Aluminum alloy casting device including a composite casting mold and a core with a built-in cooling water channel

By using the combination technology of composite casting and built-in cooling waterway core in aluminum alloy casting, the problem of low cavity accuracy and mechanical properties of aluminum alloy casting is solved, and high-precision and high-strength casting manufacturing is achieved, and metallurgical quality is improved. and wholesale pass rate.

CN115041665BActive Publication Date: 2024-11-05AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210653973.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-09
Publication Date
2024-11-05
Estimated Expiration
2042-06-09

AI Technical Summary

Technical Problem

In the existing casting process, aluminum alloy precision castings have poor cavity dimensional accuracy, low mechanical properties, many metallurgical defects, poor surface quality and finish, making it difficult to meet the high precision and high strength requirements of complex structural aluminum alloy castings.

Method used

An aluminum alloy casting device with composite casting molds and built-in cooling water circuit cores is used to achieve reasonable solidification temperature gradient distribution and cooling speed improvement through the combination of different casting materials and cooling water circuits, forming high-strength and high-toughness castings.

Benefits of technology

It significantly improves the inner cavity dimensional accuracy and surface finish of the castings, enhances mechanical properties, meets the technical requirements of complex profiles and large-scale aluminum alloy precision castings, and improves metallurgical quality and batch production pass rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115041665B_ABST
    Figure CN115041665B_ABST
Patent Text Reader

Abstract

The present invention provides an aluminum alloy casting device comprising a composite casting mold and a core with a built-in cooling water channel, wherein the device comprises the composite casting mold and the core; the aluminum alloy casting device can realize high-precision, high-strength liquid molding of large-scale aluminum alloy castings with complex thin-wall structures. Compared with the traditional single sand mold casting process, the dimension tolerance of the inner cavity of the casting prepared by the composite casting mold of the present invention can be improved by two levels, reaching CT5 level to CT7 level, and the surface finish of the inner cavity of the casting is improved by 3 times, reaching 1.6μm to 3.2μm, meeting the relevant technical requirements of large-scale aluminum alloy precision castings with complex surfaces, multiple ribs and multiple bosses and complex structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of devices for casting aluminum alloy castings, and in particular relates to a device for casting aluminum alloy castings comprising a composite casting mold and a core with a built-in cooling water channel. Background Art

[0002] Aluminum alloy has low density, high specific strength / rigidity, good corrosion resistance, good plasticity, excellent processing performance, good welding performance, excellent electrical conductivity and thermal conductivity, and has been widely used in the field of military equipment. Aluminum alloy can be divided into two categories according to the processing technology: deformed aluminum alloy and cast aluminum alloy. Among them, cast aluminum alloy has good process flow performance and medium load bearing capacity, and has been widely used in the manufacture of missile shells, fuel tank shells, engine accessory casings, engine oil pipelines, automobile engine cylinder blocks, automobile engine cylinder heads and other products.

[0003] At present, the existing casting molding process is mainly single sand casting, and quartz sand is usually used as the casting material. However, due to the low thermal conductivity of quartz sand, the cast grain size is relatively large and the overall mechanical properties are low. In addition, when designing the single sand casting process, in order to increase the chilling speed of the solidification process, it is usually necessary to paste a chilling iron in the mold. The chilling iron material is mostly medium carbon steel, but the medium carbon steel material has limited chilling capacity, and the surface of the built-in chilling iron is generally rough, resulting in low surface dimensional accuracy and smoothness of the casting after actual casting.

[0004] Castings made of metal mold materials have the advantages of high dimensional accuracy and good surface quality, and are widely used in many small and medium-sized, small and medium-sized batch aluminum alloy complex structure castings; however, metal mold materials are not suitable for the manufacture of large, complex, thin-walled aluminum alloy precision castings, and it is not suitable to set up a complex casting system, especially a shrinkage gap casting system, which makes it impossible to unpack and clean castings. In addition, the manufacturing cost of metal mold materials is high, the process optimization and adjustment space is small, and the mold structure design is complex. Therefore, there is an urgent need for a composite molding process that can increase the quenching speed of the casting process and improve the surface finish and dimensional accuracy of the casting. In addition, with the increasing production tasks in the field of military equipment, a large number of complex structure precision aluminum alloy castings also urgently need to solve the process preparation problems of high inner cavity dimensional accuracy, high mechanical performance index requirements, and high metallurgical quality requirements. Summary of the invention

[0005] In order to solve the problems of poor inner cavity dimensional accuracy, low mechanical properties, many metallurgical defects, low surface quality and surface finish of aluminum alloy precision castings in the existing single sand casting process, the present invention proposes an aluminum alloy casting device including a composite casting mold and a built-in cooling water channel core. The aluminum alloy casting device can effectively improve the overall quenching speed of the aluminum alloy melt during casting and solidification, and form a reasonable and orderly solidification temperature gradient distribution. At the same time, when the composite casting mold and the built-in cooling water channel core are used for casting, different cast structures and cast grain sizes can be obtained in the same casting, which can meet the technical index requirements of blasting separation of high-strength and toughness aluminum alloy missile shell precision castings, and realize high dimensional accuracy, high metallurgical quality and high-strength and toughness liquid molding manufacturing of large-scale complex thin-walled structure aluminum alloy castings.

[0006] The present invention provides the following technical solutions:

[0007] A device for casting an aluminum alloy, the device comprising a composite casting mold and a core; the composite casting mold comprises a cover box, an upper-upper box, an upper-middle box, an upper-lower box, a lower box and a pouring box which are sequentially connected from top to bottom; the cover box is an iron sand casting mold, the upper-upper box is a phosphate graphite casting mold, the upper-middle box is a chromite sand casting mold, the upper-lower boxes are silica sand casting molds, the lower box is a gypsum casting mold, and the pouring box is a metal casting mold;

[0008] A cooling water channel is arranged in the core, and the cooling water channel comprises an upper chilling water channel located in the upper upper box, a middle chilling water channel located in the upper middle box, and a lower chilling water channel located in the lower box.

[0009] The invention prepares a cover box, an upper box, an upper middle box, an upper and lower box, a lower box and a runner box by selecting different casting materials, and combines with a core with a built-in cooling water channel, so that a reasonable and orderly solidification temperature gradient distribution can be formed after the alloy melt is cast, and a solidification order from top to bottom is formed under a low-pressure casting process. By controlling the chilling time and water flow of the upper chilling water channel, the middle chilling water channel and the lower chilling water channel in the core, the alloy melt can be subjected to overall chilling from the inside to the outside; at the same time, the difference in thermal conductivity of different casting materials can also form different cast structures in different solidification areas of the casting, and different mechanical property partitions can be obtained on the same casting after heat treatment, so as to realize the preparation of missile shell castings with technical index requirements for explosive separation, and combine with the optimization control of low-pressure filling solidification process parameters to realize high dimensional accuracy, high metallurgical quality and high-strength and toughness liquid molding manufacturing of large-scale complex thin-walled structure aluminum alloy castings, which has broad market application prospects and remarkable economic benefits, and can realize the precision casting of complex thin-walled aluminum alloy castings for military equipment.

[0010] According to an embodiment of the present invention, the casting material for forming the cover box is iron sand, the particle size of the iron sand is 0.15 mm to 0.35 mm, the angular coefficient of the iron sand is 1.06 to 1.12, and the roundness of the iron sand is 0.92 to 0.96.

