Binder for inorganic fiber and inorganic fiber mat

By using a water-soluble binder that combines maleic anhydride copolymer and cellulose ether, the problems of recovery rate and formaldehyde release of inorganic fiber mats are solved, and the manufacturing of inorganic fiber mats with high recovery properties and low pollution is achieved.

CN115135830BActive Publication Date: 2024-10-11NISSHIN CHEM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180015316.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-02-19
Filing Date
2021-02-03
Publication Date
2024-10-11
Estimated Expiration
2041-02-03

AI Technical Summary

Technical Problem

The water-soluble phenolic resin binder used in existing inorganic fiber mats will release formaldehyde after curing, leading to volatile organic compound pollution, affecting health and the environment, and the recovery rate of alternative binders is poor.

Method used

A binder containing ammonia-modified maleic anhydride copolymer and cellulose ether is used, combined with polyvinyl alcohol resin to form a water-soluble binder. Inorganic fiber mats are manufactured through spray coating and heat curing to ensure high recovery. rate and low formaldehyde emission.

Benefits of technology

It achieves a high recovery rate of inorganic fiber mats and a very small amount of formaldehyde release, meeting excellent recovery properties and environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003803917440000051
    Figure BDA0003803917440000051
  • Figure BDA0003803917440000061
    Figure BDA0003803917440000061
  • Figure BDA0003803917440000141
    Figure BDA0003803917440000141
Patent Text Reader

Abstract

The present invention relates to a binder for inorganic fibers and an inorganic fiber mat. The binder for inorganic fibers is characterized in that it contains 3 parts by mass or more of (B) an amino-modified copolymer containing maleic anhydride, relative to 100 parts by mass of (A) cellulose ether having a viscosity (20°C) of 500 mPa·s or less in a 2% by mass aqueous solution. The inorganic fiber mat contains inorganic fibers treated with the above-mentioned binder for inorganic fibers. By using the binder for inorganic fibers of the present invention, an inorganic fiber mat having a high recovery rate equivalent to that of a phenolic resin can be produced, and the emission of volatile organic compounds from the inorganic fiber mat is extremely small.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a binder for inorganic fibers, and in particular to an inorganic fiber mat suitable for use as a heat insulating material, a sound absorbing material, etc. for construction, which has extremely low emission of volatile organic compounds, has a sufficient thickness, and has excellent restorability, as well as an inorganic fiber mat treated with the binder. Background Art

[0002] In the past, inorganic fiber mats composed of inorganic fibers such as glass wool and rock wool have been widely used as heat insulating materials and sound absorbing materials for industrial and residential use. Inorganic fiber mats are generally manufactured by fixing inorganic fibers to each other using a binder with a water-soluble phenolic resin as a main component and molding them into a mat shape (for example, Japanese Patent Publication No. 58-070760: Patent Document 1).

[0003] However, the water-soluble phenolic resin used as the main component of the above-mentioned binder generally uses formaldehyde as a crosslinking agent, so there is a problem that unreacted formaldehyde remains in the inorganic fiber mat when the binder is heated and cured. In addition, there is also a problem that formaldehyde is generated due to the hydrolysis and condensation reactions of the binder after curing. In this case, the above-mentioned formaldehyde is released from the surface and side of the inorganic fiber mat after production.

[0004] Regarding volatile organic compounds such as formaldehyde that easily volatilize into the air at normal temperature and pressure, indoor air pollution caused by volatile organic compounds has become more obvious in recent years, and health damage such as sick building syndrome, one of the causes of volatile organic compounds, has become a problem. Therefore, the amount of formaldehyde released from building materials is legally restricted. Therefore, it is believed that in order to reduce the amount of formaldehyde and other volatile organic compounds released from building materials, it is effective to reduce their content.

[0005] The volatile organic compounds released from the inorganic fiber mat are mainly formaldehyde contained in the binder, so in order to solve the above problem, it is necessary to make the composition used in the binder into a formaldehyde-free composition. However, the inorganic fiber mat using the conventional binder with phenolic resin as the main component has low raw material cost and excellent recovery rate of the mat. Therefore, it is necessary to have these properties even if the binder with the formaldehyde-free composition as the main component is used, but it is difficult to have the same performance.

