OCA optical glue and film for curved screen and preparation method thereof
By using components such as acrylate prepolymer and UV curing technology in the OCA optical film, the problem of insufficient bonding and filling performance of curved screens is solved, and an adhesive film with high stability and creep properties is achieved, which is suitable for Production and transportation of curved screens.
Patent Information
- Application Number
- CN202210842030.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-18
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-07-18
AI Technical Summary
The existing OCA optical film has insufficient mechanical tensile properties and filling properties during the bonding and filling process of curved screens, resulting in undesirable phenomena such as bubble rebound, poor stability, and intolerance to storage.
An OCA optical glue including acrylate prepolymer, photoinitiator, leveling agent, defoaming agent, antioxidant, coupling agent, cross-linking agent and polymerization inhibitor is used for one-time curing and Secondary curing to form a semi-cured state to improve bonding and filling properties, and use appropriate polymerization inhibitors to prevent the reaction of active double bonds and improve stability.
It achieves effective bonding of curved screens and ink step filling, avoids bubble rebound, improves the creep property and storage stability of the adhesive film, and is suitable for the production and transportation of curved screens.
Smart Images

Figure CN115124928B_ABST
Abstract
Description
[Technical field]
[0001] The invention relates to the technical field of optical adhesives, in particular to the technical field of OCA optical adhesives. [Background technology]
[0002] Driven by the development of the global electronics industry, the global touch display screen is developing faster and faster. The touch display era has quietly changed and enriched our daily life. Smart phones and tablets used in daily life are inseparable from touch screens. In particular, the increasingly popular curved screen technology has greatly improved our visual experience. In the assembly process of curved touch screens, OCA optical adhesive film is required to bond the special flexible curved screen and OLED. The curvature of the curved surface greatly increases the seamless bonding between the flexible screen and the OLED. The existing OCA optical adhesive film does not have excellent mechanical tensile properties and filling properties. It is difficult to meet the effective filling of the curved surface position and the ink step filling, and it is easy to have undesirable phenomena such as bubble rebound; and the stability is poor and it is not resistant to storage. [Summary of the invention]
[0003] The purpose of the present invention is to solve the problems in the prior art and to propose an OCA optical glue for a curved screen and a preparation method thereof. The adhesive film made by the OCA optical glue can not only meet the requirements of effective bonding of the flexible screen and the OLED at the curved surface position, but also meet the requirements of effective filling of the curved surface position and ink step filling, and has high stability and storage resistance.
[0004] To achieve the above purpose, the present invention proposes an OCA optical glue for a curved screen, comprising the following components in parts by weight: 100 parts of acrylate prepolymer, 0.3-1 parts of photoinitiator A, 0.5-3 parts of photoinitiator B, 0.05-0.2 parts of leveling agent, 0.1-0.3 parts of defoaming agent, 0.03-0.06 parts of antioxidant, 0.3-1 parts of coupling agent, 0.5-2 parts of cross-linking agent, and 0.01-0.05 parts of inhibitor.
[0005] Preferably, the composition includes the following components in parts by weight: 100 parts of acrylate prepolymer, 0.5 parts of photoinitiator A, 1 part of photoinitiator B, 0.1 parts of leveling agent, 0.2 parts of defoaming agent, 0.05 parts of antioxidant, 0.5 parts of coupling agent, 1 part of crosslinking agent, and 0.03 parts of inhibitor, wherein the photoinitiator A is a cationic photoinitiator.
[0006] Preferably, the acrylate prepolymer comprises the following components in parts by weight: 30-60 parts of 2-ethylhexyl acrylate, 10-25 parts of hydroxyethyl acrylate, 5-15 parts of hydroxybutyl acrylate, 3-10 parts of isobornyl methacrylate, 3-10 parts of isobornyl acrylate, 3-8 parts of acrylic acid, 5-20 parts of butyl acrylate, 1-5 parts of glycidyl methacrylate, 1-6 parts of deuterated methacrylate, 0.5-2 parts of a molecular weight regulator, and 0.3-0.7 parts of a photoinitiator C.