[0011] According to an embodiment of the present invention, the cover box is made of a binder and iron sand through stirring and hardening, wherein the binder is selected from phenol urethane resin, the mass ratio of the binder to the iron sand is 2.8 to 3.6:100, the stirring time is 15 to 20 minutes, and the hardening time is 12 to 24 minutes.

[0012] According to an embodiment of the present invention, the sand intake of the cover box is 80 mm to 140 mm.

[0013] According to an embodiment of the present invention, the casting material forming the upper box is phosphate graphite, and the phosphate graphite is prepared by mixing and drying phosphoric acid, graphite powder, water glass and aluminum oxide, wherein the weight ratio of phosphoric acid, graphite powder, water glass and aluminum oxide is: phosphoric acid 14% to 20%, aluminum oxide 12% to 14%, water glass 8% to 12%, and the remainder is graphite powder; the mixing time is 15min to 20min, the drying temperature is 580℃ to 620℃, and the drying time is 30min to 45min.

[0014] According to an embodiment of the present invention, the upper box has a tensile strength of 1.2 MPa to 1.4 MPa and a compressive strength of 6.2 MPa to 8.4 MPa.

[0015] According to an embodiment of the present invention, the sand intake of the upper box is 80 mm to 140 mm.

[0016] According to an embodiment of the present invention, the casting material forming the upper middle box is chromite sand, the particle size of the chromite sand is 0.2 mm to 0.5 mm, the angular coefficient of the chromite sand is 1.12 to 1.20, and the roundness of the chromite sand is 0.91 to 0.95.

[0017] According to an embodiment of the present invention, the upper middle box is made of a binder and chromite sand through stirring and hardening, wherein the binder is selected from phenol urethane resin, the mass ratio of the binder to the chromite sand is 2.4 to 3.0:100, the stirring time is 20 minutes to 25 minutes, and the hardening time is 15 minutes to 22 minutes.

[0018] According to an embodiment of the present invention, the room temperature tensile strength of the upper middle box is 1.3 MPa to 1.7 MPa.

[0019] According to an embodiment of the present invention, the sand intake of the upper middle box is 80 mm to 140 mm.

[0020] According to an embodiment of the present invention, the casting material forming the upper and lower boxes is silica sand, the particle size of the silica sand is 0.25 mm to 0.50 mm, the angular coefficient of the silica sand is 1.14 to 1.25, and the roundness of the silica sand is 0.92 to 0.96.

[0021] According to an embodiment of the present invention, the upper and lower boxes are made of a binder and silica sand through stirring and hardening, wherein the binder is selected from phenol urethane resin, the mass ratio of the binder to the silica sand is 3.2-4.0:100, the stirring time is 18-28 minutes, and the hardening time is 16-24 minutes.

[0022] According to an embodiment of the present invention, the room temperature compressive strength of the upper and lower boxes is 5.2 MPa to 7.0 MPa.

[0023] According to an embodiment of the present invention, the sand intake of the upper and lower boxes is 80 mm to 140 mm.

[0024] According to an embodiment of the present invention, the casting material forming the lower box is gypsum, which is prepared by mixing and drying high-strength α-hemihydrate gypsum, quartz powder, bauxite, diatomaceous earth, sodium sulfate, short ceramic fiber, citric acid, n-octanol and deionized water.

[0025] According to an embodiment of the present invention, the particle size of high-strength α-hemihydrate gypsum is 250 mesh to 350 mesh, the particle size of quartz powder is 70 mesh to 150 mesh, the particle size of bauxite is 320 mesh to 400 mesh, the particle size of diatomaceous earth is 350 mesh to 500 mesh, the length of short ceramic fiber is 40 μm to 80 μm, and the effective content of n-octanol is 96.0% to 98.5%.

[0026] According to an embodiment of the present invention, the components forming gypsum and their weight ratios are: high-strength α-hemihydrate gypsum 25% to 30%, quartz powder 4% to 6%, bauxite 8% to 10%, diatomaceous earth 2% to 3%, sodium sulfate 2% to 2.5%, short ceramic fibers 0.6% to 1.0%, citric acid 1.2% to 1.8%, n-octanol 1.6% to 2.4%, and the balance is deionized water.

[0027] According to an embodiment of the present invention, the lower box is prepared by the following method:

[0028] (1) After adding high-strength α-hemihydrate gypsum, quartz powder and bauxite to deionized water, stir at a speed of 250 r / min to 400 r / min for 15 min to 20 min, then add diatomaceous earth, sodium sulfate and citric acid to the mixed slurry, stir at a speed of 350 r / min to 500 r / min for 20 min to 25 min, then add short ceramic fiber and n-octanol to the mixed slurry, stir at a speed of 600 r / min to 800 r / min for 12 min to 15 min, then inject the mixed slurry into the lower box mold and wait for the mixed slurry to gel and harden. The gel and hardening time of the mixed slurry is 20 h to 28 h;

[0029] (2) The gelled and hardened gypsum mold is placed in a trolley furnace for heating and calcining. The heating and calcining of the gypsum mold is a step-by-step heating process: room temperature → 140℃~180℃ for 6h~8h → 200℃~280℃ for 8h~10h → 300℃~400℃ for 10h~12h → 420℃~520℃ for 6h~8h → 540℃~620℃ for 8h~12h → 620℃~750℃ for 6h~10h → slowly cool in the furnace to below 200℃ and air cool out of the furnace.

[0030] According to an embodiment of the present invention, the sand intake of the lower box is 80 mm to 140 mm.

[0031] According to an embodiment of the present invention, the casting material forming the runner box is low carbon steel, medium carbon steel or stainless steel.

[0032] According to an embodiment of the present invention, the height of the runner box is 200 mm to 300 mm.

[0033] According to an embodiment of the present invention, the surface of the runner box includes a refractory coating layer, which is sprayed with a refractory coating. The refractory coating includes zinc oxide, graphite powder, titanium dioxide, asbestos powder, water glass and deionized water.

[0034] According to an embodiment of the present invention, the components in the refractory coating and their weight ratios are: zinc oxide 4% to 6%, graphite powder 8% to 12%, titanium dioxide 8% to 10%, asbestos powder 6% to 8%, water glass 6% to 10%, and the balance is deionized water.

[0035] Wherein, when the refractory coating is prepared, the temperature of the deionized water is 70°C to 90°C.

[0036] According to an embodiment of the present invention, the preheating temperature during spraying of the refractory coating is 280°C to 340°C.

[0037] According to an embodiment of the present invention, the thickness of the refractory coating layer is 0.12 mm to 0.25 mm.

[0038] According to an embodiment of the present invention, the sand intake of the runner box is 80 mm to 140 mm.

[0039] According to an embodiment of the present invention, the runner box and the liquid riser nozzle of the low-pressure casting machine are positioned and assembled by means of positioning seat pins (such as metal seat pins).

[0040] According to an embodiment of the present invention, the core is made by mixing and hardening an inorganic binder and ceramic granular sand. The inorganic binder is an alkali metal salt inorganic binder, and the ceramic granular sand is aluminum oxide. The mass ratio of the inorganic binder to the ceramic granular sand is 2.8 to 3.6:100. The stirring time is 12 minutes to 18 minutes. The hardening method is CO2 blowing hardening. The CO2 gas flow rate is 1.8L / min to 2.4L / min, and the hardening time is 20 minutes to 28 minutes.

