A method for preparing a single-phase garnet-type lithium ion solid electrolyte with different densities
By removing the alkaline salts on the surface of the garnet-type lithium-ion electrolyte and mixing and sintering it with non-alkaline salts, the problem of low density of the single-phase garnet-type lithium-ion electrolyte is solved and the lithium-ion transmission performance and battery safety are improved. , achieving electrolyte preparation with high density and high ionic conductivity.
Patent Information
- Application Number
- CN202210866422.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-07-22
AI Technical Summary
It is difficult to prepare high-density single-phase garnet-type solid-state lithium-ion electrolytes with existing technology, and low-density electrolyte sheets will lead to low lithium-ion transmission performance and battery safety issues.
The alkaline salts on the surface of the garnet-type lithium-ion solid electrolyte are removed before high-temperature sintering, and the electrolyte powder without alkaline pore-forming salts is mixed and pressed into tablets, and then sintered at high temperature to control the density and avoid Li+/H+ Exchange reaction.
The preparation of a high-density single-phase garnet-type lithium-ion solid-state electrolyte is achieved, which improves lithium-ion transmission performance and battery safety, and enhances ionic conductivity.
Smart Images

Figure BDA0003758802910000021 
Figure HDA0003758802920000011 
Figure HDA0003758802920000021
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a single-phase garnet-type lithium ion solid electrolyte with different densities, belonging to the technical field of solid electrolyte materials. Background Art
[0002] Solid-state lithium batteries can achieve high energy density while ensuring safety, becoming a hot topic in the research and development of next-generation lithium batteries. As a key material in solid-state lithium batteries, garnet-type solid electrolytes have the advantages of high ionic conductivity, wide electrochemical window, and chemical stability to lithium metal.
[0003] However, it is difficult to obtain a high-density single-phase garnet solid electrolyte using current preparation methods. + The ionic conductivity is higher than that of LaZrO 7 The multiphase LLZTO has a lower lithium ion transport performance than the tetragonal LLZTO by tens of times or even several orders of magnitude. On the other hand, the low-density garnet-type lithium ion electrolyte sheet will lose the ability to prevent dendrites from Li + The ability to grow and penetrate, thus causing battery safety issues. Summary of the invention
[0004] The present invention aims at the difficulty in preparing the existing high-density single-phase garnet-type solid electrolyte, and proposes a method for preparing a single-phase garnet-type lithium ion solid electrolyte with different densities. The present invention creatively proposes that the difficulty in preparing the high-density garnet-type solid electrolyte is due to the formation of alkaline salts (such as lithium carbonate, etc.) on the surface of the garnet-type lithium ion solid electrolyte. Such substances are relatively stable at lower temperatures (within the calcination temperature range), but form pores in the subsequent high-temperature sintering process, causing the density to decrease. Therefore, the present invention removes the alkaline salts before the high-temperature sintering process, and avoids the Li generated in the process of removing impurities. + / H + The exchange reaction prevents the formation of impure phases with low ionic conductivity, and by artificially adding different masses of lithium carbonate, mixing it with electrolyte powder without alkaline pore-forming salts and pressing it into tablets, and sintering it at the same high temperature to control the density of the garnet-type lithium-ion solid electrolyte, thereby realizing the preparation of single-phase garnet-type solid electrolytes with different densities.
[0005] A method for preparing a single-phase garnet-type lithium-ion solid electrolyte with different densities, the specific steps are as follows:
[0006] (1) mixing lithium carbonate, zirconium oxide, lanthanum oxide and tantalum oxide to obtain a mixed powder A, wet-grinding the mixed powder A to obtain a mixed slurry, and drying the mixed slurry to obtain a mixed powder B;
[0007] (2) calcining the mixed powder B at a temperature of 800 to 950° C. for 6 to 10 hours to obtain a garnet-type electrolyte mother powder;
[0008] (3) The garnet-type electrolyte mother powder is added to hydrochloric acid to react for 30 to 60 seconds to remove alkaline salts, and the water-soluble lithium salts are removed by washing with distilled water to obtain pure LLZTO, which is then filtered and dried to obtain electrolyte powder without alkaline salts;
[0009] (4) adding different amounts of lithium carbonate to electrolyte powder without alkaline salts, mixing them evenly to obtain a mixed powder C, and pressing the mixed powder C into tablets to obtain an electrolyte body;
[0010] (5) The electrolyte body is sintered at a temperature of 1050° C. to 1250° C. to obtain a single-phase garnet-type lithium-ion solid electrolyte with different densities.
[0011] In the step (1), if the mass fraction of the mixed powder A is 100%, zirconium oxide accounts for 10-20%, lanthanum oxide accounts for 20-40%, tantalum oxide accounts for 10-20%, and the remainder is lithium carbonate.