[0006] In order to deal with the above problems, in Japanese Patent Publication No. 2005-299013 (Patent Document 2), a binder with an acrylic resin emulsion as the main component was proposed. In addition, in Japanese Patent Publication No. 2006-089906 (Patent Document 3), a binder consisting of a vinyl copolymer with functional groups such as carboxyl groups was proposed. However, the recovery rate of the inorganic fiber mat obtained using these binders is poor compared with the inorganic fiber mat obtained using a binder containing a water-soluble phenolic resin. Furthermore, the applicant also disclosed a binder containing a water-soluble polymer compound and a boron compound having a hydroxyl group in Japanese Patent Publication No. 2011-153395 (Patent Document 4). However, although the problem of volatile organic compounds in the inorganic fiber mat obtained using this binder has been eliminated, the recovery rate is slightly poor compared with the water-soluble phenolic resin.

[0007] International Publication No. 2005 / 092814 (Patent Document 5) proposes an unsaturated copolymer of maleic anhydride and an unsaturated monomer (specifically, an unsaturated copolymer of maleic anhydride and butadiene), Japanese Patent Publication No. 2012-136385 (Patent Document 6) proposes a copolymer compound of maleic anhydride and acrylic acid ester, Japanese Patent Publication No. 2016-108707 (Patent Document 7) and Japanese Patent Publication No. 2016-108708 (Patent Document 8) propose a maleic acid copolymer (considered to be a methyl vinyl ether / maleic anhydride copolymer monoalkyl ester), and Japanese Patent Publication No. 60-046951 (Patent Document 9) proposes an isobutylene-maleic anhydride copolymer. Inorganic fiber mats composed of inorganic fibers are manufactured by spraying a low concentration of a water-soluble binder onto molten glass, but the aforementioned compounds lack solubility in water and may not necessarily obtain a suitable water-soluble binder.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Laid-Open No. 58-070760

[0011] Patent Document 2: Japanese Patent Application Publication No. 2005-299013

[0012] Patent Document 3: Japanese Patent Application Publication No. 2006-089906

[0013] Patent Document 4: Japanese Patent Application Publication No. 2011-153395

[0014] Patent Document 5: International Publication No. 2005 / 092814

[0015] Patent Document 6: Japanese Patent Application Publication No. 2012-136385

[0016] Patent Document 7: Japanese Patent Application Publication No. 2016-108707

[0017] Patent Document 8: Japanese Patent Application Publication No. 2016-108708

[0018] Patent Document 9: Japanese Patent Application Laid-Open No. 60-046951 Summary of the invention

[0019] Problems to be solved by the invention

[0020] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a binder for inorganic fibers capable of producing an inorganic fiber mat having excellent restorability, and an inorganic fiber mat treated with the binder.

[0021] Means for solving problems

[0022] The present inventors have conducted intensive studies to achieve the above-mentioned object and have found that a binder comprising an amino-modified copolymer containing maleic anhydride and cellulose ether can give an inorganic fiber mat the same recovery rate as a phenolic resin and can achieve an extremely small amount of volatile organic compound emission, thereby completing the present invention.

[0023] Therefore, the present invention provides the following inorganic fiber binder and an inorganic fiber mat treated with the binder.

[0024] 1. A binder for inorganic fibers, characterized in that it contains (B) 3 parts by mass or more of an amino-modified copolymer containing maleic anhydride, relative to (A) 100 parts by mass of a cellulose ether having a viscosity (20° C.) of 500 mPa·s or less in a 2% by mass aqueous solution.

[0025] 2. The binder for inorganic fibers according to item 1 above, wherein the cellulose ether (A) contains at least one selected from the group consisting of methyl cellulose, ethyl cellulose, ethyl methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose and hydroxypropyl cellulose.

[0026] 3. The binder for inorganic fibers according to 1 or 2 above, wherein the (B) amino-modified product of the copolymer containing maleic anhydride has a weight average molecular weight of 50,000 to 300,000 and has a specific structural formula described below.

[0027] 4. The binder for inorganic fibers according to any one of 1 to 3 above, wherein the (B) ammonia-modified product of a copolymer containing maleic anhydride is an ammonia-modified product of an isobutylene-maleic anhydride copolymer.

[0028] 5. The binder for inorganic fibers according to any one of 1 to 4 above, further comprising (C) a polyvinyl alcohol-based resin having a degree of polymerization of 100 to 3,500.

[0029] 6. The binder for inorganic fibers according to 5 above, wherein the degree of saponification of the (C) polyvinyl alcohol-based resin is 70 mol% or more.

[0030] 7. The binder for inorganic fibers according to any one of 1 to 6 above, wherein the inorganic fibers are glass wool or rock wool.

