A method for manufacturing a HTCC multilayer ceramic tube shell
By using laser holes to form the side wall cavity after isostatic pressing process, the problem of collapse and deformation during the side wall cavity forming of HTCC multi-layer ceramic tube shell is solved, and stress-free processing and high-quality molding are achieved.
Patent Information
- Application Number
- CN202210879235.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-07-25
AI Technical Summary
The side wall cavity of HTCC multi-layer ceramic tube shell is prone to collapse and deform during the molding process, and cannot be achieved using conventional isostatic pressing processes.
After the isostatic pressing process, the side wall cavity is formed by laser opening method to avoid deformation and collapse of the cavity, and the HTCC multi-layer ceramic tube shell is formed through printing, stacking, hot cutting and sintering steps.
It effectively avoids deformation and collapse of the side wall cavity, and the laser processing method can flexibly process cavity of any shape, size and depth, ensuring molding quality.
Smart Images

Figure CN115087279B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high temperature ceramic tube shell processing, and in particular relates to a method for manufacturing a HTCC multilayer ceramic tube shell. Background Art
[0002] High Temperature Co-fired Ceramic HTCC (High Temperature co-fired Ceramic) is an integrated ceramic made by laminating unsintered tape-cast ceramic materials (usually alumina) and sintering at high temperature (usually greater than 1200°C) to form a multi-layer circuit. HTCC has the advantages of corrosion resistance, high temperature resistance, long life, high efficiency and energy saving, uniform temperature, good thermal conductivity, and fast thermal compensation. Therefore, it has a wide range of application prospects in high-power micro-assembly circuits. Its current main application directions include HTCC heaters, HTCC multi-layer ceramic substrates, and HTCC ceramic tube shells.
[0003] Among them, HCTT ceramic tube shells are widely used in the field of optical communications. They can provide electrical and gas connections and mechanical support protection for optical communication devices. Optical communication ceramic tube shells generally require a cavity (i.e., a side wall cavity) to be opened on the side wall of the end for welding the optical window bracket. However, the current preparation technology of HTCC multilayer ceramic tube shells is relatively complicated. The conventional molding method is isostatic pressing after printing, punching, and lamination, and the side wall cavity is formed in the isostatic pressing step. For these products that require a cavity to be opened in the middle, direct isostatic pressing will cause the cavity to collapse and deform. Therefore, the side wall cavity of the HTCC multilayer ceramic tube shell cannot be achieved using conventional isostatic pressing processes. Summary of the invention
[0004] In view of this, it is necessary for the present invention to provide a method for manufacturing a HTCC multilayer ceramic tube shell. During the forming process of the HTCC multilayer ceramic tube shell, the formation of the side wall cavity is performed after the isostatic pressing process and combined with a laser opening method, thereby solving the problem of easy collapse and deformation of the side wall cavity during the forming process of the HTCC multilayer ceramic tube shell in the existing process.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a method for manufacturing a HTCC multilayer ceramic tube shell, comprising the following steps:
[0007] Providing a green ceramic sheet, printing a metallized pattern on the green ceramic sheet, punching a cavity, and then laminating and isostatic pressing the green ceramic sheet to form a multilayer ceramic tube shell green body with a cavity structure inside;
[0008] Thermally cutting the multi-layer ceramic tube shell green body to form a single multi-layer ceramic tube shell green body unit;
[0009] Opening a cavity in the side wall of the green unit by laser to form a green unit with a side wall cavity;
[0010] The green unit with the side wall cavity is subjected to side printing and then sintered to form a HTCC multi-layer ceramic tube shell.
[0011] In a further embodiment, the raw ceramic sheet is made of alumina.
[0012] In a further embodiment, the green ceramic sheet is formed by tape casting after mixing alumina powder, and the composition is 90-96wt% ceramic.
[0013] In a further embodiment, the slurry used to print the metallization pattern is tungsten slurry or tungsten-molybdenum slurry.
[0014] In a further embodiment, the cavity is punched by mechanical punching or laser punching.
[0015] In a further embodiment, the temperature of the isostatic pressing process is 40-80° C. and the pressure is 500-5000 psi.
[0016] In a further embodiment, the temperature of the hot cutting table is 40-80°C, and the temperature of the blade is 40-80°C.
[0017] In a further embodiment, the type of the laser is selected from one or a combination of two or more of ultraviolet nanosecond, ultraviolet picosecond, green light, and optical fiber.
