Device and method for chemical plating of inner wall of aluminum alloy gas cylinder

By designing the electroless plating device of the inner wall of the aluminum alloy gas cylinder with the plating solution circulation and automatic control system, the problems of complex operation and unstable plating are solved, and a uniform, bright and corrosion-resistant plating layer is achieved, which improves product quality and production efficiency.

CN115058705BActive Publication Date: 2024-11-15INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210481758.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-05
Publication Date
2024-11-15
Estimated Expiration
2042-05-05

AI Technical Summary

Technical Problem

The electroless plating process of the inner wall of the aluminum alloy gas cylinder is complicated and inconvenient to operate, and lacks efficient and convenient devices and methods, resulting in unstable circulation of the plating solution and cumbersome reaction process, which affects product quality.

Method used

A device including an electroless plating system, heating system, control system and post-treatment system was designed, using a plating liquid circulation system and an automatic control system, spraying the treatment liquid evenly through the liquid sprayer, and the circulation pump controls the processing liquid circulation, the timer and The speed governor ensures the reaction time and speed of each step, forming a stable electroless plating environment.

Benefits of technology

The coating with uniform, bright and corrosion-resistant inner wall of the aluminum alloy cylinder is realized, with controllable thickness, simplified the process flow, improved production efficiency, reduced costs, and ensured the purity and concentration of the gas stored in the cylinder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003627766310000011
    Figure HDA0003627766310000011
  • Figure HDA0003627766310000021
    Figure HDA0003627766310000021
Patent Text Reader

Abstract

The present invention belongs to surface treatment technology, specifically, a device and method for chemical plating of the inner wall of an aluminum alloy gas cylinder. The device includes a chemical plating system, a heating system, a control system and a post-processing system. When in use, the device includes six steps: activation, water washing, pre-plating, chemical plating, water washing and drying. The present invention solves the problems of inconvenient operation and difficult control of the plating solution during chemical plating of the inner wall of the aluminum alloy gas cylinder by introducing a plating solution injection and circulation system in the chemical plating process, thereby improving production efficiency. At the same time, a smooth, uniform and corrosion-resistant coating can be obtained on the inner wall of the aluminum alloy gas cylinder, which can ensure the purity and concentration of the gas stored in the aluminum alloy gas cylinder and improve the product quality of the aluminum alloy gas cylinder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the surface treatment technology, in particular to a device and method for chemical plating of the inner wall of an aluminum alloy gas cylinder. Background Art

[0002] Chemical plating technology can be used to treat the surface of workpieces with complex shapes, and has been widely used in aluminum alloy devices. After being treated with chemical plating, aluminum alloys can have better corrosion resistance and smoother surfaces, giving aluminum alloys more functionality. For aluminum alloy gas cylinders, after the inner wall is treated with chemical plating, the original rough oxide surface is replaced by a smooth and corrosion-resistant metal coating. On the one hand, it can reduce the adsorption of gas on the inner wall of the gas cylinder to ensure that the concentration of stored gas remains unchanged; on the other hand, it can slow down the corrosion of corrosive gases on the inner wall of the aluminum alloy gas cylinder to ensure the purity of the stored gas. However, there are currently few chemical plating processes for the inner wall of aluminum alloy gas cylinders. At the same time, there are many differences between the chemical plating of the inner wall of the gas cylinder and the chemical plating process of conventional parts, such as the small mouth of the gas cylinder is inconvenient to operate, the inner wall of the gas cylinder is invisible during the plating process, the area of ​​the inner wall of the gas cylinder is too large compared with the volume of the treatment liquid in the gas cylinder, etc., which makes the chemical plating process of the inner wall of the aluminum alloy gas cylinder more complicated.

[0003] In response to the problems existing in the chemical plating of the inner wall of aluminum alloy, a very simple aluminum alloy chemical plating technology (patent publication number CN113403614A) that only requires a one-step pretreatment has been developed in the early stage, which shortens the process flow. However, when chemically plating the inner wall of the aluminum alloy gas cylinder, a feasible, efficient and easy-to-operate device and operation method are still needed. Summary of the invention

[0004] In view of the above problems, the present invention aims to provide a device and method for chemical plating of the inner wall of aluminum alloy gas cylinders. By introducing an injection and circulation system for the treatment liquid in the chemical plating process, various problems existing in the chemical plating of the inner wall of aluminum alloy gas cylinders are solved. At the same time, the device includes multiple automatic control processes, which can improve production efficiency, have high scalability, save costs, etc. After the inner wall of the gas cylinder is treated with chemical plating using this technology, the quality of the gas stored in the gas cylinder will be greatly improved, the application scope of the gas cylinder will be expanded, and it will have important driving significance for improving the product quality of related industries.

[0005] In order to achieve the object of the present invention, the technical solution of the present invention is:

[0006] A device for chemical plating of the inner wall of an aluminum alloy gas cylinder, the device comprises a chemical plating system, a heating system, a control system and a post-processing system, and the specific structure is as follows:

[0007] The chemical plating system includes an activation treatment tank, a water washing treatment tank, a pre-plating treatment tank, a chemical plating treatment tank, a gas cylinder rack, and a liquid sprayer. The liquid sprayer is tubular and extends into the aluminum alloy gas cylinder. The treatment liquid is evenly sprayed into the aluminum alloy gas cylinder through the liquid sprayer. The four treatment tanks are discharged in sequence. The gas cylinder rack is placed on each treatment tank when in use. The liquid sprayer is connected to the multi-way water pipe joint at one end of the liquid outlet pipe of the circulation pump.