[0007] Preferably, the acrylate prepolymer comprises the following components in parts by weight: 40 parts of 2-ethylhexyl acrylate, 15 parts of hydroxyethyl acrylate, 10 parts of hydroxybutyl acrylate, 5 parts of isobornyl methacrylate, 5 parts of isobornyl acrylate, 5 parts of acrylic acid, 15 parts of n-butyl acrylate, 3 parts of glycidyl methacrylate, 2 parts of deuterated methacrylate, 1 part of molecular weight regulator, and 0.5 parts of photoinitiator C.
[0008] Preferably, the photoinitiator A is photoinitiator 6992, 9-(4-hydroxyethoxyphenyl) hexafluorophosphate, 4-isobutylphenyl-4'-methylphenyl iodine hexafluorophosphate, diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate, bis(4-(diphenylsulfonium)phenyl)sulfide-bishexafluorophosphate, bis(4-tert-butylphenyl)iodine toluenesulfonate, sulfonium hexafluoroantimonate, bis(4-tert-butylphenyl)iodine hexafluorophosphate, diphenyl iodine hexafluoroarsenate, diphenyl iodine trifluoromethanesulfonate, 2-(3,4-dimethoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 4-isopropyl-4'-methyldiphenyl iodine tetra( The photoinitiator B is one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexylphenyl ketone, benzophenone, a, a-dimethoxy-a-phenylacetophenone, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone; the leveling agent is one or more of BYK-358N, BYK371, BYK370, BYK3700; the defoaming agent is TEGO Foamex 842, tegofoamex The antioxidant is one or more of antioxidant 1076, antioxidant 703, and antioxidant 1010; the coupling agent is one or more of KH550, KH560, and KH570; the crosslinking agent is one or more of 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, di-trimethylolpropane tetraacrylate, and trimethylolpropane triacrylate; the polymerization inhibitor is one or more of hydroquinone, p-hydroxyanisole, methyl hydroquinone, 2-tert-butylhydroquinone, and 2,5-di-tert-butylhydroquinone; the molecular weight regulator is one or more of n-dodecyl mercaptan, isooctyl thioglycolate, and tert-dodecyl mercaptan; the photoinitiator C is one or more of 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide.
[0009] Preferably, the photoinitiator A is photoinitiator 6992; the photoinitiator B is diphenyl-(2,4,6-trimethylbenzoyl)phosphine; the leveling agent is BYK370; the defoaming agent is TEGO foamex840; the antioxidant is antioxidant 703; the coupling agent is a one-to-one mixture of KH550 and KH560; the crosslinking agent is 1,6-hexanediol diacrylate; the inhibitor is hydroquinone; the molecular weight regulator is n-dodecyl mercaptan; and the photoinitiator C is 1-hydroxycyclohexyl phenyl ketone.
[0010] The present invention also proposes a method for preparing OCA optical glue for a curved screen, comprising the following steps:
[0011] a. Preparation of acrylic prepolymer: weigh the raw materials of prepolymer according to the ratio; add the raw materials into the glass reactor in sequence, stir them evenly for a certain period of time under the protection of nitrogen atmosphere, and then irradiate them with UV light to cause free radical polymerization reaction. The viscosity of the prepolymer is controlled to be 3000-30000mpa﹒s, the weight average molecular weight is between 600,000 and 3 million, and the glass transition temperature is between -40℃ and 20℃;
[0012] b. Add the acrylate prepolymer obtained in step a, photoinitiator A, photoinitiator B, leveling agent, defoaming agent, antioxidant, coupling agent, crosslinking agent and polymerization inhibitor into a glass reactor in order according to the proportion, and stir at room temperature for 1-3 hours to obtain OCA glue.