[0031] 8. The binder for inorganic fibers according to any one of 1 to 7 above, which is dissolved in water and used as an aqueous solution of the binder for inorganic fibers, and the viscosity of the aqueous solution of the binder for inorganic fibers is 1 to 100 mPa·s at 20°C.

[0032] 9. An inorganic fiber mat comprising inorganic fibers treated with the inorganic fiber binder according to any one of 1 to 8 above.

[0033] Effects of the Invention

[0034] By using the inorganic fiber binder of the present invention, an inorganic fiber mat having a high recovery rate can be produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a schematic diagram showing one embodiment of the process of producing an inorganic fiber mat using the inorganic fiber binder of the present invention.

[0036] Figure 2 This is a perspective view showing one embodiment of the step of applying the binder for inorganic fibers of the present invention to inorganic fibers. DETAILED DESCRIPTION

[0037] The present invention is described in detail below.

[0038] The binder for inorganic fibers of the present invention is characterized by comprising the following components (A) and (B):

[0039] (A) 100 parts by mass of cellulose ether having a viscosity of 500 mPa·s or less in a 2% by mass aqueous solution,

[0040] (B) Amino-modified product of a copolymer containing maleic anhydride: 3 parts by mass or more.

[0041] The cellulose ether of component (A) may be a polymer of the desired viscosity, and the viscosity of a 2% by mass aqueous solution is 500 mPa·s or less, preferably 100 mPa·s or less. More preferably, the viscosity may be 20 mPa·s or less. It should be noted that there is no particular restriction on the lower limit of the viscosity, but it is preferably 1 mPa·s or more. The viscosity of a 2% by mass aqueous solution is a value measured at 20°C using a B-type viscometer. If the viscosity of a 2% by mass aqueous solution exceeds 500 mPa·s, poor coating due to spraying may occur, making it impossible to obtain the desired adhesion amount, resulting in undesirable conditions such as the inability to obtain sufficient recovery of the inorganic fiber mat.

[0042] The weight average molecular weight of the cellulose ether of the component (A) is preferably 100,000 or less, and more preferably 30,000 or less. If the weight average molecular weight exceeds 100,000, the desired adhesion amount may not be obtained due to poor coating caused by spraying, and the inorganic fiber mat may not be able to obtain sufficient recovery. The weight average molecular weight is a value based on polystyrene conversion based on aqueous gel permeation chromatography (GPC) analysis.

[0043] The cellulose ether of component (A) is preferably at least one selected from methyl cellulose, ethyl cellulose, ethyl methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxyethyl methyl cellulose, and hydroxypropyl cellulose. Water-soluble cellulose ethers are particularly preferred. In addition, products obtained by substituting a part of the hydrogen atoms of the hydroxyl group of cellulose with methyl, hydroxypropyl, hydroxyethyl, carboxymethyl, etc. can be used.

[0044] The amino-modified copolymer containing maleic anhydride as the component (B) functions as a crosslinking agent in the present invention. The amino-modified copolymer containing maleic anhydride as the component (B) is not particularly limited, and examples thereof include copolymers of the following general formula.

[0045] [Chemistry 1]

[0046]

[0047] In the above formula, R 1 and R 2 Each is a linear or branched alkylene group having 2 to 5 carbon atoms and may have 1 to 2 unsaturated groups, for example, ethylene, propylene, isopropylene, n-butylene, isobutylene, ethylene-propylene, butadienyl, etc., R 1 and R 2 They may be the same as or different from each other.

[0048] Examples of the component (B) include amino-modified copolymers of maleic anhydride and isobutylene, isopropylene, ethylene, ethylene-propylene, butadiene, etc. In particular, an amino-modified isobutylene-maleic anhydride copolymer represented by the following structural formula is preferred.

[0049] [Chemistry 2]

[0050]

[0051] The weight average molecular weight of the amino-modified copolymer containing maleic anhydride as the component (B) is preferably 50,000 to 300,000, more preferably 50,000 to 200,000, and most preferably 50,000 to 100,000. The weight average molecular weight is a value in terms of polystyrene based on aqueous gel permeation chromatography (GPC) analysis.

[0052] In the above formula, n and m represent a mass ratio, and n is preferably 50 to 90 mass %, more preferably 70 to 80 mass %, relative to 100 mass % of the total of n+m.