[0008] The heating system includes a heating rod, a thermal resistor, and a secondary instrument, which are used to control the temperature of each step of the chemical plating process; each treatment tank that needs to be heated is equipped with a heating rod, a thermal resistor, and a secondary instrument connected to the thermal resistor. The heating rod is placed in the aqueous solution for water bath heating, the thermal resistor is vertically installed in the water bath in the treatment tank, and the secondary instrument is connected to the thermal resistor through an electric wire and installed outside the treatment tank;

[0009] The control system includes a circulation pump, an automatic controller, a speed regulator, a timer, and a multi-way water pipe joint. Each treatment tank is equipped with a control system for controlling the chemical plating reaction process and the circulation of the treatment liquid in the reaction; the automatic controller is provided with a speed regulator and a timer, and the speed regulator is connected to the circulation pump through the automatic controller to control the flow rate of the circulation pump when the treatment liquid circulates; a multi-way water pipe joint is installed at one end of the liquid outlet pipe of the circulation pump, and a liquid sprayer is installed at the outlet end of the multi-way water pipe joint;

[0010] The post-processing system includes a water tank, a liquid sprayer, and a drying box. One end of the water outlet pipe on the water tank is connected to the liquid sprayer and extends into the bottle mouth of the aluminum alloy gas cylinder in the water tank. The washed aluminum alloy gas cylinder is placed in the drying box for drying.

[0011] The device for chemical plating the inner wall of an aluminum alloy gas cylinder has four processing tanks, all of which are inner and outer double-tank nested structures that can be heated in a water bath, and are used to heat and hold different processing liquids. Each processing tank corresponds to a processing step, and the inner tank of each processing tank holds different processing liquids. An aqueous solution for water bath heating is installed between the outer tank and the inner tank of each processing tank.

[0012] The device for chemically plating the inner wall of the aluminum alloy gas cylinder, the gas cylinder rack is used to place and fix the aluminum alloy gas cylinder, so that the bottle body of the aluminum alloy gas cylinder remains stable during each step of the reaction process.

[0013] In the device for chemically plating the inner wall of an aluminum alloy gas cylinder, the heating rod is used to heat the treatment tanks to the required temperatures, and the thermal resistor and the secondary instrument are used to measure and control the temperatures of the four treatment tanks.

[0014] The device for chemically plating the inner wall of an aluminum alloy gas cylinder, the circulating pump is used to inject the treatment liquid into the aluminum alloy gas cylinder to be treated, and the circulating pump is an acid and alkali resistant circulating pump.

[0015] The device for chemically plating the inner wall of an aluminum alloy gas cylinder comprises an automatic controller for controlling a circulation pump to inject a treatment liquid into the aluminum alloy gas cylinder and stop after the treatment liquid is filled; a timer for measuring the reaction time of each step in the reaction process; and a multi-way water pipe joint for adjusting the number of liquid outlets of the circulation pump according to the number of aluminum alloy gas cylinders that are simultaneously subjected to chemical plating treatment.

[0016] The device for chemical plating the inner wall of the aluminum alloy gas cylinder, the water tank is used to clean the aluminum alloy gas cylinder after chemical plating, the inner wall of the aluminum alloy gas cylinder is rinsed with clean water to take away the residual treatment liquid on the bottle wall, the water is evenly sprayed on the inner wall of the aluminum alloy gas cylinder through the sprayer, and the drying box is used to completely remove the residual water on the inner wall of the aluminum alloy gas cylinder after washing.

[0017] A method for chemical plating of the inner wall of an aluminum alloy gas cylinder, comprising activation, water washing, pre-plating, chemical plating, water washing, and drying, the specific steps of which are as follows:

[0018] 1) Preparation: Wrap the outer wall of the aluminum alloy gas cylinder to be treated with plastic wrap to prevent the outer wall of the aluminum alloy gas cylinder from participating in the chemical plating process;

[0019] 2) Activation: Place the aluminum alloy gas cylinder in the gas cylinder rack on the activation tank, operate the automatic controller, and the circulation pump will inject the activation treatment liquid placed in the activation treatment tank into the aluminum alloy gas cylinder to be treated. After the activation treatment liquid is filled, the circulation pump automatically stops, and then the timer starts timing; during the activation process, the activation treatment liquid in the aluminum alloy gas cylinder does not need to be circulated, so that the inner wall of the aluminum alloy gas cylinder is fully activated; after the timer prompts that the time is up, the activation treatment liquid in the aluminum alloy gas cylinder is poured back into the activation treatment tank by the circulation pump; during the activation process, the temperature of the activation treatment liquid in the activation treatment tank is 35-65°C, and the activation time is 1-10min;

[0020] 3) Water washing: Place the aluminum alloy gas cylinder in a water washing tank, and use a circulating pump to spray the water in the water washing tank into the aluminum alloy gas cylinder through a liquid sprayer for repeated washing 2 to 5 times; until the residual activation treatment liquid on the bottle wall is completely removed. The water temperature in the water washing tank used for washing during the water washing process is 50 to 80°C, and the water washing process is completed as soon as possible within 3 minutes to avoid oxidation of the inner wall of the evenly activated aluminum alloy gas cylinder;