[0013] The present invention also proposes an OCA optical adhesive film for a curved screen, comprising a heavy release film and a light release film, wherein an optical adhesive layer is provided between the heavy release film and the light release film layer, and the optical adhesive layer is prepared by coating the above-mentioned OCA optical glue for a curved screen.
[0014] As a preferred method, the thickness of the adhesive film is 50-200um, and the antistatic value of the heavy release film and the light release film is 10 6 -10 9 Ω, thickness is between 50-150um.
[0015] Preferably, the heavy release film and the light release film are both optical grade release films with a transmittance greater than 90%, the thickness of the adhesive film is 125um, the thickness of the optical heavy release film is 100um, and the thickness of the optical light release film layer is 75um.
[0016] Preferably, the release force of the light release film is 5-10 gf / in, and the release force of the heavy release film is 15-35 gf / in.
[0017] The present invention also proposes a method for preparing an OCA optical adhesive film for a curved screen, comprising the following steps: the OCA glue prepared in step b is allowed to stand at room temperature for defoaming, the OCA glue is coated between an optical PET heavy release film and an optical PET light release film, and is cured by ultraviolet light irradiation for a certain period of time to obtain a semi-cured curved screen OCA optical adhesive film, the wavelength of the ultraviolet light is 330-420nm, and after the OCA adhesive film is initially bonded to the screen, it is cured by ultraviolet light irradiation for a certain period of time, the wavelength of the ultraviolet light is 200-310nm.
[0018] Beneficial effects of the present invention:
[0019] (1) After being cured, the OCA optical adhesive film for curved screens prepared by the present invention will remain in a semi-cured state and have good creep properties. This semi-cured state can effectively bond the flexible screen and OLED at the curved surface position, and can also effectively fill different ink step differences, and will not cause undesirable phenomena such as bubble rebound under normal temperature, high temperature and high humidity environments;
[0020] (2) The cured OCA optical adhesive film is firstly bonded to the screen, and then degassed under pressure, and then secondary cured to achieve true curing and bonding. This secondary curing adhesive film technology can be well applied to the technical field of OCA adhesive film for curved screens, which is of great significance to the future development of curved screen mobile phones;
[0021] (3) Since the unreacted active double bonds in the OCA optical film are effectively inhibited by adding an inhibitor, the creep stability is good, which ensures the effective storage of the OCA film product and ensures the stable performance of the product during transportation and in the downstream touch module factory;
[0022] (4) by adding photoinitiator A and photoinitiator B into the formula of optical glue, photoinitiator B is used as the initiator of primary curing; photoinitiator A is a cationic photoinitiator, which is used as the initiator of secondary curing to achieve true curing bonding;
[0023] (5) First, the monomers of the optical adhesive system are initiated by photoinitiator C to undergo free radical polymerization to obtain an acrylate prepolymer, and then photoinitiator A, photoinitiator B and other additives are added to the acrylate prepolymer to obtain an optical adhesive; after the optical adhesive is made into an optical adhesive film, it is first irradiated with medium-wave ultraviolet rays to activate only the photoinitiator B, so that the optical adhesive is cured once to obtain a semi-cured optical adhesive soft film; after the optical adhesive is bonded, it is irradiated with short-wave ultraviolet rays to activate the photoinitiator A and perform secondary curing to achieve true cured bonding; (meth)acrylates (such as glycidyl methacrylate) and cationic photoinitiators with cationic heterocyclic alkane structures are further cross-linked and cured when exposed to short-wavelength radiation, thereby increasing the tensile strength and bonding strength of the adhesive film. This secondary curing method facilitates the transportation and use of the optical adhesive and has a good bonding effect.
[0024] The features and advantages of the present invention will be described in detail through embodiments in conjunction with the accompanying drawings.
Brief Description of the Drawings
[0025] Figure 1 It is a schematic structural diagram of an OCA optical adhesive film for a curved screen according to the present invention.
