A stable flame retardant dispersion and preparation method thereof

By uniformly dispersing flame retardants such as decabromodiphenylethane, antimony trioxide, magnesium hydroxide, zinc borate, etc. in water, combined with specific surfactants and stirring technology, the uneven dispersion of inorganic powder flame retardants is solved. Problem, a stable and uniform flame retardant dispersion liquid is achieved, and the flame retardant effect and scope of application are enhanced.

CN115094641BInactive Publication Date: 2024-12-03SHANDONG JUZHAN NEW MATERIALS CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202210970678.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-13
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Inorganic powder flame retardant in existing flame retardant coating glues are prone to form uneven granular forms during the dispersion process, and even lead to demulsification of aqueous emulsions, affecting the flame retardant effect.

Method used

Flame retardants such as decabromodiphenylethane, antimony trioxide, magnesium hydroxide, zinc borate, etc. are uniformly dispersed in water, combined with anti-settling agent, wetting agent, defoaming agent and dispersing agent, and are stirred in three times through high-speed stirring. The added method is used to prepare a stable flame retardant dispersion liquid to ensure the synergistic effect and dispersion uniformity of the flame retardant.

Benefits of technology

The prepared stable flame retardant dispersion liquid is more uniformly dispersed in the aqueous emulsion, has strong flame retardant effect, good stability, wide application range, and does not affect the stability of the emulsion.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a stable flame retardant dispersion and a preparation method thereof, comprising the following components in parts by weight: 30-50 parts of water, 20-30 parts of decabromodiphenylethane, 10-20 parts of antimony trioxide, 10-20 parts of magnesium hydroxide, 5-10 parts of zinc borate, 0.5-3 parts of anti-settling agent, 1-1.5 parts of wetting agent, 0.5-1 part of defoamer, and 3-7 parts of dispersant. The invention has good stability and strong flame retardant effect. Decabromodiphenylethane, antimony trioxide, magnesium hydroxide, and zinc borate are uniformly dispersed in water. The prepared flame retardant dispersion is added to the emulsion, which is more uniform than directly adding the flame retardant to the emulsion for dispersion. The synergistic effect between the flame retardants will be better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardants, and in particular relates to a stable flame retardant dispersion and a preparation method thereof. Background Art

[0002] Fire pressure in public places in China is becoming increasingly severe. Flammable polymers are widely used in public places, and flame retardant polymer materials are increasingly needed. Polymers such as blackout curtains, roller blinds, and sofa fabrics in public places are flammable materials. If a fire occurs, it will cause significant losses to property and life. Flame retardant treatment of these flammable fabrics can effectively reduce the losses caused by fire.

[0003] For these flammable polymer fabrics, flame retardant coating can be applied. Through the process of scraping or dipping, the fabric can be kept beautiful and flame retardant. The coating adhesive is mainly water-based. The water-based coating adhesive is prepared by adding flame retardants to the water-based emulsion and evenly dispersing the flame retardants in it. At present, most flame retardant coating adhesives still add powdered flame retardants. By adding wetting agents, dispersants, defoaming agents, etc., inorganic powder flame retardants or organic powder flame retardants are dispersed in water-based emulsions.

[0004] However, if inappropriate additives are added during the dispersion of inorganic powders, the powders will be unevenly dispersed and form granules, and may even cause the aqueous emulsion to break. Summary of the invention

[0005] The purpose of the present invention is to provide a stable flame retardant dispersion and a preparation method thereof, which has uniform dispersion, good stability and strong flame retardant effect. Decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are uniformly dispersed in water, and the prepared flame retardant dispersion is added to the emulsion, which is more uniform than directly adding the flame retardant to the emulsion for dispersion. The synergistic effect between the flame retardants will be better.

[0006] The technical solution adopted by the present invention to solve the technical problem is: a stable flame retardant dispersion, comprising the following components in parts by weight: 30-50 parts of water, 20-30 parts of decabromodiphenylethane, 10-20 parts of antimony trioxide, 10-20 parts of magnesium hydroxide, 5-10 parts of zinc borate, 0.5-3 parts of anti-settling agent, 1-1.5 parts of wetting agent, 0.5-1 part of defoaming agent and 3-7 parts of dispersant.

