Aqueous coating compositions containing polycarboxylic acids having improved leveling properties

By combining anionic stabilizing binders and polycarboxylic acids in water-based coatings, the problem of insufficient rheological properties and storage stability of water-based coatings in the 'wet-on-wet' method is solved, excellent leveling and optical-mechanical properties are achieved, and Improves the brightness and color flop effect of metallic coatings.

CN115052937BActive Publication Date: 2024-10-15BASF COATINGS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180010150.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-01-21
Filing Date
2021-01-08
Publication Date
2024-10-15
Estimated Expiration
2041-01-08

AI Technical Summary

Technical Problem

Existing aqueous coating compositions suffer from poor rheological properties, insufficient storage stability and poor optical-mechanical properties when processed in the 'wet-on-wet' method, especially when polyamides and metal silicates are not used .

Method used

A water-based coating composition containing an anion-stabilized base material, a polycarboxylic acid and a solvent is used. The polycarboxylic acid is dissolved in a solvent and then added to the anion-stabilized base material and colored pigments to form a coating composition without effect pigments. For preparing multi-layer paint systems.

Benefits of technology

It achieves excellent leveling, storage stability and optical and mechanical properties, improves the brightness and angular color effect of the metal coating, and avoids the defects caused by the use of polyamide and metal silicates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003755057730000391
    Figure BDA0003755057730000391
  • Figure BDA0003755057730000392
    Figure BDA0003755057730000392
  • Figure BDA0003755057730000401
    Figure BDA0003755057730000401
Patent Text Reader

Abstract

The invention relates to an aqueous coating composition comprising at least one anionically stabilized binder B, at least one coloring pigment P, at least one polycarboxylic acid PC and optionally at least one solvent S. The coating composition does not contain effect pigments. The invention also relates to a method for preparing an aqueous coating composition according to the invention, comprising adding a solution of a polycarboxylic acid PC in a solvent S to a coating composition comprising at least one anionically stabilized binder B and a coloring pigment P. In addition, the invention relates to a method for preparing a multilayer paint system, comprising preparing a basecoat layer or at least two directly successive basecoat layers directly on a substrate optionally coated with a first coating layer, preparing a clearcoat layer directly on the one basecoat layer or on the uppermost basecoat layer, and jointly curing one or more basecoat layers and the clearcoat layer. At least one basecoat material comprises an aqueous coating composition according to the invention and / or an aqueous coating prepared by the method according to the invention. Finally, the invention relates to a multilayer paint system obtainable by the method according to the invention.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to an aqueous coating composition comprising at least one anionically stabilized binder B, at least one coloring pigment P, at least one polycarboxylic acid PC and optionally at least one solvent S. The coating composition does not contain effect pigments. The invention also relates to a method for preparing the aqueous coating composition of the invention by adding a solution of the polycarboxylic acid PC in the solvent S to a coating composition comprising at least one anionically stabilized binder B and the coloring pigment P. In addition, the invention relates to a method for preparing a multilayer paint system, comprising preparing a basecoat layer or at least two directly successive basecoat layers directly on a substrate optionally coated with a first coating layer, preparing a clearcoat layer directly on the one basecoat layer or the uppermost basecoat layer, and jointly curing one or more basecoat layers and the clearcoat layer. At least one of the basecoat materials comprises an aqueous coating composition of the invention and / or an aqueous coating prepared by the method of the invention. Finally, the invention relates to a multilayer paint system obtainable by the method of the invention. Prior art

[0002] In particular in automotive finishing, but also in other fields in which coatings having a high decorative effect and at the same time effective corrosion protection are required, it is known to provide a substrate with a plurality of coating films stacked one above the other.

[0003] The multicoat paint system is preferably applied by the so-called "wet-on-wet" method, which means that a pigmented basecoat material is first applied and, after a short flash-off time, overcoated with a clearcoat without a baking step. Subsequently, the basecoat layer and the clearcoat are baked together.

[0004] The "wet-on-wet" method is of particular importance in the application of automotive metallic effect paints.

[0005] Economic and environmental reasons dictate the use of waterborne basecoat compositions for the production of multicoat systems. The coating compositions used to prepare these basecoats must be processable by the currently conventional, rational "wet-on-wet" process; i.e., after a very short initial drying time, without a baking step, they must be recoatable with a clear topcoat without exhibiting defects in their visual appearance, such as those known as "pinholes".

[0006] Furthermore, the coating composition must also exhibit adequate storage stability. A routine test is to store the material at 40°C.

[0007] Furthermore, the rheological properties of the coating composition must be tailored for "wet-on-wet" application to achieve a high quality overall appearance, which is particularly influenced by effective leveling of the coating composition used. Furthermore, minimization of gel spots is a challenge.

[0008] In principle, it is known to use any of a wide range of rheology additives for adjusting the rheological properties.

[0009] For example, EP 0877063A2, WO 2009 / 100938A1, EP 2457961A1 and EP 3183303A1 describe aqueous coating compositions comprising polyamides with an acid value of ≥30 mg KOH / g polyamide or <10 mg KOH / g polyamide. However, the use of polyamides and other water-insoluble ingredients in aqueous coating compositions may lead to incompatibility between these compounds and the water-soluble components of the composition. This leads in particular to particle formation during processing by a "wet-on-wet" method and / or when the polyamide is introduced into the coating composition, and / or insufficient storage stability (separation or phase separation) of the coating composition, particularly at relatively high temperatures, such as temperatures of ≥40° C. In addition, when adding polyamides, there may be poor leveling and / or poor appearance.

[0010] EP 1153989A1 discloses an aqueous coating composition comprising a polyamide having an acid value of ≥30 mg KOH / g polyamide and a metal silicate consisting of very small, usually nano-scale particles as an additional rheological aid. However, the disadvantage of having such metal silicates in aqueous coating compositions, especially in combination with an acid value of >30 mg KOH / g polyamide, is that pinholes and / or burst holes may often occur when processed by a "wet-on-wet" method. In addition, the use of metal silicates is undesirable because, due to their high surface area, they interact strongly with other formulation ingredients, especially with dispersing additives and / or base materials with pigment affinity groups. Minimizing these interactions requires a high level of dilution. However, this dilution may adversely affect, in particular, the shear stability and circulation line stability of the coating composition.

[0011] Aqueous coating compositions comprising metal silicates are also known, which are often used as rheology aids in aqueous coating compositions, such as the commercially available metal silicates " RD". However, in this case, there are disadvantages that the incidence of pinholes increases and / or leveling is poor in processing by the above method.

[0012] Thus, it would be advantageous to have an effect pigment-free aqueous coating composition that exhibits effective leveling and minimization of gel spots and good optical and mechanical properties while being substantially free of polyamide and / or metal silicates. Such compositions would also advantageously improve the brightness and flop index of a metal coating applied "wet-on-wet" directly over a coating prepared from the aqueous coating composition. Furthermore, the aqueous coating composition should have high storage stability.

[0013] Purpose

[0014] Therefore, the object of the present invention is to provide an aqueous coating composition which contains coloring pigments and which exhibits effective leveling even without the use of polyamides and / or metal silicates. In addition, the aqueous coating composition should have good optical and mechanical properties and high storage stability. In addition, the aqueous coating composition should improve the brightness and the flop effect of a metal coating applied "wet-on-wet" directly to a coating formed by the aqueous coating composition.

[0015] Technical Solution

[0016] The above objects are achieved by the subject matter claimed in the claims and by preferred embodiments of this subject matter described in the following description.

[0017] Therefore, a first subject of the present invention is an aqueous coating composition comprising:

[0018] (a) at least one anionically stabilized binder BM,

[0019] (b) at least one coloring pigment EP,

[0020] (c) at least one polycarboxylic acid PC, and

[0021] (d) optionally at least one solvent S,

[0022] Therein the coating composition comprises 0% by weight of effect pigments.

[0023] The above-described aqueous coating composition is also referred to hereinafter as the coating composition of the invention and is therefore a subject of the present invention. Preferred embodiments of the coating composition of the invention emerge from the following description and from the dependent claims.

[0024] Even without adding polyamide and / or metal silicate, more particularly without adding polyamide and metal silicate, the coating composition of the present invention has excellent leveling. This effective leveling is achieved by using at least one polycarboxylic acid PC in combination with at least one anion-stabilized base material B and optionally at least one solvent S. When combined with anion-stabilized base material B, the polycarboxylic acid PC acts as an associative thickener and leads to high viscosity after releasing the shear stress without negatively affecting the low viscosity under shear. Therefore, due to the low viscosity under shear, the coating composition of the present invention can be easily applied. When the shear stress is released, that is, after the coating composition is applied to the substrate, the sharp increase in viscosity leads to an excellent leveling effect. The use of solvent S can increase the uniform incorporation of polycarboxylic acid PC in the aqueous coating composition, thereby preventing gel spots and particles, and achieving high storage stability. According to the present invention, the polycarboxylic acid PC can also be dissolved in solvent S before being added to the aqueous coating composition. The solution has high stability during storage and can therefore be added to the preparation method as a storage-stable intermediate in a simple manner as part of the preparation of the aqueous coating composition. Furthermore, the addition of polycarboxylic acid PC does not have any adverse effect on the optical and mechanical properties of the coating prepared with the composition of the present invention and the multi-layer coating system comprising the basecoat layer prepared with the coating composition of the present invention. Despite the addition of polycarboxylic acid PC, the coating composition of the present invention can still achieve a high solid content.

[0025] Furthermore, the use of the at least one polycarboxylic acid PC and anionically stabilized binder B, optionally in combination with at least one solvent S, results in an increased goniochromatic effect of metal coatings applied "wet-on-wet" directly on a coating prepared from the aqueous coating composition of the present invention. Without being bound by this theory, it is believed that the polycarboxylic acid PC migrates into the overlying metal coating and increases the substantially parallel orientation of the effect pigments to the underlying substrate.

[0026] Another subject of the invention is a method for producing a multi-layer paint system, comprising producing a basecoat layer or at least two directly successive basecoat layers directly on a substrate optionally coated with a first coating, producing a clearcoat layer directly on the basecoat layer or the topmost basecoat layer, and jointly curing the basecoat layer or layers and the clearcoat layer. At least one basecoat material comprises an aqueous coating composition according to the invention and / or an aqueous coating prepared by the method according to the invention.

[0027] A further subject matter of the present invention is a multicoat paint system obtainable by the process according to the invention.

[0028] Detailed Description

[0029] definition :

[0030] First, many of the terms used in the context of the present invention are explained.

[0031] The expression "aqueous coating composition" is known to those skilled in the art. It refers essentially to a coating composition that is not based solely on organic solvents. In fact, any coating composition based on organic solvents contains only organic solvents and no water for dissolving and / or dispersing components, or a coating composition to which water is not explicitly added during its preparation, water instead only enters the composition in the form of pollutants, atmospheric moisture and / or solvents for any particular additives used. In contrast to aqueous coating compositions, such compositions are referred to as solvent-based or "based on organic solvents". In the context of the present invention, "aqueous" should preferably be understood to mean that the coating composition comprises a moisture content of at least 20% by weight, preferably at least 25% by weight, very preferably at least 50% by weight, based in each case on the total amount of solvents present (i.e. water and organic solvents). The moisture content is preferably in turn 60-100% by weight, more particularly 65-90% by weight, very preferably 70-80% by weight, based in each case on the total amount of solvents present.

[0032] The term "binder" in the sense of the present invention and in accordance with DIN EN ISO 4618 (German version, date: March 2007) preferably refers to those non-volatile components of the composition of the present invention which are responsible for film formation, excluding any pigments and fillers therein, and more particularly refers to the polymer resin responsible for film formation. The non-volatile components can be determined by the method described in the Examples section.

[0033] In order to obtain an excellent flop effect, the aqueous coating composition must contain at least one anionically stabilized binder B. According to the invention, anionically stabilized binders B are understood to be binders that contain groups that can be converted into anionic groups (potentially anionic groups) by neutralizing agents. Anionic groups that can be converted into anionic groups by neutralizing agents are, for example, carboxylic acid, sulfonic acid and / or phosphonic acid groups, more particularly carboxylic acid groups.

[0034] According to the invention, the term "polycarboxylic acid" refers to an aliphatic or aromatic carboxylic acid having at least two carboxylic acid groups per molecule. These carboxylic acid groups can be converted fully or partially into anionic groups by a neutralizing agent.

[0035] The term "(meth)acrylate" shall hereinafter refer to both acrylate and methacrylate.

[0036] Applying the coating composition to a substrate or preparing a coating film on a substrate should be understood as follows: the corresponding coating composition is applied in a manner such that the coating film obtained therefrom is arranged on the substrate. However, direct contact with the substrate is not required. Therefore, other layers may be present between the coating film and the substrate. For example, in the optional step (1), a cured coating (S1) is prepared on a metal substrate (S), but a conversion coating as described below, such as a zinc phosphate coating, may be provided between the substrate and the cured coating (S1).

[0037] On the contrary, the coating composition is directly applied to the substrate or directly prepares the film on the substrate, which causes the obtained film to be in direct contact with the substrate. Therefore, more particularly, there is no other layer between the film and the substrate. Of course, the same principle is applicable to the coating composition directly applying or directly preparing the film one after another, for example in step (2) (b) of the present invention.

[0038] The term "flash evaporation" means that the organic solvent and / or water present in the coating composition evaporates after application, usually at ambient temperature (i.e. room temperature), for example 15-35° C. for a period of, for example, 0.5-30 minutes. Since the coating composition is still free-flowing at least immediately after being applied in the form of droplets, it can form a uniform, smooth coating film by leveling. However, after the flash evaporation operation, the coating film is still not in a ready-to-use state. For example, it is no longer free-flowing, but is still soft and / or sticky, and in some cases only partially dry. More particularly, as described below, the coating film is still not cured.

[0039] In contrast, intermediate drying is carried out, for example, at a higher temperature and / or for a longer time, so that a higher proportion of organic solvent and / or water evaporates from the applied coating film compared to flash evaporation. Therefore, intermediate drying is usually carried out at an elevated temperature relative to ambient temperature, for example 40-90° C., for a time of, for example, 1-60 minutes. However, intermediate drying also does not result in a coating film in a ready-to-use state, i.e. a cured coating film as described below. A typical sequence of flash evaporation and intermediate drying operations comprises, for example, flashing the applied coating film at ambient temperature for 5 minutes and then intermediate drying it at 80° C. for 10 minutes.