[0041] According to an embodiment of the present invention, the room temperature tensile strength of the core is 2.2 MPa to 3.4 MPa.

[0042] According to an embodiment of the present invention, the core is an integral core or a segmented assembled core.

[0043] According to an embodiment of the present invention, the core is assembled and positioned with the composite casting mold by means of sand blocks, preferably assembled and positioned with the runner box in the composite casting mold by means of sand blocks.

[0044] According to an embodiment of the present invention, the material forming the upper chilling waterway is brass, and the inner cavity cross-sectional area of ​​the upper chilling waterway is 800 mm 2 ~1200mm 2 The water flow rate of the upper chilling water channel is 0.8L / min~1.2L / min, and the chilling time is 2min~3min after the low-pressure filling of the alloy melt is completed. The water flow state is maintained after the chilling is completed. The upper chilling water channel is located in the upper box casting mold.

[0045] According to the embodiment of the present invention, the material forming the quenching water channel is stainless steel, and the inner cavity cross-sectional area of ​​the quenching water channel is 600mm 2 ~1000mm 2 The water flow rate of the middle water channel of the quenching is 0.6L / min~1.0L / min, and the quenching time is 3min~5min after the quenching of the upper water channel is completed. The water flow state continues to be maintained after the quenching is completed. The middle water channel of the quenching is located in the upper middle box casting mold.

[0046] According to an embodiment of the present invention, the material forming the chilled water channel is aluminum alloy, and the inner cavity cross-sectional area of ​​the chilled water channel is 500mm 2 ~800mm 2The water flow rate of the lower chilling water channel is 0.4L / min~0.7L / min, and the chilling time is 4min~6min after the chilling of the middle chilling water channel is completed. After the chilling is completed, the water flow state is maintained. The lower chilling water channel is located in the lower box casting mold.

[0047] According to an embodiment of the present invention, the upper chilling water channel, the middle chilling water channel and the lower chilling water channel are not connected to each other.

[0048] According to an embodiment of the present invention, the upper chilling water channel provides a cold source for the upper upper box, the middle chilling water channel provides a cold source for the upper middle box, and the lower chilling water channel provides a cold source for the lower box. The setting of the upper chilling water channel, the middle chilling water channel and the lower chilling water channel can adjust the chilling speed during the casting and solidification of the aluminum alloy melt, so that a reasonable and orderly solidification temperature gradient distribution is formed in the composite casting mold.

[0049] The present invention also provides a method for preparing an aluminum alloy casting, which comprises using the above-mentioned device for aluminum alloy casting.

[0050] According to an embodiment of the present invention, the preparation method comprises the following steps:

[0051] The aluminum alloy melt is cast into the above-mentioned aluminum alloy casting device. After the casting is completed, cooling water is introduced into the upper quenching water channel. The aluminum alloy melt in the upper box casting mold is quenched for 2min to 3min, then cooling water is introduced into the middle quenching water channel. The aluminum alloy melt in the upper middle box casting mold is quenched for 3min to 5min, then cooling water is introduced into the lower quenching water channel, and the aluminum alloy melt in the lower box casting mold is quenched for 4min to 6min.

[0052] According to an embodiment of the present invention, the aluminum alloy melt in the upper box casting mold can be quenched for 2 to 3 minutes, and the water flow state is continued after the quenching is completed (i.e., after quenching for 2 to 3 minutes).

[0053] According to an embodiment of the present invention, the aluminum alloy melt in the upper middle box casting mold can be quenched for 3 minutes to 5 minutes, and the water flow state is continued after the quenching is completed (i.e., after quenching for 3 minutes to 5 minutes).

[0054] According to an embodiment of the present invention, the aluminum alloy melt in the lower box casting mold can be quenched for 4 to 6 minutes, and the water flow state is continued after the quenching is completed (i.e., after 4 to 6 minutes of quenching).

[0055] According to an embodiment of the present invention, the preparation method comprises the following steps:

[0056] 1) connecting the pouring box to the rising nozzle of the low-pressure casting machine, and low-pressure casting the aluminum alloy melt into the above-mentioned aluminum alloy casting device through the rising nozzle of the low-pressure casting machine; wherein the casting temperature of the aluminum alloy melt is 700° C. to 720° C., the filling pressure is 50 kPa to 100 kPa, the pressurization rate is 0.8 kPa / s to 1.5 kPa / s, and the filling speed is 35 mm / s to 65 mm / s;

[0057] 2) After casting is completed, cooling water is introduced into the upper quenching water channel to quench the aluminum alloy melt in the upper box casting mold for 2 minutes to 3 minutes; after the quenching in the upper quenching water channel is completed, the water flow state is continued, and cooling water is introduced into the middle quenching water channel to quench the aluminum alloy melt in the upper middle box casting mold for 3 minutes to 5 minutes; after the quenching in the middle quenching water channel is completed, the water flow state is continued, and cooling water is introduced into the lower quenching water channel to quench the aluminum alloy melt in the lower box casting mold for 4 minutes to 6 minutes; during the quenching process, the crystallization boost pressure of the aluminum alloy melt is 4kPa to 10kPa, the crusting time is 40s to 60s, and the crystallization time is 600s to 1200s.

[0058] The present invention also provides the aluminum alloy casting, which is prepared by the above-mentioned preparation method.

[0059] Beneficial effects of the present invention:

[0060] The present invention provides an aluminum alloy casting device including a composite casting mold and a core with a built-in cooling water channel. The aluminum alloy casting device can realize high-precision and high-strength liquid molding of large-scale complex thin-walled aluminum alloy castings. Compared with the traditional single sand mold casting process, the inner cavity dimension tolerance of the casting prepared by the composite casting mold of the present invention can be improved by two levels, reaching CT5-CT7 level, and the surface finish of the inner cavity of the casting is improved by 3 times, reaching 1.6μm-3.2μm, meeting the relevant technical requirements of large-scale aluminum alloy precision castings with complex surfaces, multiple ribs and multiple bosses and complex structures. Because the core has a built-in cooling water channel, the quenching speed of the composite casting mold can be increased from 4℃ / s to 25℃ / s, the average grain size of the cast state can be refined from 120μm to 52μm, the tensile strength can be increased by more than 12% after T5 / T6 heat treatment, the yield strength can be increased by more than 10%, and the elongation after fracture can be increased by at least 40%, so that high-strength and high-toughness liquid molding manufacturing of aluminum alloy castings can be realized. However, due to the limited chilling capacity of traditional single sand molds, it is generally difficult to form an orderly solidification gradient distribution after casting of aluminum alloy castings. Locally thick areas or areas with variable thickness cross-sections of castings are prone to mushy solidification, resulting in ineffective solidification compensation and easy to produce looseness and shrinkage defects, resulting in large fluctuations in the production quality of engineering batch production of aluminum alloy precision castings. In addition, by controlling the material, chilling time and water flow of the built-in cooling water channel of the core, combined with the reasonable layout of different casting materials such as iron sand molds, graphite molds, and chromite sand molds, a reasonable and orderly solidification temperature gradient can be formed on the three-dimensional scale of the casting solidification, the casting as a whole is effectively compensated for shrinkage and chilled, the metallurgical quality is significantly improved, and the qualified rate of batch production of aluminum alloy precision castings is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 It is a schematic diagram of the structure of the built-in cooling water channel of the core in Example 2.

