Preparation method and application of a germanium-loaded sphalerite flotation targeted activation agent
By preparing a targeted activation agent for flotation of germanium-loaded sphalerite, and combining the grinding, slurrying and air-filled flotation processes, the problem of poor germanium recovery in flotation of germanium-loaded sphalerite was solved, and efficient germanium recovery and Resource utilization, simple process, and environmentally friendly.
Patent Information
- Application Number
- CN202210036338.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-01-13
AI Technical Summary
The existing technology lacks effective understanding of germanium and targeted agents during the flotation process of germanium-loaded sphalerite, resulting in poor germanium recovery results and serious waste of resources. In addition, the use of traditional activators under alkaline conditions results in low product quality. , affecting subsequent desulfurization and other processes.
A targeted activation agent for flotation of germanium-loaded sphalerite is prepared. A targeted activation agent for ore flotation is prepared through a combination of acetic acid, acetone, copper sulfate and 4-methoxyacetophenone. It is combined with grinding, Slurry mixing and air flotation processes improve the recovery rate of germanium.
It effectively improves the recovery rate and grade of germanium-loaded sphalerite, and achieves efficient utilization of germanium with less usage, less environmental pollution, simple process and stable indicators.
Smart Images

Figure CN115090424B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mineral processing, and in particular to a preparation method and application of a germanium-loaded sphalerite flotation targeting activation agent. Background Art
[0002] my country has rich reserves of zinc resources. Since 2000, China has been the world's largest producer and consumer of zinc metal. China's development in the lead and zinc industry has even attracted international attention. Zinc sulfide ore is the main source of zinc resources, and the main zinc-containing mineral is sphalerite. Sphalerite also often contains rare elements such as manganese, cadmium, indium, thallium, gallium, and germanium. Therefore, sphalerite is not only mainly used for refining zinc, but also a raw material for extracting other rare elements.
[0003] At present, for the flotation of germanium-bearing sphalerite, there is no correct understanding of the influence of the presence and content of germanium on the surface properties, electronic configuration, chemical properties and floatability of sphalerite. Therefore, when selecting this type of mineral, it is usually treated as ordinary sphalerite. There is a lack of theoretical basis for the formulation of pulp pH value, activator type and dosage, stirring speed, etc. when flotating germanium-bearing sphalerite, especially in the use of activators. These reasons lead to poor selection and recovery effects of germanium-bearing sphalerite, resulting in serious waste of resources. For example, copper sulfate, the activator of sphalerite, will not only activate sphalerite during use, but also have a certain activation effect on pyrite, etc., and copper sulfate activation usually needs to be carried out under alkaline conditions. This slurry adjustment process will also lead to low product quality and affect subsequent desulfurization.
[0004] Therefore, if we do not reach a comprehensive understanding of the properties and floatability of germanium-loaded sphalerite, and still use the reagent system and process flow of ordinary sphalerite for flotation, we will still not be able to effectively solve the problem of germanium recovery and efficient utilization. In summary, the influence of germanium on sphalerite in germanium-loaded sphalerite and the study of targeted reagents for germanium-loaded sphalerite and the application of targeted reagents have far-reaching significance for the recovery of rare metal germanium. Summary of the invention
[0005] The purpose of the present invention is to provide a preparation method and application of a germanium-loaded sphalerite flotation targeting activation agent. The ore flotation targeting activation agent is prepared by using acetic acid, acetone, copper sulfate, 4-methoxyacetophenone and anhydrous ethanol, so as to achieve effective activation of germanium-loaded sphalerite and germanium-loaded lead-zinc sulfide ore. The germanium-loaded sphalerite is floated by adopting the processes of ore grinding, slurry mixing and dosing, and aeration flotation. Compared with the traditional sphalerite activator copper sulfate, the recovery effect of the germanium-loaded sphalerite can be effectively improved.
