Silicon-carbon negative electrode energy storage material and preparation method thereof
By using the preparation method of silicon carbon negative electrode material in lithium-ion batteries, the silicon dioxide-coated molybdenum carbide material is formed by using magnesium thermal reduction treatment, the performance attenuation problem caused by volume expansion of silicon material in lithium-ion batteries is solved, and high Energy density and stability are improved.
Patent Information
- Application Number
- CN202210819273.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-13
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-07-13
AI Technical Summary
The electrochemical energy storage materials of existing lithium-ion batteries have shortcomings in terms of high energy density and cycle stability, especially due to the performance attenuation problems caused by volume expansion of silicon materials.
Using the preparation method of silicon-carbon negative electrode material, the high temperature reflux of molybdate, 2-methylimidazole and zinc acetate in N,N-dimethylformamide, and then the ultrasonic dispersion in water and ethanol was uniformly distributed, and the magnesium was used. Thermal reduction treatment forms a silica-coated molybdenum carbide material, reducing the external load of silicon and enhancing the stability of the material.
It significantly improves the energy density and cycle stability of lithium-ion batteries, inhibits the battery performance attenuation caused by volume expansion of silicon, provides a multi-variable negative electrode material with low silicon load, and improves the long cycle performance of the battery.
Smart Images

Figure CN115132996B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new energy and storage materials, and specifically relates to a silicon-carbon negative electrode energy storage material with a low silicon content. The present invention also relates to a method for preparing the silicon-carbon negative electrode energy storage material. Background Art
[0002] In recent years, the energy crisis and environmental pollution caused by fossil fuels have become increasingly serious. Scientists are committed to developing clean, green, renewable energy. Renewable energy sources such as solar energy and wind energy account for an increasing share of total energy consumption. The discontinuity of these energy outputs makes electrochemical energy storage and conversion technologies highly sustainable. The research and design of electrochemical energy storage electrode materials, and conversion technology can be the key to practical applications. For example, various single-crystal silicon cells, dye-sensitized cells, and perovskite cells developed in recent years can effectively convert solar energy into electrical energy. On this basis, storing the electrical energy converted from intermittent solar energy, wind energy, and tidal energy can effectively broaden the scope of application of renewable energy.
[0003] In terms of battery energy storage, lithium-ion batteries have more excellent performance in terms of energy density and service life. The new MOFs material is a crystalline porous material formed by the combination of metal ions and organic ligands through coordination bonds. It has the advantages of porosity, high specific surface area, structural diversity and designability, and has potential application prospects in the fields of optics, sensing, catalysis and energy storage. The unique structure of MOFs materials is suitable for constructing electrode materials in electrochemical devices. For example, Professor Wang Hui of Northwest University designed a material with N-doped yolk shell carbon nanocage structure derived from Zn-based and Co-based bimetallic MOFs. Due to selenization, in this special structure, ZnSe and CoSe2 nanodots are evenly distributed in the carbon grid with hollow internal structure constraints. The interface effect between the two can accelerate the diffusion of lithium ions and sodium ions in the solid, and the highly mesoporous N-doped amorphous carbon derived from MOF, as a closed reactor, can increase thermodynamic stability. The large void space of amorphous carbon can also inhibit structural instability and reduce the inevitable volume expansion of active materials, thereby improving battery performance. Summary of the invention
[0004] The purpose of the present invention is to provide a silicon-carbon negative electrode energy storage material, which can be used in high energy density lithium ion batteries.
[0005] Another object of the present invention is to provide a method for preparing the silicon-carbon negative electrode energy storage material.
[0006] The first technical solution adopted by the present invention is that the silicon-carbon negative electrode energy storage material includes a battery-specific copper foil, the copper foil is used as a current collector, and the silicon-carbon negative electrode active material is coated on the copper foil; the electrode material is a double-layer structure of copper foil and silicon-carbon negative electrode.