[0053] The content of the amino-modified copolymer containing maleic anhydride as component (B) is 3 parts by mass or more, preferably 4 parts by mass or more, more preferably 5 parts by mass or more, with respect to 100 parts by mass of the cellulose ether as component (A), and the upper limit is preferably 20 parts by mass or less, more preferably 10 parts by mass or less. If the content of the amino-modified copolymer containing maleic anhydride is less than 3 parts by mass, disadvantages such as insufficient crosslinking may occur, and if it exceeds 20 parts by mass, there may be no problem in miscibility with the cellulose ether as component (A), but the treated aqueous solution may be colored yellow, the quality of the product may be reduced, and the cost may increase.

[0054] As the copolymer containing maleic anhydride as the component (B), a commercially available item can be used, and examples thereof include "ISOBAM" manufactured by Kuraray Co., Ltd. and the like.

[0055] Furthermore, in the binder for inorganic fibers of the present invention, a polyvinyl alcohol resin may be contained as the component (C) from the viewpoint of making the coating by spraying good and improving the poor filter passability caused by insoluble matter. The degree of polymerization of the polyvinyl alcohol resin (C) may be 100 to 3500, preferably 100 to 2000, and more preferably 200 to 1800. When the degree of polymerization exceeds 3500, poor coating due to spraying may occur, so that the required adhesion amount cannot be obtained, and the inorganic fiber mat may not be able to obtain sufficient recovery. When the degree of polymerization is less than 100, the inorganic fiber mat may not be able to obtain sufficient recovery. The above-mentioned degree of polymerization is a value converted to polystyrene based on an aqueous gel permeation chromatography (GPC) analysis as a weight average degree of polymerization. In addition, the saponification degree of the polyvinyl alcohol resin is preferably 70 mol% or more, more preferably 80 mol% or more, and the upper limit is preferably less than 99.5 mol%, based on the test method of JIS K 6726. When the saponification degree is 99.5 mol % or more, the viscosity rises greatly at low temperatures, and gelation may occur.

[0056] As the polyvinyl alcohol-based resin of the component (C), a commercially available product may be used, and examples thereof include "POVAL (PVA)" manufactured by JAPAN VAM & POVAL CO., LTD., and the like.

[0057] In the case of containing (C) polyvinyl alcohol-based resin, relative to 100 parts by mass of (A) cellulose ether, it is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and as an upper limit, it is preferably 900 parts by mass or less, more preferably 250 parts by mass or less, further preferably 100 parts by mass or less, and most preferably 50 parts by mass or less. If the amount is more than 900 parts by mass, the undesirable situation of reduced resilience may occur sometimes. In addition, if the amount is less than 10 parts by mass, the coating is poor due to spraying, the filter passability is poor due to insoluble matter, and the desired adhesion amount cannot be obtained, resulting in the undesirable situation that the inorganic fiber mat cannot obtain sufficient resilience.

[0058] The inorganic fiber binder of the present invention is composed of (A) cellulose ether, (B) ammonia-modified copolymer containing maleic anhydride, and (C) polyvinyl alcohol-based resin as required. The total amount of these components is preferably 90% by mass or more, more preferably 95% by mass or more, and most preferably 100% by mass relative to 100% by mass of the inorganic fiber binder (composition). As other components, additives such as water-retaining materials such as urea, silane coupling agents, waterproofing agents, pH adjusting agents, coloring agents, etc. can be added as required. The addition amount of these additives can be arbitrarily set within the scope of not damaging the effect of the present invention. By mixing them, a binder is obtained.

[0059] The inorganic fiber binder of the present invention is preferably dissolved in water and used as an inorganic fiber binder aqueous solution. The viscosity of the inorganic fiber binder aqueous solution is preferably 1 to 100 mPa·s at 20°C, and particularly preferably 1 to 50 mPa·s. It should be noted that the viscosity value is a measured value using a rotational viscometer. When the viscosity exceeds 100 mPa·s, the jetting (spraying) is poor, and the amount of adhesive attached after processing is reduced, so the effect of the present invention is sometimes not achieved. In addition, its concentration is preferably 10% by mass or less, more preferably 5% by mass or less, and most preferably 3% by mass or less.

[0060] The pH of the aqueous solution of the inorganic fiber binder is preferably 4 to 10. When the pH is out of the above range, the crosslinking property may change, which may affect the restorability.