[0040] Curing of a coating film is therefore understood to mean converting the film into a ready-to-use state, i.e. into a state in which the substrate provided with the corresponding coating film can be transported, stored and used as intended. More particularly, a cured coating film is no longer soft or tacky, but is conditioned into a solid coating film, the properties of which, such as hardness or adhesion to the substrate, do not undergo any further significant changes even upon further exposure to curing conditions as described below.

[0041] In the context of the present invention, "physically curable" or the term "physical curing" means forming a cured coating film by releasing a solvent from a polymer solution or a polymer dispersion, the curing being achieved by the interlinking of polymer chains.

[0042] In the context of the present invention, "thermochemically curable" or the term "thermochemically curing" means that the crosslinking of the paint film (forming a cured coating film) is initiated by a chemical reaction of reactive functional groups, and activation energy can be provided for these chemical reactions by heat. This may involve different, complementary functional groups (complementary functional groups) reacting with each other and / or forming a cured layer based on the reaction of self-reactive groups (i.e., functional groups that react with similar groups). Examples of suitable complementary reactive functional groups and self-reactive functional groups are known, for example, from German patent application DE 199 30 665A1, page 7, line 28 to page 9, line 24.

[0043] The crosslinking can be self-crosslinking and / or external crosslinking. For example, self-crosslinking is present if complementary reactive functional groups are already present in the organic polymer used as binder, such as polyesters, polyurethanes or poly(meth)acrylates. External crosslinking is present, for example, when a (first) organic polymer containing specific functional groups such as hydroxyl groups is reacted with a crosslinking agent known per se, such as polyisocyanates and / or melamine resins. Thus, the crosslinking agent contains reactive functional groups that are complementary to the reactive functional groups present in the (first) organic polymer used as binder.

[0044] Especially in the case of external crosslinking, the known mono- and multi-component systems, in particular the two-component systems, are useful. In the one-component system, the components to be crosslinked, for example the organic polymer as a binder and the crosslinking agent, are present side by side with each other, i.e. in one component. The prerequisite is that the components to be crosslinked react with each other only at relatively high temperatures, for example above 100° C., i.e. participate in the curing reaction. Otherwise, the components to be crosslinked would have to be stored separately from each other and mixed with each other only shortly before application to the substrate in order to avoid premature, at least partial thermochemical curing (see two-component system). An example of a combination is a hydroxy-functional polyester and / or polyurethane in combination with a melamine resin and / or a blocked polyisocyanate as a crosslinking agent. In the two-component system, the components to be crosslinked, for example the organic polymer as a binder and the crosslinking agent, are present in at least two components respectively, which are combined only shortly before application. This form is selected when the components to be crosslinked react with each other even at ambient temperature or at a slightly elevated temperature of, for example, 40-90° C. Examples of combinations are hydroxy-functional polyesters and / or polyurethanes and / or poly(meth)acrylates with free polyisocyanates as crosslinkers.

[0045] In the context of the present invention, "actinically chemically curable" or the term "actinically chemically curing" is understood to mean that curing can be carried out using actinic radiation, i.e. electromagnetic radiation such as near infrared (NIR) and UV radiation, in particular UV radiation, and curing using particulate radiation such as electron beams. UV radiation curing is usually initiated by free radical or cationic photoinitiators. Typical actinically curable functional groups are carbon-carbon double bonds, for which free radical photoinitiators are usually used. Actinic curing is therefore also based on chemical crosslinking.

[0046] In the case of purely physically curing coating compositions, curing is preferably carried out for a period of 2 to 48 hours at 15 to 90° C. In this case, curing may therefore differ from flashing and / or intermediate drying operations only in the duration of the curing step.

[0047] In principle and in the context of the present invention, curing of thermochemically curable, particularly preferably thermochemically curable and externally crosslinking one-component systems is preferably carried out at a temperature of 80 to 250° C., more preferably 80 to 180° C., for a period of 5 to 60 minutes, preferably 10 to 45 minutes. Any flashing and / or intermediate drying stages prior to curing are therefore carried out at lower temperatures and / or for shorter times.

[0048] In principle and in the context of the present invention, the curing of thermochemically curable, particularly preferably thermochemically curable and externally crosslinkable two-component systems is carried out at a temperature of, for example, 15 to 90° C., preferably 40 to 90° C., for a period of 5 to 80 minutes, preferably 10 to 50 minutes. This does not, of course, exclude the curing of the two-component system at higher temperatures. For example, if a one-component and a two-component system are present simultaneously in the film formed according to the method of the invention, the co-curing is determined by the curing conditions required for the one-component system, thus resulting in the use of the higher curing temperatures described for the one-component system. Therefore, any flashing and / or intermediate drying stages before curing are carried out at lower temperatures and / or for shorter times.

[0049] The measurement methods used to determine certain characteristic variables in the context of the present invention are known from the examples. Unless explicitly stated otherwise, these measurement methods will be used to determine the corresponding characteristic variables.

[0050] All temperatures exemplified in the context of the present invention are to be understood as the temperature of the space in which the coated substrate is present. It is therefore not intended that the substrate itself must have this particular temperature.

[0051] All film thicknesses reported in the context of the present invention are to be understood as dry film thicknesses. They are therefore in each case the thickness of the cured film. Thus, when it is reported that a coating is applied at a specific film thickness, this means that the coating is applied in such a way that, after curing, said film thickness results.

[0052] If reference is made to an official standard in the context of the present invention, this of course refers to the version of the standard in force on the filing date or, if no version in force on that date existed, to the most recent version in force.

[0053] The water-based coating composition of the present invention:

[0054] Anion-stabilized binder B(a):

[0055] As a first essential ingredient, the coating composition of the invention comprises at least one anionically stabilized binder B. Excellent leveling properties are only achieved in combination with anionically stabilized binder B and a polycarboxylic acid PC dissolved in a solvent S. In contrast, in the case of the use of nonionically stabilized binders, the addition of a polycarboxylic acid PC does not lead to high leveling properties. In this context, nonionically stabilized binders are binders which have, in particular, a significant proportion of certain water-soluble nonionic groups, preferably polyoxyalkylene groups, polylactone groups, such as polybutyrolactone groups, polyol groups, such as polyvinyl alcohol groups, polyamide groups, such as polyacrylamide groups, and polyvinylpyrrolidone groups, more particularly polyethylene oxide and / or polypropylene oxide groups.

[0056] The anionically stabilized binder B is preferably present in the aqueous coating composition of the invention in the specified total amount. Therefore, in a preferred embodiment of the invention, the at least one anionically stabilized binder B is present in a total amount of 40-95% by weight solids, preferably 50-90% by weight solids, more particularly 55-85% by weight solids, in each case based on the total binder content of the coating composition. If more than one anionically stabilized binder B is used, the above-mentioned amount range is based on the total amount of anionically stabilized binders B in the composition. The use of the at least one anionically stabilized binder B in combination with the at least one polycarboxylic acid PC within the above-mentioned amount range results in excellent leveling properties and good optical and mechanical properties without adversely affecting the storage stability of the composition of the invention.

[0057] In the context of the present invention, it has proven to be advantageous if the anionically stabilized binder B is selected from aqueous polyurethane-polyurea dispersions which comprise anionically stabilized polyurethane-polyurea particles (PPP).

[0058] The anionically stabilized polyurethane-polyurea particles (PPP) preferably have an average particle size of 40 to 2,000 nm and a gel fraction of at least 50% and comprise in each case in reacted form:

[0059] (Z.1.1) at least one polyurethane prepolymer containing anionic groups and / or groups convertible into anionic groups and containing isocyanate groups, and

[0060] (Z.1.2.) At least one polyamine comprising two primary amino groups and one or two secondary amino groups.

[0061] The anionically stabilized polyurethane-polyurea particles (PPP) are in an aqueous dispersion or are present in the form of an aqueous dispersion. The water content in the dispersion is preferably 45 to 75% by weight, preferably 50 to 70% by weight, more preferably 55 to 65% by weight, in each case based on the total amount of the dispersion. Preferably, the dispersion consists of at least 90% by weight, preferably at least 92.5% by weight, very preferably at least 95% by weight, more preferably at least 97.5% by weight of polyurethane-polyurea particles (PPP) and water (the relevant values ​​are obtained by adding the amount of particles (i.e. the amount of polymer, determined via the solids content) and the amount of water).

[0062] Anionically stabilized polyurethane-polyurea particles (PPP) are polymer particles based on polyurethane-polyurea. Anionically stabilized polyurethane-polyurea particles (PPP) have a gel fraction of at least 50% (for the measurement method, see the Examples section) and an average particle size (also referred to as mean particle size) of 40-2,000 nanometers (nm) (for the measurement method, see the Examples section). Therefore, polyurethane-polyurea particles (PPP) constitute microgels. The reason is that, on the one hand, the polymer particles are in the form of relatively small particles or microparticles, and on the other hand, they are at least partially intramolecularly crosslinked. The latter means that the polymer structure present in the particles is equivalent to a typical macroscopic network with a three-dimensional network structure. However, from a macroscopic point of view, this microgel continues to contain discrete polymer particles.

[0063] Since microgels represent structures between branched and macroscopic crosslinked systems, they combine the properties of macromolecules with a network structure that are soluble in a suitable organic solvent and of an insoluble macroscopic network, the fraction of crosslinked polymer can be determined, for example, only after separation of the solid polymer, after removal of water and any organic solvent and subsequent extraction. The phenomenon utilized here is that the microgel particles, which are initially soluble in a suitable organic solvent, retain their internal network structure after separation and behave like a macroscopic network in the solid. Crosslinking can be verified by the experimentally obtainable gel fraction. Finally, the gel fraction is the fraction of polymer in the microgel that cannot be molecularly dissolved in the solvent as a discrete solid. Here, a further increase in the gel fraction caused by crosslinking reactions after separation of the polymer solid must be excluded. This insoluble fraction in turn corresponds to the fraction of polymer or particles that is present in the form of intramolecularly crosslinked particles.

[0064] The polyurethane-polyurea particles (PPP) preferably have a gel fraction of 50%, preferably at least 60%, more preferably at least 70%, more particularly at least 80%. Thus, the gel fraction may be up to 100% or close to 100%, for example 99% or 98%. In this case, all or almost all of the polyurethane-polyurea polymer is in the form of crosslinked particles.

[0065] The polyurethane-polyurea particles (PPP) have an average particle size of 40-2,000 nm, preferably 40-1500 nm, more preferably 100-1,000 nm, still more preferably 110-500 nm, more particularly 120-300 nm. An especially preferred range is 130-250 nm.

[0066] The polyurethane-polyurea particles (PPP) comprise in each case in reacted form (Z.1.1) at least one polyurethane prepolymer comprising isocyanate groups and comprising anionic groups and / or groups convertible into anionic groups, and (Z.1.2) at least one polyamine comprising two primary amino groups and one or two secondary amino groups. Here, the expression "the polyurethane-polyurea particles (PPP) comprise in each case in reacted form a polyurethane prepolymer (Z.1.1) and a polyamine (Z.1.2)" means that in the preparation of the polyurethane-polyurea particles (PPP) the aforementioned NCO-containing polyurethane prepolymer (Z.1.1) as well as the polyamine (Z.1.2) are used and that these two components react with one another to form a urea compound.

[0067] The polyurethane-polyurea particles (PPP) preferably consist of the two components (Z.1.1) and (Z.1.2), which means that they are prepared from these two components. The polyurethane-polyurea particles (PPP) in aqueous dispersion are obtainable, for example, by a specific three-step process.

[0068] In the first step (I) of the process, a composition (Z) is prepared. The composition (Z) comprises at least one, preferably exactly one, specific intermediate (ZL) containing isocyanate groups and blocked primary amino groups. The preparation of the intermediate (Z.1) comprises reacting at least one polyurethane prepolymer (Z.1.1) containing isocyanate groups and anionic groups and / or groups convertible into anionic groups with at least one compound (Z.1.2a) derived from a polyamine (Z.1.2) and containing at least two blocked primary amino groups and at least one free secondary amino group.

[0069] For the purposes of the present invention, component (Z.1.1) is referred to as a prepolymer for ease of understanding.

[0070] The prepolymer (Z.1.1) contains anionic groups and / or groups which can be converted into anionic groups (i.e. groups which can be converted into anionic groups by using known neutralizing agents, such as bases, which will be described in detail later below). As is known to the person skilled in the art, these groups are, for example, carboxylic acid, sulfonic acid and / or phosphonic acid groups, more particularly carboxylic acid groups (functional groups which can be converted into anionic groups by neutralizing agents), and anionic groups derived from the above functional groups, such as, more particularly, carboxylates, sulfonates and / or phosphonates, preferably carboxylates. It is known that the introduction of such groups can improve the dispersibility in water. Depending on the conditions chosen, the groups can be present in one form (e.g. carboxylic acid) or in the other form (carboxylates) in a proportionate or almost entirely manner by using, for example, neutralizing agents, which will be described later below.

[0071] To introduce the groups, during the preparation of the prepolymer (Z.1.1), starter compounds can be used which, in addition to the groups for reaction in the preparation of the urethane bonds, preferably hydroxyl groups, further contain the abovementioned groups, for example carboxylic acid groups. In this way, the groups are introduced into the prepolymer.

[0072] The corresponding compounds envisaged for the introduction of the preferred carboxylic acid groups include - insofar as they contain carboxyl groups - polyether polyols and / or polyester polyols. However, it is preferred in any case to use low molecular weight compounds having at least one carboxylic acid group and at least one functional group reactive toward isocyanate groups, preferably a hydroxyl group. In the context of the present invention, the expression "low molecular weight compound" means that the compound in question has a molecular weight of less than 300 g / mol. Preferably 100-200 g / mol. In this sense, examples of preferred compounds are monocarboxylic acids containing two hydroxyl groups, such as dihydroxypropionic acid, dihydroxysuccinic acid and dihydroxybenzoic acid. More particularly, they are α,α-dimethylolalkanoic acids, such as 2,2-dihydroxymethylacetic acid, 2,2-dihydroxymethylpropionic acid, 2,2-dihydroxymethylbutyric acid and 2,2-dihydroxymethylpentanoic acid, especially 2,2-dihydroxymethylpropionic acid.