[0006] In order to achieve the above object, the first object of the present invention is achieved in this way: a method for preparing a germanium-loaded sphalerite flotation targeting activation agent, characterized in that it comprises the following steps:
[0007] (1) preparing a 4-6% acetic acid solution, and sequentially adding the acetone solution and the copper sulfate solution to the acetic acid solution to prepare solution A;
[0008] (2) dissolving 4-methoxyacetophenone in anhydrous ethanol to prepare solution B;
[0009] (3) The solution A in step (1) and the solution B in step (2) are mixed in a ratio of 1 to 2:1 to obtain an ore flotation targeting activation agent.
[0010] Preferably, in step (1), the ratio of the acetone solution to the acetic acid solution and the ratio of the copper sulfate solution to the acetic acid solution are both 0.8-1.2:1.
[0011] Preferably, in step (1), the concentrations of acetone and copper sulfate in the acetic acid solution are both 50 g / L.
[0012] Preferably, the ratio of 4-methoxyacetophenone to anhydrous ethanol in step (2) is 1 to 2:1.
[0013] The second object of the present invention is achieved by using a targeted activation agent for flotation of germanium-loaded sphalerite, and the application of the targeted activation agent in flotation of germanium-loaded sphalerite and its germanium-loaded lead-zinc sulfide ore.
[0014] An application of a targeted activation agent for flotation of germanium-loaded sphalerite, wherein the targeted activation agent is used for flotation of germanium-loaded sphalerite, characterized in that the method for flotation of germanium-loaded sphalerite comprises the following steps:
[0015] S1: The germanium-loaded sphalerite is manually selected to remove other gangue minerals to obtain pure germanium-loaded sphalerite;
[0016] S2: crushing the pure germanium-loaded zinc sphalerite in step S1 to a particle size of -74 μm + 38 μm to prepare a pure germanium-loaded zinc sphalerite sample;
[0017] S3: taking 2 g of the pure germanium-loaded zinc sphalerite sample in step S2 and putting it into a flotation machine, adding 40 mL of deionized water to prepare a pure germanium-loaded zinc sphalerite slurry, and adding a pH regulator to the pure germanium-loaded zinc sphalerite slurry until the pH value of the pure germanium-loaded zinc sphalerite slurry is 7 to 8, thereby obtaining a weakly alkaline pure germanium-loaded zinc sphalerite slurry;
[0018] S4: adding a targeted activation agent, a collector and a frother to the pure ore pulp of the weakly alkaline germanium-loaded sphalerite in step S3 in sequence, and then performing rapid flotation separation. The froth product of the flotation is the germanium-loaded sphalerite concentrate.
[0019] Preferably, when the targeted activation agent is used for flotation of germanium-loaded sphalerite, the pH adjuster is sodium hydroxide or hydrochloric acid, and the added amount of the targeted activation agent is 2-20 mg / L; the collector is butyl xanthate, and the added amount of the butyl xanthate is 25 mg / L; the foaming agent is pine oil, and the added amount of the pine oil is 15 mg / L.
[0020] An application of a germanium-loaded sphalerite flotation targeted activation agent, wherein the targeted activation agent is used for flotation of germanium-loaded lead-zinc sulfide ore, characterized in that the method for flotation of germanium-loaded lead-zinc sulfide ore comprises the following steps:
[0021] a: After grinding 500g of germanium-loaded lead-zinc sulfide ore, the grinding fineness is controlled to -0.074mm and the content is 69.3%;
[0022] b: taking the ground germanium-loaded lead-zinc sulfide ore sample in step a and placing it in a 1500 mL flotation tank, adding water to 1500 mL to prepare a germanium-loaded lead-zinc sulfide ore slurry;
[0023] c. firstly conducting lead-sulfur mixed flotation in the slurry of the germanium-loaded lead-zinc sulfide ore, and sequentially adding a depressant, a No. 1 collector and a frother for flotation separation, and obtaining a flotation foam product lead concentrate and remaining minerals after flotation separation;
[0024] d: adding an activator, a No. 2 collector and a frother to the remaining mineral in step c in sequence, and obtaining frothed zinc concentrate and tailings after flotation separation.