[0018] In a further embodiment, the processing parameters of the laser are: laser power 10-50W, laser frequency 20-150kHz, and scanning times 10-200 times.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The manufacturing method of the HTCC multilayer ceramic tube shell in the present invention places the side wall cavity forming step after the isostatic pressing process and combines it with laser cavity opening, which can effectively avoid the deformation and collapse of the cavity. Specifically, the side wall cavity is opened by laser processing after the isostatic pressing process. Since the laser processing method is stress-free, it will not damage the appearance of the HTCC multilayer ceramic tube shell, and the laser processing method is flexible and can be processed to form a cavity of any shape, size and depth. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of the printing patterns of L01, L14, L19 and L23-BOT layers in a typical embodiment of the present invention;
[0022] Figure 2 A schematic diagram of a first cavity pattern and a second cavity pattern in a typical embodiment of the present invention;
[0023] Figure 3 This is a comparison diagram of the green body of the ceramic tube shell with no cavity and a circular cavity on one side of the end in Example 1 of the present invention;
[0024] Figure 4 This is a real picture of the ceramic tube shell green body after side printing in Example 1 of the present invention. DETAILED DESCRIPTION
[0025] Embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0027] A typical embodiment of the present invention provides a method for manufacturing a HTCC multilayer ceramic tube shell, comprising the following steps:
[0028] Providing a green ceramic sheet, printing a metallized pattern on the green ceramic sheet, punching a cavity, and then laminating and isostatic pressing the green ceramic sheet to form a multilayer ceramic tube shell green body with a cavity structure inside;
[0029] Thermally cutting the multi-layer ceramic tube shell green body to form a single multi-layer ceramic tube shell green body unit;
[0030] Opening a cavity in the side wall of the green unit by laser to form a green unit with a side wall cavity;
[0031] The green unit with the side wall cavity is subjected to side printing and then sintered to form a HTCC multi-layer ceramic tube shell.
[0032] In the present invention, on the basis of the conventional HTCC multilayer ceramic tube shell process, the side wall cavity is opened after isostatic pressing, and the formed tube shell green body is opened by laser, thereby avoiding the problem of easy collapse and deformation of the side wall cavity caused by isostatic pressing in the original process. In addition, the laser opening method is flexible and stress-free, and the side wall cavity of any shape, size and depth can be formed according to actual needs.
[0033] In a further embodiment, the type of the green ceramic sheet used in this article is not particularly limited, and can be a material commonly used for HTCC ceramics. In some specific embodiments of the present invention, the green ceramic sheet used is an alumina green ceramic sheet, and its processing method is not particularly limited. According to an embodiment of the present invention, the green ceramic sheet is formed by casting after mixing alumina powder, and its composition is 90%-96wt% porcelain.
[0034] The printing of metallized patterns, punching of cavities, lamination and isostatic pressing processes described herein can all be carried out in conventional ways in the art. Specifically, the metallized patterns can be printed on the raw ceramic sheet according to design requirements. The slurry for printing the metallized patterns can be tungsten slurry or tungsten-molybdenum slurry. It is understood that any slurry that can be used for printing raw ceramic sheets in the art can be used. In addition, it is understood that the specific metallized pattern printing can be adjusted according to the number of layers of the raw ceramic sheet and the overall thickness of the tube shell. Figure 1 2 is a schematic diagram of printing metallized patterns on green ceramic sheets in a typical embodiment of the present invention, where L01, L14, L19 and L23-BOT patterns are printed on corresponding green ceramic sheets respectively.
[0035] The punched cavity is specifically punched on a separate raw porcelain sheet according to design requirements. It should be noted that the punched cavity here is the internal cavity of the tube shell, and does not include the punching of the side wall cavity. Figure 2 2 shows a typical embodiment of the present invention, in which a cavity pattern is punched on a green ceramic sheet, and a first cavity pattern and a second cavity pattern are processed respectively. The punching method of the cavity is not particularly limited, and a conventional method in the art can be used. Specific examples include but are not limited to mechanical punching, laser punching, etc. Other punching methods in the art can also be used, which will not be described in detail here.
[0036] The lamination refers to laminating the raw ceramic sheets in a corresponding order according to the product structure design, which will not be elaborated here. The laminated raw ceramic sheets are subjected to isostatic pressing. The specific isostatic pressing process can be adjusted according to the actual situation (such as the thickness and number of layers of the raw ceramic sheets). In some specific embodiments of the present invention, the temperature of the isostatic pressing process is 40-80°C and the pressure is 500-5000psi.
[0037] A multilayer ceramic tube shell green body with a cavity inside can be formed by the isostatic pressing process. The multilayer ceramic tube shell green body can be cut into several multilayer ceramic tube shell green body units as needed. The specific cutting method can be a conventional choice in the art, such as hot cutting. In some specific embodiments of the present invention, the hot cutting is performed by a hot cutting machine, the table temperature is 40-80°C, and the blade temperature is 40-80°C.