[0073] The prepolymers (Z.1.1) therefore preferably comprise carboxylic acid groups. Based on the solids content, they preferably have an acid number of 10 to 30 mg KOH / g, more particularly 15 to 23 mg KOH / g (for the measurement method, see the Examples section).

[0074] The prepolymer (Z.1.1) is preferably prepared by the reaction of a diisocyanate with a polyol. Examples of suitable polyols are saturated or olefinically unsaturated polyester polyols and / or polyether polyols, as described, for example, in WO 2018 / 011311A1 and WO2016 / 091546A1. Polyols preferably used to prepare the prepolymer (Z.1.1) are polyester diols prepared using dimer fatty acids. Particularly preferred are polyester diols prepared using dicarboxylic acids, wherein at least 50% by weight, preferably 55-75% by weight, of the dicarboxylic acids used are dimer fatty acids. Dimer fatty acids are oligomeric forms of unsaturated monomeric fatty acids. Fatty acids are saturated or unsaturated, especially non-branched, monocarboxylic acids having 8-64 carbon atoms.

[0075] In addition, for the preparation of the polymer (Z.1.1), polyamines such as diamines and / or amino alcohols can also be used. Examples of diamines include hydrazine, alkyl- or cycloalkyldiamines such as propylenediamine and 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, and examples of amino alcohols include ethanolamine or diethanolamine.

[0076] With regard to polyisocyanates suitable for preparing isocyanate-containing polyurethane prepolymers (Z.1.1), reference is made to the publications WO 2018 / 011311A1 and WO 2016 / 091546A1. Preferably, aliphatic diisocyanates are used, such as hexamethylene diisocyanate, isophorone diisocyanate (IPDI), dicyclohexylmethane 4,4'-diisocyanate, 2,4- or 2,6-diisocyanato-1-methylcyclohexane and / or m-tetramethylxylene diisocyanate (m-TMXDI).

[0077] The number-average molecular weight of the prepolymers can vary within wide ranges, for example in the range from 2000 to 20 000 g / mol, preferably in the range from 3500 to 6000 g / mol (for the determination methods, see the Examples section).

[0078] The prepolymer (Z.1.1) contains isocyanate groups and preferably has an isocyanate content of 0.5 to 6.0% by weight, preferably 1.0 to 5.0% by weight, particularly preferably 1.5 to 4.0% by weight, based on the solids content (for the measurement method, see the Examples section).

[0079] The hydroxyl number of the prepolymer is preferably less than 15 mg KOH / g, more particularly less than 10 mg KOH / g, still more preferably less than 5 mg KOH / g, based on the solids content (for the measurement method, see the Examples section).

[0080] The prepolymer (Z.1.1) can be prepared as described in WO 2018 / 011311 A1 and WO 2016 / 091546 A1.

[0081] As already mentioned above, the groups which are convertible into anionic groups present in the prepolymer (Z.1.1) can also be present in proportion as corresponding anionic groups, for example by using a neutralizing agent. In this way, the water dispersibility of the prepolymer (Z.1.1) and therefore also of the intermediate (Z.1) can be adjusted. Contemplated neutralizing agents include in particular the known alkaline neutralizing agents, for example carbonates, bicarbonates or hydroxides of alkali metals and alkaline earth metals, for example LiOH, NaOH, KOH or Ca(OH)2. Also suitable for neutralization and preferably used in the context of the present invention are organic nitrogen bases, for example amines, such as ammonia, trimethylamine, triethylamine, tributylamine, dimethylaniline, triphenylamine, dimethylethanolamine, methyldiethanolamine or triethanolamine, and mixtures thereof.

[0082] If it is necessary to neutralize groups convertible into anionic groups, in particular carboxylic acid groups, the neutralizing agent can be added, for example, in such an amount that 35-65% of the group fraction is neutralized (neutralization degree), preferably 40-60% (for calculation method, see the Examples section).

[0083] Compound (Z.1.2a) contains two blocked primary amino groups and one or two free secondary amino groups.

[0084] As is known, a blocked amino group is an amino group in which the hydrogen radical on the nitrogen which is inherently present as a free amino group has been replaced by a reversible reaction with a blocking agent. Due to the blocking, the amino group cannot react by condensation or addition reactions like the free amino group and is therefore non-reactive in this respect and therefore differs from the free amino group. The primary amino group of compound (Z.1.2a) can be blocked with blocking agents known per se, for example with ketones and / or aldehydes. In the case of such blocking, ketimines and / or aldimines are then produced, with the release of water. Such groups can be unblocked when water is added.

[0085] If it is neither indicated that the amino group is blocked nor that it is free, the free amino group is referred to.

[0086] Preferred blocking agents for blocking the primary amino groups of compound (Z.1.2a) are ketones. Among the ketones, those organic solvents (Z.2) which will be described later below are particularly preferred. The reason is that this solvent (Z.2) must in any case be present in the composition (Z) to be prepared in step (I) of the process. By using ketones (Z.2) for blocking, it is therefore possible to use the corresponding preferred methods for preparing blocked amines without having to separate the blocking agent, which may be undesirable in terms of cost and inconvenience. Instead, the solution of the blocked amine can be used directly for the preparation of the intermediate (Z.1). Preferred blocking agents are acetone, methyl ethyl ketone, methyl isobutyl ketone, diisopropyl ketone, cyclopentanone or cyclohexanone; particularly preferred are ketones (Z.2), methyl ethyl ketone and methyl isobutyl ketone.

[0087] Furthermore, the preferred blocking with ketones and / or aldehydes, especially ketones, and the associated preparation of ketimines and / or aldimines have the advantage of selectively blocking primary amino groups. The secondary amino groups present are obviously not blocked and therefore remain free. Thus, compounds (Z.1.2a) which contain one or two free secondary amino groups in addition to two blocked primary amino groups can easily be prepared by the preferred blocking reaction described from the corresponding polyamines (Z.1.2) containing free secondary and primary amino groups.

[0088] The compounds (Z.1.2a) preferably have two blocked primary amino groups and one or two free secondary amino groups, the primary amino groups they have are exclusively blocked primary amino groups, and the secondary amino groups they have are exclusively free secondary amino groups.

[0089] Compound (Z.1.2a) preferably has a total of 3 or 4 amino groups, these being selected from blocked primary amino groups and free secondary amino groups.

[0090] Particularly preferred compounds (Z.1.2a) are those which consist of two blocked primary amino groups, one or two free secondary amino groups and an aliphatic saturated hydrocarbon group.

[0091] Similar preferred embodiments apply to polyamines (Z.1.2) when these contain free primary amino groups instead of blocked primary amino groups. Examples of preferred polyamines (Z.1.2) from which compounds (Z.1.2a) can also be prepared by blocking primary amino groups are diethylenetriamine, 3-(2-aminoethyl)aminopropylamine, dipropylenetriamine, as well as N1-(2-(4-(2-aminoethyl)piperazin-1-yl)ethyl)-ethane-1,2-diamine (one secondary amino group, two primary amino groups to be blocked) and triethylenetetramine, as well as N,N'-bis(3-aminopropyl)ethylenediamine (two secondary amino groups, two primary amino groups to be blocked).

[0092] If a certain amount of the polyamine is blocked, the blocking may result in, for example, a fraction of 95 mol % or more of the primary amino groups being blocked (this fraction can be determined by IR spectroscopy; see the Examples section). For example, when a polyamine in the unblocked state has two free primary amino groups, and when a certain amount of the primary amino groups of this amine is subsequently blocked, then in the context of the present invention, the amine is said to have two blocked primary amino groups if a fraction of more than 95 mol % of the primary amino groups present in the amount used is blocked.

[0093] The preparation of the intermediate (Z.1) involves the reaction of the prepolymer (Z.1.1) with the compound (Z.1.2a) by addition reaction of the isocyanate groups of (Z.1.1) with the free secondary amino groups of (Z.1.2a). This reaction is known per se and then leads to the attachment of the compound (Z.1.2a) to the prepolymer (Z.1.1) to form a urea bond, ultimately giving the intermediate (Z.1).

[0094] Intermediate (Z.1) can be prepared as described in WO 2018 / 011311A1 and WO 2016 / 091546A1.

[0095] The fraction of intermediate (Z.1) is 15 to 65% by weight, preferably 25 to 60% by weight, more preferably 30 to 55% by weight, particularly preferably 35 to 52.5% by weight and in a very particular embodiment 40 to 50% by weight, in each case based on the total amount of composition (Z).

[0096] The composition (Z) further comprises at least one specific organic solvent (Z.2). The solvent (Z.2) has a water solubility of up to 38% by weight at a temperature of 20° C. (for the measurement method, see the Examples section). The solubility in water at a temperature of 20° C. is preferably less than 30% by weight. The preferred range is 1 to 30% by weight. Therefore, the solvent (Z.2) has a rather moderate solubility in water, more particularly, is not completely miscible with water, or does not have an infinite solubility in water.

[0097] Examples of solvents (Z.2) are methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, diethyl ether, dibutyl ether, dipropylene glycol dimethyl ether, ethylene glycol diethyl ether, toluene, methyl acetate, ethyl acetate, butyl acetate, propylene carbonate, cyclohexanone or mixtures of these solvents. Preference is given to methyl ethyl ketone, which has a solubility of 24% by weight in water at 20° C. Thus, solvent (Z.2) is not a solvent such as acetone, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, tetrahydrofuran, dioxane, N-formylmorpholine, dimethylformamide or dimethyl sulfoxide.

[0098] The effect of choosing a specific solvent (Z.2) with only limited water solubility is, in particular, that when the composition (Z) is dispersed in the aqueous phase in step (II) of the process, a homogeneous solution cannot be formed directly; instead, the crosslinking reaction (addition reaction of free primary amino groups and isocyanate groups to form urea bonds) that occurs in step (II) takes place within a limited volume, thus enabling the formation of microparticles as defined above.

[0099] The fraction of the at least one organic solvent (Z.2) is 35 to 85% by weight, preferably 40 to 75% by weight, more preferably 45 to 70% by weight, particularly preferably 47.5 to 65% by weight and in a very particular embodiment 50 to 60% by weight, in each case based on the total amount of the composition (Z).

[0100] In the present invention, it has been found that due to the targeted combination of the above-mentioned fractions of the intermediate (Z.1) in the composition (Z) and the selection of a specific solvent (Z.2), a polyurethane-polyurea dispersion comprising polyurethane-polyurea particles (PPP) having the desired particle size and gel fraction can be provided according to steps (II) and (III) described below.

[0101] The components (Z.1) and (Z.2) preferably together make up at least 90% by weight of the composition (Z). The two components preferably make up at least 95% by weight of the composition (Z), more particularly at least 97.5% by weight. Very particularly preferably, the composition (Z) consists of these two components. In this context, it can be noted that when neutralizing agents as described above are used, these neutralizing agents are included together with the intermediates when calculating the amount of intermediates (Z.1). Therefore, the solid content of the composition (Z) preferably corresponds to the fraction of the intermediates (Z.1) in the composition (Z). Therefore, the composition (Z) preferably has a solid content of 15-65% by weight, preferably 25-60% by weight, more preferably 30-55% by weight, particularly preferably 35-52.5% by weight, and in a very particular embodiment, 40-50% by weight.

[0102] Particularly preferred compositions (Z) therefore comprise a total of at least 90% by weight of components (Z.1) and (Z.2) and, apart from the intermediate (Z.1), exclusively organic solvents.

[0103] In step (II) of the process described here, the composition (Z) is then dispersed in water, accompanied by deblocking of the blocked primary amino groups of the intermediate (Z.1) and reaction of the resulting free primary amino groups with the isocyanate groups of the intermediate (Z.1) and with the isocyanate groups of the deblocked intermediate obtained from the intermediate (Z.1), the reaction being an addition reaction.

[0104] Step (II) of the method can be carried out as described in WO 2018 / 011311A1 and WO 2016 / 091546A1.

[0105] The fraction of polyurethane-polyurea particles (PPP) in the dispersion is preferably 25 to 55% by weight, preferably 30 to 50% by weight, more preferably 35 to 45% by weight, in each case based on the total amount of the dispersion (determined analogously to the solids content determined above for intermediate (Z.1)).

[0106] The polyurethane-polyurea particles (PPP) preferably have an acid number of 10 to 35 mg KOH / g, more particularly 15 to 23 mg KOH / g (for the measurement method, see the Examples section). In addition, the polyurethane-polyurea particles have very few hydroxyl groups or no hydroxyl groups. Thus, the OH number of the particles is less than 15 mg KOH / g, more particularly less than 10 mg KOH / g, more preferably less than 5 mg KOH / g (for the measurement method, see the Examples section).

[0107] It is particularly preferred to use an anionically stabilized binder having a certain electrophoretic mobility at pH 8.0. Here, the electrophoretic mobility can be determined as described in the Examples section. Therefore, in a preferred embodiment of the present invention, the at least one anionically stabilized binder B has an electrophoretic mobility of -2.5 to -15 (μm / s) / (V / cm), preferably -2.5 to -10 (μm / s) / (V / cm), more preferably -4 to -8 (μm / s) / (V / cm), more particularly -5 to -8 (μm / s) / (V / cm) at pH 8.0. The use of at least one anionically stabilized binder B having the above electrophoretic mobility in combination with the at least one polycarboxylic acid PC results in an excellent leveling effect without adversely affecting the performance characteristics and the optical and color properties of the coating prepared with the composition of the present invention.

[0108] The coating composition may contain a total amount of 1-60% by weight solids, preferably 5-50% by weight solids, more preferably 10-40% by weight solids, most preferably 15-40% by weight solids of the polyurethane-polyurea aqueous dispersion, in each case based on the total binder content of the coating composition. The use of the above total amounts of polyurethane-polyurea aqueous dispersions in combination with the at least one polycarboxylic acid PC results in excellent leveling properties without negatively affecting the mechanical and optical properties of the resulting coating.