[0025] Preferably, when the targeted activation agent is used for flotation of germanium-loaded lead-zinc sulfide ore, the inhibitor in step c is zinc sulfate, the amount of zinc sulfate is 2000 g / t, the No. 1 collector is ethyl xanthate, the amount of ethyl xanthate is 120 g / t; the activator in step d is copper sulfate and the targeted activation agent, the No. 2 collector is butyl xanthate, the amount of butyl xanthate is 100 g / t; the foaming agent in step c and step d is pine oil, wherein the amount of the foaming agent in step c is 20 g / t, and the amount of the foaming agent in step d is 30 g / t.
[0026] Preferably, when the targeted activation agent is used for flotation of germanium-loaded lead-zinc sulfide ore, the total amount of copper sulfate and the targeted activation agent is 400 g / t, and the ratio of copper sulfate to the targeted activation agent is 0:1, 1:3, 1:1, 3:1 or 1:0.
[0027] In summary, compared with the prior art, the beneficial effects of the present invention are:
[0028] 1. The targeted activation agent prepared by the present invention has stable properties; it has a strong ability to target and activate germanium-bearing sphalerite in combination with the processes of ore grinding, slurry mixing and dosing, and aeration flotation. Compared with the copper sulfate activator in the prior art, it can effectively improve the recovery of germanium-bearing sphalerite, and can effectively improve the grade and recovery rate of zinc and germanium in actual ore flotation.
[0029] 2. The targeted activation agent prepared by the present invention can not only realize the effective activation flotation of germanium-loaded sphalerite, but also realize the effective activation flotation of germanium-loaded lead-zinc sulfide ore.
[0030] 3. When the present invention utilizes targeted activation agents for ore flotation, the dosage is small and the environmental pollution is small.
[0031] 4. The present invention is not only easy to implement, but can also be used without changing the original production process; it is also simple to use, has a good process sorting effect, and has stable indicators. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The present invention is a test flow chart of flotation of germanium-loaded sphalerite;
[0033] Figure 2 This is a test flow chart of the flotation of germanium-containing lead-zinc sulfide ore according to the present invention;. DETAILED DESCRIPTION
[0034] The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without carrying out creative work are within the scope of protection of the present invention. The techniques, methods and equipment known to ordinary technicians in the relevant fields may not be discussed in detail, but where appropriate, the techniques, methods and equipment should be regarded as part of the authorization specification. In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0035] Example 1
[0036] This specific embodiment provides a method for preparing a targeted activation agent for flotation of germanium-bearing sphalerite, and the application of the targeted activation agent in flotation of germanium-bearing sphalerite.
[0037] 1.1 Preparation of flotation targeting activation agent
[0038] (1) preparing a 4-6% acetic acid solution, and sequentially adding an acetone solution and a copper sulfate solution to the acetic acid solution, wherein the ratio of the acetone solution to the acetic acid solution and the ratio of the copper sulfate solution to the acetic acid solution are both 1:1, and the concentration of acetone and copper sulfate in the acetic acid solution is 50 g / L, to prepare solution A;
[0039] (2) dissolving 4-methoxyacetophenone in anhydrous ethanol, with the ratio of 4-methoxyacetophenone to anhydrous ethanol being 1:1, to prepare solution B;
[0040] (3) Solution A and solution B are mixed in a ratio of 2:1 to obtain an ore flotation targeted activation agent.