[0021] 4) Pre-plating: Place the aluminum alloy gas cylinder on the gas cylinder rack of the pre-plating treatment tank, operate the automatic controller, and the circulating pump will inject the pre-plating treatment liquid placed in the pre-plating treatment tank into the aluminum alloy gas cylinder to be plated. After the pre-plating treatment liquid is filled, the circulating pump will automatically stop and the timer will start timing. During this process, the pre-plating treatment liquid in the aluminum alloy gas cylinder does not need to be circulated, so that the inner wall of the aluminum alloy gas cylinder is quickly deposited with a full coating; after the timer prompts that the time is up, the pre-plating treatment liquid in the aluminum alloy gas cylinder is poured back into the pre-plating treatment tank by the circulating pump; during the pre-plating process, the treatment liquid temperature in the pre-plating treatment tank is 70-90°C, and the pre-plating process is 5-30min;

[0022] 5) Chemical plating: Place the aluminum alloy gas cylinder on the gas cylinder rack of the chemical plating treatment tank, operate the automatic controller, and the circulation pump will inject the chemical plating treatment solution placed in the chemical plating treatment tank into the aluminum alloy gas cylinder. After the chemical plating treatment solution is filled, the circulation pump will automatically stop and the timer will start timing; use the speed regulator to adjust the circulation pump speed to 0.01m / s. 3 / h~0.04m 3 / h, to ensure a suitable circulation speed of the chemical plating treatment solution; the automatic controller controls the circulation pump to automatically update the chemical plating treatment solution in the aluminum alloy cylinder during the chemical plating process; after the timer prompts that the time is up, the chemical plating treatment solution in the aluminum alloy cylinder is returned to the chemical plating treatment tank by the circulation pump; during the chemical plating process, the temperature of the chemical plating treatment solution in the plating tank is 60-90°C, and the chemical plating time is 20-60min;

[0023] 6) Water washing: Take out the aluminum alloy gas cylinder and place it in the water tank, and use a sprayer connected to the tap water pipe to fully rinse the aluminum alloy gas cylinder until the residual chemical plating treatment liquid on the bottle wall is completely removed;

[0024] 7) Drying: Place the aluminum alloy gas cylinder in a drying oven at a temperature of 50-100°C for 10-30 minutes to remove the residual moisture on the inner wall of the aluminum alloy gas cylinder.

[0025] In the method for chemical plating the inner wall of an aluminum alloy gas cylinder, all automatic controllers and timers are pre-set with time according to the corresponding treatment tanks.

[0026] In the method for chemical plating the inner wall of an aluminum alloy gas cylinder, the chemical plating treatment liquid inside the aluminum alloy gas cylinder circulates once within 10 to 15 minutes during the chemical plating process to ensure the stability of the chemical plating treatment liquid and allow the reaction process to proceed normally; during the circulation of the chemical plating treatment liquid, the injection pipe of the circulation pump is placed at the bottom of the aluminum alloy gas cylinder, and after the new chemical plating treatment liquid is injected, the original chemical plating treatment liquid in the bottle automatically overflows from the bottle mouth and flows back into the plating tank, and after the circulation pump is filled with the new chemical plating treatment liquid, the automatic controller controls the circulation pump to stop working.

[0027] The design concept of the present invention is:

[0028] First, for the chemical plating of the inner wall of aluminum alloy gas cylinders, there are problems such as complex operation process, invisible state during the whole process, small space in the gas cylinder, and excessive loading. The present invention designs a plating solution circulation system to solve the problems of excessive loading, unstable reaction process, easy decomposition of plating solution, etc. Secondly, the chemical plating process is complicated and cumbersome, and too many factors need to be controlled at the same time. The present invention designs an automatic control system, which can well integrate the above complex processes efficiently, so that the entire production process can be carried out in an orderly manner. The device with a certain degree of automation also reduces the number of production personnel and saves factory costs.

[0029] The present invention has the following advantages and beneficial effects:

[0030] 1. The process provided by the present invention can form a coating with good bonding strength, high brightness and uniform surface on the inner wall of the aluminum alloy gas cylinder, and the thickness can be controlled within the range of 5 to 20 μm, meeting the actual use needs.

[0031] 2. The device and method provided by the present invention integrate the complex chemical plating process, making the originally cumbersome process more professional and orderly.

[0032] 3. The device provided by the present invention is provided with an automatic plating solution circulation system, which prevents the plating solution from decomposing, makes the reaction process more stable, and simplifies the complicated operation process of manually replacing the plating solution.

[0033] 4. In addition to being applicable to chemical plating of the inner wall of aluminum alloy gas cylinders, the present invention is also applicable to the chemical composite plating process of the inner wall of aluminum alloy gas cylinders.

