A carbon / nickel surface modified titanium-based metal bipolar plate and its preparation method and application

The carbon/nickel surface modification layer was prepared on the titanium-based bipolar plate by electrodeposition and autocatalytic methods, which solved the problem of high cost of surface modification process of titanium-based bipolar plates, and achieved low-cost, simple process and high-efficiency titanium Basic bipolar plate production, suitable for large-scale fuel cell production.

CN115172792BActive Publication Date: 2024-11-15ZHENGZHOU UNIVERSITY OF LIGHT INDUSTRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210852053.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-19
Publication Date
2024-11-15
Estimated Expiration
2042-07-19

AI Technical Summary

Technical Problem

The existing titanium-based bipolar plate surface modification process is costly and is not suitable for large-scale production. In particular, the preparation of carbon film modified layers requires high temperature and complex equipment, and commercial production cannot be achieved.

Method used

Using electrodeposition combined with autocatalysis method, a nickel layer is prepared on the surface of the titanium-based bipolar plate, and a carbon/nickel surface modified layer is prepared by cracking catalysis using carbon materials in the discarded medical masks, reducing costs and simplifying the process.

Benefits of technology

It realizes low-cost, simple process, and large-scale production of carbon/nickel surface modified titanium-based bipolar plates, improves corrosion resistance and electrical conductivity, and is suitable for efficient production of fuel cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115172792B_ABST
    Figure CN115172792B_ABST
Patent Text Reader

Abstract

The present invention relates to a carbon / nickel surface-modified titanium-based metal bipolar plate and a preparation method and application thereof, and belongs to the field of fuel cell technology. The method comprises the following steps: after degreasing and washing the titanium-based metal plate, a nickel transition layer is first electrodeposited; the discarded medical masks are disinfected, disassembled, dried, and crushed; the titanium-based metal after the surface electrodeposition of nickel and the treated discarded medical masks are mixed and put into a tubular furnace together and evacuated; the vacuumized tubular furnace is heated at 200-600°C for 1-10 hours to obtain. The present invention first prepares a nickel transition layer on the surface of the titanium-based metal bipolar plate, and then uses nickel metal to crack the discarded medical masks to prepare carbon materials with catalytic properties. A carbon / nickel surface modification layer is successfully prepared on the surface of the titanium-based metal bipolar plate, thereby improving the corrosion resistance of the titanium-based metal and reducing its surface contact resistance. The process is simple, the preparation time is short, the cost is low, and it is green and environmentally friendly, and can be applied to large-scale fuel cell production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a carbon / nickel surface-modified titanium-based metal bipolar plate and a preparation method and application thereof, belonging to the field of fuel cells. Background Art

[0002] Proton exchange membrane fuel cells (PEMFCs) have the characteristics of high energy conversion efficiency, low temperature operation, and environmental friendliness, and have become one of the mainstream technologies for the application and promotion of fuel cells worldwide. Bipolar plates are one of the important components of fuel cell stacks, accounting for more than 70% of the total mass, about 50% of the total volume, and about 30% of the total cost. They play the role of conducting current, supporting the battery structure, evenly distributing the reaction gases of the cathode and anode, and discharging the reaction products. Therefore, bipolar plates are required to have high conductivity, high air tightness, good mechanical properties, corrosion resistance, low cost, and easy batch processing.

