectively reduce the sintering temperature when the LATP solid-state electrolyte material is prepared by a solid-phase method, so that the sintering temperature is reduced to below 1000°C, which reduces energy consumption and saves costs. At the same time, due to the low-temperature sintering process, the LATP maintains a pure phase structure, thereby improving the intercrystalline bonding strength and ionic conductivity of the LATP solid-state electrolyte material.
[0095] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A TiO2-based inorganic composite material, characterized in that: The general chemical formula of the TiO2-based inorganic composite material is: Li 1+x Al y Ti 2y-1 O 3z+4 (PO4) z , where 0.1 <x<1,0<y<2,0<z<1; The X-ray diffraction pattern of the TiO2-based inorganic composite material contains characteristic diffraction peaks in the range of 10°-60°, wherein the positions of the main peaks are located at 2θ angles of 18.8°, 21.6°, 22.6°, 25.2°, 27.3°, 37.8°, 48.1°53.9° and 55.1°; the peak intensity ratio of the secondary peak to the highest peak in the X-ray diffraction pattern of the TiO2-based inorganic composite material is I=0.51; The crystal structure of the TiO2-based inorganic composite material is an anatase crystal structure.
2. The TiO2-based inorganic composite material according to claim 1, characterized in that: The pH value of the TiO2-based inorganic composite material is 7-8.
3. The TiO2-based inorganic composite material according to claim 1, characterized in that: The particle size of the TiO2-based inorganic composite material is between 10 μm and 20 μm.
4. A method for preparing the TiO2-based inorganic composite material according to any one of claims 1 to 3, characterized in that: The preparation method comprises: Weigh titanium dioxide, lithium source material, aluminum source material and phosphorus source material in molar ratio, put them into a mixer and mix them evenly to obtain a mixed material; Placing the mixed material in a reaction furnace for sintering, setting the sintering temperature between 500° C. and 700° C., and the heat preservation time between 3 hours and 15 hours, to obtain a sintered product; The sintered product is crushed to obtain a TiO2-based inorganic composite material; The general chemical formula of the TiO2-based inorganic composite material is: Li 1+x Al y Ti 2y-1 O 3z+4 (PO4) z , where 0.1 <x<1,0<y<2,0<z<1; The X-ray diffraction pattern of the TiO2-based inorganic composite material contains characteristic diffraction peaks in the range of 10°-60°, wherein the positions of the main peaks are located at 2θ angles of 18.8°, 21.6°, 22.6°, 25.2°, 27.3°, 37.8°, 48.1°53.9° and 55.1°; the peak intensity ratio of the secondary peak to the highest peak in the X-ray diffraction pattern of the TiO2-based inorganic composite material is I=0.51; The crystal structure of the TiO2-based inorganic composite material is an anatase crystal structure.
5. The preparation method according to claim 4, characterized in that: The pH value of the TiO2-based inorganic composite material is 7-8; The particle size of the TiO2-based inorganic composite material is between 10 μm and 20 μm.
6. The preparation method according to claim 4, characterized in that: The lithium source material includes: one or more of lithium carbonate, lithium hydroxide, lithium nitrate or lithium acetate; The phosphorus source material includes: one or more of red phosphorus, white phosphorus, black phosphorus, phosphorus pentoxide, phosphorus trioxide, phosphoric acid, diammonium dihydrogen phosphate or diammonium hydrogen phosphate; The aluminum source material includes: one or more of aluminum oxide, aluminum hydroxide, aluminum acetate, aluminum nitrate or aluminum chloride.
7. The preparation method according to claim 6, characterized in that: The phosphorus source material is phosphoric acid, the lithium source material is lithium carbonate, and the aluminum source material is aluminum oxide.
8. The preparation method according to claim 4, characterized in that: The reaction furnace comprises: a rotary furnace, a tubular furnace, a bell furnace or a fluidized bed; The sintering temperature is 500° C. and the heat preservation time is 10 hours.
9. The preparation method according to claim 4, characterized in that: The crushing process is specifically as follows: the sintered product is primarily crushed by a ball mill or a roller mill to obtain precursor particles; the precursor particles are then crushed by a jet mill to obtain a TiO2-based inorganic composite material.
10. An application of the TiO2-based inorganic composite material according to any one of claims 1 to 3, wherein the TiO2-based inorganic composite material is used to prepare a LATP solid electrolyte material; and the sintering temperature for preparing the LATP solid electrolyte material is between 850°C and 900°C.
Citation Information
Patent Citations
Phase-shift-free lithium aluminum titanium phosphate, and method for the production thereof and use thereof
CN102648154A
Inorganic solid-state electrolyte material and preparation method therefor
CN105609881A
Nanometer lithium aluminium titanium phosphate solid electrolyte material and preparation method therefor
CN105680090A
Sagger for preparing lithium aluminum titanium phosphate solid electrolyte material and preparation method of sagger
CN113943151A