[0034] 5. The present invention can obtain a smooth, uniform, corrosion-resistant coating on the inner wall of the gas cylinder, which can ensure the purity and concentration of the gas stored in the gas cylinder and improve the product quality of the aluminum alloy gas cylinder. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 . A schematic diagram of a device for chemical plating and chemical composite plating of the inner wall of an aluminum alloy gas cylinder. In the figure, 1 is an activation treatment tank, 2 is a water washing treatment tank, 3 is a pre-plating treatment tank, 4 is a chemical plating treatment tank, 5 is a gas cylinder rack, 6 is a liquid sprayer, 7 is a heating rod, 8 is a thermal resistor, 9 is a secondary instrument, 10 is a circulating pump, 11 is an automatic controller, 12 is a speed regulator, 13 is a timer, 14 is a multi-way water pipe joint, 15 is a water tank, 16 is a drying box, 17 is a liquid outlet pipe, and 18 is an aluminum alloy gas cylinder.

[0036] Figure 2 . Macroscopic photograph of the chemical plating on the inner wall of the aluminum alloy gas cylinder in Example 1 (conditions in Example 1). DETAILED DESCRIPTION

[0037] like Figure 1 As shown, the device for chemical plating of the inner wall of an aluminum alloy gas cylinder of the present invention is composed of a chemical plating system, a heating system, a control system and a post-processing system, and mainly includes: an activation treatment tank 1, a water washing treatment tank 2, a pre-plating treatment tank 3, a chemical plating treatment tank 4, a gas cylinder rack 5, a liquid sprayer 6, a heating rod 7, a thermal resistor 8, a secondary instrument 9, a circulating pump 10, an automatic controller 11, a speed regulator 12, a timer 13, a multi-way water pipe joint 14, a water tank 15, a drying box 16, a liquid outlet pipe 17, and an aluminum alloy gas cylinder 18. The specific structure is as follows:

[0038] The chemical plating system includes four treatment tanks (activation treatment tank 1, water washing treatment tank 2, pre-plating treatment tank 3, chemical plating treatment tank 4), gas cylinder rack 5, and liquid sprayer 6. The main operations of chemical plating treatment are all carried out in this system. The four treatment tanks are all nested structures with inner and outer double tanks that can be heated in a water bath, which are used to heat and hold different treatment liquids. Each treatment tank corresponds to a treatment step. The inner tank of each treatment tank holds different treatment liquids, and the outer tank and inner tank of each treatment tank are filled with aqueous solutions for water bath heating; the gas cylinder rack 5 is used to place and fix the aluminum alloy gas cylinder 18, so that the body of the aluminum alloy gas cylinder 18 remains stable during each step of the reaction process; the liquid sprayer 6 is tubular and can be inserted into the small-caliber aluminum alloy gas cylinder 18. The liquid sprayer 6 can evenly spray the treatment liquid in the aluminum alloy gas cylinder 18. The four processing tanks are arranged in sequence. The gas cylinder rack 5 is placed on each processing tank when in use and corresponds to the inner tank of the processing tank. The gas cylinder rack 5 can be removed when not in use. The liquid sprayer 6 is connected to the multi-way water pipe joint 14 at one end of the liquid outlet pipe 17 of the circulation pump 10. The gas cylinder rack 5 and the processing tank can be adjusted according to the number and size of the aluminum alloy gas cylinders 18 to be processed.

[0039] The heating system includes a heating rod 7, a thermal resistor 8, and a secondary instrument 9, which are used to control the temperature of each step of the chemical plating process. The heating rod 7 is used to heat the treatment tank to the required temperature, and the thermal resistor 8 and the secondary instrument 9 are used to measure and control the temperature of the four treatment tanks. Each treatment tank that needs to be heated is equipped with a heating rod 7, a thermal resistor 8, and a secondary instrument 9 connected to the thermal resistor 8. The heating rod 7 is placed in the aqueous solution for water bath heating, the thermal resistor 8 is vertically installed in the water bath in the treatment tank, and the secondary instrument 9 is connected to the thermal resistor 8 through an electric wire and installed outside the treatment tank. The thermal resistor 8 and the secondary instrument 9 are connected in series to test the water temperature after heating.

[0040] The control system includes a circulation pump 10, an automatic controller 11, a speed regulator 12, a timer 13, and a multi-way water pipe joint 14. Each treatment tank is equipped with a control system for controlling the chemical plating reaction process and the circulation of the treatment liquid in the reaction. The circulation pump 10 is used to inject the treatment liquid into the aluminum alloy gas cylinder 18 to be treated, and the circulation pump 10 is an acid and alkali resistant circulation pump. The automatic controller 11 is provided with a speed regulator 12 and a timer 13. The speed regulator 12 is connected to the circulation pump 10 through the automatic controller 11, and the flow rate of the circulation pump 10 when the treatment liquid circulates can be controlled. A multi-way water pipe joint 14 is installed at one end of the liquid outlet pipe 17 of the circulation pump 10, and a liquid sprayer 6 is installed at the outlet end of the multi-way water pipe joint 14. The multi-way water pipe joint 14 can adjust the number of liquid outlets of the circulation pump 10 according to the number of aluminum alloy gas cylinders 18 that are simultaneously subjected to chemical plating treatment. The automatic controller 11 is used to control the circulation pump 10 to inject the treatment liquid into the aluminum alloy gas cylinder 18, and stop after the treatment liquid is filled. The timer 13 is used to measure the reaction time of each step in the reaction process.