[0012] The concentration of hydrochloric acid in step (3) is 0.1-2 mol / L.
[0013] The drying temperature in step (3) is 60-90°C.
[0014] The amount of lithium carbonate added in step (4) is 0.5-20% of the mass of the mixed powder C.
[0015] Ionic conductivity measurements can be calculated using the following formula,
[0016]
[0017] Wherein, σ is the obtained conductivity; d is the thickness of the sample; S is the area of the electrode on the measured sample; and R is the resistance of the sample obtained by the AC impedance test.
[0018] The beneficial effects of the present invention are:
[0019] (1) The present invention creatively proposes that the difficulty in preparing a high-density garnet-type solid electrolyte is due to the formation of alkaline salts on the surface of the garnet-type lithium-ion solid electrolyte. These alkaline salts are relatively stable during calcination, but decompose to form pores during the subsequent high-temperature sintering process, causing the density to decrease. Therefore, the present invention removes the alkaline salts before the high-temperature sintering process, thereby achieving the preparation of a high-density garnet-type solid electrolyte;
[0020] (2) The traditional acid dissolution method will produce Li + / H + The exchange reaction results in the generation of La with extremely low ionic conductivity.2 Zr 2 O 7 , and the surface morphology of the mother powder will be corroded during the reaction, resulting in a decrease in sinterability; the present invention selects hydrochloric acid with the slowest reaction kinetics, and strictly controls the acid concentration and reaction time, thereby inhibiting side reactions while also ensuring the removal effect of alkaline salts;
[0021] (3) The present invention adds different amounts of lithium carbonate before tableting to ensure that different densities can be produced at the same sintering temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Table 1 Performance comparison of garnet-type lithium-ion solid electrolytes;
[0023] Figure 1 is the X-ray diffraction pattern of the comparative example garnet type solid electrolyte mother powder;
[0024] Figure 2 This is an X-ray diffraction diagram of the mother powder without alkaline salt after calcination of the garnet-type solid electrolyte in Example 1;
[0025] Figure 3 is a cross-sectional scan of a comparative example garnet-type solid electrolyte;
[0026] Figure 4 is a cross-sectional scan of the garnet-type solid electrolyte without alkaline salts in Example 1;
[0027] Figure 5 is the impedance diagram of the comparative example garnet-type solid electrolyte;
[0028] Figure 6 This is the impedance diagram of the garnet-type solid electrolyte without alkaline salts in Example 1. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0030] Comparative Example: A method for preparing a garnet-type lithium-ion solid electrolyte, the specific steps are as follows:
[0031] (1) lithium carbonate, zirconium oxide, lanthanum oxide and tantalum oxide are mixed to obtain a mixed powder A, the mixed powder A is added to a zirconium oxide ball mill, zirconium oxide grinding balls and isopropanol are added, and a mixed slurry is obtained by wet grinding, and the mixed slurry is dried at a temperature of 80° C. to obtain a mixed powder B; wherein, based on the mass fraction of the mixed powder A being 100%, zirconium oxide accounts for 15%, lanthanum oxide accounts for 28%, tantalum oxide accounts for 15%, and the remainder is lithium carbonate, and the molar ratio of Li, La, Zr and Ta is 6.4:3:1.4:0.6; the ball mill speed is 300 rpm, and the ball milling time is 10 h;
[0032] (2) calcining the mixed powder B at 900° C. for 10 h to obtain a garnet-type electrolyte mother powder;
[0033] (3) The garnet-type electrolyte mother powder is pressed into tablets under a pressure of 200 MPa and sintered at a temperature of 1200°C for 3 h to obtain a garnet-type lithium-ion solid electrolyte.