[0038] In a further solution, the green unit is subjected to laser processing to open the side wall cavity. There is no particular limitation on the specific laser type. Examples include, but are not limited to, one or a combination of two or more of ultraviolet nanosecond, ultraviolet picosecond, green light, and optical fiber. The specific processing parameters are actually adjusted according to the type of laser and the side wall cavity. In some typical embodiments of the present invention, the laser power is 10-50W, the laser frequency is 20-150kHz, and the number of scans is 10-200 times. Laser opening of the side wall cavity has the advantages of stress-free processing and flexible processing methods. Side wall cavities of any shape, depth or size can be formed as needed. And because the side wall cavity is formed after isostatic pressing, the problem of cavity collapse or deformation caused by isostatic pressing is avoided.
[0039] The present invention is described below by means of specific examples. It should be noted that the following specific examples are only for illustrative purposes and do not limit the scope of the present invention in any way. In addition, unless otherwise specified, methods without specific conditions or steps are conventional methods, and the reagents and materials used can be obtained from commercial channels.
[0040] Example 1
[0041] The manufacturing method of the HTCC multilayer ceramic tube shell in this embodiment has the following specific steps:
[0042] Green ceramic sheet printing: prepare 23 alumina green ceramic sheets of the same batch with a thickness of 0.25 mm, label the individual green ceramic sheets in sequence, and print the metallized patterns of L01, L14, L19, and L23-BOT on the back of the 1st, 14th, 19th, and 23rd layers of green ceramic sheets respectively;
[0043] Green Ceramic Sheet Punching: Use a mechanical punching machine to punch the 1st to 13th layers of green ceramic sheets. Figure 2 The first cavity pattern shown in FIG. 1 is used to punch out the 14th to 18th layers of raw porcelain sheets. Figure 2 In the second cavity pattern shown in , the 19th to 23rd layers do not need to be flushed;
[0044] Lamination and isostatic pressing: Lamination is performed sequentially from the 23rd layer to the 1st layer, followed by hot pressing in a warm water isostatic press. The hot pressing temperature is 50°C, the hot pressing pressure is 2000psi, and the heat and pressure holding time is 10min;
[0045] Hot cutting: hot cutting the green body after isostatic pressing to form a single tube shell green body;
[0046] Laser processing of side wall cavity: a single tube shell green body is fixed on the positioning fixture, and a UV nanosecond laser punching machine is used to open a cavity on the side wall of the tube shell. The cavity opening effect is adjusted by adjusting the laser power, frequency and other parameters. Specifically, the laser power is 13.5W, the frequency is set to 50kHz, the scanning speed is 500mm / s, and the number of scanning passes is set to 50 times; Figure 3 shows a comparison of the tube shell before and after the side wall cavity is opened;
[0047] Side printing: metallization patterns are printed on both sides of the tube shell, and metallization patterns are printed on the end of the tube shell cavity;
[0048] Sintering: The processed ceramic tube shell green body is sintered in a high temperature co-firing furnace, the sintering temperature is controlled at 1500-1600°C, and the sintering time is 1-2 hours. The final product of the HTCC multilayer ceramic tube shell prepared in this embodiment is as follows: Figure 4 As shown in .
[0049] Example 2
[0050] The manufacturing method of the HTCC multilayer ceramic tube shell in this embodiment has the following specific steps:
[0051] Green ceramic sheet printing: prepare 23 green ceramic sheets of the same batch with a thickness of 0.25 mm, label the individual green ceramic sheets in sequence, and print the metallized patterns of L01, L14, L19, and L23-BOT on the back of the 1st, 14th, 19th, and 23rd layers respectively;
[0052] Punching cavities of raw ceramic sheets: Use a laser punching machine to punch the first cavity pattern for the 1st to 13th layers of raw ceramic sheets, and punch the second cavity pattern for the 14th to 18th layers of raw ceramic sheets. There is no need to punch cavities for the 19th to 23rd layers.
[0053] Lamination and isostatic pressing: Lamination is performed sequentially from the 23rd layer to the 1st layer, followed by hot pressing in a warm water isostatic press at a temperature of 60°C, a hot pressing pressure of 3000 psi, and a holding time of 10 minutes;
[0054] Hot cutting: cutting the green body after isostatic pressing into single tube shell green body;
[0055] Laser processing of side wall cavity: a single tube shell green body is fixed on the positioning fixture, and a UV nanosecond laser punching machine is used to open a cavity on the side wall of the tube shell; the cavity opening effect is adjusted by adjusting the laser power, frequency and other parameters. Specifically, the laser power is 12W, the frequency is set to 100kHz, the scanning speed is 500mm / s, and the number of scanning passes is set to 70 times;
[0056] Side printing: metallization patterns are printed on both sides of the tube shell, and metallization patterns are printed on the end of the tube shell cavity;
[0057] Sintering: The processed ceramic green body is sintered in a high-temperature co-firing furnace. The sintering temperature is controlled at 1500-1600℃ and the sintering time is 1-2h.