[0041] The post-processing system includes a water tank 15, a liquid sprayer 6, and a drying box 16. One end of the water outlet pipe on the water tank 15 is connected to the liquid sprayer, and the liquid sprayer can be extended into the bottle mouth of the aluminum alloy gas cylinder 18 in the water tank 15. The aluminum alloy gas cylinder 18 after water washing is placed in the drying box 16 for drying. The water tank 15 is used to clean the aluminum alloy gas cylinder 18 after chemical plating treatment, and the inner wall of the aluminum alloy gas cylinder 18 is rinsed with clean water to remove the residual treatment liquid on the bottle wall. The water can be evenly sprayed on the inner wall of the aluminum alloy gas cylinder 18 through the liquid sprayer. The drying box 16 is used to completely remove the water remaining on the inner wall of the aluminum alloy gas cylinder 18 after water washing.

[0042] The device includes six steps of activation, water washing, pre-plating, chemical plating, water washing and drying when in use, as follows:

[0043] 1) Preparation: Wrap the outer wall of the aluminum alloy gas cylinder to be treated with plastic wrap to prevent the outer wall of the aluminum alloy gas cylinder from participating in the chemical plating process.

[0044] 2) Activation: Place the aluminum alloy gas cylinder in the gas cylinder rack on the activation tank, operate the automatic controller, and the circulation pump will inject the activation treatment liquid placed in the activation treatment tank into the aluminum alloy gas cylinder to be treated. After the activation treatment liquid is filled, the circulation pump will automatically stop, and then the timer will start timing. During the activation process, the activation treatment liquid in the aluminum alloy gas cylinder does not need to be circulated, so that the inner wall of the aluminum alloy gas cylinder is fully activated. After the timer prompts that the time is up, the activation treatment liquid in the aluminum alloy gas cylinder is poured back into the activation treatment tank by the circulation pump. During the activation process, the temperature of the activation treatment liquid in the activation treatment tank is 35-65°C, and the activation time is 1-10 minutes.

[0045] 3) Water washing: Place the aluminum alloy gas cylinder in a water washing tank, and use a circulating pump to spray the water in the water washing tank into the aluminum alloy gas cylinder through a liquid sprayer for repeated washing 2 to 5 times. This process is continued until the residual activation treatment liquid on the cylinder wall is completely removed. The water temperature in the water washing tank used for washing is 50 to 80°C, and the water washing process must be completed as soon as possible within 3 minutes to avoid oxidation of the inner wall of the evenly activated aluminum alloy gas cylinder.

[0046] 4) Pre-plating: Place the aluminum alloy cylinder on the cylinder rack of the pre-plating treatment tank, operate the automatic controller, and the circulating pump will inject the pre-plating treatment liquid placed in the pre-plating treatment tank into the aluminum alloy cylinder to be plated. After the pre-plating treatment liquid is filled, the circulating pump will automatically stop and the timer will start timing. During this process, the pre-plating treatment liquid in the aluminum alloy cylinder does not need to be circulated, so that the inner wall of the aluminum alloy cylinder is quickly deposited with a full coating. After the timer prompts that the time is up, the pre-plating treatment liquid in the aluminum alloy cylinder is poured back into the pre-plating treatment tank by the circulating pump. During the pre-plating process, the treatment liquid temperature in the pre-plating treatment tank is 70-90°C, and the pre-plating process takes 5-30 minutes.

[0047] 5) Chemical plating: Place the aluminum alloy gas cylinder on the gas cylinder rack of the chemical plating treatment tank, operate the automatic controller, and the circulation pump will inject the chemical plating treatment solution placed in the chemical plating treatment tank into the aluminum alloy gas cylinder. After the chemical plating treatment solution is filled, the circulation pump will automatically stop and the timer will start timing. Use the speed regulator to adjust the circulation pump speed to 0.01m 3 / h~0.04m 3 / h, to ensure the appropriate circulation speed of the chemical plating treatment solution. The automatic controller controls the circulation pump to automatically update the chemical plating treatment solution in the aluminum alloy cylinder during the chemical plating process. After the timer prompts that the time is up, the chemical plating treatment solution in the aluminum alloy cylinder is returned to the chemical plating treatment tank by the circulation pump. The temperature of the chemical plating treatment solution in the plating tank during the chemical plating process is 60-90℃, and the chemical plating time is 20-60min.

[0048] 6) Water washing: Take out the aluminum alloy gas cylinder and place it in the sink. Use a sprayer connected to the tap water pipe to fully rinse the aluminum alloy gas cylinder until the chemical plating treatment liquid remaining on the bottle wall is completely removed.

[0049] 7) Drying: Place the aluminum alloy gas cylinder in a drying oven at a temperature of 50-100°C for 10-30 minutes to remove the residual moisture on the inner wall of the aluminum alloy gas cylinder.

[0050] All automatic controllers and timers must be pre-set according to the corresponding treatment tank. The chemical plating treatment liquid inside the aluminum alloy cylinder during the chemical plating process must be circulated once within 10 to 15 minutes to ensure the stability of the chemical plating treatment liquid and allow the reaction process to proceed normally. During the circulation of the chemical plating treatment liquid, the injection pipe of the circulation pump is placed at the bottom of the aluminum alloy cylinder. After the new chemical plating treatment liquid is injected, the original chemical plating treatment liquid in the bottle automatically overflows from the bottle mouth and flows back into the plating tank. After the circulation pump is filled with the new chemical plating treatment liquid, the automatic controller controls the circulation pump to stop working. The coating thickness of the inner wall of the aluminum alloy cylinder after treatment is controllable within the range of 5 to 20μm, and the bonding strength of the coating is ≤ level 1, which meets the use requirements.