[0109] In addition to the above-mentioned polyurethane-polyurea aqueous dispersions, the coating composition of the invention may also contain anionically stabilized binders B. Suitable anionically stabilized binders B that can be used according to the invention are, for example, self-crosslinking aqueous dispersions that contain at least one polyhydrazide and at least one carbonyl-containing urethane-vinyl hybrid polymer. Suitable self-crosslinking aqueous dispersions are described, for example, in EP 0 649 865A1. The total amount of the anionically stabilized binder B is generally 0 to 45% by weight solids, based on the total binder content of the coating composition.

[0110] Coloring Pigment P(b):

[0111] As a second essential component (b), the coating composition of the invention comprises at least one coloring pigment P. Such coloring pigments are known to the person skilled in the art and are described, for example, in - Lexikon Lacke and Druckfarben, Georg Thieme Verlag, Stuttgart, New York, 1998, pp. 176 and 451. The terms "coloring pigment" and "colored pigment" are interchangeable.

[0112] Suitable colored pigments P are preferably selected from (i) white pigments, for example titanium dioxide, zinc white, zinc sulfide or lithopone; (ii) black pigments, for example carbon black, iron manganese black or spinel black; (iii) colored pigments, for example ultramarine green, ultramarine blue, manganese blue, ultramarine violet, manganese violet, iron oxide red, molybdenum red, ultramarine red, iron oxide brown, mixed brown, spinel phase and corundum phase, iron oxide yellow, bismuth vanadate; (iv) organic pigments, for example monoazo pigments, disazo pigments, anthraquinone pigments, benzimidazole pigments, quinacridone pigments, quinophthalone pigments, diketopyrrolopyrrole pigments, dioxazine pigments, indanthrone pigments, isoindoline pigments, isoindolinone pigments, azomethine pigments, thioindigo pigments, metal complex pigments, prinone pigments, perylene pigments, phthalocyanine pigments, aniline black; and (v) mixtures thereof.

[0113] The at least one coloring pigment P is preferably used in a specific total amount. Therefore, in a preferred embodiment of the first subject of the present invention, the aqueous coating composition comprises a total amount of 1 to 40% by weight, preferably 2 to 35% by weight, more preferably 5 to 30% by weight of the at least one coloring pigment P, in each case based on the total weight of the coating composition.

[0114] The aqueous coating composition of the present invention does not contain any effect pigments, ie the amount of effect pigments in the composition of the present invention is 0% by weight, based on the total weight of the coating composition.

[0115] Polycarboxylic acid PC(c):

[0116] As a third essential ingredient, the aqueous coating composition of the present invention comprises at least one polycarboxylic acid PC.

[0117] The neutralization level of the at least one polycarboxylic acid PC is preferably at least 5%, preferably at least 10%, more preferably 10-100%. The neutralization level is the amount of carboxylic acid groups neutralized by the base. The above neutralization level leads to improved dissolution of the polycarboxylic acid PC in the aqueous coating composition, thereby minimizing gel spots, while improving the leveling properties and storage stability of the coating composition.

[0118] The at least one polycarboxylic acid PC is more preferably a dicarboxylic acid.Dicarboxylic acids according to the invention are compounds having exactly two carboxylic acid groups per molecule.

[0119] In this context, particular preference is given to dicarboxylic acids having the general formula (I):

[0120] K +- OOC-R-COO - K +

[0121] in:

[0122] R is a straight chain or branched saturated C4-C 30 Alkyl, linear or branched unsaturated C 10 -C 72 Alkyl, cycloalkyl or aryl, preferably a straight chain saturated C7 alkyl,

[0123] K + It is hydrogen or a cation.

[0124] Preferred K + is a cation. More preferably K + is a base used to at least partially neutralize the polycarboxylic acid PC. Very preferably it is N,N'-dimethylethanolamine which is cationic.

[0125] Particularly preferred dicarboxylic acids are selected from the group consisting of azelaic acid, pimelic acid, suberic acid, sebacic acid, dodecanedioic acid and phthalic acid and mixtures thereof. Particularly preferably, the coating composition of the invention comprises exactly one of the abovementioned dicarboxylic acids.

[0126] The use of the above-mentioned dicarboxylic acids in combination with the at least one anionically stabilized binder B has proven to be particularly advantageous for achieving excellent leveling properties without negatively affecting the storage stability of the coating compositions and the optical and mechanical properties of the coatings produced from these compositions. In addition, the use of these polycarboxylic acids, preferably azelaic acid, pimelic acid, suberic acid, sebacic acid, dodecanedioic acid and phthalic acid and mixtures thereof, in combination with at least one anionically stabilized binder B leads to an improvement in the goniochromatic effect of metal coatings applied directly on coatings produced from the coating compositions of the invention. The polycarboxylic acids used according to the invention are commercially available, for example from Merck.

[0127] The at least one polycarboxylic acid PC is preferably used in a specific total amount. Therefore, it is particularly preferred according to the invention that the aqueous coating composition comprises a total amount of 0.01-4% by weight, more preferably 0.02-2% by weight, more particularly 0.05-1% by weight of the at least one polycarboxylic acid PC, in each case based on the total weight of the coating composition. The use of polycarboxylic acid PC, especially a dicarboxylic acid of the above-mentioned formula (I), in combination with the at least one anionically stabilized binder B in the total amount leads to excellent leveling properties without negatively affecting the good optical and mechanical properties of the coating prepared from the coating composition of the invention. In addition, the storage stability of the coating composition is not reduced when the polycarboxylic acid PC is added. In addition, the addition of only a small amount of polycarboxylic acid PC improves the angular color change effect of the metal coating directly applied on the coating prepared from the coating composition of the invention.

[0128] Solvent S(d):

[0129] As an optional ingredient, the aqueous coating composition of the present invention may include at least one solvent S. The solvent S may be used to solubilize the at least one polycarboxylic acid PC and may promote uniform incorporation of the polycarboxylic acid PC into the coating composition, thereby resulting in high storage stability and effective leveling properties of the coating composition.

[0130] The at least one solvent S is preferably selected from water, alkoxy C2-C 10 alcohols, ketones, esters, amides, methylals, butyrals, 1,3-dioxolane, glycerol formal and mixtures thereof, more particularly selected from water and / or alkoxy C2-C 10 In particular, water and / or alkoxy C2-C 10 The use of alcohols to solubilize the polycarboxylic acid PC has proven to be advantageous with regard to uniform incorporation, thereby leading to high storage stability and excellent leveling properties of the compositions of the invention.

[0131] If the at least one solvent S is present in the aqueous coating composition, the solvent S, more particularly water and / or an alkoxy C2-C 10 The total amount of alcohol is 0.01 to 15% by weight, preferably 0.05 to 10% by weight, more preferably 0.1 to 5% by weight, more particularly 0.2 to 2% by weight, in each case based on the total weight of the coating composition. In the case of using water as solvent S, the amount of solvent S is taken into account when calculating the total amount of water present in the aqueous coating composition. The at least one solvent S used in the above amounts, more particularly water and / or alkoxy C2-C 10 The alcohol causes the at least one polycarboxylic acid PC to be fully dissolved in the aqueous coating composition and in this way ensures excellent leveling properties and high storage stability. In addition, it enables the polycarboxylic acid PC to be uniformly incorporated into the aqueous coating composition.

[0132] Other ingredients (e):

[0133] In addition to the above-mentioned mandatory components (a) to (d), the aqueous coating composition of the present invention may further comprise other ingredients selected from the group consisting of a neutralizer, a thickener, a crosslinker and mixtures thereof.

[0134] The neutralizing agent is preferably selected from inorganic bases, primary amines, secondary amines, tertiary amines and mixtures thereof, in particular N,N'-dimethylethanolamine. It is particularly preferred to use a neutralizing agent, in particular N,N'-dimethylethanolamine, to neutralize the at least one polycarboxylic acid PC. In this way, the solubility of the polycarboxylic acid PC in the solvent S and the aqueous coating composition can be increased.

[0135] In this context, it is preferred that the at least one neutralizing agent, especially N,N'-dimethylethanolamine, is present in a total amount of 0.05 to 5% by weight, preferably 0.05 to 4% by weight, more preferably 0.05 to 1% by weight, more particularly 0.05 to 0.2% by weight, in each case based on the total weight of the coating composition. The use of a neutralizing agent, especially N,N'-dimethylethanolamine, in the above-mentioned amount range, optionally in combination with the at least one solvent S, ensures sufficient solubilization of the polycarboxylic acid PC and thus ensures uniform incorporation and high storage stability of the coating composition according to the invention.

[0136] The thickener is preferably selected from the group consisting of phyllosilicates, (meth)acrylic acid-(meth)acrylate copolymers, nonionic polyurethanes, hydrophobically modified polyethers, hydroxyalkylcelluloses, polyamides and mixtures thereof, in particular nonionic polyurethanes. (Meth)acrylic acid-(meth)acrylate copolymers are obtainable by reacting (meth)acrylic acid with (meth)acrylate esters. Depending on the carbon chain length in the (meth)acrylate ester, these copolymers have an associative thickening effect (ASE or HASE thickeners). Copolymers containing only C1-C4 alkyl (meth)acrylates do not have an associative thickening effect (ASE thickeners). In contrast, copolymers containing (meth)acrylates with a chain length of more than 4 carbon atoms have an associative thickening effect (HASE thickeners). Hydrophobically modified ethoxylated polyurethanes are obtainable by reacting diisocyanates with polyethers and subsequently reacting the prepolymers with hydrophobic alcohols. Such polyurethanes are also referred to as HEUR thickeners. Particular preference is given to using a combination of non-associative thickening (meth)acrylic acid-(meth)acrylate copolymers and hydrophobically modified ethoxylated polyurethanes.

[0137] In this context, it is preferred that the at least one thickener, more particularly the nonionic polyurethane, is present in a total amount of 0.015 to 3% by weight, preferably 0.03 to 2% by weight, more preferably 0.04 to 1% by weight, more particularly 0.05 to 0.7% by weight, in each case based on the total weight of the coating composition.

[0138] According to a particularly preferred embodiment of the present invention, the aqueous coating composition does not contain phyllosilicates and / or polyamides, more particularly does not contain phyllosilicates and polyamides. This means that the coating composition contains 0% by weight of phyllosilicates, more particularly sodium magnesium silicate and / or lithium aluminum magnesium silicate, and / or polyamides, based on the total weight of the coating composition. Surprisingly, the use of polycarboxylic acid PC without the additional use of polyamides and / or phyllosilicates results in excellent leveling properties comparable to the use of polyamides and / or phyllosilicates. However, when using the at least one polycarboxylic acid PC, undesirable separation phenomena do not occur and the shear stability is not reduced.

[0139] The crosslinking agent is preferably selected from melamine-formaldehyde resins, free and / or blocked polyisocyanates, polycarbodiimides and mixtures thereof, more particularly melamine-formaldehyde resins.

[0140] In this context, it is preferred that at least one crosslinker, in particular a melamine-formaldehyde resin, is present in a total amount of 5 to 50% by weight, preferably 7 to 45% by weight, very preferably 10 to 40% by weight, in each case based on the total weight of the coating composition. The above total amounts ensure sufficient crosslinking of the aqueous coating composition.

[0141] Despite the use of polycarboxylic acid PC, the coating composition of the invention still has a relatively high solids content. It is therefore preferred that the composition has a solids content of 15 to 60% by weight, in each case based on the total weight of the coating composition and measured in accordance with DIN EN ISO 3251 (June 2008). Due to the high solids content, the coating composition of the invention has good environmental properties without any adverse effects on its storage stability. Storage stability can be described, for example, by measuring the liquid viscosity over time.

[0142] The coating compositions of the invention preferably have a pH of from 7 to 10, more particularly from 7 to 9, measured in each case at 23°C.

[0143] The method for preparing the water-based coating composition of the present invention:

[0144] The coating composition of the present invention is preferably obtained by the following steps:

[0145] (1) providing a solution comprising at least one polycarboxylic acid PC, at least one solvent S and optionally at least one neutralizing agent, and

[0146] (2) Adding the solution provided in step (1) to an aqueous composition comprising at least one anionically stabilized binder B and at least one coloring pigment P.

[0147] The preparation of the solution in step (1) ensures uniform incorporation of the polycarboxylic acid PC in the aqueous composition. Furthermore, the use of the solution prepared in step (1) minimizes the risk of the formation of undesirable gel spots during the addition of the polycarboxylic acid PC to the aqueous composition comprising the anionically stabilized binder B and the at least one coloring pigment P. Furthermore, the solution is storage-stable and can therefore be easily integrated as an intermediate product into the process for the preparation of an aqueous coating composition.

[0148] With regard to the polycarboxylic acid PC, the solvent S, the anionically stabilized binder B, the coloring pigment P and the neutralizing agent, the statements made with regard to the coating composition of the invention apply mutatis mutandis.

[0149] The method for preparing a multi-layer paint system according to the present invention:

[0150] The method according to the invention for producing a multilayer coating system (M) on a substrate (S) comprises the following steps:

[0151] (1) optionally, preparing a cured first coating (S1) on a substrate (S) by applying a composition (Z1) to a substrate (S) and subsequently curing the applied composition (Z1),

[0152] (2) preparing a basecoat layer (BL2a) or at least two directly successive basecoat layers (BL2-x) directly on the first coating layer (S1) by applying a water-based basecoat material (bL2a) directly on the first coating layer (S1) or applying at least two water-based basecoat materials (bL2-x) directly and successively on the first coating layer (S1),

[0153] (3) preparing a clear coating (C) directly on the basecoat layer (BL2a) or the uppermost basecoat layer (BL2-z) by applying a clear coating (cm) directly on the basecoat layer (BL2a) or the uppermost basecoat layer (BL2-z),

[0154] (4) curing the base paint layer (BL2a) and the clear coating layer (C) or the base paint layer (BL2-x) and the clear coating layer (C) together,

[0155] Wherein at least one of the at least one basecoat material (bL2a) or the at least one of the basecoat materials (bL2-x) comprises the aqueous coating composition of the present invention and / or at least one of the at least one basecoat material (bL2a) or the at least one of the basecoat materials (bL2-x) is an aqueous coating composition prepared by the method of the present invention.