[0041] 1.2 The flotation method of germanium-loaded sphalerite includes the following steps: Figure 1 As shown:
[0042] S1: The germanium-loaded sphalerite is manually selected to remove other gangue minerals to obtain pure germanium-loaded sphalerite;
[0043] S2: crushing the pure germanium-loaded zinc sphalerite in step S1 to a particle size of -74 μm + 38 μm to prepare a pure germanium-loaded zinc sphalerite sample;
[0044] S3: taking 2 g of the pure germanium-loaded zinc sphalerite sample in step S2 and putting it into an XFG type hanging trough flotation machine, adding 40 mL of deionized water to prepare a pure germanium-loaded zinc sphalerite slurry, and adding sodium hydroxide or hydrochloric acid solution as a pH regulator to the pure germanium-loaded zinc sphalerite slurry to adjust the pH value of the pure germanium-loaded zinc sphalerite slurry to 7.5, thereby obtaining a weakly alkaline pure germanium-loaded zinc sphalerite slurry;
[0045] S4: Add 2-20 mg / L of the targeted activation agent prepared in 1.1 to the weakly alkaline germanium-loaded sphalerite pure ore pulp in turn and react for 5 minutes, then add 25 mg / L of the collector butyl xanthate and react for 2 minutes, then add 15 mg / L of the foaming agent pine oil and react for 1 minute, and perform rapid flotation separation for 3 minutes. The froth product of the flotation is the germanium-loaded sphalerite concentrate, and the product at the bottom of the flotation machine tank is the tailings.
[0046] Example 2
[0047] The mineral raw material of the germanium-bearing sphalerite in this embodiment: the mineral raw material used is the pure mineral of the germanium-bearing sphalerite after artificial selection and removal of other gangue minerals, wherein the zinc content is 63.35%, the sulfur content is 34.09%, the germanium content is 1221.5g / t, the iron and copper contents are extremely low and no other elements are contained.
[0048] In the flotation method of germanium-bearing sphalerite in this embodiment, the dosage of the targeted activation agent prepared in 1.1 is 2 mg / L, and the rest is the same as described in Example 1.
[0049] The results show that the above reagent conditions can effectively activate germanium-bearing sphalerite, and its recovery rate can reach 62.3%. Under the same copper sulfate activator dosage conditions, the recovery rate of germanium-bearing sphalerite is only 51.2%.
[0050] Example 3
[0051] The mineral raw material of the germanium-bearing sphalerite in this embodiment: the mineral raw material used is the pure mineral of the germanium-bearing sphalerite after artificial selection and removal of other gangue minerals, wherein the zinc content is 63.35%, the sulfur content is 34.09%, the germanium content is 1221.5g / t, the iron and copper contents are extremely low and no other elements are contained.
[0052] In the flotation method of germanium-bearing sphalerite in this embodiment, the dosage of the targeted activation agent prepared in 1.1 is 6 mg / L, and the rest is the same as described in Example 1.
[0053] The results show that the above reagent conditions can effectively activate germanium-bearing sphalerite, and its recovery rate can reach 84.3%. Under the same copper sulfate activator dosage conditions, the recovery rate of germanium-bearing sphalerite is only 71.4%.
[0054] Example 4
[0055] The mineral raw material of the germanium-bearing sphalerite in this embodiment: the mineral raw material used is the pure mineral of the germanium-bearing sphalerite after artificial selection and removal of other gangue minerals, wherein the zinc content is 63.35%, the sulfur content is 34.09%, the germanium content is 1221.5g / t, the iron and copper contents are extremely low and no other elements are contained.
[0056] In the flotation method of germanium-bearing sphalerite in this embodiment, the dosage of the targeted activation agent prepared in 1.1 is 10 mg / L, and the rest is the same as described in Example 1.
[0057] The results show that the above reagent conditions can effectively activate germanium-loaded sphalerite, and its recovery rate can reach 93.2%. However, under the same copper sulfate activator dosage conditions, the recovery rate of germanium-loaded sphalerite is only 86.6%.
[0058] Example 5
[0059] The mineral raw material of the germanium-bearing sphalerite in this embodiment: the mineral raw material used is the pure mineral of the germanium-bearing sphalerite after artificial selection and removal of other gangue minerals, wherein the zinc content is 63.35%, the sulfur content is 34.09%, the germanium content is 1221.5g / t, the iron and copper contents are extremely low and no other elements are contained.