[0051] Below, an apparatus and method for chemical plating of the inner wall of an aluminum alloy gas cylinder of the present invention are described through examples and in combination with the accompanying drawings, but the examples only represent a part of the present invention, and the present invention is not limited to the following examples.

[0052] Example 1

[0053] The aluminum alloy gas cylinder selected in this embodiment has a capacity of 300 ml, a bottle mouth diameter of 1.5 cm, a bottle body diameter of 10 cm, and a height of 27 cm. Figure 1As shown, the aluminum alloy gas cylinder is placed in the gas cylinder rack on the activation treatment tank heated to 58°C, and the automatic controller is used to control the acid-base resistant circulation pump to inject the activation treatment liquid into the aluminum alloy gas cylinder. After the activation treatment liquid is filled, the circulation pump automatically stops. The timer starts timing, and after 3 minutes, the activation treatment liquid in the aluminum alloy gas cylinder is poured back into the activation treatment tank by the circulation pump, and then the aluminum alloy gas cylinder is taken out of the activation treatment tank and placed in the water washing treatment tank. The water temperature in the water washing treatment tank is 70°C, and the high temperature resistant circulation pump is used to inject the water in the water washing treatment tank into the aluminum alloy gas cylinder using a sprayer for repeated water washing. After washing twice, pour out the clean water in the bottle and place the aluminum alloy gas cylinder in the pre-plating treatment tank. The temperature of the pre-plating treatment liquid in the pre-plating treatment tank is 85°C, and the automatic controller is used to operate the acid-base resistant and high temperature resistant circulation pump to inject the pre-plating treatment liquid into the aluminum alloy gas cylinder. After the treatment liquid is filled, the circulation pump automatically stops, and the timer starts working at the same time. After 18 minutes of pre-plating, the aluminum alloy gas cylinder is placed in the gas cylinder rack of the chemical plating treatment tank. The temperature of the treatment liquid in the chemical plating treatment tank is 80°C. After the chemical plating treatment liquid is filled, the circulation pump stops automatically and the timer starts working. The chemical plating treatment liquid in the gas cylinder is automatically replaced every 15 minutes, and each cycle of updating the chemical plating treatment liquid takes 3 minutes. After 51 minutes of chemical plating, the chemical plating treatment liquid in the aluminum alloy gas cylinder is poured back into the chemical plating treatment tank by the circulation pump. Take out the aluminum alloy gas cylinder from the gas cylinder rack, place it in the water tank for cleaning 3 times, and then place it in a 70°C drying oven for 15 minutes.

[0054] Cut open the treated aluminum alloy cylinder for testing. Figure 2 As shown, from the macroscopic photograph of the chemical plating of the aluminum alloy gas cylinder in Example 1, it can be seen that the inner wall of the aluminum alloy gas cylinder is a uniform and bright silver coating, the coating has good bonding strength with the substrate, the coating at the edge of the cut is intact, there is no falling off or cracking, and the coating thickness is about 9μm.

[0055] Example 2

[0056] In this embodiment, four aluminum alloy gas cylinders are selected, each with a volume of 300 ml, a bottle mouth diameter of 1.5 cm, a bottle body diameter of 10 cm, and a height of 27 cm. Figure 1As shown, four aluminum alloy gas cylinders are placed in the gas cylinder rack of the activation treatment tank heated to 50°C, and the acid-alkali resistant circulation pump is controlled by the automatic controller to inject the activation treatment liquid into the aluminum alloy gas cylinder. After the activation treatment liquid is filled, the circulation pump automatically stops. After 5 minutes, the activation treatment liquid in the aluminum alloy gas cylinder is poured back into the activation treatment tank by the circulation pump, and the aluminum alloy gas cylinder is taken out and placed in the water washing treatment tank. The water temperature in the water washing treatment tank is 65°C. The water in the water washing treatment tank is injected into the aluminum alloy gas cylinder by the sprayer using a high temperature resistant circulation pump and repeatedly washed 4 times. Then the aluminum alloy gas cylinder is placed in the gas cylinder rack of the pre-plating treatment tank. The temperature of the pre-plating treatment liquid in the pre-plating treatment tank is 88°C. The acid-alkali resistant and high temperature resistant circulation pump is operated by the automatic controller to inject the pre-plating treatment liquid into the aluminum alloy gas cylinder. After the pre-plating treatment liquid is filled, the circulation pump automatically stops, and the timer starts working. After 25 minutes of pre-plating, the aluminum alloy gas cylinder is placed in the chemical plating treatment tank. The temperature of the treatment liquid in the chemical plating treatment tank is 83°C. Use an automatic controller to operate an acid-base-resistant and high-temperature-resistant circulating pump to inject the chemical plating solution into the aluminum alloy cylinder. After the chemical plating solution is filled, the circulating pump automatically stops and the timer starts working. The chemical plating solution in the aluminum alloy cylinder is automatically replaced every 10 minutes. Each cycle requires 4 minutes to update the chemical plating solution. After 62 minutes of chemical plating, take out the aluminum alloy cylinder and use a circulating pump to pour the chemical plating solution in the aluminum alloy cylinder back into the chemical plating tank. Take out the aluminum alloy cylinder, place it in a water tank and wash it repeatedly for 3 times, and then place it in a 60℃ drying oven to dry for 20 minutes.