[0007] Further: the anti-settling agent is one or more of fumed silica, YB-121 anti-settling agent, and compound anti-settling agent.

[0008] Further: the wetting agent is one or both of HT-110 wetting agent and HT-116 wetting agent.

[0009] Further: the dispersant is one or both of AKN-255 dispersant and AKN-298 dispersant.

[0010] Further: the defoamer is THI ® X-318 defoamer.

[0011] A method for preparing a stable flame retardant dispersion comprises the following steps:

[0012] (1) Decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are mixed together to obtain a flame retardant mixture;

[0013] (2) The wetting agent, defoaming agent and dispersant are uniformly dispersed in water and stirred at a high speed of 800-1200 r / min. After dispersion for 3-7 minutes, the flame retardant mixture mixed in step (1) is added three times at a stirring speed of 800-1200 r / min. After the viscosity of the mixture changes from viscous to thin, an anti-settling agent is added, and the stirring speed is adjusted to 2800-3500 r / min. The mixture is stirred for 20-40 minutes. The uniformly dispersed flame retardant liquid is passed through a 60-mesh sieve to obtain a stable flame retardant dispersion.

[0014] The invention has the following beneficial effects: the stable flame retardant dispersion prepared by the invention has good stability and strong flame retardant effect, decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are uniformly dispersed in water, and the prepared flame retardant dispersion is added to the emulsion, which is more uniform than directly adding the flame retardant to the emulsion for dispersion, and the synergistic effect between the flame retardants will be better.

[0015] The added surfactants are all anionic or nonionic, and the pH of the flame retardant dispersion is between 7-8, which is weakly alkaline. Mixing with most aqueous emulsions will not affect the stability of the emulsion.

[0016] The prepared flame retardant dispersion can be directly added into an aqueous emulsion, has simple operation, strong flame retardant effect and wide application range. DETAILED DESCRIPTION

[0017] The present invention will be further described below in conjunction with embodiments.

[0018] A stable flame retardant dispersion comprises the following components in parts by weight: 30-50 parts of water, 20-30 parts of decabromodiphenylethane, 10-20 parts of antimony trioxide, 10-20 parts of magnesium hydroxide, 5-10 parts of zinc borate, 0.5-3 parts of an anti-settling agent, 1-1.5 parts of a wetting agent, 0.5-1 parts of a defoaming agent and 3-7 parts of a dispersant.

[0019] The anti-settling agent is one or more of fumed silica, YB-121 anti-settling agent, and a compound anti-settling agent.

[0020] The wetting agent is one or both of HT-110 wetting agent and HT-116 wetting agent.

[0021] The dispersant is one or both of AKN-255 dispersant and AKN-298 dispersant.

[0022] The defoamer is THI ® X-318 defoamer.

[0023] A method for preparing a stable flame retardant dispersion comprises the following steps:

[0024] (1) Decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are mixed together to obtain a flame retardant mixture;

[0025] (2) The wetting agent, defoaming agent and dispersant are uniformly dispersed in water and stirred at a high speed of 800-1200 r / min. After dispersion for 3-7 minutes, the flame retardant mixture mixed in step (1) is added three times at a stirring speed of 800-1200 r / min. After the viscosity of the mixture changes from viscous to thin, an anti-settling agent is added, and the stirring speed is adjusted to 2800-3500 r / min. The mixture is stirred for 20-40 minutes. The uniformly dispersed flame retardant liquid is passed through a 60-mesh sieve to obtain a stable flame retardant dispersion.

[0026] Example 1

[0027] A stable flame retardant dispersion comprises the following components in parts by weight: 35 parts of water, 30 parts of decabromodiphenylethane, 10 parts of antimony trioxide, 10 parts of magnesium hydroxide, 5 parts of zinc borate, 3 parts of fumed silica, 1.5 parts of HT-116 wetting agent, 0.5 parts of THI®X-318 defoaming agent, and 5 parts of AKN-255 dispersant.