[0062] Figure 2 It is a schematic diagram of the principle of the built-in cooling water channel in the core in Example 2 for the overall cooling of the tail section metal shell casting during the casting process.

[0063] Figure 3 It is a schematic diagram of the structure of some components of the aluminum alloy casting device in Example 3 before assembly and positioning are completed.

[0064] Figure 4 It is a schematic diagram of the structure of the device for aluminum alloy casting in Example 3 after assembly and positioning are completed.

[0065] Figure 5 It is a structural schematic diagram of an aluminum alloy casting device according to a preferred embodiment of the present invention;

[0066] Figure numerals: 11 is a cover box, 12 is an upper box, 13 is an upper middle box, 14 is an upper and lower box, 15 is a lower box, 16 is a runner box, 17 is a low-pressure casting machine, 18 is a positioning seat pin, 21 is an upper chilling water channel, 22 is a middle chilling water channel, and 23 is a lower chilling water channel. DETAILED DESCRIPTION

[0067] The present invention will be described in further detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0068] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.

[0069] Embodiment 1:

[0070] like Figure 5 As shown, a device for aluminum alloy casting, the device includes a composite mold and a core; the composite mold includes a cover box 11, an upper-upper box 12, an upper-middle box 13, an upper-lower box 14, a lower box 15 and a runner box 16 which are connected in sequence from top to bottom; the cover box 11 is an iron sand mold, the upper-upper box 12 is a phosphate graphite mold, the upper-middle box 13 is a chromite sand mold, the upper-lower box 14 is a silica sand mold, the lower box 15 is a gypsum mold, and the runner box 16 is a metal mold; a cooling water channel is arranged in the core, and the cooling water channel includes a quenching upper water channel 21 located in the upper-upper box, a quenching middle water channel 22 located in the upper-middle box and a quenching lower water channel 23 located in the lower box.

[0071] The casting material of the cover box is iron sand with a particle size of 0.25mm, an angular coefficient of 1.09, and a roundness of 0.94. The cover box is made of a binder and iron sand that are stirred and hardened. The binder is phenol urethane resin, and the mass ratio of the binder to the iron sand is 3.2:100. The stirring time is 17min, the hardening time is 18min, and the sand consumption of the cover box is 100mm.

[0072] The casting material of the upper box is phosphate graphite, which is prepared by mixing and drying phosphoric acid, graphite powder, water glass and aluminum oxide. The weight ratio of phosphoric acid, graphite powder, water glass and aluminum oxide is: 17% phosphoric acid, 13% aluminum oxide, 10% water glass, and the remainder is graphite powder; the mixing time is 17 minutes, the drying temperature is 600°C, the drying time is 40 minutes, the tensile strength of the upper box is 1.3MPa, the compressive strength is 7.4MPa, and the sand consumption of the upper box is 100mm.

[0073] The casting material of the upper middle box is chromite sand with a particle size of 0.35mm, an angular coefficient of 1.16, and a roundness of 0.93; the upper middle box is made of a binder and chromite sand through stirring and hardening. The binder is phenol urethane resin, and the mass ratio of the binder to the chromite sand is 2.7:100. The stirring time is 22min, the hardening time is 18min, the room temperature tensile strength of the upper middle box is 1.5MPa, and the sand consumption of the upper middle box is 100mm.

[0074] The casting material of the upper and lower boxes is silica sand with a particle size of 0.40mm, an angular coefficient of 1.19, and a roundness of 0.94; the upper and lower boxes are made of a binder and silica sand that are stirred and hardened. The binder is phenol urethane resin, and the mass ratio of the binder to silica sand is 3.6:100. The stirring time is 23min, the hardening time is 20min, the room temperature compressive strength of the upper and lower boxes is 6.1MPa, and the sand consumption of the upper and lower boxes is 100mm.

[0075] The lower box casting material is gypsum, which is prepared by mixing and drying high-strength α-semihydrate gypsum, quartz powder, bauxite, diatomaceous earth, sodium sulfate, short ceramic fiber, citric acid, n-octanol and deionized water. The particle size of the high-strength α-semihydrate gypsum is 300 meshes, the particle size of the quartz powder is 110 meshes, the particle size of the bauxite is 360 meshes, the particle size of the diatomaceous earth is 420 meshes, the sodium sulfate is chemically pure, the length of the short ceramic fiber is 60 μm, the citric acid is chemically pure, and the effective content of n-octanol is 97.4%; the components forming the gypsum and their weight ratios are: 27% of high-strength α-semihydrate gypsum, 5% of quartz powder, 9% of bauxite, 2.5% of diatomaceous earth, 2.2% of sodium sulfate, 0.8% of short ceramic fiber, 1.5% of citric acid, 2.0% of n-octanol, and the balance is deionized water. The lower box is prepared by the following method: add high-strength α-hemihydrate gypsum, quartz powder and bauxite to deionized water, and stir continuously at 320r / min for 17 minutes; then add diatomaceous earth, sodium sulfate and citric acid to the mixed slurry, and stir continuously at 460r / min for 24 minutes; then add short ceramic fiber and n-octanol to the mixed slurry, and stir continuously at 700r / min for 13.5 minutes; then inject the mixed slurry into the lower box mold and wait for the mixed slurry to gel and harden; the gel and hardening time of the mixed slurry is 26h. The gelled and hardened gypsum mold is placed in a trolley furnace for heating and roasting. The heating and roasting of the gypsum mold is a step-by-step heating process: room temperature → 160℃ insulation for 7h → 240℃ insulation for 9h → 350℃ insulation for 11h → 470℃ insulation for 7h → 580℃ insulation for 10h → 680℃ insulation for 8h → slowly cool to 180℃ in the furnace and air cool out of the furnace. The sand intake of the lower box is 100mm.

[0076] The casting material of the runner box is medium carbon steel with a height of 250mm. Before casting, refractory coating is sprayed on the surface of the runner box. The refractory coating is composed of zinc oxide, graphite powder, titanium dioxide, asbestos powder, water glass and deionized water. The temperature of deionized water is 80°C. The components in the refractory coating and their weight ratio are: zinc oxide 5%, graphite powder 10%, titanium dioxide 9%, asbestos powder 7%, water glass 8%, and the balance is deionized water; the preheating temperature for spraying the refractory coating is 310°C, the thickness of the refractory coating spray is 0.18mm, the sand consumption of the runner box is 100mm, and the runner box is positioned and assembled with a metal positioning pin and a liquid riser nozzle of a low-pressure casting machine.

[0077] The core is made of an inorganic binder and ceramic granular sand mixed and hardened. The inorganic binder is an alkali metal salt inorganic binder, and the ceramic granular sand is alumina. The mass ratio of the inorganic binder to the ceramic granular sand is 3.2:100. The stirring time is 15 minutes. The hardening method is CO2 blowing hardening. The CO2 gas flow rate is 2.1L / min, and the hardening time is 24 minutes. The room temperature tensile strength of the core is 2.8MPa. The core is an integral core, and is assembled and positioned with the runner box 16 in the composite casting through sand blocks.