[0007] The second technical solution adopted by the present invention is a method for preparing a silicon-carbon negative electrode material, and the specific operating steps are as follows:
[0008] Step 1, molybdic acid, 2-methylimidazole and zinc acetate are mixed in N,N-dimethylformamide, added into a round-bottom flask, refluxed at 120° C., cooled to room temperature, filtered, and dried to obtain a white precursor powder A;
[0009] Step 2: uniformly disperse the white precursor powder A in a mixed solution of water and ethanol by ultrasound, then add hexadecyltrimethylammonium bromide and ethyl orthosilicate in sequence, stir, collect the precipitate by centrifugation, and dry at 60° C. to obtain a silica-coated white precursor powder B.
[0010] Step 3, the precursor powder B is mixed with magnesium powder and sodium chloride in a certain mass ratio, ground evenly and placed in a corundum porcelain boat, and placed in a programmable temperature-controlled tube furnace under the protection of a N2 atmosphere, and heated to 600°C at a heating rate of 2°C / min, kept warm for 6 hours, and then naturally cooled to room temperature to obtain silicon-coated molybdenum carbide black powder C;
[0011] Step 4, washing the black powder C with dilute hydrochloric acid HCl to remove unreacted magnesium powder and NaCl, washing with water until neutral, and drying at 60° C. to obtain black powder D.
[0012] Step 5: Mix the black powder D with carbon black and polyvinylidene fluoride in proportion, grind thoroughly, add N-methylpyrrolidone dropwise, and continue grinding to form a uniform slurry E.
[0013] Step 6: Ultrasonic treatment of copper foil of a certain thickness in an ethanol solution, and then drying in a forced air drying oven.
[0014] Step 7, the slurry E obtained in step 6 is scraped onto the copper foil with a scraper to a certain thickness, and then placed in an 80° C. forced air drying oven for drying.
[0015] Step 8: Use a sheet pressing machine to press the prepared electrode into a circular electrode sheet with a diameter of 14 mm, place it in a vacuum drying oven at 60° C. to dry it, and make it into a negative electrode sheet M.
[0016] Step 9, assemble the negative electrode M and the positive electrode lithium sheet into a button battery in a glove box filled with argon Ar in the order of positive electrode shell, negative electrode sheet, electrolyte, diaphragm, lithium sheet, gasket, spring and negative electrode shell for subsequent performance testing.
[0017] The present invention is also characterized in that:
[0018] In step 1, zinc acetate can be replaced by any one of zinc chloride, zinc nitrate and zinc sulfate.
[0019] The reflux temperature in step 1 can be selected within the range of 100 to 160° C., the reflux time can be between 3 and 34 hours, water or ethanol can be used for washing, the drying temperature is between 60 and 100° C., and the drying time is between 1 and 6 hours.
[0020] In step 2, the volume ratio of ethanol to water is 1:1, the ultrasonic time is 30 to 60 minutes, the stirring time is 1 to 3 hours, the drying temperature is 60 to 100° C., and the drying time is 1 to 6 hours.
[0021] In step 3, the mass ratio of white powder B to magnesium powder Mg and sodium chloride NaCl is 1:1:1.
[0022] In step 4, the molar concentration of the dilute hydrochloric acid used is 1.0 mol / L.
[0023] In step 5, the mixed mass ratio of the washed and dried silicon-coated molybdenum carbide powder D, carbon black and polyvinylidene fluoride PVDF is 8:1:1.
[0024] The temperature of the drying oven in step 6 and step 7 is 60-100°C.
[0025] The synthesis principle of the key steps in the present invention is:
[0026] (i) Synthesis of precursors: Synthesis of ZnMo-bimetallic organic framework with highly ordered crystalline structure;
[0027] (ii) Synthesis of core-shell silica-coated precursor powder: The room temperature solution phase synthesis method was used to coat ethyl orthosilicate and dry it to obtain silica-coated precursor powder. The capacity of the electrode material was increased and the stability was enhanced by low silicon doping.
[0028] (III) Synthesis of reduced silicon-coated molybdenum carbide powder: By means of magnesium thermal reduction heat treatment, the silicon dioxide coated on the surface of the ZnMo crystalline support precursor is reduced to silicon element, while a very small amount of silicon enters the interior of the molybdenum carbide / carbon material and converts the material into a molybdenum carbide / carbon material.