[0028] A method for preparing a stable flame retardant dispersion comprises the following steps:

[0029] (1) Decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are mixed together to obtain a flame retardant mixture;

[0030] (2) The wetting agent, defoaming agent and dispersant are uniformly dispersed in water and stirred at a high speed of 1000 r / min. After dispersion for 5 minutes, the flame retardant mixture mixed in step (1) is added three times at a stirring speed of 1000 r / min. After the viscosity of the mixture changes from viscous to thin, an anti-settling agent is added, and the stirring speed is adjusted to 3000 r / min. The mixture is stirred for 30 minutes. The uniformly dispersed flame retardant liquid is passed through a 60-mesh sieve to obtain a stable flame retardant dispersion.

[0031] Example 2

[0032] A stable flame retardant dispersion comprises the following components in parts by weight: 35 parts of water, 30 parts of decabromodiphenylethane, 10 parts of antimony trioxide, 10 parts of magnesium hydroxide, 5 parts of zinc borate, 3 parts of YB-121 anti-settling agent, 1.5 parts of HT-116 wetting agent, 0.5 parts of THI®X-318 defoaming agent, and 5 parts of AKN-255 dispersant.

[0033] A method for preparing a stable flame retardant dispersion comprises the following steps:

[0034] (1) Decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are mixed together to obtain a flame retardant mixture;

[0035] (2) The wetting agent, defoaming agent and dispersant are uniformly dispersed in water and stirred at a high speed of 1000 r / min. After dispersion for 5 minutes, the flame retardant mixture mixed in step (1) is added three times at a stirring speed of 1000 r / min. After the viscosity of the mixture changes from viscous to thin, an anti-settling agent is added, and the stirring speed is adjusted to 3000 r / min. The mixture is stirred for 30 minutes. The uniformly dispersed flame retardant liquid is passed through a 60-mesh sieve to obtain a stable flame retardant dispersion.

[0036] Example 3

[0037] A stable flame retardant dispersion comprises the following components in parts by weight: 35 parts of water, 30 parts of decabromodiphenylethane, 10 parts of antimony trioxide, 10 parts of magnesium hydroxide, 5 parts of zinc borate, 1.5 parts of YB121 anti-settling agent, 1.5 parts of fumed silica, 1.5 parts of HT-116 wetting agent, 0.5 parts of THI®X-318 defoaming agent, and 5 parts of AKN-255 dispersant.

[0038] A method for preparing a stable flame retardant dispersion comprises the following steps:

[0039] (1) Decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are mixed together to obtain a flame retardant mixture;

[0040] (2) The wetting agent, defoaming agent and dispersant are uniformly dispersed in water and stirred at a high speed of 1000 r / min. After dispersion for 5 minutes, the flame retardant mixture mixed in step (1) is added three times at a stirring speed of 1000 r / min. After the viscosity of the mixture changes from viscous to thin, an anti-settling agent is added, and the stirring speed is adjusted to 3000 r / min. The mixture is stirred for 30 minutes. The uniformly dispersed flame retardant liquid is passed through a 60-mesh sieve to obtain a stable flame retardant dispersion.

[0041] Example 4

[0042] A stable flame retardant dispersion comprises the following components in parts by weight: 35 parts of water, 30 parts of decabromodiphenylethane, 10 parts of antimony trioxide, 10 parts of magnesium hydroxide, 5 parts of zinc borate, 3 parts of a compound anti-settling agent, 1.5 parts of an HT-116 wetting agent, 0.5 parts of a THI®X-318 defoaming agent, and 5 parts of an AKN-255 dispersant.