[0057] The treated aluminum alloy gas cylinder was cut open for testing, and the inner wall of the aluminum alloy gas cylinder was a uniform and bright silver coating with a thickness of about 13μm.

[0058] 1. Plating status

[0059] The inner wall coatings of the five aluminum alloy gas cylinders produced in Examples 1 and 2 are uniform, complete and bright.

[0060] 2. Coating bonding strength

[0061] According to GB / T 9286-1998 standard, the coating adhesion of the inner wall of the five aluminum alloy gas cylinders produced in Examples 1 and 2 was tested, and the coating adhesion of all samples was level 0, which met the use requirements.

[0062] Combined with the above results, it can be seen that the device and method for chemical plating of the inner wall of an aluminum alloy gas cylinder of the present invention includes multiple automatic control and plating solution circulation systems, which solves the problems of inconvenient operation and difficult control of plating solution faced in chemical plating of the inner wall of an aluminum alloy gas cylinder, and improves production efficiency. At the same time, batch production of chemical plating of the inner wall of an aluminum alloy gas cylinder can be carried out, and the coating of the inner wall of the aluminum alloy gas cylinder is uniform and bright, with good bonding strength. The entire process is simple to operate and easy to control. The chemical plating improves the quality of the inner wall of the aluminum alloy gas cylinder and improves the quality of the aluminum alloy gas cylinder products.

Claims

1. A method for chemical plating of the inner wall of an aluminum alloy gas cylinder, characterized in that: The device for chemical plating of the inner wall of aluminum alloy gas cylinders includes a chemical plating system, a heating system, a control system and a post-processing system. The specific structure is as follows: The chemical plating system includes an activation treatment tank, a water washing treatment tank, a pre-plating treatment tank, a chemical plating treatment tank, a gas cylinder rack, and a liquid sprayer. The liquid sprayer is tubular and extends into the aluminum alloy gas cylinder. The treatment liquid is evenly sprayed into the aluminum alloy gas cylinder through the liquid sprayer. The four treatment tanks are discharged in sequence. The gas cylinder rack is placed on each treatment tank when in use. The liquid sprayer is connected to the multi-way water pipe joint at one end of the liquid outlet pipe of the circulation pump. The heating system includes a heating rod, a thermal resistor, and a secondary instrument, which are used to control the temperature of each step of the chemical plating process; each treatment tank that needs to be heated is equipped with a heating rod, a thermal resistor, and a secondary instrument connected to the thermal resistor. The heating rod is placed in the aqueous solution for water bath heating, the thermal resistor is vertically installed in the water bath in the treatment tank, and the secondary instrument is connected to the thermal resistor through an electric wire and installed outside the treatment tank; The control system includes a circulation pump, an automatic controller, a speed regulator, a timer, and a multi-way water pipe joint. Each treatment tank is equipped with a control system for controlling the chemical plating reaction process and the circulation of the treatment liquid in the reaction; the automatic controller is provided with a speed regulator and a timer, and the speed regulator is connected to the circulation pump through the automatic controller to control the flow rate of the circulation pump when the treatment liquid circulates; a multi-way water pipe joint is installed at one end of the liquid outlet pipe of the circulation pump, and a liquid sprayer is installed at the outlet end of the multi-way water pipe joint; The post-processing system includes a water tank, a liquid sprayer, and a drying box. One end of the water outlet pipe on the water tank is connected to the liquid sprayer and extends into the bottle mouth of the aluminum alloy gas cylinder in the water tank. The washed aluminum alloy gas cylinder is placed in the drying box for drying; The method for chemical plating of the inner wall of an aluminum alloy gas cylinder includes activation, water washing, pre-plating, chemical plating, water washing, and drying. The specific steps are as follows: 1) Preparation: Wrap the outer wall of the aluminum alloy gas cylinder to be treated with plastic wrap to prevent the outer wall of the aluminum alloy gas cylinder from participating in the chemical plating process; 2) Activation: Place the aluminum alloy gas cylinder in the gas cylinder rack on the activation tank, operate the automatic controller, and the circulation pump will inject the activation treatment liquid placed in the activation treatment tank into the aluminum alloy gas cylinder to be treated. After the activation treatment liquid is filled, the circulation pump will automatically stop, and then the timer will start timing; during the activation process, the activation treatment liquid in the aluminum alloy gas cylinder does not need to be circulated, so that the inner wall of the aluminum alloy gas cylinder is fully activated; when the timer prompts that the time is up, the activation treatment liquid in the aluminum alloy gas cylinder is poured back into the activation treatment tank by the circulation pump; The temperature of the activation treatment liquid in the activation treatment tank during the activation process is 35-65°C, and the activation time is 1-10 minutes; 3) Water washing: Place the aluminum alloy gas cylinder in a water washing tank, and use a circulating pump to spray the water in the water washing tank into the aluminum alloy gas cylinder through a liquid sprayer for repeated washing 2 to 5 times; Until the residual activation treatment liquid on the cylinder wall is completely removed, the water temperature in the washing tank used for washing during the washing process is 50-80°C, and the washing process is completed as soon as possible within 3 minutes to avoid the re-oxidation of the inner wall of the uniformly activated aluminum alloy cylinder; 4) Pre-plating: Place the aluminum alloy gas cylinder on the gas cylinder rack of the pre-plating treatment tank, operate the automatic controller, and the circulating pump will inject the pre-plating treatment liquid placed in the pre-plating treatment tank into the aluminum alloy gas cylinder to be plated. After the pre-plating treatment liquid is filled, the circulating pump will automatically stop and the timer will start timing. During this process, the pre-plating treatment liquid in the aluminum alloy gas cylinder does not need to be circulated, so that the inner wall of the aluminum alloy gas cylinder is quickly deposited with a full coating; after the timer prompts that the time is up, the pre-plating treatment liquid in the aluminum alloy gas cylinder is poured back into the pre-plating treatment tank by the circulating pump; during the pre-plating process, the treatment liquid temperature in the pre-plating treatment tank is 70-90°C, and the pre-plating process is 5-30min; 5) Chemical plating: Place the aluminum alloy gas cylinder on the gas cylinder rack of the chemical plating treatment tank, operate the automatic controller, and the circulation pump will inject the chemical plating treatment solution placed in the chemical plating treatment tank into the aluminum alloy gas cylinder. After the chemical plating treatment solution is filled, the circulation pump will automatically stop and the timer will start timing; use the speed regulator to adjust the circulation pump speed to 0.01m / s. 3 / h~0.04m 3 / h, to ensure a suitable circulation speed of the chemical plating treatment solution; the automatic controller controls the circulation pump to automatically update the chemical plating treatment solution in the aluminum alloy cylinder during the chemical plating process; after the timer prompts that the time is up, the chemical plating treatment solution in the aluminum alloy cylinder is returned to the chemical plating treatment tank by the circulation pump; during the chemical plating process, the temperature of the chemical plating treatment solution in the plating tank is 60-90°C, and the chemical plating time is 20-60min; 6) Water washing: Take out the aluminum alloy gas cylinder and place it in the water tank, and use a sprayer connected to the tap water pipe to fully rinse the aluminum alloy gas cylinder until the residual chemical plating treatment liquid on the bottle wall is completely removed; 7) Drying: Place the aluminum alloy gas cylinder in a drying oven at a temperature of 50-100°C for 10-30 minutes to remove the residual moisture on the inner wall of the aluminum alloy gas cylinder.