[0026] In the figure: 1-heavy release film, 2-light release film layer, 3-optical adhesive layer. [Specific implementation method]
[0027] Embodiment 1:
[0028] The present embodiment provides an OCA optical glue for a curved screen, comprising the following components in parts by weight: 100 parts of acrylate prepolymer, 0.5 parts of photoinitiator 6992, 1 part of photoinitiator TPO, 0.1 parts of leveling agent BYK370, 0.2 parts of defoaming agent TEGOfoamex 840, 0.05 parts of antioxidant 703, 0.5 parts of a mixture of KH550 and KH560 in a mass ratio of 1:1, 1 part of 1,6-hexanediol diacrylate, and 0.01 parts of hydroquinone.
[0029] The acrylate prepolymer includes the following components in parts by weight: 40 parts of 2-ethylhexyl acrylate, 15 parts of hydroxyethyl acrylate, 10 parts of hydroxybutyl acrylate, 5 parts of isobornyl methacrylate, 5 parts of isobornyl acrylate, 5 parts of acrylic acid, 15 parts of n-butyl acrylate, 3 parts of glycidyl methacrylate, 2 parts of deuterated methacrylate, 1 part of n-dodecyl mercaptan, and 0.5 parts of photoinitiator 184 (1-hydroxycyclohexyl phenyl ketone).
[0030] Preparation method:
[0031] a. Add the raw materials for preparing acrylate prepolymer into a glass reactor in order according to the ratio, stir evenly under the protection of nitrogen atmosphere, and irradiate with UV light to cause free radical polymerization reaction. The wavelength of the ultraviolet light is 246-350nm, and the viscosity of the prepolymer is controlled to be 3000-30000mpa﹒s.
[0032] The average molecular weight is between 600,000 and 3 million, and the glass transition temperature is between -40℃ and 20℃;
[0033] b. Add the above-prepared acrylate prepolymer and other raw materials for preparing optical adhesive into a glass reactor in sequence, and stir for 1-3 hours at room temperature to obtain an OCA optical adhesive product for curved screens;
[0034] c. The prepared OCA optical glue was allowed to stand at room temperature for 2 hours to defoam, and then the OCA glue was coated between the optical PET heavy release film and the optical PET light release film, and cured by ultraviolet light irradiation for a certain period of time. The ultraviolet light energy used was 6000mj / cm 2 The wavelength of ultraviolet light is 365nm, the curing time is 400s, and the thickness of the film is controlled to be 125um. After irradiation, a semi-cured curved screen OCA optical film product is obtained. The structure is as follows Figure 1 shown.
[0035] After the initial bonding of the module and the curved cover, the OCA optical film is pressurized at room temperature to remove bubbles, and then secondary cured under a UV wavelength of 288nm with an energy of 3500mj / cm 2 , curing time 40s, completing the bonding of the module and the curved cover.
[0036] Embodiment 2:
[0037] The present embodiment provides an OCA optical glue for a curved screen, comprising the following components in parts by weight: 100 parts of acrylate prepolymer, 0.5 parts of photoinitiator 6992, 1 part of photoinitiator TPO, 0.1 parts of leveling agent BYK370, 0.2 parts of defoaming agent TEGOfoamex 840, 0.05 parts of antioxidant 703, 0.5 parts of a mixture of KH550 and KH560 in a mass ratio of 1:1, 1 part of 1,6-hexanediol diacrylate, and 0.02 parts of hydroquinone.
[0038] The proportion of the acrylic ester prepolymer is the same as that in Example 1.
[0039] The preparation method is the same as that in Example 1.
[0040] Embodiment 3:
[0041] The present embodiment provides an OCA optical glue for a curved screen, comprising the following components in parts by weight: 100 parts of acrylate prepolymer, 0.5 parts of photoinitiator 6992, 1 part of photoinitiator TPO, 0.1 parts of leveling agent BYK370, 0.2 parts of defoaming agent TEGOfoamex 840, 0.05 parts of antioxidant 703, 0.5 parts of a mixture of KH550 and KH560 in a mass ratio of 1:1, 1 part of 1,6-hexanediol diacrylate, and 0.03 parts of hydroquinone.