[0078] The material of the quenching water channel is brass, and the cross-sectional area of ​​the inner cavity of the water channel is 1000mm 2 The water flow rate is 1.0L / min, and the quenching time is 2.5min after the alloy melt is filled at low pressure. It is located in the upper box casting mold. The water channel material of the quenching is stainless steel, and the cross-sectional area of ​​the inner cavity of the water channel is 800mm 2 The water flow rate is 0.8L / min, and the chilling time is 4 minutes after the upper water channel is chilled. It is located in the upper and middle box casting mold; the material of the chilled lower water channel is aluminum alloy, and the cross-sectional area of ​​the lower water channel cavity is 650mm 2 The water flow rate is 0.5L / min, and the quenching time is 5 minutes after the quenching in the middle water channel is completed. It is located in the lower box casting mold.

[0079] The pouring box 16 and the liquid riser of the low-pressure casting machine 17 are positioned and assembled through the positioning seat pin 18, and the pouring box is ensured to be connected with the liquid riser of the low-pressure casting machine, and the aluminum alloy melt is low-pressure casted into the above-mentioned aluminum alloy casting device through the liquid riser of the low-pressure casting machine, wherein the casting temperature of the aluminum alloy melt is 710° C., the filling pressure is 75 kPa, the pressurization rate is 1.2 kPa / s, and the filling speed is 50 mm / s;

[0080] After the casting is completed, cooling water is introduced into the upper quenching water channel to quench the aluminum alloy melt in the upper box casting mold for 2 minutes to 3 minutes; after the quenching in the upper quenching water channel is completed, the water flow state is continued, and cooling water is introduced into the middle quenching water channel to quench the aluminum alloy melt in the upper middle box casting mold for 3 minutes to 5 minutes; after the quenching in the middle quenching water channel is completed, the water flow state is continued, and cooling water is introduced into the lower quenching water channel to quench the aluminum alloy melt in the lower box casting mold for 4 minutes to 6 minutes; during the quenching process, the crystallization boost pressure of the aluminum alloy melt is 7 kPa, the crusting time is 50 seconds, and the crystallization time is 900 seconds.

[0081] The inner cavity dimension tolerance of the casting prepared by the composite casting mold of the present invention can be improved by two levels, reaching CT5-CT7, and the surface finish of the inner cavity of the casting is improved by 3 times, reaching 1.6μm-3.2μm, meeting the relevant technical requirements of large aluminum alloy precision castings with complex surfaces, multiple ribs and multiple bosses, and complex structures. Since the core is built with a cooling water channel, the quenching speed of the composite casting mold can be increased from 4℃ / s to 25℃ / s, the average grain size of the cast state can be refined from 120μm to 52μm, the tensile strength can be increased by more than 12% after T5 / T6 heat treatment, the yield strength can be increased by more than 10%, and the elongation after fracture can be increased by at least 40%, which can realize the high-strength and high-toughness liquid molding manufacturing of aluminum alloy castings.

[0082] Table 1 Mechanical properties test results of various regions of the casting prepared in Example 1

[0083]

[0084] Comparative Example 1:

[0085] The other operations are the same as those in Example 1, except that a single chromite sand casting mold is used to replace the composite casting mold in Example 1.

[0086] Table 2 Comparison of properties of castings prepared in Example 1 and Comparative Example 1

[0087]

[0088] Embodiment 2:

[0089] A device for casting aluminum alloy, the device comprising a composite casting mold and a core; wherein the composite casting mold comprises a cover box, an upper-upper box, an upper-middle box, an upper-lower box, a lower box and a pouring box which are sequentially connected from top to bottom; the cover box is an iron sand casting mold, the upper-upper box is a phosphate graphite casting mold, the upper-middle box is a chromite sand casting mold, the upper-lower boxes are silica sand casting molds, the lower box is a gypsum casting mold, and the pouring box is a metal casting mold;

[0090] A cooling water channel is arranged in the core, and the cooling water channel comprises an upper chilling water channel located in the upper upper box, a middle chilling water channel located in the upper middle box, and a lower chilling water channel located in the lower box.

[0091] The casting material of the cover box is iron sand with a particle size of 0.15mm, an angular coefficient of 1.06, and a roundness of 0.92; the cover box is made of a binder and iron sand that are stirred and hardened. The binder is phenol urethane resin, and the mass ratio of the binder to iron sand is 2.8:100. The stirring time is 15min, the hardening time is 12min, and the sand consumption of the cover box is 80mm.

[0092] The casting material of the upper box is phosphate graphite, which is prepared by mixing and drying phosphoric acid, graphite powder, water glass and aluminum oxide. The weight ratio of phosphoric acid, graphite powder, water glass and aluminum oxide is: 14% phosphoric acid, 12% aluminum oxide, 8% water glass, and the remainder is graphite powder; the mixing time is 15 minutes, the drying temperature is 580°C, the drying time is 30 minutes, the tensile strength of the upper box is 1.2MPa, the compressive strength is 6.2MPa, and the sand consumption of the upper box is 80mm.

[0093] The casting material of the upper middle box is chromite sand with a particle size of 0.2mm, an angular coefficient of 1.12, and a roundness of 0.91; the upper middle box is made of a binder and chromite sand by stirring and hardening. The binder is phenol urethane resin, and the mass ratio of the binder to the chromite sand is 2.4:100. The stirring time is 20min, the hardening time is 15min, the room temperature tensile strength of the upper middle box is 1.3MPa, and the sand consumption of the upper middle box is 80mm.

[0094] The casting material of the upper and lower boxes is silica sand with a particle size of 0.25mm, an angular coefficient of 1.14, and a roundness of 0.92; the upper and lower boxes are made of a binder and silica sand that are stirred and hardened. The binder is phenol urethane resin, and the mass ratio of the binder to silica sand is 3.2:100. The stirring time is 18min, the hardening time is 16min, the room temperature compressive strength of the upper and lower boxes is 5.2MPa, and the sand consumption of the upper and lower boxes is 80mm.

[0095] The lower box casting material is gypsum, which is prepared by mixing and drying high-strength α-semihydrate gypsum, quartz powder, bauxite, diatomaceous earth, sodium sulfate, short ceramic fiber, citric acid, n-octanol and deionized water. The particle size of the high-strength α-semihydrate gypsum is 250 meshes, the particle size of the quartz powder is 70 meshes, the particle size of the bauxite is 320 meshes, the particle size of the diatomaceous earth is 350 meshes, the sodium sulfate is chemically pure, the length of the short ceramic fiber is 40 μm, the citric acid is chemically pure, and the effective content of n-octanol is 96.0%; the components forming the gypsum and their weight ratios are: 25% of high-strength α-semihydrate gypsum, 4% of quartz powder, 8% of bauxite, 2% of diatomaceous earth, 2% of sodium sulfate, 0.6% of short ceramic fiber, 1.2% of citric acid, 1.6% of n-octanol, and the balance is deionized water. The lower box is prepared by the following method: add high-strength α-hemihydrate gypsum, quartz powder and bauxite to deionized water, and stir continuously at 250r / min for 15 minutes, then add diatomaceous earth, sodium sulfate and citric acid to the mixed slurry, and stir continuously at 350r / min for 20 minutes, then add short ceramic fiber and n-octanol to the mixed slurry, and stir continuously at 600r / min for 12 minutes, then inject the mixed slurry into the lower box mold and wait for the mixed slurry to gel and harden, and the gel and hardening time of the mixed slurry is 20 hours. The gelled and hardened gypsum mold is placed in a trolley furnace for heating and roasting. The heating and roasting of the gypsum mold is a step-by-step heating process: room temperature → 140℃ insulation for 6h → 200℃ insulation for 8h → 300℃ insulation for 10h → 420℃ insulation for 6h → 540℃ insulation for 8h → 620℃ insulation for 6h → slowly cool to 160℃ in the furnace and air cool out of the furnace. The sand intake of the lower box is 80mm.