[0060] In the flotation method of germanium-bearing sphalerite in this embodiment, the dosage of the targeted activation agent prepared in 1.1 is 16 mg / L, and the rest is the same as described in Example 1.
[0061] The results show that the above reagent conditions can effectively activate germanium-loaded sphalerite, and its recovery rate can reach 93.5%. Under the same copper sulfate activator dosage conditions, the recovery rate of germanium-loaded sphalerite is only 86.8%.
[0062] Example 6
[0063] The mineral raw material of the germanium-bearing sphalerite in this embodiment: the mineral raw material used is the pure mineral of the germanium-bearing sphalerite after artificial selection and removal of other gangue minerals, wherein the zinc content is 63.35%, the sulfur content is 34.09%, the germanium content is 1221.5g / t, the iron and copper contents are extremely low and no other elements are contained.
[0064] In the flotation method of germanium-bearing sphalerite in this embodiment, the dosage of the targeted activation agent prepared in 1.1 is 20 mg / L, and the rest is the same as described in Example 1.
[0065] The results show that the above reagent conditions can effectively activate germanium-bearing sphalerite, and its recovery rate can reach 93.7%. Under the same copper sulfate activator dosage conditions, the recovery rate of germanium-bearing sphalerite is only 90.1%.
[0066] Example 7
[0067] This specific embodiment provides a method for preparing an ore flotation targeted activation agent for flotation of germanium-containing lead-zinc sulfide ore, and the application of the targeted activation agent in the flotation of germanium-containing lead-zinc sulfide ore.
[0068] The preparation method of the targeted activation agent for flotation of germanium-loaded lead-zinc sulfide ore is consistent with that in Example 1.
[0069] The flotation method of germanium-loaded lead-zinc sulfide ore comprises the following steps: Figure 2 As shown:
[0070] a: After grinding 500g of germanium-loaded lead-zinc sulfide ore, the grinding fineness is controlled to -0.074mm and the content is 69.3%;
[0071] b: taking the ground germanium-loaded lead-zinc sulfide ore sample in step a and placing it in a 1500 mL flotation tank, adding water to 1500 mL to prepare a germanium-loaded lead-zinc sulfide ore slurry;
[0072] c. Conducting a lead-sulfur mixed selection test on the germanium-loaded lead-zinc sulfide ore pulp, sequentially adding 2000 g / t of zinc sulfate inhibitor, 120 g / t of No. 1 collector ethyl xanthate, and 20 g / t of pine oil frother to the germanium-loaded lead-zinc sulfide ore pulp for flotation separation, and obtaining a froth product lead concentrate and a residue after flotation separation;
[0073] d: Add a certain amount of copper sulfate and targeted activation agent activator, No. 2 collector butyl xanthate 100g / t, pine alcohol oil frother 30g / t to the residue in step c in sequence, and obtain the froth product zinc concentrate and tailings after flotation separation.
[0074] Example 8
[0075] The mineral raw material of the germanium-containing lead-zinc sulfide ore in this embodiment: the mineral raw material used is a lead-zinc ore in a certain place in Yunnan, and the test results of the original ore grade are: 6.82% lead, 21.03% zinc, and 32.3g / t germanium. The content of Pb and Zn in the ore is higher than the lowest industrial grade for the development and utilization of mineral resources, and the content of Ag and Ge reaches the comprehensive utilization grade; the S content is relatively high, and the ore type is mainly sulfide ore; the As content is relatively low, which is relatively favorable for lead concentrate and zinc concentrate. The results of the ore zinc phase analysis show that the total zinc content of the original ore is 21.0%, mainly in the form of sulfide ore, accounting for 95.86% of the total zinc. Germanium mainly exists in the form of isomorphism, accounting for 3.70% in galena; accounting for 85.11% in sphalerite, and the highest grade of germanium in sphalerite can reach 87.6g / t; accounting for 4.25% in pyrite and marcasite, and accounting for 6.94% in gangue minerals such as calcite and dolomite. Germanium in sulfides can be recovered along with sulfides, but germanium in gangue minerals is difficult to recover.