[0061] Furthermore, the aqueous solution of the inorganic fiber binder preferably does not generate formaldehyde. For example, in JIS-A9504, it is divided into three levels of F☆☆ to F☆☆☆☆. 2 If the concentration is less than 5 μg / m 2 h and 20 μg / m 2 · If the concentration is less than 20 μg / m 2 h and 120 μg / m 2 When ·h is less than or equal to F☆☆ type, the F☆☆☆☆ type is the most excellent, and when the inorganic fiber binder of the present invention is used, an F☆☆☆☆ type inorganic fiber mat described below can be produced.

[0062] The binder for inorganic fibers of the present invention can be used for various inorganic fibers, and particularly exhibits excellent effects on glass wool and rock wool.

[0063] The inorganic fiber mat of the present invention is formed by treating inorganic fibers with the inorganic fiber binder. The inorganic fibers used in the inorganic fiber mat are not particularly limited, but are preferably glass wool or rock wool.

[0064] As a method for fiberizing the inorganic fibers, conventionally known methods such as centrifugal method and blowing method can be used. Furthermore, the density of the inorganic fiber mat can be the density used in common thermal insulation materials and sound absorbing materials, preferably 40 kg / m 3 Below, more preferably 32kg / m 3 The thickness of the inorganic fibers used may be any desired thickness, and is preferably selected from a thickness of 1 to 20 μm.

[0065] The amount of the inorganic fiber binder used is preferably 1 to 10% by mass, more preferably 1 to 5% by mass, relative to the inorganic fiber in terms of solid content ratio. If it is less than 1% by mass, there may be disadvantages such as the inorganic fiber mat lacking in recovery being formed, and if it exceeds 10% by mass, there may be disadvantages such as the inorganic fiber mat being formed into a firmly crushed inorganic fiber mat.

[0066] Reference Figure 1 and Figure 2 An example of a method for producing an inorganic fiber mat using the inorganic fiber binder of the present invention will be described. Figure 1 is a schematic diagram showing one embodiment of a process for producing an inorganic fiber mat using the inorganic fiber binder of the present invention, Figure 2 This is a perspective view showing one embodiment of the step of applying the binder for inorganic fibers of the present invention to inorganic fibers.

[0067] First, a fiberizing process is performed to spin inorganic fibers such as glass wool using a fiberizing device 1. Here, there is no particular limitation on the fiberizing method using the fiberizing device 1, and examples include conventionally known centrifugal methods, blowing methods, etc. In addition, a plurality of fiberizing devices 1 may be provided according to the density, thickness, and width direction length of the inorganic fiber mat 7 to be manufactured.

[0068] Then, if Figure 2 As shown in the figure, the binder imparting device 2 is used to impart the binder of the present invention to the inorganic fibers 3 spun from the fiberizing device 1. As a method for imparting the binder, a conventionally known method can be used, for example, the binder aqueous solution can be used and imparted by a spray method, an immersion method, etc. The binder is attached mainly to the intersections of the fibers directly from the upper layer of the fibers or from an oblique direction, and the binder is also attached to the portions other than the intersections to perform the treatment.

[0069] The conveyor 41 is a device for stacking the inorganic fibers 3 to which the uncured binder is attached on a perforated conveyor. In order to stack the fibers uniformly, the conveyor 41 is preferably a perforated conveyor having a suction device.

[0070] Here, the amount of adhesive bonded in the present invention is measured by a method called loss on ignition or LOI (Loss of Ignition), and refers to the mass of material lost by burning and reducing the amount of a dry sample of the inorganic fiber mat to which the adhesive is bonded at about 550°C x sec.

[0071] Through the above steps, the inorganic fibers 3 to which the binder is applied are accumulated on the conveyor 41 disposed below the fiberizing device 1, and are continuously moved to the conveyor 42 disposed along the production line direction. Then, the accumulated inorganic fibers 3 are compressed to a predetermined thickness by the conveyor 42 and the conveyor 5 disposed opposite to the conveyor 42 at a predetermined interval, and enter the molding furnace 6 disposed at the positions of the conveyor 42 and the conveyor 5.

[0072] In the forming furnace 6, the binder of the present invention applied to the inorganic fiber 3 is heated and cured to form an inorganic fiber mat 7 of a predetermined thickness. In addition, the processing conditions vary greatly due to the length of the production line, etc., so they can be set appropriately. For example, in the case of the present embodiment, the heating temperature is preferably 150 to 300°C, and more preferably 180 to 250°C. If the heating temperature is lower than 150°C, the moisture of the inorganic fiber mat 7 may not be completely evaporated, and if it is higher than 300°C, the binder treated on the inorganic fiber mat 7 may be carbonized. In addition, the heating time is preferably 120 to 360 seconds, and more preferably 180 to 300 seconds. If the heating temperature is shorter than 120 seconds, the moisture of the inorganic fiber mat 7 may not be completely evaporated, and if it is longer than 360 seconds, the binder treated on the inorganic fiber mat 7 may be carbonized. Moreover, the formed inorganic fiber mat 7 is cut into a predetermined product size by a cutting machine 8 provided in the part of the conveyor 43, and then transported, packaged, and bundled by the conveyor 44.