[0042] The proportion of the acrylic ester prepolymer is the same as that in Example 1.
[0043] The preparation method is the same as that in Example 1.
[0044] Embodiment 4:
[0045] The present embodiment provides an OCA optical glue for a curved screen, comprising the following components in parts by weight: 100 parts of acrylate prepolymer, 0.5 parts of photoinitiator 6992, 1 part of photoinitiator TPO, 0.1 parts of leveling agent BYK370, 0.2 parts of defoaming agent TEGOfoamex 840, 0.05 parts of antioxidant 703, 0.5 parts of a mixture of KH550 and KH560 in a mass ratio of 1:1, 1 part of 1,6-hexanediol diacrylate, and 0.04 parts of hydroquinone.
[0046] The proportion of the acrylic ester prepolymer is the same as that in Example 1.
[0047] The preparation method is the same as that in Example 1.
[0048] Embodiment 5:
[0049] The present embodiment provides an OCA optical glue for a curved screen, comprising the following components in parts by weight: 100 parts of acrylate prepolymer, 0.5 parts of photoinitiator 6992, 1 part of photoinitiator TPO, 0.1 parts of leveling agent BYK370, 0.2 parts of defoaming agent TEGOfoamex 840, 0.05 parts of antioxidant 703, 0.5 parts of a mixture of KH550 and KH560 in a mass ratio of 1:1, 1 part of 1,6-hexanediol diacrylate, and 0.05 parts of hydroquinone.
[0050] The proportion of the acrylic ester prepolymer is the same as that in Example 1.
[0051] The preparation method is the same as that in Example 1.
[0052] Embodiment 6:
[0053] The present embodiment provides an OCA optical glue for a curved screen, comprising the following components in parts by weight: 100 parts of acrylate prepolymer, 69921 parts of photoinitiator, 3 parts of photoinitiator TPO, 0.2 parts of leveling agent BYK370, 0.3 parts of defoaming agent TEGO foamex840, 0.06 parts of antioxidant 703, 1 part of KH550, 2 parts of 1,6-hexanediol diacrylate, and 0.03 parts of hydroquinone.
[0054] The acrylate prepolymer includes the following components in parts by weight: 30 parts of 2-ethylhexyl acrylate, 10 parts of hydroxyethyl acrylate, 5 parts of hydroxybutyl acrylate, 3 parts of isobornyl methacrylate, 3 parts of isobornyl acrylate, 3 parts of acrylic acid, 5 parts of n-butyl acrylate, 1 part of glycidyl methacrylate, 1 part of deuterated methacrylate, 0.5 parts of n-dodecyl mercaptan, and 0.3 parts of photoinitiator 184 (1-hydroxycyclohexyl phenyl ketone).
[0055] The preparation method is the same as that in Example 1.
[0056] Embodiment 7:
[0057] The present embodiment provides an OCA optical glue for a curved screen, comprising the following components in parts by weight: 100 parts of acrylate prepolymer, 0.3 parts of photoinitiator 6992, 0.5 parts of photoinitiator TPO, 0.05 parts of leveling agent BYK370, 0.1 parts of defoaming agent TEGOfoamex 840, 0.03 parts of antioxidant 703, 0.3 parts of KH550, 0.5 parts of 1,6-hexanediol diacrylate, and 0.03 parts of hydroquinone.
[0058] The acrylate prepolymer includes the following components in parts by weight: 60 parts of 2-ethylhexyl acrylate, 25 parts of hydroxyethyl acrylate, 15 parts of hydroxybutyl acrylate, 10 parts of isobornyl methacrylate, 10 parts of isobornyl acrylate, 8 parts of acrylic acid, 20 parts of n-butyl acrylate, 5 parts of glycidyl methacrylate, 6 parts of deuterated methacrylate, 2 parts of n-dodecyl mercaptan, and 0.7 parts of photoinitiator 184 (1-hydroxycyclohexyl phenyl ketone).