[0156] The substrate (S) is preferably selected from metal substrates, metal substrates coated with a cured electrophoretic coating, plastic substrates, reinforced plastic substrates and substrates comprising metal and plastic components, and particularly preferably selected from metal substrates.

[0157] In this context, preferred metal substrates (S) are selected from iron, aluminum, copper, zinc, magnesium and alloys thereof and steel. Preferred substrates are those of iron and steel, examples being typical iron and steel substrates used in the automotive industry. The substrate itself can be of any shape - i.e. it can be, for example, a simple metal sheet or a complex component, such as, in particular, a car body and parts thereof.

[0158] Preferred plastic substrates (S) are substrates which essentially comprise or consist of (i) polar plastics, such as polycarbonates, polyamides, polystyrenes, styrene copolymers, polyesters, polyphenylene ethers and blends of these plastics, (ii) synthetic resins, such as polyurethane RIM, SMC, BMC, and (iii) polyolefin substrates of the polyethylene and polypropylene type with a high rubber content, such as PP-EPDM, and surface-activated polyolefin substrates. In addition, the plastics may be fiber-reinforced, in particular using carbon fibers and / or metal fibers.

[0159] Furthermore, substrates (S) which contain both metal and plastic parts can also be used. Such substrates are, for example, vehicle bodies containing plastic parts.

[0160] The substrate (S) can be pretreated in any customary manner before step (1) of the process according to the invention or before the application of the composition (Z1) - i.e., for example, cleaned (e.g. mechanically and / or chemically) and / or provided with known conversion coatings (e.g. by phosphating and / or chromating) or surface activation pretreatments (e.g. by flame treatment, plasma treatment and corona discharge).

[0161] Step (1):

[0162] In step (1) of the process according to the invention, a cured first coating (S1) can be prepared on a substrate (S) by applying the composition (Z1) to the substrate (S) and subsequently curing the composition (Z1). This step is preferably carried out if the substrate (S) is a metal substrate.

[0163] The composition (Z1) can be an electrophoretic coating or a primer. However, the primer of the present invention is not the basecoat applied in step (2) of the method of the present invention. The method of the present invention is preferably carried out with a metal substrate (S). Therefore, the first coating (S1) is more particularly a cured electrophoretic coating (E1). Therefore, in a preferred embodiment of the method of the present invention, the composition (Z1) is an electrophoretic coating applied electrophoretically to the substrate (S). Suitable electrophoretic coatings and their curing are described in WO 2017 / 088988A1 and contain a hydroxyl-functional polyetheramine as a base material and a blocked polyisocyanate as a crosslinker.

[0164] The applied composition (Z1) is flashed, for example, at 15-35° C. for a period of, for example, 0.5-30 minutes and / or intermediately dried, for example, at a temperature of preferably 40-90° C. for a period of, for example, 1-60 minutes. Preferably, the applied composition (Z1) is cured at a temperature of 100-250° C., preferably 140-220° C., for a period of 5-60 minutes, preferably 10-45 minutes, which produces a cured first coating (S1).

[0165] The layer thickness of the cured first coating (C1) is, for example, 10 to 40 μm, preferably 15 to 25 μm.

[0166] Step (2):

[0167] Step (2) of the method of the present invention includes preparing exactly one basecoat layer (BL2a) (step (2) (a)) or preparing at least two directly successive basecoat layers (BL2-a) and (BL2-z) (step (2) (b)). The basecoat layer is prepared by (a) directly applying an aqueous basecoat composition (bL2a) to a substrate (S) or a cured first coating (S1) or (b) directly and successively applying at least two basecoat compositions (bL2-a) and (bL2-z) to a substrate (S) or a cured first coating (S1). Therefore, after preparation, the basecoat film (BL2a) according to step (2) (a) is directly arranged on the substrate (S) or directly arranged on the cured first coating (S1).

[0168] Therefore, applying at least two, i.e. multiple, basecoat compositions directly and successively to the substrate (S) or the cured first coating (S1) should be understood to mean applying the first basecoat composition (bL2-a) directly to the substrate (S) or the cured first coating (S1), and then applying the second basecoat composition (bL2-b) directly to the layer of the first basecoat composition. Then, any third basecoat composition (bL2-c) is applied directly to the layer of the second basecoat composition. Then, the operation can be repeated similarly for other basecoat compositions (i.e. the fourth, fifth, etc. basecoat compositions). The topmost basecoat layer obtained after step (2) (b) of the method of the present invention is represented as basecoat layer (BL2-z).

[0169] Therefore, the basecoat layer (BL2a) or the first basecoat layer (BL2-a) is arranged directly on the substrate (S) or the cured first coating layer (S1).

[0170] For the sake of greater clarity, the terms "basecoat composition" and "basecoat layer" are used in connection with the coating composition applied in step (2) of the process of the present invention and the coating film obtained. The basecoat layer or layers are cured together with the clearcoat material, so that the curing is achieved similarly to the curing of the so-called basecoat composition used in the standard method described in the introduction. More particularly, the coating composition used in step (2) of the process of the present invention is not cured separately, like the coating composition known as a top-surfacer mixed primer in the case of the standard method. With respect to step (2)(b), the basecoat composition and the basecoat layer are generally indicated as (bL2-x) and (BL2-x), where x is replaced by other suitable letters in the nomenclature of the specific individual basecoat composition and basecoat layer.

[0171] A preferred embodiment of the variant (b) of the method step (2) of the present invention is to use exactly two basecoat compositions. Therefore, two aqueous basecoat compositions (bL2-a) and (bL2-z) are directly applied to the cured first coating (S1) in succession to form two basecoat layers (BL2-a) and (BL2-z) directly superimposed on each other. The basecoat materials may be the same or different. It is also possible to prepare two or more basecoat films (BL2-x) with the same basecoat material, and to prepare one or more other basecoat films (BL2-x) with one or more other basecoat materials. However, at least one of the aqueous basecoat materials (bL2-x) used in step (2) (b) comprises an aqueous coating composition of the present invention and / or an aqueous coating composition prepared by the method of the present invention.

[0172] In a particularly preferred embodiment of step (2)(b), the first aqueous basecoat composition (bL2-a) corresponds to the coating composition of the invention, while the second basecoat composition (bL2-z) is a basecoat composition containing effect pigments. This leads to an improvement in the brightness and the goniochromatic index of the metallic coating composition used as the second basecoat composition (bL2-z), without negatively affecting the mechanical properties of the resulting multilayer coating system (M).

[0173] The basecoat composition (bL2-z) used in step (2) (b) of the method of the present invention comprises at least one binder. Therefore, the preferred aqueous basecoat composition (bL2-z) comprises at least one hydroxy-functional polymer as a binder, and the at least one hydroxy-functional polymer is selected from polyurethanes, polyesters, copolymers, copolymers thereof and mixtures of these polymers. Preferred polyurethane-acrylate copolymers (acrylated polyurethanes) and their preparation are described, for example, in WO 91 / 15528A1, page 3, line 21 to page 20, line 33 and DE 4437535A1, page 2, line 27 to page 22. The basecoat preferably has an OH value of 20-200 mg KOH / g, more preferably 40-150 mg KOH / g.

[0174] The proportion of the binder, preferably the at least one polyurethane-acrylate copolymer, is preferably 0.5 to 20% by weight, more preferably 1 to 15% by weight, particularly preferably 1.5 to 10% by weight, in each case based on the total weight of the aqueous basecoat material composition.

[0175] Advantageously, the basecoat composition (bL2-z) used in step (2) (b) of the method according to the invention is colored, i.e. it preferably comprises at least one coloring and / or effect pigment. Therefore, the aqueous basecoat composition (bL2-z) preferably comprises at least one coloring and / or effect pigment, more preferably at least one coloring and effect pigment. The combined use of a coating composition (bL2-z) comprising at least one effect pigment with the coating composition of the invention as an aqueous basecoat composition (bL2-a) results in improved brightness and angular color flop index. This improved brightness and angular color flop index is due to the presence of a combination of polycarboxylic acid PC, anionically stabilized binder B and solvent S in the first aqueous basecoat composition (bL2-a).

[0176] Preferred colored pigments in this context are the pigments described with respect to the colored pigments P present in the aqueous coating composition of the invention.

[0177] Useful effect pigments are selected from (i) platelet-shaped metal effect pigments, such as lamellar aluminum pigments, (ii) gold bronzes; (iii) bronze oxides and / or iron oxide-aluminum pigments; (iv) pearlescent pigments, such as pearl powders; (v) basic lead carbonate; (vi) bismuth oxychloride and / or metal oxide-mica pigments; (vii) lamellar pigments, such as lamellar graphite, lamellar iron oxide; (viii) multilayer effect pigments consisting of PVD films; (ix) liquid crystal polymer pigments; and (x) mixtures thereof.

[0178] The at least one coloring and / or effect pigment is preferably present in the at least one aqueous basecoat composition (bL2-z) in a total amount of 1 to 40% by weight, preferably 2 to 35% by weight, more preferably 5 to 30% by weight, in each case based on the total weight of the aqueous basecoat composition (bL2-z).

[0179] Furthermore, the basecoat composition (bL2-z) used in step (2) (b) of the method according to the invention preferably comprises at least one typical crosslinking agent known per se. Advantageously, the aqueous basecoat (bL2-z) comprises at least one crosslinking agent selected from blocked polyisocyanates and / or aminoplast resins, preferably aminoplast resins. Among aminoplast resins, melamine resins are particularly preferred.

[0180] The proportion of crosslinkers, in particular aminoplast resins and / or blocked polyisocyanates, more preferably aminoplast resins, among which melamine resins are preferred, is preferably 5 to 50% by weight, more preferably 7 to 45% by weight and particularly preferably 10 to 40% by weight, in each case based on the total binder content of the coating composition.

[0181] Preferably, the basecoat composition (bL2-z) used in step (2) (b) of the method of the present invention additionally comprises at least one thickener. Suitable thickeners are disclosed above with respect to the aqueous coating composition of the present invention. Particularly preferred thickeners are selected from phyllosilicates. The proportion of thickener is preferably 0.01-5% by weight, preferably 0.02-4% by weight, more preferably 0.05-3% by weight, in each case based on the total weight of the aqueous basecoat composition (bL2-z).

[0182] In addition, the aqueous basecoat composition (bL2-z) may also contain at least one additive. Examples of such additives are salts that can be thermally decomposed without residue or substantially without residue, resins that can be cured by physical, thermal and / or actinic radiation and are different from the polymers already mentioned as base materials, other crosslinking agents, organic solvents, reactive diluents, transparent pigments, fillers, dyes that can be dissolved in a molecularly dispersed manner, nanoparticles, light stabilizers, antioxidants, degassing agents, emulsifiers, slip additives, polymerization inhibitors, free radical polymerization initiators, tackifiers, flow regulators, film-forming aids, sag regulators (SCA), flame retardants, corrosion inhibitors, waxes, desiccants, biocides and matting agents. Suitable additives of the above-mentioned kind are known, for example, from German patent application DE 199 48 004 A1, page 14, line 4 to page 17, line 5, German patent DE 100 43 405 C1, column 5, paragraphs

[0031] -

[0033] . They are used in customary and known amounts. For example, their proportion may be 1.0 to 20% by weight, in each case based on the total weight of the aqueous basecoat material (bL2-z).

[0183] The solid content of the basecoat composition (bL2-z) can vary according to the requirements of the individual case. The solid content is mainly determined by the viscosity required for application, more particularly the viscosity required for spraying, so the skilled person can adjust it based on his or her general technical knowledge, optionally with the help of a small amount of exploratory tests. The solid content of the basecoat composition (bL2-z) is preferably 5-70% by weight, more preferably 8-60% by weight, and most preferably 12-55% by weight. The solid content can be determined as described in the examples.

[0184] The basecoat compositions (bL2a) and (bL2-x) are aqueous and preferably contain a moisture content of at least 40% by weight, preferably at least 45% by weight, very preferably at least 50% by weight, in each case based on the total amount of solvents present (i.e. water and organic solvents). Preferably, the moisture content is again 40-95% by weight, more particularly 45-90% by weight, very preferably 50-85% by weight, in each case based on the total amount of solvents present.

[0185] The basecoat compositions used according to the invention can be prepared using customary and known mixing apparatus and mixing techniques for preparing basecoat materials.

[0186] The basecoat layer (BL2a) or (BL2-x) is cured together with the clearcoat layer. In particular, the coating composition used in step (2) of the method according to the invention is not cured separately. Therefore, the basecoat layer (BL2a) or (BL2-x) is preferably not exposed to a temperature above 100° C. for a period of more than 1 minute, and particularly preferably not exposed to a temperature above 100° C. at all.

[0187] The basecoat materials (bL2a) and (bL2-x) are applied in such a way that, after curing in step (4), the basecoat layer (BL2a) or each basecoat layer (BL2-x) each has a film thickness of, for example, 5-50 μm, preferably 6-40 μm, and particularly preferably 7-35 μm. In step (2)(a), a basecoat layer (BL2a) having a relatively high film thickness of 15-50 μm, preferably 15-45 μm, is preferably prepared. In step (2)(b), each basecoat layer (BL2-x) often has a relatively low film thickness, while the film thickness of the entire system is again within the order of magnitude of one basecoat layer (BL2a). For example, in the case of two basecoat layers, the first basecoat layer (BL2-a) preferably has a film thickness of 5-35 μm, more particularly 10-30 μm, the second basecoat layer (BL2-z) preferably has a film thickness of 5-35 μm, more particularly 10-30 μm, and the total film thickness generally does not exceed 50 μm.

[0188] Step (3):

[0189] In step (3) of the method of the present invention, a clear coating (K) is prepared directly on the basecoat layer (BL2a) or the topmost basecoat layer (BL2-z). The preparation is accomplished by applying a clearcoat (k) accordingly. Suitable clearcoats are described, for example, in WO 2006042585A1, WO 2009077182A1 or WO 2008074490A1.