[0029] The beneficial effects of the present invention are
[0030] (1) Synthesis of ZnMo bimetallic organic crystalline framework precursor, which can be converted into molybdenum carbide / carbon material during subsequent heat treatment.
[0031] (2) Through solution coating and in-situ magnesium thermal reduction treatment, a very small amount of silicon is coated on the surface of the molybdenum carbide / carbon material, and a very small amount of silicon also enters the interior of the molybdenum carbide / carbon material, so that during the battery cycle, the battery performance can be inhibited from being attenuated due to the volume expansion of part of the silicon itself.
[0032] (3) The present invention provides a method for preparing a multi-element negative electrode material with low silicon loading, and the energy density and stability of the battery assembled using the electrodes are greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a flow chart of the method for preparing the silicon-carbon negative electrode energy storage material of the present invention;
[0034] Figure 2 It is a relationship diagram between current and voltage of the silicon-carbon negative electrode energy storage material of the present invention at a scanning rate of 0.2mV / s;
[0035] Figure 3 It is the electrochemical impedance diagram of the silicon-carbon negative electrode energy storage material of the present invention;
[0036] Figure 4 This is the long cycle performance diagram of the silicon-carbon negative electrode energy storage material of the present invention at a current density of 500mA / g DETAILED DESCRIPTION
[0037] The silicon-carbon negative electrode energy storage material provided by the present invention comprises a copper foil specially used for batteries. The copper foil is used as a current collector and coated with a silicon-carbon negative electrode active material. The electrode material is a double-layer structure of the copper foil and the silicon-carbon negative electrode.
[0038] The present invention will be further described below in conjunction with specific embodiments.
[0039] Embodiment 1:
[0040] Preparation method of silicon carbon negative electrode material Figure 1 The specific steps are as follows:
[0041] Step 1, molybdic acid, 2-methylimidazole and zinc acetate are mixed in 120 ml of DMF, refluxed at 160° C. for 12 hours, cooled to room temperature, filtered, and dried in an oven at 60° C. for 8 hours to obtain a white precursor powder A;
[0042] Step 2: uniformly disperse the white precursor powder A in a mixed solution of water and ethanol by ultrasound, then add hexadecyltrimethylammonium bromide and ethyl orthosilicate in sequence, perform ultrasonic treatment for 40 minutes, stir for 2 hours, collect the precipitate by centrifugation, and dry at 60° C. to obtain a silica-coated white precursor powder B.
[0043] Step 3, white powder B is mixed with magnesium powder and sodium chloride in a mass ratio of 1:1:0.8 and placed in a corundum porcelain boat, and placed in a programmable temperature-controlled tube furnace under the protection of a N2 atmosphere, and heated to 600°C at a heating rate of 2°C / min, kept warm for 7 hours, and then naturally cooled to room temperature to obtain silicon-coated molybdenum carbide black powder C;
[0044] Step 4, washing the black powder C with dilute hydrochloric acid HCl to remove unreacted magnesium powder and NaCl, washing with water until neutral, and drying at 60° C. to obtain black powder D.
[0045] Step 5: Mix the black powder D with carbon black and polyvinylidene fluoride in proportion, grind thoroughly, add N-methylpyrrolidone dropwise, and continue grinding to form a uniform slurry E.
[0046] Step 6: Ultrasonic treatment of copper foil of a certain thickness in an ethanol solution, and then drying in a 60° C. forced air drying oven.
[0047] Step 7, the slurry E obtained in step 5 is scraped onto the copper foil with a scraper to a certain thickness, and then placed in a 60° C. forced air drying oven for drying.
[0048] Step 8: Use a sheet pressing machine to press the prepared electrode into a circular electrode sheet with a diameter of 14 mm, place it in a vacuum drying oven at 60° C. to dry it, and make it into a negative electrode sheet M.