[0003] At present, bipolar plate materials can be divided into three categories: carbon-based materials, metal materials and composite materials. Among them, metal materials have good electrical conductivity, thermal conductivity, and mechanical processing properties, and can achieve thin bipolar plates (0.05~1 mm), which are increasingly widely used, especially in occasions where fuel cell power density is required to be high, such as passenger cars. At present, almost all major automobile companies use metal bipolar plates for fuel cells used in passenger cars. Light metals represented by titanium have a low density and have a competitive advantage in further improving the power density of fuel cells. However, the surface of titanium is prone to generate a passivation film with very low conductivity. This passivation film greatly increases the ohmic loss inside the battery stack, so surface modification is required. The surface modification layer mainly includes transition metals and their compounds, carbon film, etc. Among them, the carbon film modification layer has good electrical conductivity and corrosion resistance as well as a relatively low cost, which is currently a hot material for surface modification of titanium-based bipolar plates. The main preparation methods for carbon film modification layers are currently chemical vapor deposition (CVD) (such as Toyota's patented technology (US2014356764)) and physical vapor deposition (PVD) (such as multi-arc ion plating and magnetron sputtering). The PVD technology for preparing coating films has high requirements for the cleanliness of the substrate, and has strict requirements for equipment, and the process cost is high. When using CVD to prepare carbon layers, a high-temperature (generally above 700°C) carbon-containing reducing atmosphere or complex plasma-assisted equipment is usually required. There are also problems such as high process costs and inability to carry out large-scale commercial production.

[0004] The main component material of discarded medical masks is polypropylene (PP). In view of this, the present invention proposes to use discarded medical masks as a carbon source and prepare a carbon / nickel modified layer with high corrosion resistance, low contact resistance and high stability on the surface of a titanium-based bipolar plate through a simple and feasible electrodeposition combined with autocatalysis method. Summary of the invention

[0005] The purpose of the present invention is to provide a carbon / nickel surface modified titanium-based metal bipolar plate and its preparation method and application with low cost, simple process and large-scale production. The present invention first prepares a nickel transition layer on the surface of the titanium-based metal bipolar plate, and then uses the catalytic property of nickel metal to crack discarded medical masks to prepare carbon materials. The carbon / nickel surface modification layer is successfully prepared on the surface of the titanium-based metal bipolar plate, which not only improves the corrosion resistance of the titanium-based metal but also reduces its surface contact resistance. At the same time, the process is simple, the preparation time is short, the cost is low, and it is green and environmentally friendly, and can be applied to large-scale fuel cell production.

[0006] In order to achieve the above purpose, the technical solution adopted by the present invention is:

[0007] A method for preparing a carbon / nickel surface-modified titanium-based bipolar plate comprises the following steps:

[0008] 1) Place the titanium-based metal in an alkaline solution to remove oil, then place it in a hydrochloric acid solution for pickling, then wash it with distilled water, and dry it for later use;

[0009] 2) Disinfect, disassemble, dry and crush the discarded medical masks to obtain powder for later use;

[0010] 3) placing the titanium-based metal treated in step 1) in an electrodeposition tank, and using a three-electrode system to uniformly electrodeposit a nickel layer on the surface of the titanium sheet;

[0011] 4) The powder obtained in step 2) and the titanium-based metal after surface nickel electrodeposition in step 3) are placed in an ark together, and then placed in a tube furnace and the tube furnace is vacuumed.

[0012] 5) The tube furnace after evacuation in step 4) is kept warm and heated to obtain a titanium-based metal bipolar plate with a carbon / nickel surface modification.

[0013] Furthermore, in step 1), the degreasing process requires ultrasonic treatment for 5-10 min using a mixed solution of 60 g / L NaOH, 50 g / L Na2CO3, 20 g / L Na3PO4•12H2O, and 10 g / L Na2SiO3, and the acid washing process requires ultrasonic treatment for 3 min using a 3M hydrochloric acid solution, followed by washing with water for 10 min and drying for later use.

[0014] Furthermore, the solution used in the degreasing process in step 1) is prepared by weighing 6g NaOH, 5g Na2CO3, 2g Na3PO4•12H2O, and 1g Na2SiO3 reagents, making a 100ml solution into a volumetric flask, shaking it well, and taking it out for later use.

[0015] Furthermore, the titanium-based metal in step 1) is one or more of pure titanium or titanium alloy.

[0016] Furthermore, in step 2), the disinfectant solution used is 84 disinfectant, the drying temperature is 70°C, the nose bridge part of the mask is disassembled, and the rest is crushed with a grinder, and the powder size obtained after crushing is 1~10μm.