[0073] The inorganic fiber mat of the present invention thus produced has a superior recovery rate compared to inorganic fiber mats treated with binders proposed hitherto, such as phenolic resins, and emits very little volatile organic compounds.

[0074] When the inorganic fiber binder of the present invention is used, an F☆☆☆☆-shaped inorganic fiber mat can be produced.

[0075] In addition, the recovery rate of the inorganic fiber mat in the present invention is expressed as the ratio of the thickness of the inorganic fiber mat after the external force is removed and the inorganic fiber mat is restored after being compressed by an external force to the thickness of the inorganic fiber mat before compression. In order to improve the efficiency of storage and transportation, a certain number of inorganic fiber mats are sometimes compressed and packaged together. Therefore, when the inorganic fiber mat obtained by unpacking the package cannot ensure the thickness before compression, that is, when the recovery rate of the inorganic fiber mat is poor, sometimes it is not possible to fully obtain the performance such as thermal insulation and sound absorption.

[0076] Example

[0077] The present invention will be described in detail below with reference to the following production examples, embodiments and comparative examples, but the present invention is not limited to the following embodiments. In the following examples, parts and % represent parts by mass and % by mass, respectively.

[0078] [Examples 1 to 6]

[0079] 100 parts of the cellulose ether listed in Table 1 and 5 parts of the amino-modified product of isobutylene-maleic anhydride copolymer were dissolved in ion exchange water to prepare an aqueous solution of an inorganic fiber binder (sometimes referred to as a "treatment solution") having a concentration of 2% by mass. 3 The glass wool was used as inorganic fiber, and the prepared aqueous solution of inorganic fiber binder was sprayed and coated to treat the glass wool, and then heated and dried under the treatment conditions in the embodiment at 200°C for 300 seconds to prepare 12 inorganic fiber mats. The inorganic fiber mats were stacked in such a way that the thickness was 10 cm, and a density of 0.015 g / cm 3 The amount of the inorganic fiber binder used (the amount attached) to the inorganic fiber mat was adjusted to a solid content ratio of 4% by mass relative to the inorganic fibers, based on the mass of the treated inorganic fiber mat.

[0080] [Examples 7 to 9]

[0081] An inorganic fiber mat was prepared by the same method as in Example 1 except that 90 parts of cellulose ether, 10 parts of polyvinyl alcohol and 5 parts of an amino-modified isobutylene-maleic anhydride copolymer were used.

[0082] [Examples 10 to 13]

[0083] In Example 7, except that the ratio of cellulose ether to polyvinyl alcohol was changed to 70:30, 50:50, 30:70, and 10:90, respectively, an aqueous solution of an inorganic fiber binder was prepared by the same production method as in Example 1 to produce an inorganic fiber mat.

[0084] [Examples 14 and 15]

[0085] An inorganic fiber mat was prepared by preparing an inorganic fiber binder aqueous solution in the same manner as in Example 1 except that the amounts of the amino-modified isobutylene-maleic anhydride copolymer were changed to 3 parts and 10 parts, respectively.

[0086] [Example 16]

[0087] An inorganic fiber mat was prepared by the same method as in Example 1 except that the amino-modified isobutylene-maleic anhydride copolymer "ISOBAM-104" was replaced with "ISOBAM-110".

[0088] [Comparative Example 1]

[0089] An inorganic fiber mat was prepared by preparing an aqueous solution of an inorganic fiber binder in the same manner as in Example 1 except that phenol resin "FG-1032" (water-soluble phenol: manufactured by DIC Corporation) was used instead of cellulose ether.

[0090] [Comparative Example 2]

[0091] An inorganic fiber mat was prepared by preparing an aqueous solution of an inorganic fiber binder by the same production method as in Example 1 except that the amount of the amino-modified isobutylene-maleic anhydride copolymer was changed to 1 part.

[0092] [Comparative Example 3]

[0093] An inorganic fiber mat was prepared by preparing an aqueous solution of an inorganic fiber binder by the same production method as in Example 1 except that polyvinyl alcohol was used instead of cellulose ether.