[0049] Step 9, assemble the negative electrode M and the positive electrode lithium sheet into a button battery in a glove box filled with argon Ar in the order of positive electrode shell, negative electrode sheet, electrolyte, diaphragm, lithium sheet, gasket, spring and negative electrode shell for subsequent performance testing.
[0050] Embodiment 2:
[0051] Preparation method of silicon carbon negative electrode material Figure 1 The specific steps are as follows:
[0052] Step 1, molybdic acid, 2-methylimidazole and zinc chloride are mixed in 120 ml of DMF, refluxed at 180° C. for 10 hours, cooled to room temperature, filtered, and dried in an oven at 80° C. for 3 hours to obtain a white precursor powder A;
[0053] Step 2: dissolve the white precursor powder A in 48 mL of water and 72 mL of ethanol, then add hexadecyltrimethylammonium bromide and ethyl orthosilicate in sequence, perform ultrasonic treatment for 1 hour, stir for 2 hours, collect the precipitate by centrifugation, and dry at 80°C for 4 hours to obtain a silica-coated white precursor powder B.
[0054] Step 3, white powder B is mixed with magnesium powder and sodium chloride in a mass ratio of 1:1:1 and placed in a corundum porcelain boat, and placed in a programmable temperature-controlled tube furnace under the protection of a N2 atmosphere, and heated to 600°C at a heating rate of 2°C / min, and kept warm for 6 hours, and then naturally cooled to room temperature to obtain silicon-coated molybdenum carbide black powder C;
[0055] Step 4, washing the black powder C with dilute hydrochloric acid HCl to remove unreacted magnesium powder and NaCl, washing with water until neutral, and drying at 60° C. to obtain black powder D.
[0056] Step 5: Mix the black powder D with carbon black and polyvinylidene fluoride in proportion, grind thoroughly, add N-methylpyrrolidone dropwise, and continue grinding to form a uniform slurry E.
[0057] Step 6: ultrasonically treat a copper foil of a certain thickness in an ethanol solution, and then dry it in a 70° C. forced air drying oven.
[0058] Step 7, the slurry E obtained in step 5 is scraped onto the copper foil with a scraper to a certain thickness, and then placed in a 70° C. forced air drying oven for drying.
[0059] Step 8: Use a sheet pressing machine to press the prepared electrode into a circular electrode sheet with a diameter of 14 mm, place it in a vacuum drying oven at 60° C. to dry it, and make it into a negative electrode sheet M.
[0060] Step 9, assemble the negative electrode M and the positive electrode lithium sheet into a button battery in a glove box filled with argon Ar in the order of positive electrode shell, negative electrode sheet, electrolyte, diaphragm, lithium sheet, gasket, spring and negative electrode shell for subsequent performance testing.
[0061] Embodiment 3:
[0062] Preparation method of silicon carbon negative electrode material Figure 1 The specific steps are as follows:
[0063] Step 1, molybdic acid, 2-methylimidazole and zinc nitrate are mixed in 120 ml of DMF, refluxed at 190° C. for 8 hours, cooled to room temperature, filtered, and dried in an oven at 70° C. for 5 hours to obtain a white precursor powder A;
[0064] Step 2: dissolve the white precursor powder A in water and ethanol, then add hexadecyltrimethylammonium bromide and ethyl orthosilicate in sequence, perform ultrasonic treatment for 1 hour, stir for 2 hours, collect the precipitate by centrifugation, and dry at 60° C. for 12 hours to obtain a silica-coated white precursor powder B.
[0065] Step 3, weigh 1g of white powder B, 1g of magnesium powder and 1g of sodium chloride, mix them evenly, put them in a corundum porcelain boat, and place them in a program-controlled temperature tube furnace under the protection of N2 atmosphere, heat them to 600°C at a heating rate of 2°C / min, keep them warm for 6 hours, and then cool them naturally to room temperature to obtain silicon-coated molybdenum carbide black powder C;
[0066] Step 4, washing the black powder C with dilute hydrochloric acid HCl to remove unreacted magnesium powder and NaCl, washing with water until neutral, and drying at 60° C. to obtain black powder D.