[0096] The casting material of the runner box is low carbon steel with a height of 200mm. Before casting, refractory coating is sprayed on the surface of the runner box. The refractory coating is composed of zinc oxide, graphite powder, titanium dioxide, asbestos powder, water glass and deionized water. The temperature of deionized water is 70°C. The components in the refractory coating and their weight ratio are: zinc oxide 4%, graphite powder 8%, titanium dioxide 8%, asbestos powder 6%, water glass 6%, and the balance is deionized water; the preheating temperature for spraying the refractory coating is 280°C, the thickness of the refractory coating spray is 0.12mm, the sand consumption of the runner box is 80mm, and the runner box is positioned and assembled with a metal positioning pin and a liquid riser nozzle of a low-pressure casting machine.

[0097] The core is made of an inorganic binder and ceramic granular sand mixed and hardened. The inorganic binder is an alkali metal salt inorganic binder, and the ceramic granular sand is alumina. The mass ratio of the inorganic binder to the ceramic granular sand is 2.8:100. The stirring time is 12 minutes. The hardening method is CO2 blowing hardening. The CO2 gas flow rate is 1.8L / min, and the hardening time is 20 minutes. The room temperature tensile strength of the core is 2.2MPa. The core is an integral core, and is assembled and positioned with the runner box by sand blocks.

[0098] The material of the quenching water channel is brass, and the cross-sectional area of ​​the inner cavity of the water channel is 800mm 2 The water flow rate is 0.8L / min, and the quenching time is 2min after the alloy melt is filled with low pressure. It is located in the upper box casting mold; the water channel material of the quenching is stainless steel, and the cross-sectional area of ​​the inner cavity of the water channel is 600mm 2 The water flow rate is 0.6L / min, and the chilling time is 3 minutes after the upper water channel is chilled. It is located in the upper and middle box casting mold; the material of the chilled lower water channel is aluminum alloy, and the cross-sectional area of ​​the lower water channel cavity is 500mm 2 The water flow rate is 0.4L / min, and the quenching time is 4 minutes after the quenching in the middle water channel is completed. It is located in the lower box casting mold.

[0099] The pouring box and the low-pressure casting machine liquid riser are positioned and assembled by the positioning seat pin, and the pouring box is ensured to be connected with the low-pressure casting machine liquid riser, and the aluminum alloy melt is low-pressure casted into the above-mentioned aluminum alloy casting device through the low-pressure casting machine liquid riser, wherein the casting temperature of the aluminum alloy melt is 700° C., the filling pressure is 50 kPa, the pressurization rate is 0.8 kPa / s, and the filling speed is 35 mm / s;

[0100] After the casting is completed, cooling water is introduced into the upper quenching water channel to quench the aluminum alloy melt in the upper box casting mold for 2 minutes to 3 minutes; after the quenching in the upper quenching water channel is completed, the water flow state is continued, and cooling water is introduced into the middle quenching water channel to quench the aluminum alloy melt in the upper middle box casting mold for 3 minutes to 5 minutes; after the quenching in the middle quenching water channel is completed, the water flow state is continued, and cooling water is introduced into the lower quenching water channel to quench the aluminum alloy melt in the lower box casting mold for 4 minutes to 6 minutes; during the quenching process, the crystallization boost pressure of the aluminum alloy melt is 4kPa, the crusting time is 40s, and the crystallization time is 600s.

[0101] Table 3 Mechanical properties test results of each region of the casting prepared in Example 2

[0102]

[0103] Comparative Example 2:

[0104] The other operations are the same as those in Example 2, except that a single phosphate graphite casting mold is used to replace the composite casting mold in Example 2.

[0105] Table 4 Performance comparison of castings prepared in Example 2 and Comparative Example 2

[0106]

[0107] Embodiment 3:

[0108] A device for casting aluminum alloy, the device comprising a composite casting mold and a core; wherein the composite casting mold comprises a cover box, an upper-upper box, an upper-middle box, an upper-lower box, a lower box and a pouring box which are sequentially connected from top to bottom; the cover box is an iron sand casting mold, the upper-upper box is a phosphate graphite casting mold, the upper-middle box is a chromite sand casting mold, the upper-lower boxes are silica sand casting molds, the lower box is a gypsum casting mold, and the pouring box is a metal casting mold;

[0109] A cooling water channel is arranged in the core, and the cooling water channel comprises an upper chilling water channel located in the upper upper box, a middle chilling water channel located in the upper middle box, and a lower chilling water channel located in the lower box.

[0110] The casting material of the cover box is iron sand with a particle size of 0.35mm, an angular coefficient of 1.12, and a roundness of 0.96; the cover box is made of a binder and iron sand that are stirred and hardened. The binder is phenol urethane resin, and the mass ratio of the binder to the iron sand is 3.6:100. The stirring time is 20min, the hardening time is 24min, and the sand consumption of the cover box is 140mm.

[0111] The casting material of the upper box is phosphate graphite, which is prepared by mixing and drying phosphoric acid, graphite powder, water glass and aluminum oxide. The weight ratio of phosphoric acid, graphite powder, water glass and aluminum oxide is: 20% phosphoric acid, 14% aluminum oxide, 12% water glass, and the remainder is graphite powder; the mixing time is 20 minutes, the drying temperature is 620°C, the drying time is 45 minutes, the tensile strength of the upper box is 1.4MPa, the compressive strength is 8.4MPa, and the sand consumption of the upper box is 140mm.

[0112] The casting material of the upper middle box is chromite sand with a particle size of 0.5mm, an angular coefficient of 1.20, and a roundness of 0.95; the upper middle box is made of a binder and chromite sand by stirring and hardening. The binder is phenol urethane resin, and the mass ratio of the binder to the chromite sand is 3.0:100. The stirring time is 25min, the hardening time is 22min, the room temperature tensile strength of the upper middle box is 1.7MPa, and the sand consumption of the upper middle box is 140mm.

[0113] The casting material of the upper and lower boxes is silica sand with a particle size of 0.50mm, an angular coefficient of 1.25, and a roundness of 0.96; the upper and lower boxes are made of a binder and silica sand that are stirred and hardened. The binder is phenol urethane resin, and the mass ratio of the binder to silica sand is 4.0:100. The stirring time is 28min, the hardening time is 24min, the room temperature compressive strength of the upper and lower boxes is 7.0MPa, and the sand consumption of the upper and lower boxes is 140mm.