[0034] Example 1: A method for preparing a high-density single-phase garnet-type lithium-ion solid electrolyte, the specific steps are as follows:
[0035] (1) lithium carbonate, zirconium oxide, lanthanum oxide and tantalum oxide are mixed to obtain a mixed powder A, the mixed powder A is added to a zirconium oxide ball mill, zirconium oxide grinding balls and isopropanol are added, and a mixed slurry is obtained by wet grinding, and the mixed slurry is dried at a temperature of 80° C. to obtain a mixed powder B; wherein, based on the mass fraction of the mixed powder A being 100%, zirconium oxide accounts for 15%, lanthanum oxide accounts for 38%, tantalum oxide accounts for 15%, and the remainder is lithium carbonate, and the molar ratio of Li, La, Zr and Ta is 6.4:3:1.4:0.6; the ball mill speed is 300 rpm, and the ball milling time is 10 h;
[0036] (2) calcining the mixed powder B at 900° C. for 10 h to obtain a garnet-type electrolyte mother powder;
[0037] (3) The garnet-type electrolyte mother powder was added to hydrochloric acid and reacted for 60 seconds to remove the alkaline salt, and the electrolyte powder was washed with distilled water 5 times to remove the soluble neutral lithium salt generated in the acid reaction to obtain pure LLZTO, which was filtered and dried at 80°C for 8 hours to obtain an electrolyte powder without alkaline salts; wherein the concentration of hydrochloric acid was 1 mol / L;
[0038] (4) adding lithium carbonate to the electrolyte powder without alkaline salt, mixing them evenly to obtain a mixed powder C, and pressing the mixed powder C into a tablet under a pressure of 200 MPa to obtain an electrolyte body; wherein the amount of lithium carbonate added is 0.5% by weight of the mixed powder C;
[0039] (5) the electrolyte body is sintered at a temperature of 1200° C. for 3 h to obtain a single-phase garnet-type lithium-ion solid electrolyte;
[0040] The X-ray diffraction pattern of the comparative example garnet solid electrolyte mother powder is shown in Figure 1 The X-ray diffraction pattern of the electrolyte powder without alkaline salts in this embodiment is shown in Figure 2 ,from Figure 1 and Figure 2 It can be seen that after acid treatment, the garnet-type lithium-ion solid electrolyte is still single-phase and Li 2 CO 3The diffraction peak of the comparative example garnet-type solid electrolyte is shown in the cross-sectional scanning diagram. Figure 3 ; The cross-sectional scanning diagram of the garnet-type solid electrolyte without alkaline salts in this embodiment is shown in Figure 4 ,from Figure 3 and Figure 4 It can be seen that the density of the acid-treated garnet-type lithium-ion solid electrolyte after high-temperature sintering is greatly improved compared with the control example, from 90.2% to 94.6%. The impedance spectrum of the control example garnet-type solid electrolyte is shown in Figure 5 The impedance spectrum of the garnet-type solid electrolyte without alkaline salts in this embodiment is shown in Figure 6 ,from Figure 5 and Figure 6 It can be seen that the internal resistance of the acid-treated garnet-type lithium-ion solid electrolyte is greatly reduced after high-temperature sintering compared with the control ratio, thereby enhancing the ionic conductivity from 2.8*10 ^-4 S cm -1 Increased to 5.2*10 ^-4 S cm -1 .
[0041] Example 2: A method for preparing a high-density single-phase garnet-type lithium-ion solid electrolyte, the specific steps are as follows:
[0042] (1) lithium carbonate, zirconium oxide, lanthanum oxide and tantalum oxide are mixed to obtain a mixed powder A, the mixed powder A is added to a zirconium oxide ball mill, zirconium oxide grinding balls and isopropanol are added, and a mixed slurry is obtained by wet grinding, and the mixed slurry is dried at a temperature of 90° C. to obtain a mixed powder B; wherein, based on the mass fraction of the mixed powder A being 100%, zirconium oxide accounts for 18%, lanthanum oxide accounts for 32%, tantalum oxide accounts for 15%, and the remainder is lithium carbonate, and the molar ratio of Li, La, Zr and Ta is 6.6:3:1.6:0.4; the ball mill speed is 200 rpm, and the ball milling time is 14 h;
[0043] (2) The mixed powder B is calcined at 850° C. for 8 h to obtain a garnet-type electrolyte mother powder;
[0044] (3) The garnet-type electrolyte mother powder was added to hydrochloric acid and reacted for 40 seconds to remove the alkaline salt, and washed with distilled water for 4 times to remove the soluble neutral lithium salt generated in the acid washing reaction to obtain pure LLZTO, which was filtered and dried at 70°C for 9 hours to obtain an electrolyte powder without alkaline salts; wherein the concentration of hydrochloric acid was 0.5 mol / L;
[0045] (4) adding lithium carbonate to the electrolyte powder without alkaline salt, mixing them evenly to obtain a mixed powder C, and pressing the mixed powder C under a pressure of 300 MPa to obtain an electrolyte body; wherein the amount of lithium carbonate added is 5% by weight of the mixed powder C;
[0046] (5) the electrolyte body is sintered at a temperature of 1150° C. for 6 h to obtain a single-phase garnet-type lithium-ion solid electrolyte;
[0047] The density of the acid-treated garnet-type lithium-ion solid electrolyte in this embodiment after high-temperature sintering is greatly improved compared with the control example, from 90.2% to 92.7%.