2. The method for chemical plating of the inner wall of an aluminum alloy gas cylinder according to claim 1, characterized in that: The four processing tanks are all nested structures with inner and outer double tanks that can be heated in a water bath and are used to heat and hold different processing liquids. Each processing tank corresponds to a processing step, and the inner tank of each processing tank holds different processing liquids. An aqueous solution for water bath heating is installed between the outer tank and the inner tank of each processing tank.

3. The method for chemical plating of the inner wall of an aluminum alloy gas cylinder according to claim 1, characterized in that: The gas cylinder rack is used to place and fix the aluminum alloy gas cylinder so that the body of the aluminum alloy gas cylinder remains stable during each step of the reaction process.

4. The method for chemical plating of the inner wall of an aluminum alloy gas cylinder according to claim 1, characterized in that: The heating rod is used to heat the processing tanks to the required temperature, and the thermal resistor and secondary instrument are used to measure and control the temperature of the four processing tanks.

5. The method for chemical plating of the inner wall of an aluminum alloy gas cylinder according to claim 1, characterized in that: The circulation pump is used to inject the treatment liquid into the aluminum alloy gas cylinder to be treated, and the circulation pump is an acid and alkali resistant circulation pump.

6. The method for chemical plating of the inner wall of an aluminum alloy gas cylinder according to claim 1, characterized in that: The automatic controller is used to control the circulation pump to inject the treatment liquid into the aluminum alloy cylinder and stop after the treatment liquid is filled; the timer is used to measure the reaction time of each step in the reaction process; the multi-way water pipe connector adjusts the number of the circulation pump outlets according to the number of aluminum alloy cylinders undergoing chemical plating treatment at the same time.

7. The method for chemical plating of the inner wall of an aluminum alloy gas cylinder according to claim 1, characterized in that: The water tank is used to clean the aluminum alloy gas cylinder after chemical plating. The inner wall of the aluminum alloy gas cylinder is rinsed with clean water to remove the residual treatment liquid on the cylinder wall. The water is evenly sprayed on the inner wall of the aluminum alloy gas cylinder through the sprayer. The drying box is used to completely remove the residual water on the inner wall of the aluminum alloy gas cylinder after washing.

8. The method for chemical plating of the inner wall of an aluminum alloy gas cylinder according to claim 1, characterized in that: All automatic controllers and timers are pre-set according to the corresponding processing tanks.

9. The method for chemical plating of the inner wall of an aluminum alloy gas cylinder according to claim 1, characterized in that: During the chemical plating process, the chemical plating solution inside the aluminum alloy cylinder is circulated once within 10 to 15 minutes to ensure the stability of the chemical plating solution and allow the reaction process to proceed normally. During the circulation of the chemical plating solution, the injection pipe of the circulation pump is placed at the bottom of the aluminum alloy cylinder. After the new chemical plating solution is injected, the original chemical plating solution in the bottle automatically overflows from the bottle mouth and flows back into the plating tank. After the circulation pump is filled with the new chemical plating solution, the automatic controller controls the circulation pump to stop working.