[0114] The lower box casting material is gypsum, which is prepared by mixing and drying high-strength α-semihydrate gypsum, quartz powder, bauxite, diatomaceous earth, sodium sulfate, short ceramic fiber, citric acid, n-octanol and deionized water. The particle size of the high-strength α-semihydrate gypsum is 350 meshes, the particle size of the quartz powder is 150 meshes, the particle size of the bauxite is 400 meshes, the particle size of the diatomaceous earth is 500 meshes, the sodium sulfate is chemically pure, the length of the short ceramic fiber is 80 μm, the citric acid is chemically pure, and the effective content of n-octanol is 98.5%; the components forming the gypsum and their weight ratios are: 30% of high-strength α-semihydrate gypsum, 6% of quartz powder, 10% of bauxite, 3% of diatomaceous earth, 2.5% of sodium sulfate, 1.0% of short ceramic fiber, 1.8% of citric acid, 2.4% of n-octanol, and the balance is deionized water. The lower box is prepared by the following method: add high-strength α-hemihydrate gypsum, quartz powder and bauxite to deionized water, and stir continuously at 400r / min for 20min, then add diatomaceous earth, sodium sulfate and citric acid to the mixed slurry, and stir continuously at 500r / min for 25min, then add short ceramic fiber and n-octanol to the mixed slurry, and stir continuously at 800r / min for 15min, then inject the mixed slurry into the lower box mold and wait for the mixed slurry to gel and harden, and the gel and hardening time of the mixed slurry is 28h. The gelled and hardened gypsum mold is placed in a trolley furnace for heating and roasting. The heating and roasting of the gypsum mold is a step-by-step heating process: room temperature → 180℃ insulation for 8h → 280℃ insulation for 10h → 400℃ insulation for 12h → 520℃ insulation for 8h → 620℃ insulation for 12h → 750℃ insulation for 10h → slowly cool to 150℃ in the furnace and air cool out of the furnace. The sand intake of the lower box is 140mm.

[0115] The casting material of the runner box is stainless steel, with a height of 300mm. Before casting, refractory coating is sprayed on the surface of the runner box. The refractory coating is composed of zinc oxide, graphite powder, titanium dioxide, asbestos powder, water glass and deionized water. The temperature of deionized water is 90°C. The components in the refractory coating and their weight ratio are: zinc oxide 6%, graphite powder 12%, titanium dioxide 10%, asbestos powder 8%, water glass 10%, and the balance is deionized water; the preheating temperature for spraying the refractory coating is 340°C, the thickness of the refractory coating spray is 0.25mm, the sand consumption of the runner box is 140mm, and the runner box is positioned and assembled with a metal positioning pin and a liquid riser nozzle of a low-pressure casting machine.

[0116] The core is made of an inorganic binder and ceramic granular sand mixed and hardened. The inorganic binder is an alkali metal salt inorganic binder, and the ceramic granular sand is alumina. The mass ratio of the inorganic binder to the ceramic granular sand is 3.6:100. The stirring time is 18 minutes. The hardening method is CO2 blowing hardening. The CO2 gas flow rate is 2.4L / min, and the hardening time is 28 minutes. The room temperature tensile strength of the core is 3.4MPa. The core is an integral core, and is assembled and positioned with the runner box by sand blocks.

[0117] The material of the quenching water channel is brass, and the cross-sectional area of ​​the inner cavity of the water channel is 1200mm 2 The water flow rate is 1.2L / min. The quenching time is 3 minutes after the alloy melt is filled at low pressure. It is located in the upper box casting mold. The water channel material for the quenching is stainless steel, and the cross-sectional area of ​​the inner cavity of the water channel is 1000mm. 2 The water flow rate is 1.0L / min, and the chilling time is 5 minutes after the upper water channel is chilled. It is located in the upper and middle box casting mold; the material of the chilled lower water channel is aluminum alloy, and the cross-sectional area of ​​the lower water channel is 800mm 2 The water flow rate is 0.7L / min, and the quenching time is 6 minutes after the quenching in the middle water channel is completed. It is located in the lower box casting mold.

[0118] The pouring box and the low-pressure casting machine liquid riser are positioned and assembled by the positioning seat pin, and the pouring box is ensured to be connected with the low-pressure casting machine liquid riser, and the aluminum alloy melt is low-pressure casted into the above-mentioned aluminum alloy casting device through the low-pressure casting machine liquid riser, wherein the casting temperature of the aluminum alloy melt is 720° C., the filling pressure is 100 kPa, the pressurization rate is 1.5 kPa / s, and the filling speed is 65 mm / s;

[0119] After the casting is completed, cooling water is introduced into the upper quenching water channel to quench the aluminum alloy melt in the upper box casting mold for 2 minutes to 3 minutes; after the quenching in the upper quenching water channel is completed, the water flow state is continued, and cooling water is introduced into the middle quenching water channel to quench the aluminum alloy melt in the upper middle box casting mold for 3 minutes to 5 minutes; after the quenching in the middle quenching water channel is completed, the water flow state is continued, and cooling water is introduced into the lower quenching water channel to quench the aluminum alloy melt in the lower box casting mold for 4 minutes to 6 minutes; during the quenching process, the crystallization boost pressure of the aluminum alloy melt is 10kPa, the crusting time is 60s, and the crystallization time is 1200s.

[0120] Table 5 Mechanical properties test results of each region of the casting prepared in Example 3

[0121]

[0122] Comparative Example 3:

[0123] The other operations are the same as those in Example 3, except that a single quartz sand casting mold is used to replace the composite casting mold in Example 1.

[0124] Table 6 Comparison of properties of castings prepared in Example 3 and Comparative Example 3

[0125]

[0126]

[0127] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An aluminum alloy casting device, characterized in that: The device comprises a composite casting mold and a core; the composite casting mold comprises a cover box, an upper-upper box, an upper-middle box, an upper-lower box, a lower box and a pouring box which are sequentially connected from top to bottom; the cover box is an iron sand casting mold, the upper-upper box is a phosphate graphite casting mold, the upper-middle box is a chromite sand casting mold, the upper-lower boxes are silica sand casting molds, the lower box is a gypsum casting mold, and the pouring box is a metal casting mold; The core is made by mixing and hardening an inorganic binder and ceramic granular sand, wherein the inorganic binder is an alkali metal salt inorganic binder and the ceramic granular sand is aluminum oxide; A cooling water channel is arranged in the core, and the cooling water channel comprises an upper chilling water channel located in the upper upper box, a middle chilling water channel located in the upper middle box, and a lower chilling water channel located in the lower box; The upper chilling water channel, the middle chilling water channel and the lower chilling water channel are not connected to each other; The material forming the upper cooling water channel is brass, and the inner cross-sectional area of ​​the upper cooling water channel is 800mm 2 ~1200mm 2 The water flow rate of the upper chilling water channel is 0.8L / min to 1.2L / min, and the chilling time is 2min to 3min after the alloy melt is filled with low pressure. After the chilling, the water is kept flowing. The upper chilling water channel is located in the upper box casting mold; The material forming the quenching water channel is stainless steel, and the inner cross-sectional area of ​​the quenching water channel is 600mm 2 ~1000mm 2 The water flow rate of the middle water channel of the quenching is 0.6L / min~1.0L / min, and the quenching time is 3min~5min after the quenching of the upper water channel is completed. After the quenching is completed, the water flow state is maintained. The middle water channel of the quenching is located in the upper middle box casting mold; The material forming the chilled water channel is aluminum alloy, and the inner cross-sectional area of ​​the chilled water channel is 500mm 2 ~800mm 2 The water flow rate of the lower chilling water channel is 0.4L / min~0.7L / min, and the chilling time is 4min~6min after the chilling of the middle chilling water channel is completed. After the chilling is completed, the water flow state is maintained. The lower chilling water channel is located in the lower box casting mold.