[0017] Furthermore, in step 3), the composition of the plating solution used for the electrodeposition of nickel is as follows: 300-400 g / L nickel sulfate, 50-80 g / L nickel chloride, 30-40 g / L boric acid, 0.05-2 g / L sodium dodecyl sulfate, pH 5-6.

[0018] Furthermore, in step 3), the auxiliary electrode is a Pt sheet, the reference electrode is a saturated calomel electrode (SCE), and the current density is 1~100×10 -5 A / cm 2 , the potential is -1.0~-0.5V, and the deposition time is 10~1000s.

[0019] Furthermore, in step 3), the mass ratio of the powder to the titanium-based metal after nickel electrodeposition is 1:(1-10).

[0020] Furthermore, the vacuum degree of the vacuum in step 4) is 0.01~1Pa.

[0021] Furthermore, the heat preservation heating in step 5) is to increase the temperature to 200-600° C. at a rate of 1-10° C. / min and keep the temperature for 1-10 hours.

[0022] The invention provides a carbon / nickel surface-modified titanium-based metal bipolar plate prepared by the method.

[0023] Another object of the present invention is to provide the use of the carbon / nickel surface modified titanium-based metal bipolar plate prepared by the above method in the preparation of fuel cells.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The present invention uses electrodeposited nickel as a catalyst to catalyze the cracking of the treated waste medical supplies, and obtains a carbon / nickel modified layer in situ on the surface of the titanium-based metal, and the obtained product is densely and evenly distributed on the metal surface. Not only does it improve the corrosion resistance of the titanium-based metal as a bipolar plate, but it also greatly improves its surface conductivity.

[0026] (2) The carbon source used in preparing the carbon modified layer is the pyrolysis atmosphere of discarded medical masks, and no other additional carbon-containing gas, reducing gas and inert atmosphere are required.

[0027] (3) The method of the present invention has simple process, short preparation time, low cost, green and environmental protection, is suitable for large-scale production, and has good application prospects.

[0028] (4) The bipolar plate obtained by the present invention is applied to proton exchange membrane fuel cells, which can not only improve the energy density and service life of the fuel cell and reduce the cost of the fuel cell stack, but also solve the environmental problems caused by the disposal of discarded medical masks. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The XRD spectrum of the carbon / nickel surface modified pure titanium bipolar plate of Example 4 of the present invention;

[0030] Figure 2 This is a surface SEM image of a pure titanium bipolar plate modified with carbon / nickel according to Example 4 of the present invention;

[0031] Figure 3 This is a cross-sectional SEM image of a carbon / nickel surface-modified pure titanium bipolar plate according to Example 4 of the present invention;

[0032] Figure 4 The polarization curve of the carbon / nickel surface modified pure titanium bipolar plate of Example 4 of the present invention in a simulated proton exchange membrane fuel cell environment (0.5 mol / L H2SO4+2ppm HF, 80°C);

[0033] Figure 5 The time current line of the carbon / nickel surface modified pure titanium bipolar plate of Example 4 of the present invention at a constant potential of 0.6 V for 4 hours in a simulated proton exchange membrane fuel cell cathode environment (0.5 mol / L H2SO4+2ppm HF, 80°C, oxygen);

[0034] Figure 6 The time current line of the carbon / nickel surface modified pure titanium bipolar plate of Example 4 of the present invention at a constant potential of -0.1 V for 4 hours in a simulated proton exchange membrane fuel cell anode environment (0.5 mol / L H2SO4+2ppm HF, 80°C, hydrogen flow);

[0035] Figure 7 This is a graph showing the variation of the interface contact resistance (ICR) of the carbon / nickel surface modified pure titanium bipolar plate according to Example 4 of the present invention with the assembly pressure. DETAILED DESCRIPTION

[0036] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention easier to understand, the present invention is described in detail below with reference to the accompanying drawings and specific implementation methods.