[0067] Step 5: Mix the black powder D with carbon black and polyvinylidene fluoride in proportion, grind thoroughly, add N-methylpyrrolidone dropwise, and continue grinding to form a uniform slurry E.
[0068] Step 6: ultrasonically treat a copper foil of a certain thickness in an ethanol solution, and then dry it in an air drying oven at 80° C.
[0069] Step 7, the slurry E obtained in step 5 is scraped onto the copper foil with a scraper to a certain thickness, and then placed in an 80° C. forced air drying oven for drying.
[0070] Step 8: Use a sheet pressing machine to press the prepared electrode into a circular electrode sheet with a diameter of 14 mm, place it in a vacuum drying oven at 60° C. to dry it, and make it into a negative electrode sheet M.
[0071] Step 9, assemble the negative electrode M and the positive electrode lithium sheet into a button battery in a glove box filled with argon Ar in the order of positive electrode shell, negative electrode sheet, electrolyte, diaphragm, lithium sheet, gasket, spring and negative electrode shell for subsequent performance testing.
[0072] Embodiment 4:
[0073] Preparation method of silicon carbon negative electrode material Figure 1 The specific steps are as follows:
[0074] Step 1, molybdic acid, 2-methylimidazole and zinc sulfate are mixed in 120 ml of DMF, refluxed at 200° C. for 6 hours, cooled to room temperature, filtered, and dried in an oven at 60° C. for 6 hours to obtain a white precursor powder A;
[0075] Step 2: dissolve the white precursor powder A in 80 mL of water and 80 mL of ethanol, then add hexadecyltrimethylammonium bromide and ethyl orthosilicate in sequence, perform ultrasonic treatment for 30 minutes, stir for 3 hours, collect the precipitate by centrifugation, and dry at 60°C for 6 hours to obtain a silica-coated white precursor powder B.
[0076] Step 3, weigh 1g of white powder B, 1g of magnesium powder and 1g of sodium chloride, mix them evenly, put them in a corundum porcelain boat, and place them in a program-controlled temperature tube furnace under the protection of N2 atmosphere, heat them to 600°C at a heating rate of 2°C / min, keep them warm for 6 hours, and then cool them naturally to room temperature to obtain silicon-coated molybdenum carbide black powder C;
[0077] Step 4, washing the black powder C with dilute hydrochloric acid HCl to remove unreacted magnesium powder and NaCl, washing with water until neutral, and drying at 60° C. to obtain black powder D.
[0078] Step 5: Mix the black powder D with carbon black and polyvinylidene fluoride in proportion, grind thoroughly, add N-methylpyrrolidone dropwise, and continue grinding to form a uniform slurry E.
[0079] Step 6: Ultrasonic treatment of copper foil of a certain thickness in an ethanol solution, and then drying in a 90° C. forced air drying oven.
[0080] Step 7, the slurry E obtained in step 5 is scraped onto the copper foil with a scraper to a certain thickness, and then placed in a 90° C. forced air drying oven for drying.
[0081] Step 8: Use a sheet pressing machine to press the prepared electrode into a circular electrode sheet with a diameter of 14 mm, place it in a vacuum drying oven at 60° C. to dry it, and make it into a negative electrode sheet M.
[0082] Step 9, assemble the negative electrode M and the positive electrode lithium sheet into a button battery in a glove box filled with argon Ar in the order of positive electrode shell, negative electrode sheet, electrolyte, diaphragm, lithium sheet, gasket, spring and negative electrode shell for subsequent performance testing.
[0083] like Figure 1 Shown is a schematic diagram of the preparation process of silicon-containing silicon-carbon negative electrode energy storage materials.
[0084] like Figure 2 The silicon-carbon negative electrode energy storage material of the present invention has a 0.2mVs -1 The relationship between current and voltage at a scan rate of , shows the curve of the electrode at this scan rate. Obviously, for the first cycle of discharge process, a clear peak appeared near the voltage of 0.6V, indicating that the solid electrolyte membrane (SEI membrane) was formed here. In each subsequent cycle, all CV curves showed similar curve shapes in terms of peak shape and amplitude, and a pair of obvious redox peaks appeared near 1.4V and 1.25V, indicating that the electrode mainly achieves storage through the surface capacitance effect.