2. The device according to claim 1, characterized in that The casting material for forming the cover box is iron sand, the particle size of the iron sand is 0.15 mm to 0.35 mm, the angular coefficient of the iron sand is 1.06 to 1.12, and the roundness of the iron sand is 0.92 to 0.96; And / or, the cover box is made by stirring and hardening a binder and iron sand, wherein the binder is selected from phenol urethane resin, the mass ratio of the binder to the iron sand is 2.8-3.6:100, the stirring time is 15-20 minutes, and the hardening time is 12-24 minutes; And / or, the sand intake of the cover box is 80 mm to 140 mm; And / or, the casting material forming the upper upper box is phosphate graphite, which is prepared by mixing and drying phosphoric acid, graphite powder, water glass and aluminum oxide, wherein the weight ratio of phosphoric acid, graphite powder, water glass and aluminum oxide is: phosphoric acid 14% to 20%, aluminum oxide 12% to 14%, water glass 8% to 12%, and the remainder is graphite powder; the mixing time is 15min to 20min, the drying temperature is 580°C to 620°C, and the drying time is 30min to 45min; And / or, the upper box has a tensile strength of 1.2 MPa to 1.4 MPa and a compressive strength of 6.2 MPa to 8.4 MPa; And / or, the sand intake of the upper box is 80mm to 140mm; And / or, the casting material forming the upper middle box is chromite sand, the particle size of the chromite sand is 0.2 mm to 0.5 mm, the angular coefficient of the chromite sand is 1.12 to 1.20, and the roundness of the chromite sand is 0.91 to 0.95; And / or, the upper middle box is made by stirring and hardening a binder and chromite sand, wherein the binder is selected from phenol urethane resin, the mass ratio of the binder to the chromite sand is 2.4-3.0:100, the stirring time is 20min-25min, and the hardening time is 15min-22min; And / or, the room temperature tensile strength of the upper middle box is 1.3MPa to 1.7MPa; And / or, the sand intake of the upper middle box is 80mm to 140mm; And / or, the casting material forming the upper and lower boxes is silica sand, the particle size of the silica sand is 0.25 mm to 0.50 mm, the angular coefficient of the silica sand is 1.14 to 1.25, and the roundness of the silica sand is 0.92 to 0.96; And / or, the upper and lower boxes are made of a binder and silica sand by stirring and hardening, wherein the binder is selected from phenol urethane resin, the mass ratio of the binder to the silica sand is 3.2-4.0:100, the stirring time is 18-28 minutes, and the hardening time is 16-24 minutes; And / or, the room temperature compressive strength of the upper and lower boxes is 5.2MPa to 7.0MPa; And / or, the sand intake of the upper and lower boxes is 80mm to 140mm.

3. The device according to claim 1, characterized in that The casting material forming the lower box is gypsum, which is prepared by mixing and drying high-strength α-hemihydrate gypsum, quartz powder, bauxite, diatomaceous earth, sodium sulfate, short ceramic fiber, citric acid, n-octanol, and deionized water; the particle size of high-strength α-hemihydrate gypsum is 250 mesh to 350 mesh, the particle size of quartz powder is 70 mesh to 150 mesh, the particle size of bauxite is 320 mesh to 400 mesh, the particle size of diatomaceous earth is 350 mesh to 500 mesh, and the length of short ceramic fiber is 100 mesh to 150 mesh. The particle size is 40 μm to 80 μm, and the effective content of n-octanol is 96.0% to 98.5%. The components and weight ratios of the gypsum are as follows: 25% to 30% high-strength α-hemihydrate gypsum, 4% to 6% quartz powder, 8% to 10% bauxite, 2% to 3% diatomaceous earth, 2% to 2.5% sodium sulfate, 0.6% to 1.0% short ceramic fiber, 1.2% to 1.8% citric acid, 1.6% to 2.4% n-octanol, and the balance is deionized water. And / or, the sand intake of the lower box is 80mm to 140mm.

4. The device according to claim 1, characterized in that The casting material forming the pouring box is low carbon steel, medium carbon steel or stainless steel; And / or, the height of the runner box is 200 mm to 300 mm; And / or, the surface of the runner box includes a refractory coating layer, the refractory coating layer is formed by spraying the refractory coating, the refractory coating includes zinc oxide, graphite powder, titanium dioxide, asbestos powder, water glass and deionized water; the components in the refractory coating and their weight ratios are: zinc oxide 4% to 6%, graphite powder 8% to 12%, titanium dioxide 8% to 10%, asbestos powder 6% to 8%, water glass 6% to 10%, and the balance is deionized water; And / or, the sand intake of the runner box is 80 mm to 140 mm; And / or, the runner box and the liquid riser nozzle of the low-pressure casting machine are positioned and assembled by means of positioning seat pins.

5. The device according to claim 1, characterized in that The mass ratio of inorganic binder to ceramic granular sand is 2.8-3.6:100, the stirring time is 12-18 minutes, the hardening method is CO2 blowing hardening, the CO2 gas flow rate is 1.8L / min-2.4L / min, and the hardening time is 20-28 minutes; And / or, the room temperature tensile strength of the core is 2.2 MPa to 3.4 MPa; And / or, the core and the runner box in the composite casting mold are assembled and positioned by sand blocks.

6. A method for preparing an aluminum alloy casting, characterized in that: The preparation method comprises using the aluminum alloy casting device according to any one of claims 1 to 5, and the preparation method comprises the following steps: The aluminum alloy melt is cast into the above-mentioned aluminum alloy casting device. After the casting is completed, cooling water is introduced into the upper quenching water channel. The aluminum alloy melt in the upper box casting mold is quenched for 2min to 3min, then cooling water is introduced into the middle quenching water channel. The aluminum alloy melt in the upper middle box casting mold is quenched for 3min to 5min, then cooling water is introduced into the lower quenching water channel, and the aluminum alloy melt in the lower box casting mold is quenched for 4min to 6min.

7. The preparation method according to claim 6, characterized in that: The preparation method comprises the following steps: 1) connecting the pouring box to the rising nozzle of the low-pressure casting machine, and low-pressure casting the aluminum alloy melt into the above-mentioned aluminum alloy casting device through the rising nozzle of the low-pressure casting machine; wherein the casting temperature of the aluminum alloy melt is 700° C. to 720° C., the filling pressure is 50 kPa to 100 kPa, the pressurization rate is 0.8 kPa / s to 1.5 kPa / s, and the filling speed is 35 mm / s to 65 mm / s; 2) After casting is completed, cooling water is introduced into the upper quenching water channel to quench the aluminum alloy melt in the upper box casting mold for 2 minutes to 3 minutes; after the quenching in the upper quenching water channel is completed, the water flow state is continued, and cooling water is introduced into the middle quenching water channel to quench the aluminum alloy melt in the upper middle box casting mold for 3 minutes to 5 minutes; after the quenching in the middle quenching water channel is completed, the water flow state is continued, and cooling water is introduced into the lower quenching water channel to quench the aluminum alloy melt in the lower box casting mold for 4 minutes to 6 minutes; during the quenching process, the crystallization boost pressure of the aluminum alloy melt is 4kPa to 10kPa, the crusting time is 40s to 60s, and the crystallization time is 600s to 1200s.

8. An aluminum alloy casting, which is prepared by the preparation method according to claim 6 or 7.