[0076] In the flotation method of the germanium-loaded lead-zinc sulfide ore of this embodiment, the usage ratio of copper sulfate and the targeted activation agent is 1:1, that is, the usage ratio of copper sulfate and the targeted activation agent is 200 g / t. The rest is the same as that in Example 7.
[0077] Example 9
[0078] The mineral raw material of the germanium-loaded lead-zinc sulfide ore in this example is consistent with the raw material in Example 8.
[0079] In the flotation method of the germanium-containing lead-zinc sulfide ore of this embodiment, the usage ratio of copper sulfate and the targeted activation agent is 3:1, that is, copper sulfate is 300 g / t and the targeted activation agent is 100 g / t. The rest is consistent with that described in Example 8.
[0080] Example 10
[0081] The mineral raw material of the germanium-loaded lead-zinc sulfide ore in this example is consistent with the raw material in Example 8.
[0082] In the flotation method of the germanium-loaded lead-zinc sulfide ore of this embodiment, the usage ratio of copper sulfate and the targeted activation agent is 1:3, that is, copper sulfate is 100 g / t and the targeted activation agent is 300 g / t. The rest is consistent with that described in Example 8.
[0083] Embodiment 11
[0084] The mineral raw material of the germanium-loaded lead-zinc sulfide ore in this example is consistent with the raw material in Example 8.
[0085] In the flotation method of the germanium-containing lead-zinc sulfide ore of this embodiment, the usage ratio of copper sulfate and the targeted activation agent is 0:1, that is, copper sulfate is 0 g / t and the targeted activation agent is 400 g / t. The rest is consistent with that described in Example 8.
[0086] Example 12
[0087] The mineral raw material of the germanium-loaded lead-zinc sulfide ore in this example is consistent with the raw material in Example 8.
[0088] In the flotation method of the germanium-loaded lead-zinc sulfide ore of this embodiment, the usage ratio of copper sulfate and targeted activation agent (LKA) is 1:0, that is, copper sulfate is 400 g / t and targeted activation agent is 0 g / t. The rest is consistent with that described in Example 8.
[0089] In Examples 8-12, the test results of different activator dosage conditions are shown in Table 1.
[0090]
[0091]
[0092] Table 1
[0093] It can be seen from the test results in Table 1 that when flotation is performed on sulfur-containing lead-zinc ores, when the ratio of copper sulfate to targeted activation agent is 1:1, that is, both are 200 g / t, the recovery effect of zinc minerals is the best, and the recovery rate of germanium is also high.
[0094] The above description enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a germanium-loaded sphalerite flotation targeting activation agent, characterized in that: The following steps are involved: (1) Prepare 4-6% acetic acid solution, and add acetone solution and copper sulfate solution to the acetic acid solution in sequence to prepare solution A; (2) dissolving 4-methoxyacetophenone in anhydrous ethanol to prepare solution B; (3) mixing the solution A in step (1) with the solution B in step (2) in a ratio of 1 to 2:1 to obtain an ore flotation targeting activation agent; The ratio of the acetone solution to the acetic acid solution and the ratio of the copper sulfate solution to the acetic acid solution in step (1) are both 0.8 to 1.2:1; Application of the targeted activation agent in the flotation of germanium-loaded sphalerite and germanium-loaded lead-zinc sulfide ore; When the targeted activation agent is used for flotation of germanium-loaded sphalerite, the method for flotation of germanium-loaded sphalerite comprises the following steps: S1: The germanium-loaded sphalerite is manually selected to remove other gangue minerals to obtain pure germanium-loaded sphalerite; S2: crushing the pure germanium-loaded zinc sphalerite in step S1 to a particle size of -74 μm + 38 μm to prepare a pure germanium-loaded zinc sphalerite sample; S3: taking 2 g of the pure germanium-loaded zinc sphalerite sample in step S2 and putting it into a flotation machine, adding 40 mL of deionized water to prepare a pure germanium-loaded zinc sphalerite slurry, and adding a pH regulator to the pure germanium-loaded zinc sphalerite slurry until the pH value of the pure germanium-loaded zinc sphalerite slurry is 7-8, thereby obtaining a weakly alkaline pure germanium-loaded zinc sphalerite slurry; S4: adding a targeted activation agent, a collector and a frother to the pure ore pulp of the weakly alkaline germanium-loaded sphalerite in step S3 in sequence, and then performing rapid flotation separation. The froth product of the flotation is the germanium-loaded sphalerite concentrate.