[0085] like Figure 3This is the electrochemical impedance diagram of the silicon-carbon negative electrode energy storage material of the present invention. The impedance curve is mainly composed of two parts, one part makes a semicircle in the high-frequency area and a slant line in the low-frequency area. The semicircle represents the charge transfer resistance (RCT), which mainly depends on the hydrophilicity, conductivity and microstructure of the electrode, which can facilitate the charge transfer process. The diameter of the circle is smaller at high frequencies, and the corresponding Faraday charge transfer resistance (Rct) is smaller. The straight line is the Warburg impedance, which represents the electrolyte and ion diffusion / transport in the active material. Therefore, the introduction of silicon-carbon negative electrode materials reduces the ion diffusion resistance and improves the conductivity of the performance composite material in the Faraday reaction.
[0086] like Figure 4 This is the long cycle performance diagram of the silicon-carbon negative electrode energy storage material of the present invention at a current density of 0.5A / g. In order to detect the long-term stability of the silicon-carbon negative electrode, we further characterized the charge and discharge cycle performance diagram of the material at a current density of 0.5A / g. After 200 cycles, the electrode still maintains a specific capacity of 506.7mAh / g, indicating that the silicon-coated molybdenum carbide material has a good heterogeneous interface and efficient synergistic effect during the cycle process.
Claims
1. Silicon-carbon negative electrode energy storage material, characterized in that: The invention comprises a copper foil for battery, the copper foil is used as a current collector, and a silicon-carbon negative electrode active material is coated on the copper foil; the electrode material is a double-layer structure of copper foil and silicon-carbon negative electrode; the specific operation steps of the preparation method of the silicon-carbon negative electrode energy storage material are as follows: Step 1: Mix molybdic acid, 2-methylimidazole and zinc acetate in N,N-dimethylformamide and add to a flask at 160 o C, reflux at high temperature, then cool to room temperature, filter, and dry to obtain a white precursor powder A; Step 2: uniformly disperse the white precursor powder A in a mixed solution of water and ethanol by ultrasonication, then add hexadecyltrimethylammonium bromide and ethyl orthosilicate in sequence, stir, collect the precipitate by centrifugation, and o C is dried to obtain a white precursor powder B coated with silica; Step 3: Precursor powder B is mixed with magnesium powder and sodium chloride in a certain mass ratio, ground evenly and placed in a corundum porcelain boat, and placed in a programmable temperature-controlled tube furnace under the protection of N2 atmosphere for 2 hours. o C / min heating rate to 600 o C, keep warm for 7 hours, and then cool naturally to room temperature to obtain silicon-coated molybdenum carbide powder C; Step 4: Wash the molybdenum carbide powder C with dilute hydrochloric acid HCl to remove unreacted magnesium powder and NaCl, and then wash with water until neutral. o C is dried to obtain black powder D; Step 5, mixing black powder D with carbon black and polyvinylidene fluoride in proportion, grinding thoroughly, adding N-methylpyrrolidone dropwise, and continuing grinding to form a uniform slurry E; Step 6, ultrasonically treating the copper foil in an ethanol solution, and then placing it in a forced air drying oven for drying; Step 7: Scrape the slurry E obtained in step 5 onto the copper foil dried in step 6 with a scraper, and then place it at 60 o C. Dry in a blast drying oven to form an electrode; Step 8: Use a tablet press to make a circular electrode sheet with a diameter of 14 mm and place it on a 60 o C is dried in a vacuum drying oven to form a negative electrode sheet M; Step 9, assemble the negative electrode sheet M and the positive electrode lithium sheet into a button battery in a glove box filled with argon Ar in the order of positive electrode shell, negative electrode sheet, electrolyte, diaphragm, lithium sheet, gasket, spring and negative electrode shell, and finally perform performance test.