[0059] The preparation method is the same as that in Example 1.
[0060] Comparative Example 1: An OCA optical glue for a curved screen comprises the following components in parts by weight: 100 parts of acrylate prepolymer, 0.5 parts of photoinitiator 6992, 1 part of photoinitiator TPO, 0.1 parts of leveling agent BYK370, 0.2 parts of defoaming agent TEGO foamex840, 0.05 parts of antioxidant 703, 0.5 parts of a mixture of KH550 and KH560 in a mass ratio of 1:1, and 1 part of 1,6-hexanediol diacrylate.
[0061] The proportion of the acrylic ester prepolymer is the same as that in Example 1.
[0062] The preparation method is the same as that in Example 1.
[0063] The optical adhesives prepared in Examples 1-5 and Comparative Example 1 were tested for performance, and the results are shown in Tables 1 and 2.
[0064] Table 1
[0065]
[0066]
[0067] Table 2
[0068]
[0069] (Note: The creep values in Table 1 are the creep values of the OCA film products tested after being placed for 1 day, 7 days, 14 days, 30 days, 60 days and 120 days respectively; the test method is: the OCA film products are stacked into 800um thickness, and the creep value is measured by a rheometer (TA company model ARES-G2) with a parallel plate fixture. The test conditions are constant stress 1000Pa, temperature 40℃, and strain time 360 seconds;
[0070] BF refers to the semi-cured OCA film product before secondary curing; AF refers to the cured film obtained by curing the OCA film product before secondary curing in an LED curing box;
[0071] In Table 2, the BF 1D film product is the OCA film sample that was placed for 1 day before secondary curing, and the AF 1D film product is the film product that was placed for 1 day before secondary curing and cured in an LED curing box, and the LED energy is 3500mj / cm 2 ;
[0072] In Table 2, the tensile strength of BF 1D and AF 1D is tested by cutting the OCA film into 25mm*5cm strips, pasting them on two 150um thick PET films, placing them under constant temperature and humidity conditions for 30MIN, and then testing them with a tensile machine to obtain the tensile strength values;
[0073] In Table 2, the adhesion test method is: cut the OCA film product into 25mm*15cm strips, tear off the light release film, and stick it on the 50umPET substrate, then tear off the heavy release film and stick it on the bare glass cover, use a 2kg roller to roll back and forth three times at a speed of 300mm / min, let it stand for 30MIN under constant temperature and humidity conditions, and use a tensile machine to test the adhesion of the OCA film to the bare glass cover at a speed of 300mm / min; In Table 2, the normal temperature ink step filling experiment is to stick the OCA film on the CG glass cover with an ink step height of 20um, use an automatic vacuum laminating machine for laminating, set the laminating pressure to 2kg, the negative pressure to 100Kpa, and the laminating time to 20 seconds; then put it into a high-pressure degassing machine for degassing, and set the condition to pressurize and degas for 30MIN at room temperature under a pressure of 0.4Mpa; finally, observe the filling property of the OCA film on the ink step CG cover under normal temperature conditions;
[0074] In Table 2, the reverse disassembly performance of the OCA film was verified by reverse disassembly under the condition of 80℃*10sec.
[0075] It can be concluded from Examples 1-5 that too low an inhibitor content cannot achieve a good inhibitory effect, while too high an inhibitor content will seriously affect the cross-linking and curing effect of the OCA film, resulting in a very low tensile strength, which is not conducive to the downstream reprocessing of the OCA film.
[0076] Example 3 has a good implementation effect. The addition of a suitable amount of hydroquinone inhibitor effectively inhibits the polymerization of the unreacted active double bonds in the OCA film, so the product has a stable creep value and is relatively stable over time. Example 3 has a high tensile strength before and after secondary curing, which ensures that the OCA film has excellent anti-disassembly performance and has a high bonding force, ensuring effective bonding to the CG cover plate and the module.