[0094] [Evaluation method]

[0095] The viscosity, pH, formaldehyde concentration, storage stability, spray suitability, and filter passability of the aqueous solutions of the inorganic fiber binder (treatment solutions) of Examples 1 to 16 and Comparative Examples 1 to 3 were measured.

[0096] In addition, the recovery rate speed of the inorganic fiber mats of Examples 1 to 16 and Comparative Examples 1 to 3 was measured.

[0097] 〈Viscosity of treatment fluid〉

[0098] The viscosity of an aqueous solution of the inorganic fiber binder having a concentration of 2% by mass was measured at 20° C. using a B-type viscometer.

[0099] 〈PH of treatment liquid〉

[0100] The pH of an aqueous solution of an inorganic fiber binder having a concentration of 2% by mass was measured at 20° C. by a glass electrode method.

[0101] 〈Formaldehyde concentration in treatment fluid〉

[0102] Using the MBTH colorimetric method, add K-1 reagent (1 small package) of the product name "Package Test Formaldehyde" (Model: WAK-FOR) of Kyoritsu RIKEN to 1.5 mL of the treated liquid, shake it 5 to 6 times at room temperature to react, and let it stand for 3 minutes. Suck it all into a polyethylene tube, shake it 5 to 6 times to color it, and let it stand for 1 minute. After standing, compare the color with the standard color and measure the concentration (color) close to the standard color. The results are recorded in Table 1.

[0103] 〈Storage stability of treatment solution〉

[0104] The state of the treatment liquid after being left to stand at room temperature for one month was visually observed.

[0105] ○: No separation was observed in the treated liquid.

[0106] ×: The treatment liquid separated or gelled.

[0107] When the treatment liquid separates or gels, the nozzle may be clogged and spraying may become impossible.

[0108] 〈Spray suitability〉

[0109] When the treatment liquid was sprayed by a spray (trigger type), the spray amount and coating unevenness were observed.

[0110] ○: A specified amount can be uniformly discharged.

[0111] △: The discharge amount and coating are uneven.

[0112] ×: Cannot be ejected.

[0113] <Filter permeability>

[0114] The treated liquid was passed through a filter (300 mesh) and the recovered product from the filter was observed.

[0115] ○: The amount of the recovered product from the filter is less than 0.1% relative to the total amount of the treated liquid.

[0116] Δ: The amount of the recovered product from the filter is 0.1% or more and less than 1.0% based on the total amount of the treated liquid.

[0117] ×: The amount of material recovered from the filter is 1.0% or more relative to the total amount of the treatment liquid.

[0118] 〈Recovery rate of inorganic fiber mat〉

[0119] When manufacturing the inorganic fiber mat, a sample of 10 cm×10 cm×10 cm was taken out, a load of 20 kg was applied for 1 hour, the thickness (dx) of the inorganic fiber mat after the load was applied was measured, and the recovery rate (n=5) was calculated according to the following formula (1). The results are recorded in Table 1.

[0120] The recovery rate is preferably 65% ​​or more, more preferably 70% or more.

[0121] R=(dx / d)×100 (1)

[0122] R: Recovery rate (%)

[0123] dx: Thickness of the restored inorganic fiber mat (mm)

[0124] d: Nominal thickness of the inorganic fiber mat before the test (mm)

[0125] [Table 1]

[0126]

[0127] **The above mixing ratios are calculated based on solid content.

[0128] The details of the cellulose ethers in the above table are as follows.

[0129] "METROSE SM-4" (methylcellulose manufactured by Shin-Etsu Chemical Co., Ltd., viscosity of 2 mass % aqueous solution is 5 mPa·s or less, methoxyl substitution degree is 1.8)

[0130] "METROSE SM-100" (methylcellulose manufactured by Shin-Etsu Chemical Co., Ltd., viscosity of 2 mass % aqueous solution 100 mPa·s, methoxyl substitution degree 1.8)

[0131] "METROSE 60SH-03" (hydroxypropyl methylcellulose manufactured by Shin-Etsu Chemical Co., Ltd., 2% aqueous solution with a viscosity of 5 mPa·s or less, methoxyl substitution degree 1.9, hydroxypropoxyl substitution molar number 0.25)

[0132] "METROSE 60SH-50" (hydroxypropyl methylcellulose manufactured by Shin-Etsu Chemical Co., Ltd., viscosity of 2 mass % aqueous solution 50 mPa·s, methoxyl substitution degree 1.9, hydroxypropoxyl substitution molar number 0.25)