2. A method for preparing a silicon-carbon negative electrode material, characterized in that: The specific steps are as follows: Step 1: Mix molybdic acid, 2-methylimidazole and zinc acetate in N,N-dimethylformamide and add to a flask at 160 o C, reflux at high temperature, then cool to room temperature, filter, and dry to obtain a white precursor powder A; Step 2: uniformly disperse the white precursor powder A in a mixed solution of water and ethanol by ultrasonication, then add hexadecyltrimethylammonium bromide and ethyl orthosilicate in sequence, stir, collect the precipitate by centrifugation, and o C is dried to obtain a white precursor powder B coated with silica; Step 3: Precursor powder B is mixed with magnesium powder and sodium chloride in a certain mass ratio, ground evenly and placed in a corundum porcelain boat, and placed in a programmable temperature-controlled tube furnace under the protection of N2 atmosphere for 2 hours. o C / min heating rate to 600 o C, keep warm for 7 hours, and then cool naturally to room temperature to obtain silicon-coated molybdenum carbide powder C; Step 4: Wash the molybdenum carbide powder C with dilute hydrochloric acid HCl to remove unreacted magnesium powder and NaCl, and then wash with water until neutral. o C is dried to obtain black powder D; Step 5, mixing black powder D with carbon black and polyvinylidene fluoride in proportion, grinding thoroughly, adding N-methylpyrrolidone dropwise, and continuing grinding to form a uniform slurry E; Step 6, ultrasonically treating the copper foil in an ethanol solution, and then placing it in a forced air drying oven for drying; Step 7: Scrape the slurry E obtained in step 5 onto the copper foil dried in step 6 with a scraper, and then place it at 60 o C. Dry in a blast drying oven to form an electrode; Step 8: Use a tablet press to make a circular electrode sheet with a diameter of 14 mm and place it on a 60 o C is dried in a vacuum drying oven to form a negative electrode sheet M; Step 9, assemble the negative electrode sheet M and the positive electrode lithium sheet into a button battery in a glove box filled with argon Ar in the order of positive electrode shell, negative electrode sheet, electrolyte, diaphragm, lithium sheet, gasket, spring and negative electrode shell, and finally perform performance test.
3. The method for preparing the silicon-carbon negative electrode material according to claim 2, characterized in that: The reflux time in step 1 is 12 hours and the drying temperature is 60 o C, drying time 8 hours.
4. The method for preparing the silicon-carbon negative electrode material according to claim 2, characterized in that: In step 2, the volume ratio of ethanol to water is 1:1, the ultrasonic time is 40 minutes, the stirring time is 2 hours, and the drying time is 1 to 6 hours.
5. The method for preparing the silicon-carbon negative electrode material according to claim 2, characterized in that: In step 3, the mass ratio of precursor powder B to magnesium powder and sodium chloride is 1:1:0.
8.
6. The method for preparing the silicon-carbon negative electrode material according to claim 2, characterized in that: In step 4, the molar concentration of the dilute hydrochloric acid used is 1.0 mol / L.
7. The method for preparing the silicon-carbon negative electrode material according to claim 2, characterized in that: In step 5, the mixing mass ratio of black powder D to carbon black and polyvinylidene fluoride PVDF is 8:1:
1.
8. The method for preparing the silicon-carbon negative electrode material according to claim 2, characterized in that: The drying temperature in step 6 is 60 o C.
Citation Information
Patent Citations
Silicon carbon composite material and preparation method thereof
CN102185128A
Method for preparing silicon-carbon anode material for lithium ion power battery
CN109686941A
High-performance transition metal oxide negative electrode material and battery assembling method
CN110808365A
Etched nano-silicon double-layer carbon-coated lithium ion battery negative electrode material, negative electrode pole piece and preparation method of etched nano-silicon double-layer carbon-coated lithium ion battery negative electrode material
CN111525115A
One-dimensional porous silicon-carbon composite negative electrode material, preparation method, and application thereof
WO2022121137A1