[0043] A method for preparing a stable flame retardant dispersion comprises the following steps:

[0044] (1) Decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are mixed together to obtain a flame retardant mixture;

[0045] (2) The wetting agent, defoaming agent and dispersant are uniformly dispersed in water and stirred at a high speed of 1000 r / min. After dispersion for 5 minutes, the flame retardant mixture mixed in step (1) is added three times at a stirring speed of 1000 r / min. After the viscosity of the mixture changes from viscous to thin, an anti-settling agent is added, and the stirring speed is adjusted to 3000 r / min. The mixture is stirred for 30 minutes. The uniformly dispersed flame retardant liquid is passed through a 60-mesh sieve to obtain a stable flame retardant dispersion.

[0046] Example 5

[0047] A stable flame retardant dispersion comprises the following components in parts by weight: 30 parts of water, 20 parts of decabromodiphenylethane, 10 parts of antimony trioxide, 10 parts of magnesium hydroxide, 5 parts of zinc borate, 0.5 parts of fumed silica, 1 part of HT-110 wetting agent, and THI ® 0.5 parts of X-318 defoamer and 3 parts of AKN-255 dispersant.

[0048] A method for preparing a stable flame retardant dispersion comprises the following steps:

[0049] (1) Decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are mixed together to obtain a flame retardant mixture;

[0050] (2) The wetting agent, defoaming agent and dispersant are uniformly dispersed in water and stirred at a high speed of 800 r / min. After dispersion for 3 minutes, the flame retardant mixture mixed in step (1) is added three times at a stirring speed of 800 r / min. After the viscosity of the mixture changes from viscous to thin, an anti-settling agent is added, and the stirring speed is adjusted to 2800 r / min. The mixture is stirred for 20 minutes. The uniformly dispersed flame retardant liquid is passed through a 60-mesh sieve to obtain a stable flame retardant dispersion.

[0051] Example 6

[0052] A stable flame retardant dispersion comprises the following components in parts by weight: 50 parts of water, 30 parts of decabromodiphenylethane, 20 parts of antimony trioxide, 20 parts of magnesium hydroxide, 10 parts of zinc borate, 3 parts of fumed silica, 1.5 parts of HT-110 moistening agent, and THI ® 1 part of X-318 defoamer and 7 parts of AKN-255 dispersant.

[0053] A method for preparing a stable flame retardant dispersion comprises the following steps:

[0054] (1) Decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are mixed together to obtain a flame retardant mixture;

[0055] (2) The wetting agent, defoaming agent and dispersant are uniformly dispersed in water and stirred at a high speed of 1200 r / min. After dispersion for 7 minutes, the flame retardant mixture mixed in step (1) is added three times at a stirring speed of 1200 r / min. After the viscosity of the mixture changes from viscous to thin, an anti-settling agent is added, and the stirring speed is adjusted to 3500 r / min. The mixture is stirred for 40 minutes. The uniformly dispersed flame retardant liquid is passed through a 60-mesh sieve to obtain a stable flame retardant dispersion.

[0056] The flame retardant dispersion was tested to observe its stability. The experimental data are shown in Table 1.

[0057] Table 1

[0058] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Test Container 100ml measuring cylinder 100ml measuring cylinder 100ml measuring cylinder 100ml measuring cylinder 100ml measuring cylinder 100ml measuring cylinder Testing time September - February of the following year September - February of the following year September - February of the following year September - February of the following year September - February of the following year September - February of the following year Minimum room temperature -10 degrees -10 degrees -10 degrees -10 degrees -10 degrees -10 degrees Whether frozen no no no no no no pH 7-8 7-8 7-8 7-8 7-8 7-8 Storage 2 months 1 ml of water precipitates out from the upper layer, but no precipitation occurs at the bottom 1 ml of water precipitates out from the upper layer, but no precipitation occurs at the bottom No water precipitated from the upper layer and no sediment was found at the bottom No water precipitated from the upper layer and no sediment was found at the bottom 1.5 ml of water precipitated from the upper layer, but no precipitation occurred at the bottom. 1.5 ml of water precipitated from the upper layer, but no precipitation occurred at the bottom. Storage 4 months 4 ml of water precipitated from the upper layer, but no precipitation occurred at the bottom 4 ml of water precipitated from the upper layer, but no precipitation occurred at the bottom 2 ml of water precipitated from the upper layer, but no precipitation occurred at the bottom 2 ml of water precipitated from the upper layer, but no precipitation occurred at the bottom 6 ml of water precipitated from the upper layer and precipitated from the bottom 4.5 ml of water precipitated from the upper layer, but no precipitation occurred at the bottom. Storage 6 months 7ml of water precipitates from the upper layer and there are lumps at the bottom 10ml of water precipitates out from the upper layer, and there are lumps at the bottom 5ml of water precipitates from the upper layer, and there is no hard lump at the bottom, but the bottom is sticky, the color is darker at the bottom and lighter at the top 3ml of water precipitates on the upper layer, no lumps at the bottom, not sticky, and the color is basically uniform 9ml of water precipitates from the upper layer, and there are lumps at the bottom 7ml of water precipitates from the upper layer and there are lumps at the bottom