[0077] The present invention focuses on screening the types and amounts of suitable photoinitiators A and B, and adding a suitable amount of inhibitors. When the OCA optical adhesive is cured once, the wavelength of ultraviolet rays only activates the photoinitiator B to trigger the OCA optical adhesive to undergo a certain cross-linking and curing reaction, thereby obtaining a semi-cured adhesive film. When the OCA optical adhesive is cured for the second time, short-wave ultraviolet rays will activate the photoinitiator A, triggering the epoxy groups in the OCA optical adhesive to undergo further cross-linking and curing reaction, thereby obtaining a completely cured adhesive film. The effect of the inhibitor prevents the adhesive film after the once-curing from undergoing a slow cross-linking and curing reaction during a long period of storage, thereby improving the stable creep property of the adhesive film.
[0078] The above embodiments are intended to illustrate the present invention, not to limit the present invention. Any solution that is a simple transformation of the present invention belongs to the protection scope of the present invention.
Claims
1. An OCA optical glue for curved screens, It is characterized in that The invention comprises the following components in parts by weight: 100 parts of acrylate prepolymer, 0.3-1 parts of photoinitiator A, 0.5-3 parts of photoinitiator B, 0.05-0.2 parts of leveling agent, 0.1-0.3 parts of defoaming agent, 0.03-0.06 parts of antioxidant, 0.3-1 parts of coupling agent, 0.5-2 parts of crosslinking agent and 0.01-0.05 parts of polymerization inhibitor, wherein the photoinitiator A can be activated by ultraviolet light with a wavelength of 200-310 nm, the photoinitiator B can be activated by ultraviolet light with a wavelength of 330-420 nm, and the photoinitiator A is a cationic photoinitiator; The acrylate prepolymer comprises the following components in parts by weight: 30-60 parts of 2-ethylhexyl acrylate, 10-25 parts of hydroxyethyl acrylate, 5-15 parts of hydroxybutyl acrylate, 3-10 parts of isobornyl methacrylate, 3-10 parts of isobornyl acrylate, 3-8 parts of acrylic acid, 5-20 parts of butyl acrylate, 1-5 parts of glycidyl methacrylate, 1-6 parts of deuterated methacrylate, 0.5-2 parts of a molecular weight regulator and 0.3-0.7 parts of a photoinitiator C.
2. The OCA optical glue for curved screen according to claim 1, It is characterized in that The invention comprises the following components in parts by weight: 100 parts of acrylate prepolymer, 0.5 parts of photoinitiator A, 1 part of photoinitiator B, 0.1 parts of leveling agent, 0.2 parts of defoaming agent, 0.05 parts of antioxidant, 0.5 parts of coupling agent, 1 part of crosslinking agent and 0.03 parts of polymerization inhibitor.
3. The OCA optical glue for curved screen according to claim 1, It is characterized in that The acrylate prepolymer comprises the following components in parts by weight: 40 parts of 2-ethylhexyl acrylate, 15 parts of hydroxyethyl acrylate, 10 parts of hydroxybutyl acrylate, 5 parts of isobornyl methacrylate, 5 parts of isobornyl acrylate, 5 parts of acrylic acid, 15 parts of n-butyl acrylate, 3 parts of glycidyl methacrylate, 2 parts of deuterated methacrylate, 1 part of molecular weight regulator, and 0.5 parts of photoinitiator C.