[0190] After application, the clearcoat material (k) or the corresponding clearcoat (K) is preferably flashed and / or intermediately dried at 15 to 35° C. for a period of 0.5 to 30 minutes.

[0191] The clear coating material (k) is applied in such a manner that the film thickness of the clear coating after curing in step (4) is, for example, 15 to 80 μm, preferably 20 to 65 μm, and particularly preferably 25 to 60 μm.

[0192] Step (4):

[0193] In step (4) of the method of the present invention, the basecoat layer (BL2a) and the clearcoat layer (K) or the basecoat layer (BL2-x) and the clearcoat layer (K) are cured together.

[0194] Co-curing is preferably carried out at a temperature of 60-250°C, preferably 80-200°C, more preferably 80-160°C for a period of 5-60 minutes.

[0195] The method of the invention allows the production of multilayer paint systems on substrates without a separate curing step. However, the multilayer paint systems produced by applying the method of the invention have good optical and mechanical properties. If the coating composition of the invention is used in combination with a subsequently applied coating composition comprising metal effect pigments, the angular chromatic effect of the coating comprising metal effect pigments can be increased. The increased angular chromatic effect in the multilayer paint system is due to the presence of polycarboxylic acid PC, anionically stabilized binder B and optional solvent S in the first aqueous basecoat composition (bL2-a) used to produce the first basecoat layer (BL2-a).

[0196] Thus, a basecoat composition comprising metal effect pigments which exceeds the specification with respect to the angular flop effect can still be used as a coating immediately above a coating obtained from the coating composition of the invention. Thus, the use of the coating composition of the invention as first basecoat layer (bL2-a) in the method of the invention reduces the need to set up batches of basecoat compositions containing metal effect pigments which exceed the specification with respect to the angular flop effect obtained. Thus, the method of the invention has an increased environmental balance and efficiency.

[0197] With regard to further preferred embodiments of the process according to the invention, in particular with regard to the basecoat compositions used therein and the components of these basecoat compositions, the statements made with regard to the coating compositions according to the invention are valid mutatis mutandis.

[0198] The multi-layer paint system of the invention:

[0199] After step (4) of the process according to the invention, the multicoat paint system (M) according to the invention is obtained.

[0200] With regard to further preferred embodiments of the multicoat paint system according to the invention, the comments made with regard to the coating composition according to the invention and the method according to the invention apply mutatis mutandis.

[0201] In particular, the present invention is described by the following embodiments:

[0202] Embodiment 1: A water-based coating composition comprising, based on the total weight of the coating composition:

[0203] (a) at least one anionically stabilized binder B,

[0204] (b) at least one coloring pigment P,

[0205] (c) at least one polycarboxylic acid PC, and

[0206] (d) optionally at least one solvent S,

[0207] Therein the coating composition comprises 0% by weight of effect pigments.

[0208] Embodiment 2: An aqueous coating composition according to embodiment 1, wherein the at least one anionically stabilized binder B is present in a total amount of 40 to 95% by weight solids, preferably 50 to 90% by weight solids, more particularly 55 to 85% by weight solids, in each case based on the total binder content of the coating composition.

[0209] Embodiment 3: The aqueous coating composition according to embodiment 1 or 2, wherein the at least one anionically stabilized binder B is selected from aqueous polyurethane-polyurea dispersions comprising anionically stabilized polyurethane-polyurea particles (PPP).

[0210] Embodiment 4: The aqueous coating composition according to embodiment 3, wherein the anionically stabilized polyurethane-polyurea particles (PPP) have an average particle size of 40 to 2,000 nm and a gel fraction of at least 50%, and the polyurethane-polyurea particles (PPP) comprise in each case in reacted form:

[0211] (Z.1.1) at least one polyurethane prepolymer containing anionic groups and / or groups convertible into anionic groups and containing isocyanate groups, and

[0212] (Z.1.2) At least one polyamine comprising two primary amino groups and one or two secondary amino groups.

[0213] Embodiment 5: An aqueous coating composition according to embodiment 3 or 4, wherein the polyurethane-polyurea particles (PPP) have an average particle size of 110-500 nm, more particularly 130-250 nm, and / or a gel fraction of 60-100%, preferably 70-100%, more particularly 80-100%.

[0214] Embodiment 6: The aqueous coating composition according to any one of the preceding embodiments 4 or 5, wherein the prepolymer (Z.1.1) comprises carboxylic acid groups.

[0215] Embodiment 7: An aqueous coating composition according to any one of Embodiments 4 to 6, wherein the prepolymer (Z.1.1) comprises at least one polyester diol, which is prepared using a diol and a dicarboxylic acid, provided that at least 50% by weight, preferably 55-75% by weight, of the dicarboxylic acid is a dimer fatty acid.

[0216] Embodiment 8: The aqueous coating composition according to any one of Embodiments 4 to 7, wherein the polyamine (Z.1.2) consists of one or two secondary amino groups, two primary amino groups and an aliphatic saturated hydrocarbon group.

[0217] Embodiment 9: An aqueous coating composition according to any one of Embodiments 4 or 8, wherein the at least one polyamine (Z.1.2) is selected from diethylenetriamine, 3-(2-aminoethyl)aminopropylamine, dipropylenetriamine, N1-(2-(4-(2-aminoethyl)piperazine-1-yl)ethyl)ethane-1,2-diamine, triethylenetetramine and N,N'-bis(3-aminopropyl)ethylenediamine, preferably diethylenetriamine.

[0218] Embodiment 10: An aqueous coating composition according to any one of Embodiments 3 to 9, wherein the polyurethane-polyurea aqueous dispersion has an electrophoretic mobility of -2.5 to -15 (μm / s) / (V / cm), preferably -2.5 to -10 (μm / s) / (V / cm), more preferably -4 to -8 (μm / s) / (V / cm), and more particularly -6 to -8 (μm / s) / (V / cm) at pH 8.0.

[0219] Embodiment 11: An aqueous coating composition according to any of Embodiments 3 to 10, wherein the aqueous polyurethane-polyurea dispersion is present in a total amount of 1 to 60% by weight solids, preferably 5 to 50% by weight solids, more preferably 10 to 40% by weight solids, very preferably 15 to 40% by weight solids, in each case based on the total binder content of the coating composition.

[0220] Embodiment 12: An aqueous coating composition according to any one of the preceding embodiments, wherein the at least one pigment P is selected from (i) white pigments, such as titanium dioxide, zinc white, zinc sulfide or zinc lithopone; (ii) black pigments, such as carbon black, iron manganese black or spinel black; (iii) color pigments, such as ultramarine green, ultramarine blue, manganese blue, ultramarine violet, manganese violet, iron oxide red, molybdenum red, ultramarine red, iron oxide brown, mixed brown, spinel phase and corundum phase, iron oxide yellow , bismuth vanadate; (iv) organic pigments, such as monoazo pigments, disazo pigments, anthraquinone pigments, benzimidazole pigments, quinacridone pigments, quinophthalone pigments, diketopyrrolopyrrole pigments, dioxazine pigments, indanthrone pigments, isoindoline pigments, isoindolinone pigments, azomethine pigments, thioindigo pigments, metal complex pigments, prinone pigments, perylene pigments, phthalocyanine pigments, aniline black; and (v) mixtures thereof.

[0221] Embodiment 13: An aqueous coating composition according to any of the preceding embodiments, wherein the at least one pigment P is present in a total amount of 1-40% by weight, preferably 2-35% by weight, more preferably 5-30% by weight, in each case based on the total weight of the coating composition.

[0222] Embodiment 14: The aqueous coating composition according to any one of the preceding embodiments, wherein the neutralization level of the at least one polycarboxylic acid PC is at least 5%, preferably at least 10%, more preferably 10-100%.

[0223] Embodiment 15: The aqueous coating composition according to any one of the preceding embodiments, wherein the at least one polycarboxylic acid PC is a dicarboxylic acid.

[0224] Embodiment 16: The aqueous coating composition according to Embodiment 15, wherein the dicarboxylic acid has the general formula (I):

[0225] K +- OOC-R-COO - K +

[0226] in:

[0227] R is a straight chain or branched saturated C4-C 30 Alkyl, linear or branched unsaturated C10 -C 72 Alkyl, cycloalkyl or aryl, preferably a straight chain saturated C7 alkyl,

[0228] K + It is hydrogen or a cation.

[0229] Embodiment 17: The aqueous coating composition according to any of the preceding embodiments, wherein the dicarboxylic acid is selected from azelaic acid, pimelic acid, suberic acid, sebacic acid, dodecanedioic acid and phthalic acid, and mixtures thereof.

[0230] Embodiment 18: An aqueous coating composition according to any of the preceding embodiments, wherein the at least one polycarboxylic acid PC, more particularly a dicarboxylic acid of the general formula (I), is present in a total amount of 0.01-4 wt. %, more preferably 0.02-2 wt. %, more particularly 0.05-1 wt. %, in each case based on the total weight of the coating composition.

[0231] Embodiment 19: The aqueous coating composition according to any one of the preceding embodiments, wherein the at least one solvent S is selected from water, an alkoxy C2-C 10 Alcohols, ketones, esters, amides, methylals, butyrals, 1,3-dioxolane, glycerol formal and mixtures thereof, more particularly alkoxy C2-C 10 alcohol.

[0232] Embodiment 20: An aqueous coating composition according to any one of the preceding embodiments, wherein the aqueous coating composition comprises a total amount of 0.01-15 wt %, preferably 0.05-10 wt %, more preferably 0.1-5 wt %, more particularly 0.2-2 wt % of the at least one solvent S, more particularly water and / or alkoxy C2-C 10 Alcohol, in each case based on the total weight of the coating composition.

[0233] Embodiment 21: An aqueous coating composition according to any one of the preceding embodiments, wherein the coating composition additionally comprises at least one neutralizing agent, the neutralizing agent is preferably selected from inorganic bases, primary amines, secondary amines, tertiary amines and mixtures thereof, more particularly N,N'-dimethylethanolamine.

[0234] Embodiment 22: An aqueous coating composition according to embodiment 20, wherein the at least one neutralizing agent, preferably N,N'-dimethylethanolamine, is present in a total amount of 0.05-5% by weight, preferably 0.05-4% by weight, more preferably 0.05-1% by weight, more particularly 0.05-0.2% by weight, in each case based on the total weight of the coating composition.

[0235] Embodiment 23: An aqueous coating composition according to any one of the preceding embodiments, wherein the coating composition comprises 0 wt% of phyllosilicate, more particularly sodium magnesium silicate and / or lithium aluminum magnesium silicate, and / or polyamide, based on the total weight of the coating composition.

[0236] Embodiment 24: An aqueous coating composition according to any one of the preceding embodiments, wherein the coating composition additionally comprises at least one crosslinking agent, the crosslinking agent is preferably selected from melamine-formaldehyde resins, free and / or blocked polyisocyanates, polycarbodiimides and mixtures thereof, more particularly melamine-formaldehyde resins.

[0237] Embodiment 25: An aqueous coating composition according to embodiment 24, wherein the at least one crosslinker, in particular a melamine-formaldehyde resin, is present in a total amount of 5 to 50% by weight, preferably 7 to 45% by weight, more preferably 10 to 40% by weight, in each case based on the total binder content of the coating composition.

[0238] Embodiment 26: The aqueous coating composition according to any of the preceding embodiments, wherein the composition has a solids content of 15 to 60 wt. %, in each case based on the total weight of the coating composition and measured in accordance with DIN EN ISO 3251 (June 2008).

[0239] Embodiment 27: The aqueous coating composition according to any of the preceding embodiments, having a pH of 7 to 10, more particularly 7 to 9, measured in each case at 23°C.

[0240] Embodiment 28: A method for preparing an aqueous coating composition, comprising:

[0241] (1) providing a solution comprising at least one polycarboxylic acid PC, at least one solvent S and optionally at least one neutralizing agent, and

[0242] (2) Adding the solution provided in step (1) to an aqueous composition comprising at least one anionically stabilized binder B and at least one coloring pigment P.

[0243] Embodiment 29: A method for preparing a multilayer paint system (M) on a substrate (S), comprising the following steps:

[0244] (1) optionally, preparing a cured first coating (S1) on a substrate (S) by applying a composition (Z1) to a substrate (S) and subsequently curing the applied composition (Z1),

[0245] (2) preparing a basecoat layer (BL2a) or at least two directly successive basecoat layers (BL2-x) directly on the first coating layer (S1) by applying a water-based basecoat material (bL2a) directly on the first coating layer (S1) or applying at least two water-based basecoat materials (bL2-x) directly and successively on the first coating layer (S1),

[0246] (3) preparing a clear coating (C) directly on the basecoat layer (BL2a) or the uppermost basecoat layer (BL2-z) by applying a clear coating (cm) directly on the basecoat layer (BL2a) or the uppermost basecoat layer (BL2-z),

[0247] (4) curing the base paint layer (BL2a) and the clear coating layer (C) or the base paint layer (BL2-x) and the clear coating layer (C) together,

[0248] Wherein, at least one of the at least one basecoat material (bL2a) or the at least one basecoat material (bL2-x) comprises the aqueous coating composition according to any one of Embodiments 1 to 27, and / or at least one of the at least one basecoat material (bL2a) or the at least one basecoat material (bL2-x) is an aqueous coating composition prepared by the method described in Embodiment 28.

[0249] Embodiment 30: A method according to Embodiment 29, wherein the substrate (S) is selected from a metal substrate, a metal substrate coated with a cured electrophoretic coating, a plastic substrate, a reinforced plastic substrate, and a substrate comprising metal and plastic components, with a metal substrate being particularly preferred.

[0250] Embodiment 31: A method according to embodiment 29 or 30, wherein the first aqueous basecoat material (bL2-a) comprises a coating composition according to any one of embodiments 1 to 27 or a basecoat material (bL2-a) obtained by the method according to embodiment 28 and wherein the second basecoat material (bL2-z) comprises a basecoat composition containing effect pigments.