[0133] "CELLOGEN 5A" (carboxymethyl cellulose manufactured by Daiichi Kogyo Seiyaku Co., Ltd., viscosity of 2 mass % aqueous solution is 5 mPa·s or less, degree of carboxymethyl substitution is 0.75)

[0134] "CELLOGEN 7A" (carboxymethyl cellulose manufactured by Daiichi Kogyo Seiyaku Co., Ltd., viscosity of 2% by mass aqueous solution 20 mPa·s, degree of carboxymethyl substitution 0.75)

[0135] In addition, the viscosity of the 2 mass % aqueous solution is the viscosity measured at 20 degreeC using the Brookfield viscometer.

[0136] The degree of methoxy substitution is the average number of hydroxyl groups substituted with methoxy groups per glucose ring unit of cellulose. The number of moles of substitution is the average number of moles of hydroxypropoxy groups or hydroxyethoxy groups added per glucose ring unit of cellulose.

[0137] The details of the polyvinyl alcohol in the above table are as follows.

[0138] JP-05 (partially saponified Poval: saponification degree 87-89%, degree of polymerization 500)

[0139] · "JM-17" (Intermediate saponification Poval: saponification degree 95-97%, degree of polymerization 1700)

[0140] "JC-25" (Completely saponified Poval: saponification degree 99-99.4%, degree of polymerization 2500)

[0141] The above products are all manufactured by JAPAN VAM&POVAL CO.,LTD.

[0142] "ISOBAM-104" in the above table is an amine-modified isobutylene-maleic anhydride copolymer manufactured by Kuraray Co., Ltd., and has the following chemical structure, a weight average molecular weight of 55,000 to 65,000, n=70 to 80% by mass, and m=20 to 30% by mass.

[0143] [Chemistry 3]

[0144]

[0145] "ISOBAM-110" in the above table is an amine-modified isobutylene-maleic anhydride copolymer manufactured by Kuraray Co., Ltd., and has the following chemical structure, a weight average molecular weight of 160,000 to 170,000, n=70 to 80% by mass, and m=20 to 30% by mass.

[0146] [Chemistry 4]

[0147]

[0148] Description of Reference Numerals

[0149] 1 Fibrosis device

[0150] 2. Adhesive applying device

[0151] 3 Inorganic fiber

[0152] 41, 42, 43, 44, 5 Conveyor

[0153] 6 Molding furnace

[0154] 7 Inorganic fiber mat

[0155] 8 Cutting machine

Claims

1. A binder for inorganic fibers, characterized in that: (A) 100 parts by mass of a cellulose ether having a viscosity of 500 mPa·s or less in a 2% by mass aqueous solution at 20° C., (B) 3 parts by mass or more of an amino-modified copolymer containing maleic anhydride, and (C) 5 parts by mass or more of a polyvinyl alcohol-based resin having a degree of polymerization of 100 to 3500, The cellulose ether (A) contains at least one selected from the group consisting of methyl cellulose, ethyl cellulose, ethyl methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose.

2. The binder for inorganic fibers according to claim 1, wherein The (B) amino-modified copolymer containing maleic anhydride has a weight average molecular weight of 50,000 to 300,000 and has the following structural formula: [Chemistry 1] In the above formula, R 1 and R 2 Each is a linear or branched alkylene group having 2 to 5 carbon atoms, n and m are positive numbers, and the content of n is 50 to 90 mass % based on 100 mass % of the total of n+m.

3. The binder for inorganic fibers according to claim 1 or 2, wherein: The (B) amine-modified product of the copolymer containing maleic anhydride is an amine-modified product of an isobutylene-maleic anhydride copolymer.

4. The binder for inorganic fibers according to claim 1 or 2, wherein The (C) polyvinyl alcohol-based resin has a saponification degree of 70 mol% or more.

5. The binder for inorganic fibers according to claim 1 or 2, wherein: The inorganic fiber is glass wool or asbestos.

6. The binder for inorganic fibers according to claim 1 or 2, wherein: The inorganic fiber binder aqueous solution is dissolved in water and used as the inorganic fiber binder aqueous solution, and the viscosity of the inorganic fiber binder aqueous solution is 1 to 100 mPa·s at 20°C.

7. An inorganic fiber mat comprising inorganic fibers treated with the inorganic fiber binder according to any one of claims 1 to 6.