[0048] Example 3: A method for preparing a high-density single-phase garnet-type lithium-ion solid electrolyte, the specific steps are as follows:
[0049] (1) lithium carbonate, zirconium oxide, lanthanum oxide and tantalum oxide are mixed to obtain a mixed powder A, the mixed powder A is added to a zirconium oxide ball mill, zirconium oxide grinding balls and isopropanol are added, and a mixed slurry is obtained by wet grinding, and the mixed slurry is dried at a temperature of 95° C. to obtain a mixed powder B; wherein, based on the mass fraction of the mixed powder A being 100%, zirconium oxide accounts for 16%, lanthanum oxide accounts for 26%, tantalum oxide accounts for 20%, and the remainder is lithium carbonate, and the molar ratio of Li, La, Zr and Ta is 6.8:3:1.8:0.2; the ball mill speed is 280 rpm, and the ball milling time is 16 h;
[0050] (2) calcining the mixed powder B at 800° C. for 10 h to obtain a garnet-type electrolyte mother powder;
[0051] (3) The garnet-type electrolyte mother powder was added to hydrochloric acid and reacted for 50 seconds to remove the alkaline salt, and washed with distilled water for 3 times to remove the soluble neutral lithium salt generated in the acid washing reaction to obtain pure LLZTO, which was filtered and dried at 90°C for 6 hours to obtain an electrolyte powder without alkaline salts; wherein the concentration of hydrochloric acid was 0.3 mol / L;
[0052] (4) adding lithium carbonate to the electrolyte powder without alkaline salt, mixing them evenly to obtain a mixed powder C, and pressing the mixed powder C into a tablet under a pressure of 400 MPa to obtain an electrolyte body; wherein the amount of lithium carbonate added is 10% by weight of the mixed powder C;
[0053] (5) the electrolyte body is sintered at a temperature of 1100° C. for 6 h to obtain a single-phase garnet-type lithium-ion solid electrolyte;
[0054] The density of the acid-treated garnet-type lithium-ion solid electrolyte in this embodiment after high-temperature sintering is greatly improved compared with the comparative example, from 90.2% to 91.5%;
[0055] The performance comparison of the garnet-type lithium ion solid electrolytes of the comparative example and Examples 1 to 3 is shown in Table 1.
[0056] Table 1 Performance comparison of garnet-type lithium-ion solid electrolytes
[0057] Relative density% Ionic conductivity S / cm Comparative Example 90.2% <![CDATA[2.8*10 ^-4 S cm -1 ]]> Example 1 94.6% <![CDATA[5.2*10 ^-4 S cm -1 ]]> Example 2 92.7% <![CDATA[3.9*10 ^-4 S cm -1 ]]> Example 3 91.5% <![CDATA[3.3*10 ^-4 S cm -1 ]]>
[0058] As shown in Table 1, the relative density of garnet-type lithium-ion solid electrolyte can be as high as 94.6%, and the ionic conductivity can reach 5.2*10 ^-4 S cm -1 .
[0059] The specific implementation modes of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for preparing a single-phase garnet-type lithium ion solid electrolyte with different densities, characterized in that: The specific steps are as follows: (1) mixing lithium carbonate, zirconium oxide, lanthanum oxide and tantalum oxide to obtain a mixed powder A, wet-grinding the mixed powder A to obtain a mixed slurry, and drying the mixed slurry to obtain a mixed powder B; (2) calcining the mixed powder B at a temperature of 800 to 950° C. for 6 to 10 hours to obtain a garnet-type electrolyte mother powder; (3) The garnet-type electrolyte mother powder is added to hydrochloric acid to react for 30 to 60 seconds to remove alkaline salts, and the water-soluble lithium salts are removed by washing with distilled water to obtain pure LLZTO, which is then filtered and dried to obtain electrolyte powder without alkaline salts; (4) adding different amounts of lithium carbonate to electrolyte powder without alkaline salts, mixing them evenly to obtain a mixed powder C, and pressing the mixed powder C into tablets to obtain an electrolyte body; (5) The electrolyte body is sintered at a temperature of 1050° C. to 1250° C. to obtain a single-phase garnet-type lithium-ion solid electrolyte with different densities.
2. The method for preparing the single-phase garnet-type lithium ion solid electrolyte with different densities according to claim 1, characterized in that: Step (1) The mass fraction of the mixed powder A is 100%, wherein zirconium oxide accounts for 10-20%, lanthanum oxide accounts for 20-40%, tantalum oxide accounts for 10-20%, and the remainder is lithium carbonate.
3. The method for preparing the single-phase garnet-type lithium ion solid electrolyte with different densities according to claim 1, characterized in that: The concentration of hydrochloric acid in step (3) is 0.1-2 mol / L.
4. The method for preparing the single-phase garnet-type lithium ion solid electrolyte with different densities according to claim 1, characterized in that: The drying temperature in step (3) is 60-90°C.
5. The method for preparing the single-phase garnet-type lithium ion solid electrolyte with different densities according to claim 1, characterized in that: The amount of lithium carbonate added in step (4) is 0.5 to 20% of the mass of the mixed powder C.