[0059] The experimental conclusions are as follows:

[0060] Compared with Examples 1-6, the composite anti-settling agent has the best anti-settling effect.

[0061] The flame retardant dispersion prepared by the following components in parts by weight: 35 parts of water, 30 parts of decabromodiphenylethane, 10 parts of antimony trioxide, 10 parts of magnesium hydroxide, 5 parts of zinc borate, 3 parts of compound anti-settling agent, 1.5 parts of wetting agent HT-116, 0.5 parts of defoaming agent THI®X-318 and 0.5 parts of dispersant AKN-2555 has no lumps at the bottom after being stored for 6 months, can still be easily uniformed by simple stirring and has good storage stability.

[0062] The stable flame retardant dispersion prepared by the present invention has good stability and strong flame retardant effect. Decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are uniformly dispersed in water. The prepared flame retardant dispersion is added to the emulsion, which is more uniform than directly adding the flame retardant to the emulsion for dispersion. The synergistic effect between the flame retardants will be better.

[0063] The prepared flame retardant dispersion can be directly added into an aqueous emulsion, has simple operation, strong flame retardant effect and wide application range.

Claims

1. A method for preparing a stable flame retardant dispersion, characterized in that: The following steps are involved: (1) Decabromodiphenylethane, antimony trioxide, magnesium hydroxide and zinc borate are mixed together to obtain a flame retardant mixture; (2) Dispersing the wetting agent, defoaming agent and dispersant uniformly in water and stirring at a high speed of 800-1200 r / min. After dispersion for 3-7 minutes, adding the flame retardant mixture mixed in step (1) in three times at a stirring speed of 800-1200 r / min. After the viscosity of the mixture changes from viscous to thin, adding an anti-settling agent, adjusting the stirring speed to 2800-3500 r / min, stirring for 20-40 minutes, and passing the uniformly dispersed flame retardant liquid through a 60-mesh sieve to obtain a stable flame retardant dispersion; The stable flame retardant dispersion comprises the following components in parts by weight: 30-50 parts of water, 20-30 parts of decabromodiphenylethane, 10-20 parts of antimony trioxide, 10-20 parts of magnesium hydroxide, 5-10 parts of zinc borate, 0.5-3 parts of anti-settling agent, 1-1.5 parts of wetting agent, 0.5-1 part of defoaming agent, and 3-7 parts of dispersant; The anti-settling agent is fumed silica; The wetting agent is HT-116 wetting agent; The dispersant is AKN-255 dispersant; The defoamer is THI® X-318 defoamer.

Citation Information

Patent Citations

  • Low-smoke density additive-type flame retardant resin and application thereof

    CN102070869A

  • Phosphor nitrogen fire retardant dispersion and preparation method thereof

    CN102383210A

  • Efficient low-smoke flame-retardant textile coating adhesive and preparation method thereof

    CN103498341A

  • Fire-retardant thermoplastic polyolefin waterproof roll and preparation method thereof

    CN104441887A

  • Water-based suspension fire retardant containing red phosphorus micro-powder and preparation method and application of fire retardant

    CN104861203A