[0251] Embodiment 32: A method according to embodiment 31, wherein the water-based basecoat material (bL2-z) comprises at least one hydroxy-functional polymer as a binder, and the at least one hydroxy-functional polymer is selected from polyurethanes, polyesters, copolymers, copolymers thereof and mixtures of these polymers.

[0252] Embodiment 33: A method according to embodiment 31 or 32, wherein the effect pigment is selected from the following group: (i) platelet-shaped metal effect pigments, such as lamellar aluminum pigments, (ii) gold bronze; (iii) bronze oxide and / or iron oxide-aluminum pigments; (iv) pearlescent pigments, such as pearlescent powder; (v) basic lead carbonate; (vi) bismuth oxychloride and / or metal oxide-mica pigments; (vii) lamellar pigments, such as lamellar graphite, lamellar iron oxide; (viii) multilayer effect pigments composed of PVD films; (ix) liquid crystal polymer pigments; and (x) mixtures thereof.

[0253] Embodiment 34: A method according to any of embodiments 31 to 33, wherein the effect pigment is present in the aqueous basecoat material (bL2-z) in a total amount of 1 to 40% by weight, preferably 2 to 35% by weight, more preferably 5 to 30% by weight, in each case based on the total weight of the aqueous basecoat composition (bL2-z).

[0254] Embodiment 35: A method according to any one of embodiments 31 to 34, wherein the basecoat material (bL2-z) comprises at least one crosslinking agent selected from blocked polyisocyanates and / or aminoplast resins, preferably aminoplast resins.

[0255] Embodiment 36: The method according to any one of Embodiments 29-35, wherein the co-curing in step (4) is carried out at a temperature of 60-250°C, preferably 80-200°C, more preferably 80-160°C, for a period of 5-60 minutes.

[0256] Embodiment 37: A multi-layer paint system (M) produced by the method according to any one of Embodiments 29 to 36. Example

[0257] The present invention will now be explained in more detail by using working examples, but the present invention is by no means limited to these working examples. In addition, the terms "part", "%" and "ratio" in the examples represent "part by mass", "mass %" and "mass ratio" respectively, unless otherwise indicated.

[0258] 1. Determination method:

[0259] 1. Solid content (solid, non-volatile matter )

[0260] The non-volatile fraction is determined in accordance with DIN EN ISO 3251 (date: June 2008). It involves weighing 1 g of sample into a pre-dried aluminum pan, drying it in a drying cabinet at 125° C. for 60 minutes, cooling it in a desiccator and then weighing it again. The residue relative to the total amount of sample used corresponds to the non-volatile fraction. If desired, the volume of the non-volatile fraction can optionally be determined in accordance with DIN 53219 (date: August 2009).

[0261] 1.2 Granularity

[0262] The average particle size is determined by dynamic light scattering (photon correlation spectroscopy (PCS)) according to DIN ISO 13321 (date: October 2004). Here, the average particle size means the average particle diameter (Z-average) measured. The measurement is carried out at 25 ± 1 ° C using a Malvern Nano S90 (obtained from Malvern Instruments). The instrument covers a size range of 3-3000nm and is equipped with a 4mW He-Ne laser at 633nm. Each sample is diluted with particle-free deionized water as a dispersion medium and then measured in a 1ml polystyrene cell with a suitable scattering intensity. The evaluation is carried out using a digital correlator with the aid of Zetasizer analysis software, version 7.11 (obtained from Malvern Instruments). The measurement is carried out 5 times and the measurement is repeated for a second freshly prepared sample. The average particle size refers to the arithmetic mean (volume average) of the average particle size. Here, the standard deviation of 5 determinations is ≤4%.

[0263] 1.3 Determination of acid value

[0264] The acid number is determined in accordance with DIN EN ISO 2144 (date: June 2002) using "Method A". The acid number corresponds to the mass of potassium hydroxide in mg required to neutralize 1 g of sample under the conditions specified in DIN EN ISO 2114. The acid number reported here corresponds to the total acid number specified in the DIN standard and is based on the solids content.

[0265] 1.4 Determination of OH value

[0266] The OH value is determined according to DIN 53240-2 (date: November 2007). In this method, OH groups are reacted with excess acetic anhydride by acetylation. The excess acetic anhydride is subsequently cleaved by adding water to form acetic acid, and the total acetic acid is back-titrated with ethanolic KOH solution. The OH value expresses the amount of KOH in mg (based on solids) which is equivalent to the amount of acetic acid bound in the acetylation of 1 g of sample.

[0267] 1.5 Determination of number average molecular weight and weight average molecular weight

[0268] The number average molecular weight (Mn) is determined by gel permeation chromatography (GPC) according to DIN 55672-1 (date: August 2007). In addition to the number average molecular weight, this method can also be used to determine the weight average molecular weight (Mw) and the polydispersity d (ratio of weight average molecular weight (Mw) to number average molecular weight (Mn)). Tetrahydrofuran is used as eluent. The determination is carried out relative to a polystyrene standard. The column material consists of a styrene-divinylbenzene copolymer.

[0269] 1.6 Determination of gel fraction of polyurethane-polyurea particles (PPP)

[0270] In the context of the present invention, the gel fraction of the polyurethane-polyurea particles (PPP) is determined gravimetrically. Here, first, the polymer present is separated from a sample of the aqueous dispersion (initial mass 1.0 g) by freeze drying. After determining the solidification temperature, i.e. the temperature above which the electrical resistance of the sample no longer shows further changes when the temperature is further reduced, the completely frozen sample undergoes its main drying, which is usually carried out at a drying temperature of 10° C. below the solidification temperature in a drying vacuum pressure range of 5-0.05 mbar. Rapid freeze drying of the polymer is achieved by gradually increasing the temperature of the heating surface below the polymer to 25° C.; after a drying time of typically 12 hours, the amount of separated polymer (solids, determined via freeze drying) is constant and no longer undergoes any changes even in the case of prolonged freeze drying. Subsequent drying at a surface temperature below the polymer of 30° C., while the ambient pressure is reduced to the maximum extent (typically between 0.05 and 0.03 mbar), results in optimal drying of the polymer.

[0271] The isolated polymer was subsequently sintered in a forced-air furnace at 130° C. for 1 minute and then extracted in excess tetrahydrofuran (tetrahydrofuran to solids ratio = 300:1) at 25° C. for 24 hours. The insoluble fraction (gel fraction) of the isolated polymer separated on a suitable glass frit was then dried in a forced-air oven at 50° C. for 4 hours and then weighed again.

[0272] It was further determined that at a sintering temperature of 130°C, the sintering time varied between 1 and 20 minutes, and the measured particle gel fraction was independent of the sintering time. Therefore, it can be ruled out that a crosslinking reaction after the separation of the polymer solids further increases the gel fraction.

[0273] The gel fraction determined in this way according to the invention is also referred to as gel fraction (freeze-dried).

[0274] In parallel, the gel fraction (solids content), also referred to below as gel fraction (130° C.), was determined gravimetrically by isolating a polymer sample from the aqueous dispersion (initial mass 1.0 g) for 60 minutes at 130° C. The mass of the polymer was determined and then, analogously to the procedure described above, the polymer was extracted in excess tetrahydrofuran at 25° C. for 24 hours, the insoluble fraction (gel fraction) was separated off, dried and weighed again.

[0275] 1.7 Solubility in water

[0276] The solubility of an organic solvent in water at 20°C is determined as follows. The organic solvent and water are combined and mixed in a suitable glass container, and the mixture is then allowed to equilibrate. The amounts of water and solvent are selected here so that equilibrium produces two phases that are separated from each other. After equilibration, a sample of the aqueous phase (i.e., the phase containing more water than organic solvent) is drawn with a syringe, the sample is diluted with tetrahydrofuran in a ratio of 1 / 10, and then subjected to gas chromatography analysis to determine the solvent fraction (conditions see Section 8, Solvent Content).

[0277] If two phases are not formed, the solvent is miscible with water in any weight ratio, regardless of the amounts of water and solvent. Therefore, such an infinitely water-soluble solvent (e.g. acetone) is not a solvent (Z.2) in any way.

[0278] 1.8 Determination of surface charge by electrophoresis

[0279] The surface charge was determined by measuring with a Zetasizer Nano from Malvern in the pH range of 3-10. The measurement started from the pH of the diluted sample. The pH was adjusted with HCl and / or NaOH. The samples were measured in 10 mmol / l KCl.

[0280] 1.9 degree of neutralization

[0281] The degree of neutralization of component x is calculated from the amount of carboxylic acid groups present in this component (determined by the acid number) and the amount of neutralizer used.

[0282] 1.10 Preparation of multi-layer paint systems

[0283] Cathodic electrodeposition coating ( The galvanized rolled steel test panels were coated with CG 800, BASF Coatings GmbH) and cured at 180° C. for 22 minutes. The resulting dry film thickness of the cured electrophoretic coating obtained was 18 μm.

[0284] On these panels, each water-based basecoat material (BC-C1) to (BC-C8) and (BC-I1) to (BC-I8) was electrostatically applied and dried at 23°C for 4 minutes to obtain a first basecoat layer (BL2-a) having a dry film thickness of 18 μm.

[0285] Subsequently, an aqueous basecoat material (BC-E1) or (BC-E2) containing effect pigments is applied using two subsequent electrostatic application processes in the bell jar method, so that the dry film thickness of the resulting second basecoat layer (BL2-z) is 12-14 μm. The basecoat material (BC-E1) or (BC-E2) is flashed at 23°C for 1 minute and dried at 70°C for 10 minutes.

[0286] After the basecoat material has dried, a commercially available clearcoat (2K clearcoat) is pneumatically applied. Supplied by BASF Coatings GmbH) such that the resulting dry film thickness was 40 μm. The clear coat was flashed at 23° C. for 20 minutes and the resulting multi-coat system was then cured at 140° C. for 20 minutes.

[0287] 1.11 Determination of dry film thickness

[0288] The film thickness was determined according to DIN EN ISO 2808 (date: May 2007), method 12A, using a Measured by 3100-4100 instrument.

[0289] 1.12 Determination of angle-dependent brightness

[0290] To determine the brightness, the coated substrate (i.e. the multi-coat system described in point 1.10) is measured using a spectrophotometer (e.g. an X-Rite MA60B+BA multi-angle spectrophotometer). The surface is illuminated with a light source. Spectral detection is carried out in the visible light range at various angles. Taking into account the standardized spectral values ​​and also the reflection spectrum of the light source used, the spectral determination values ​​obtained in this way can be used to calculate the color value in the CIEL*a*b* color space, where L* characterizes the brightness, a* the red-green value and b* the yellow-blue value.

[0291] The brightness (ΔL), red-green value (Δa) and yellow-blue value (Δb) were calculated using a non-inventive multi-coat paint system comprising BC-C1 or BC-C3 as the first basecoat layer (BL2-a) and BC-E1 or BC-E2 as the second basecoat layer (BL2-z) as a reference.

[0292] 2. Preparation of water-based basecoat materials

[0293] With regard to the formulation ingredients and their amounts described in the table below, the following factors should be considered: When reference is made to commercial products or preparation protocols described elsewhere, independently of the primary name chosen for the ingredient in question, the reference is to exactly the commercial product or exactly the product prepared with the protocol mentioned.

[0294] Thus, when a formulation ingredient has the main name "melamine-formaldehyde resin" and when a commercial product is used to represent this ingredient, the melamine-formaldehyde resin is used exactly in the form of this commercial product. Therefore, if conclusions are to be drawn about the amount of active substance (melamine-formaldehyde resin), any other ingredients present in the commercial product, such as solvents, must be taken into account.

[0295] Thus, if a preparation scheme for a formulation ingredient is mentioned, and if this preparation results in, for example, a polymer dispersion with a defined solids content, then exactly this dispersion is used. The most important factor is not whether the main name chosen is the term "polymer dispersion" or just the active substance, such as "polymer", "polyester" or "polyurethane-modified polyacrylate". This must be taken into account if conclusions are to be drawn about the amount of active substance (polymer).

[0296] 2.1 Preparation of aqueous dispersion of anionically stabilized polyurethane-polyurea particles (D1)

[0297] An aqueous dispersion (D1) of anionically stabilized polyurethane-polyurea particles was prepared according to the preparation example "PD1" on pages 75 and 76 of WO 2018 / 011311A1. The dispersion has an electrophoretic mobility of -6.7 (μm / s) / (V / cm) at pH 8.0 (measured as shown in point 1.8 above).

[0298] 2.2 Preparation of color paste and mica paste

[0299] 2.2.1 Preparation of white pulp P1

[0300] 50 parts by weight of Titan Rutil R-960-38, 11 parts by weight of a polyester prepared according to DE A 40 09 858 A1, column 16, lines 37-59, Example D, 16 parts by weight of a binder dispersion prepared according to EP 0 228 003 B2, page 8, lines 6-18, 1.5 parts by weight of White paste P1 was prepared from P900 (BASF SE), 17 parts by weight of deionized water, 1.5 parts by weight of aqueous N,N′-dimethylethanolamine solution (10% by weight in deionized water) and 3 parts by weight of butyl glycol.

[0301] 2.2.2 Preparation of carbon black slurry P2

[0302] 10.1 parts by weight of carbon black FW 2, 5 parts by weight of a polyester prepared according to DE A 40 09 858 A1, column 16, lines 37-59, Example D, 58.9 parts by weight of a binder dispersion prepared according to patent application WO 92 / 15405, page 14, line 13 to page 15, line 13, 2.2 parts by weight of Carbon black slurry P2 was prepared by mixing P900 (BASF SE), 8.4 parts by weight of deionized water, 7.8 parts by weight of an aqueous solution of N,N′-dimethylethanolamine (10% by weight in deionized water) and 7.6 parts by weight of butanediol.

[0303] 2.2.3 Preparation of yellow paste P3

[0304] Yellow paste P3 was prepared from 17.3 parts by weight of Sicotrans-Gelb L 1916, 18.3 parts by weight of a polyester prepared according to Example D in DE 40 09 858 A1, column 16, lines 37-59, 43.6 parts by weight of a binder dispersion prepared according to EP 022 8003 B2, page 8, lines 6-18, 16.5 parts by weight of deionized water and 4.3 parts by weight of butyl diglycol.