[0058] Example 3
[0059] The manufacturing method of the HTCC multilayer ceramic tube shell in this embodiment mainly comprises the following steps:
[0060] Green ceramic sheet printing: prepare 23 green ceramic sheets of the same batch with a thickness of 0.25 mm, label the individual green ceramic sheets in sequence, and print the metallized patterns of L01, L14, L19, and L23-BOT on the back of the 1st, 14th, 19th, and 23rd layers respectively;
[0061] Punching cavities of raw ceramic sheets: Use a laser punching machine to punch the first cavity pattern for the 1st to 13th layers of raw ceramic sheets, and punch the second cavity pattern for the 14th to 18th layers of raw ceramic sheets. There is no need to punch cavities for the 19th to 23rd layers.
[0062] Lamination and isostatic pressing: Lamination is performed sequentially from the 23rd layer to the 1st layer, followed by hot pressing in a warm water isostatic press; the hot pressing temperature is 70°C, the hot pressing pressure is 3000psi, and the heat and pressure holding time is 10 minutes each;
[0063] Hot cutting: cutting the green body after isostatic pressing into single tube shell green body;
[0064] Laser processing of side wall cavity: fix a single tube shell green body on the positioning fixture, and use a fiber laser punching machine to open the cavity on the side wall of the tube shell; adjust the cavity opening effect by adjusting the laser power, frequency and other parameters. Specifically, the laser power is 40W, the frequency is set to 150kHz, the scanning speed is 1000mm / s, and the number of scanning passes is set to 10 times;
[0065] Side printing: metallization patterns are printed on both sides of the tube shell, and metallization patterns are printed on the end of the tube shell cavity;
[0066] Sintering: The processed ceramic green body is sintered in a high-temperature co-firing furnace. The sintering temperature is controlled at 1500-1600℃ and the sintering time is 1-2h.
[0067] The side wall cavity of the HTCC multi-layer ceramic tube shell prepared in the above embodiment has no collapse or deformation, and has good molding quality.
[0068] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0069] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for manufacturing a HTCC multilayer ceramic tube shell, characterized in that: The following steps are involved: Providing a green ceramic sheet, printing a metallized pattern on the green ceramic sheet, punching a cavity, and then laminating and isostatic pressing the green ceramic sheet to form a multilayer ceramic tube shell green body with a cavity structure inside; Thermally cutting the multi-layer ceramic tube shell green body to form a single multi-layer ceramic tube shell green body unit; Opening a cavity on the side wall of the green unit by laser to form a green unit with a side wall cavity, wherein the processing parameters of the laser are laser power of 10-50W, laser frequency of 20-150kHz, and scanning times of 10-200 times; The green unit with the side wall cavity is subjected to side printing and then sintered to form a HTCC multi-layer ceramic tube shell.
2. The method for manufacturing the HTCC multilayer ceramic tube package according to claim 1, characterized in that: The material of the green porcelain sheet is alumina.
3. The method for manufacturing the HTCC multilayer ceramic tube package according to claim 2, characterized in that: The green ceramic sheet is formed by casting after mixing alumina powder, and the composition is 90-96wt% ceramic.
4. The method for manufacturing the HTCC multilayer ceramic tube package according to claim 1, characterized in that: The slurry for printing the metallization pattern is tungsten slurry or tungsten-molybdenum slurry.
5. The method for manufacturing the HTCC multilayer ceramic tube package according to claim 1, characterized in that: The method of punching the cavity is mechanical punching or laser punching.
6. The method for manufacturing the HTCC multilayer ceramic tube package according to claim 1, characterized in that: The isostatic pressing process is performed at a temperature of 40-80°C and a pressure of 500-5000 psi.
7. The method for manufacturing the HTCC multilayer ceramic tube package according to claim 1, characterized in that: The table temperature of the hot cutting is 40-80°C, and the temperature of the blade is 40-80°C.
8. The method for manufacturing the HTCC multilayer ceramic tube package according to claim 1, characterized in that: The type of the laser is selected from one or a combination of two or more of ultraviolet nanosecond, ultraviolet picosecond, green light, and optical fiber.