2. The method for preparing a germanium-loaded sphalerite flotation targeting activation agent according to claim 1, characterized in that: In step (1), the concentrations of acetone and copper sulfate in the acetic acid solution are both 50 g / L.
3. The method for preparing a germanium-loaded sphalerite flotation targeting activation agent according to claim 1, characterized in that: The ratio of 4-methoxyacetophenone to anhydrous ethanol in step (2) is 1 to 2:
1.
4. The method for preparing a germanium-loaded sphalerite flotation targeting activation agent according to claim 1, characterized in that: When the targeted activation agent is used for flotation of germanium-loaded sphalerite, the pH regulator is sodium hydroxide or hydrochloric acid, and the added amount of the targeted activation agent is 2-20 mg / L; the collector is butyl xanthate, and the added amount of the butyl xanthate is 25 mg / L; the foaming agent is pine oil, and the added amount of the pine oil is 15 mg / L.
5. The method for preparing a germanium-loaded sphalerite flotation targeting activation agent according to claim 1, characterized in that: When the targeted activation agent is used for flotation of germanium-loaded lead-zinc sulfide ore, the method for flotation of germanium-loaded lead-zinc sulfide ore comprises the following steps: a: After grinding 500g of germanium-loaded lead-zinc sulfide ore, the grinding fineness was controlled to −0.074 mm, accounting for 69.3%; b: taking the ground germanium-loaded lead-zinc sulfide ore sample in step a and placing it in a 1500 mL flotation tank, adding water to 1500 mL to prepare a germanium-loaded lead-zinc sulfide ore slurry; c. firstly conducting lead-sulfur mixed flotation in the slurry of the germanium-loaded lead-zinc sulfide ore, and sequentially adding a depressant, a No. 1 collector and a frother for flotation separation, and obtaining a flotation foam product lead concentrate and remaining minerals after flotation separation; d: adding an activator, a No. 2 collector and a frother to the remaining mineral in step c in sequence, and obtaining frothed zinc concentrate and tailings after flotation separation.
6. The method for preparing a germanium-loaded sphalerite flotation targeting activation agent according to claim 5, characterized in that: When the targeted activation agent is used for flotation of germanium-loaded lead-zinc sulfide ore, the inhibitor in step c is zinc sulfate, the dosage of the zinc sulfate is 2000 g / t, the No. 1 collector is ethyl xanthate, and the dosage of the ethyl xanthate is 120 g / t; the activator in step d is copper sulfate and the targeted activation agent, the No. 2 collector is butyl xanthate, and the dosage of the butyl xanthate is 100 g / t; the foaming agent in step c and step d is pine oil, wherein the dosage of the foaming agent in step c is 20 g / t, and the dosage of the foaming agent in step d is 30 g / t.
7. The method for preparing a germanium-loaded sphalerite flotation targeting activation agent according to claim 6, characterized in that: When the targeted activation agent is used for flotation of germanium-loaded lead-zinc sulfide ore, the total amount of the copper sulfate and the targeted activation agent is 400 g / t, and the ratio of the copper sulfate to the targeted activation agent is 0:1, 1:3, 1:1, 3:1 or 1:0.