[0305] 2.2.4 Preparation of red pulp P4

[0306] 49.7 parts by weight of an acrylated polyurethane dispersion prepared according to "Bendemitteldispersion A" (polymer A) of patent application WO 91 / 15528, 12 parts by weight of red (BASF SE), 3 parts by weight Red paste P4 was prepared from P900 (BASF SE), 2 parts by weight of butyl glycol, 1 part by weight of N,N′-dimethylethanolamine aqueous solution (10% by weight in deionized water) and 32.3 parts by weight of deionized water.

[0307] 2.2.4 Preparation of blue paste P5

[0308] 69.8 parts by weight of an acrylated polyurethane dispersion prepared according to patent application WO 91 / 15528 "Bindemitteldispersion A" (polymer A), 12.5 parts by weight of Paliogen Blue L 6482 (BASF SE), 1.2 parts by weight of Blue paste P5 was prepared from P900 (BASF SE), 1.5 parts by weight of an aqueous solution of N,N′-dimethylethanolamine (10% by weight in deionized water) and 15 parts by weight of deionized water.

[0309] 2.2.5 Preparation of mica slurry MI1

[0310] A mica slurry was prepared by mixing 1.5 parts by weight of butyl glycol, 1.5 parts by weight of a polyester prepared according to DE 4 009 858 A, column 16, lines 37-59, and 1.3 parts by weight of Mica Mearlin ext. Super Orange 339Z (Merck KGaA) using a stirring apparatus.

[0311] 2.2.6 Preparation of mica slurry MI2

[0312] A mica slurry was prepared by mixing 1.5 parts by weight of butyl glycol, 1.5 parts by weight of a polyester prepared according to DE 4 009 858 A, column 16, lines 37-59, Example D, and 1.3 parts by weight of Iriodin 9225 SQB (Merck KGaA) using a stirring apparatus.

[0313] 2.3 Preparation of solutions (SOL1) to (SOL11) of different carboxylic acids in solvent S

[0314] Solutions SOL1 to SOL11 were prepared by mixing corresponding amounts of carboxylic acid, neutralizing agent, and solvent S as listed in Table 1.

[0315] Table 1: Compounds of solutions SOL1 to SOL11 (amounts given in % by weight)

[0316]

[0317] 1) 10 wt% N,N'-dimethylethanolamine aqueous solution

[0318] 2.4 Preparation of water-based basecoat materials BC-C1 to BC-C7 (comparison)

[0319] Waterborne basecoat materials BC-C1 to BC-C7 were prepared by mixing the ingredients listed in Table 2 in the stated order. After stirring for 10 minutes, the mixture was then adjusted to pH 8.0 with deionized water and N,N'-dimethylethanolamine and adjusted to 1000 s -1 The spray viscosity at shear number is 85 mPa*s, measured at 23°C using a rotational viscometer (Rheolab QC instrument with C-LTD80 / QC control system, obtained from Anton Paar). BC-C1 to BC-C3 do not contain any di- or monocarboxylic acids. BC-C4 to BC-C7 each contain a different monocarboxylic acid.

[0320] Table 2: Compounding materials for waterborne basecoat materials BC-C1 to BC-C7

[0321]

[0322]

[0323] 1)Prepared according to Example BM2 on page 45 of WO 2016 / 116299

[0324] 2) Prepared according to Example BE 1 on page 28, lines 13 to 33 of WO 2014 / 033135A1

[0325] 2.5 Preparation of Water-Based Base Coat Materials BC-I1 to BC-I8 (Present Embodiment)

[0326] The waterborne coatings BC-I1 to BC-I8 of the present invention are prepared by adding corresponding amounts of polycarboxylic acid solutions SOL1 to SOL7 prepared according to point 2.3 to corresponding amounts of comparative waterborne basecoat materials BC-C1 to BC-C3 under stirring (see Table 3).

[0327] Table 3: Compounding materials of water-based basecoat materials BC-I3 to BC-I8 of the present invention (amount in weight %)

[0328]

[0329] 2.6 Preparation of water-based basecoat materials BC-E1 and BC-E2 containing effect pigments

[0330] The ingredients listed under "Aqueous Phase" in Table 4 were mixed in the order described to obtain an aqueous mixture. In addition, the ingredients listed under "Organic Phase" in Table 2 were mixed in the order described to obtain an organic mixture. The organic mixture was added to the aqueous mixture under stirring and stirring was continued for 10 minutes. The mixture was then adjusted to pH 8.0 using deionized water and N,N'-dimethylethanolamine and heated for 1000 s. -1 The spray viscosity is 65 mPa*s under a shear load of 1000 nm, measured at 23° C. using a rotational viscometer (Rheolab QC instrument with C-LTD80 / QC control system from Anton Paar or Rheomat RM 180 from Mettler-Toledo).

[0331] Table 4: Compounding materials of water-based basecoat material BC-E (amounts in wt%)

[0332]

[0333] 1) Prepared according to WO 92 / 15405 (page 14, line 13 to page 15, line 28),

[0334] 2) Prepared according to DE 4 009 858 A, column 16, lines 37-59, Example D,

[0335] 3) Prepared according to DE 4 437 535 A1, page 7, line 55 to page 8, line 23.

[0336] 3. Viscosity measurement

[0337] The effect of adding polycarboxylic acid (azelaic acid) on the viscosity of water-based coatings can be measured by using The Rheostress device measures the oscillatory viscosity to determine:

[0338] 0.5 ml of the corresponding aqueous coating was added to the measuring plate of the apparatus and the mixture was stirred for 1000 s. -1 The shear stress was then reduced to 1 s -1 , and the progression of the sol curve is measured as a function of time. The important parameter is the shear stress reduction to 1 s -1 Values ​​obtained after 1 and 8 min.

[0339] The obtained results and the solid content of the waterborne basecoat material are shown in Table 5.

[0340] Table 5: Viscosity of the prepared water-based basecoat material

[0341]

[0342] A solution of a polycarboxylic acid in a solvent S (azelaic acid (BC-I1, BC-I2, BC-I3), pimelic acid (BC-I4), suberic acid (BC-I5), sebacic acid (BC-I6), dodecanedioic acid (BC-I7) and phthalic acid (BC-I8)) is added to an aqueous basecoat composition comprising at least one anionically stabilized binder B and a color pigment P, which results in a reduction of the shear stress to 1 s compared to aqueous basecoat compositions not comprising the polycarboxylic acid PC (BC-C1 to BC-C3) or aqueous basecoat compositions comprising monocarboxylic acids (BC-C4 to BC-C7). -1 After 1000s, the viscosity increases significantly. -1 The spraying viscosity at 100% remained almost unchanged, so that the coating of the present invention has good application performance. Due to this significant increase in viscosity, the water-based coatings BC-I1 to BC-I8 of the present invention have better leveling properties than the comparative coatings without any polycarboxylic acid (BC-C1 to BC-C3) or the comparative coatings containing monocarboxylic acids (BC-C4 to BC-C7).

[0343] 4. Brightness measurement

[0344] The brightness of the multicoat paint systems produced according to point 1.10 was measured as described in point 1.12.

[0345] 4.1 Multilayer coatings containing BC-E1 as the second metal coating (BL2-z)

[0346] Relative to the reference (a multilayer paint system comprising BC-C1 or BC-C2 as the first basecoat layer (BL2-a) and BC-E1 as the second basecoat layer (BL2-z)), the weighted color values ​​of the multilayer paint system of the present invention are shown in Table 6.

[0347] Table 6: Gloss measurements of multi-coat paint systems

[0348]

[0349] A solution of a polycarboxylic acid (azelaic acid) in a solvent S is added to an aqueous basecoat composition comprising at least one anionically stabilized binder B and colored pigments P (BC-I1 and BC-I2), which results in a significantly increased angular-variant effect of the directly adjacent basecoat layer comprising metallic effect pigments, as compared to a multi-layer coating system in which no polycarboxylic acid is used in the first basecoat layer (BC-C1 or BC-C2), due to the large positive ΔL values ​​obtained at measuring angles of 15° and 25°.

[0350] 4.2 Multilayer coatings containing BC-E2 as the second metal coating (BL2-z)

[0351] The weighted color values ​​of the multi-layer paint system of the present invention obtained relative to the reference (a multi-layer paint system comprising BC-C3 as the first basecoat layer (BL2-a) and BC-E2 as the second basecoat layer (BL2-z)) are shown in Table 7.

[0352] Table 7: Gloss measurements of multi-coat paint systems

[0353]

[0354]

[0355] The addition of solutions of different polycarboxylic acids (azelaic acid, pimelic acid, suberic acid, sebacic acid, dodecanedioic acid and phthalic acid) in solvent S to aqueous basecoat compositions (BC-I3 and BC-I8) comprising at least one anionically stabilized binder B and color pigments P resulted in an increased flop effect in the directly overlying basecoat layer comprising metallic effect pigments, due to the positive ΔL values ​​obtained at a measuring angle of 15°, compared to multicoat paint systems in which monocarboxylic acids were used in the first basecoat layer (BC-C3). Furthermore, no significant flop effect was obtained when using comparative basecoat compositions containing monocarboxylic acids (BC-C4 to BC-C7), since no positive ΔL values ​​were obtained at 15°.

Claims

1. A method for producing a multi-coat paint system (M) on a substrate (S), wherein The following steps are involved: (1) optionally, preparing a cured first coating (S1) on a substrate (S) by applying a composition (Z1) to a substrate (S) and subsequently curing the applied composition (Z1), (2) by applying two aqueous basecoat materials (bL2-a, bL2-z) directly and successively onto the first coating layer (S1), and preparing two directly successive basecoat layers (BL2-a, bL2-z) directly on the first coating layer (S1); BL2-z), (3) preparing a clear coating (C) directly on the uppermost basecoat layer (BL2-z) by applying a clear coating (cm) directly on the uppermost basecoat layer (BL2-z), (4) The base paint layer (BL2-a, BL2-z) and the clear coating layer (C) are cured together, The first basecoat material (bL2-a) comprises an aqueous coating composition, which comprises, based on the total weight of the coating composition: (a) at least one anionically stabilized binder B, (b) at least one coloring pigment P, (c) at least one polycarboxylic acid PC, wherein the at least one polycarboxylic acid PC is a dicarboxylic acid selected from azelaic acid, pimelic acid, suberic acid, sebacic acid, dodecanedioic acid and phthalic acid and mixtures thereof, and (d) optionally at least one solvent S, wherein the coating composition comprises 0% by weight of effect pigments, The second basecoat material (bL2-z) contains at least one effect pigment.

2. The process according to claim 1, wherein the at least one anionically stabilized binder B is present in a total amount of 40 to 95% by weight solids, based in each case on the total binder content of the coating composition.

3. The process according to claim 2, wherein the at least one anionically stabilized binder B is present in a total amount of 50 to 90% by weight solids, based in each case on the total binder content of the coating composition.

4. The process according to claim 3, wherein the at least one anionically stabilized binder B is present in a total amount of 55 to 85% by weight solids, based in each case on the total binder content of the coating composition. 5 . The process according to claim 1 , wherein the at least one anionically stabilized binder B is selected from aqueous polyurethane-polyurea dispersions comprising anionically stabilized polyurethane-polyurea particles.

6. The process according to claim 5, wherein the anionically stabilized polyurethane-polyurea particles have an average particle size of 40 to 2,000 nm and a gel fraction of at least 50%, and the polyurethane-polyurea particles comprise in each case in reacted form: (Z.1.1) at least one polyurethane prepolymer containing anionic groups and / or groups convertible into anionic groups and containing isocyanate groups, and (Z.1.2) At least one polyamine comprising two primary amino groups and one or two secondary amino groups.

7. The process according to claim 5, wherein the aqueous polyurethane-polyurea dispersion is present in a total amount of 1 to 60% by weight solids, based in each case on the total binder content of the coating composition.

8. The process according to claim 7, wherein the aqueous polyurethane-polyurea dispersion is present in a total amount of 5 to 50% by weight solids, based in each case on the total binder content of the coating composition.

9. The process according to claim 8, wherein the aqueous polyurethane-polyurea dispersion is present in a total amount of 10 to 40% by weight solids, based in each case on the total binder content of the coating composition.

10. The process according to claim 9, wherein the aqueous polyurethane-polyurea dispersion is present in a total amount of 15 to 45% by weight solids, based in each case on the total binder content of the coating composition.

11. The process according to any one of claims 1 to 4, wherein the at least one colored pigment P is present in a total amount of 1 to 40% by weight, based in each case on the total weight of the coating composition. 12 . The process according to claim 11 , wherein the at least one colored pigment P is present in a total amount of 2 to 35% by weight, based in each case on the total weight of the coating composition.

13. The process according to claim 12, wherein the at least one colored pigment P is present in a total amount of 5 to 30% by weight, based in each case on the total weight of the coating composition.

14. The method according to any one of claims 1 to 4, wherein the neutralization level of the at least one polycarboxylic acid PC is at least 5%.

15. The method according to claim 14, wherein the neutralization level of the at least one polycarboxylic acid PC is at least 10%.

16. The method according to claim 15, wherein the neutralization level of the at least one polycarboxylic acid PC is 10-100%.

17. The process according to any one of claims 1 to 4, wherein the at least one polycarboxylic acid PC is present in a total amount of 0.01 to 4% by weight, based in each case on the total weight of the coating composition.

18. The process according to claim 17, wherein the at least one polycarboxylic acid PC is present in a total amount of 0.02 to 2% by weight, based in each case on the total weight of the coating composition.

19. The process according to claim 18, wherein the at least one polycarboxylic acid PC is present in a total amount of 0.05 to 1% by weight, based in each case on the total weight of the coating composition.

20. The method according to any one of claims 1 to 4, wherein the at least one solvent S is selected from water, alkoxy C 2 -C 10 Alcohols, ketones, esters, amides, methylal, butyral, 1,3-dioxolane, glycerol formal and mixtures thereof.

21. The method according to claim 20, wherein the at least one solvent S is an alkoxy C 2 -C 10 Alcohol and / or water.

22. Multicoat paint system obtainable by the process according to any one of claims 1 to 21.