4. The OCA optical glue for curved screen according to claim 1, Features: The photoinitiator A is photoinitiator 6992, 9-(4-hydroxyethoxyphenyl) hexafluorophosphate, 4-isobutylphenyl-4'-methylphenyl iodonium hexafluorophosphate, diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate, bis(4-(diphenylsulfonium)phenyl)sulfide-bishexafluorophosphate, bis(4-tert-butylphenyl)iodonium p-toluenesulfonate, sulfonium hexafluoroantimonate, bis(4-tert-butylphenyl)iodonium hexafluorophosphate, diphenyl iodonium hexafluoroarsenate, diphenyl iodonium trifluoromethanesulfonate, 2-(3,4-dimethoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 4-isopropyl-4'-methyldiphenyl iodonium tetra(pentafluoro) The photoinitiator B is one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexylphenyl ketone, benzophenone, a, a-dimethoxy-a-phenylacetophenone, diphenyl-(2,4,6-trimethylbenzoyl)phosphine, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone; the leveling agent is one or more of BYK-358N, BYK371, BYK370, BYK3700; the defoaming agent is TEGO Foamex 842, tego foamex The antioxidant is one or more of antioxidant 1076, antioxidant 703, and antioxidant 1010; the coupling agent is one or more of KH550, KH560, and KH570; the crosslinking agent is one or more of 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, di-trimethylolpropane tetraacrylate, and trimethylolpropane triacrylate; the polymerization inhibitor is one or more of hydroquinone, p-hydroxyanisole, methyl hydroquinone, 2-tert-butylhydroquinone, and 2,5-di-tert-butylhydroquinone; the molecular weight regulator is one or more of n-dodecyl mercaptan, isooctyl thioglycolate, and tert-dodecyl mercaptan; the photoinitiator C is one or more of 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide.
5. The OCA optical glue for curved screen as claimed in claim 4, Features: The photoinitiator A is photoinitiator 6992; the photoinitiator B is diphenyl-(2,4,6-trimethylbenzoyl)phosphine; the leveling agent is BYK370; the defoaming agent is TEGO foamex 840; the antioxidant is antioxidant 703; the coupling agent is a 1:1 mixture of KH550 and KH560; the crosslinking agent is 1,6-hexanediol diacrylate; the inhibitor is hydroquinone; the molecular weight regulator is n-dodecyl mercaptan; and the photoinitiator C is 1-hydroxycyclohexyl phenyl ketone.
6. A method for preparing the OCA optical glue for curved screens as claimed in any one of claims 1 to 5, It is characterized in that The following steps are involved: a. Preparation of acrylic prepolymer: weigh the raw materials of prepolymer according to the ratio; add the raw materials into the glass reactor in sequence, stir them evenly under the protection of nitrogen atmosphere, and then irradiate them with UV light to cause free radical polymerization reaction. The viscosity of the prepolymer is controlled to be 3000-30000mpa﹒s, the weight average molecular weight is between 600,000 and 3 million, and the glass transition temperature is between -40℃ and 20℃; b. Add the acrylate prepolymer obtained in step a, photoinitiator A, photoinitiator B, leveling agent, defoaming agent, antioxidant, coupling agent, crosslinking agent and polymerization inhibitor into a glass reactor in order according to the proportion, and stir at room temperature for 1-3 hours to obtain OCA glue.
7. An OCA optical film for curved screens, Features: It comprises a heavy release film (1) and a light release film (2), wherein an optical adhesive layer (3) is provided between the heavy release film (1) and the light release film layer (2), and the optical adhesive layer (3) is prepared by coating the OCA optical adhesive for curved screens according to any one of claims 1 to 5.
8. A method for preparing an OCA optical adhesive film for a curved screen, It is characterized in that The method comprises the following steps: allowing the OCA glue prepared in claim 7 to stand for defoaming, coating the OCA glue between a heavy release film and a light release film, and curing the film by irradiating the film with ultraviolet light for a certain period of time to obtain a semi-cured curved screen OCA optical adhesive film, wherein the wavelength of the ultraviolet light is 330-420nm.
9. A method for preparing an OCA optical adhesive film for a curved screen. It is characterized in that The method comprises the following steps: after initially bonding the OCA adhesive film prepared in claim 8 to the screen, secondary curing is performed by irradiating ultraviolet light for a certain period of time, wherein the wavelength of the ultraviolet light is 200-310 nm.