[0037] Example 1

[0038] The method for preparing the carbon / nickel surface modified titanium-based metal bipolar plate of this embodiment comprises the following steps:

[0039] 1) Cut commercial pure titanium into 1×2cm size, prepare a mixed solution of 60g / L NaOH, 50g / L Na2CO3, 20g / L Na3PO4•12H2O, and 10g / L Na2SiO3, ultrasonicate for 10min, ultrasonicate with 3M hydrochloric acid solution for 3min, and wash with water for 10min. After the treatment, dry it in a drying oven at 70℃ for 12h for later use;

[0040] The collected discarded medical masks are disinfected, disassembled, dried, and crushed to obtain powder for use. The disinfection solution used is 84 disinfectant, and the drying temperature is 70°C. The nose bridge part of the mask is disassembled and the rest is crushed with a grinder. The powder size after crushing is 1~10μm.

[0041] 2) Place the pure titanium treated in step 1) in an electrodeposition tank and use a three-electrode system to uniformly electrodeposit a nickel layer on the surface of the titanium sheet. The plating solution used is 350 g / L nickel sulfate, 60 g / L nickel chloride, 35 g / L boric acid, 1 g / L sodium dodecyl sulfate, and the pH is 5. During electrodeposition, the auxiliary electrode is a Pt sheet, the reference electrode is a saturated calomel electrode (SCE), and the current density is 1×10 -5 A / cm 2 , potential is -0.7 V, deposition time is 1000 s.

[0042] 3) Take the titanium sheet with nickel deposited on the surface obtained in step 2) and lay it flat on the bottom of the ark, and evenly place the discarded medical masks treated in step 1) on it, with the mass ratio of the titanium sheet to the treated discarded masks being 1:1. Place the ark in a tube furnace and evacuate it to 0.1 Pa, heat the tube furnace to 200°C at a heating rate of 5°C / min, and keep it warm for 2h to obtain the product.

[0043] Example 2

[0044] The method for preparing the carbon / nickel surface modified titanium-based metal bipolar plate of this embodiment comprises the following steps:

[0045] 1) Same as step 1) in Example 1.

[0046] 2) Place the pure titanium treated in step 1) in an electrodeposition tank and use a three-electrode system to uniformly electrodeposit a nickel layer on the surface of the titanium sheet. The plating solution used is 350 g / L nickel sulfate, 60 g / L nickel chloride, 35 g / L boric acid, 1 g / L sodium dodecyl sulfate, and the pH is 5. During electrodeposition, the auxiliary electrode is a Pt sheet, the reference electrode is a saturated calomel electrode (SCE), and the current density is 1×10 -4 A / cm 2 , potential is -0.8 V, deposition time is 200 s.

[0047] 3) Take the titanium sheet with nickel deposited on the surface obtained in step 2) and lay it flat on the bottom of the ark, and evenly place the discarded medical masks treated in step 1) on it, with the mass ratio of titanium sheet to treated discarded masks being 1:2. Place the ark in a tube furnace and evacuate it to 0.1 Pa, heat the tube furnace to 300°C at a heating rate of 5°C / min, and keep it warm for 2h to obtain the product.

[0048] Example 3

[0049] The method for preparing the carbon / nickel surface modified titanium-based metal bipolar plate of this embodiment comprises the following steps:

[0050] 1) Same as step 1) in Example 1.

[0051] 2) Take the pure titanium treated in step 1) and place it in an electrodeposition tank. Use a three-electrode system to uniformly electrodeposit a nickel layer on the surface of the titanium sheet. The plating solution used is 350g / L nickel sulfate, 60g / L nickel chloride, 35g / L boric acid, 1g / L sodium dodecyl sulfate, and the pH is 5. During electrodeposition, the auxiliary electrode is a Pt sheet, the reference electrode is a saturated calomel electrode (SCE), and the current density is 2×10 -4 A / cm 2 , potential is -0.9 V, deposition time is 60 s.

[0052] 3) Take the titanium sheet obtained in step 2) and spread it on the bottom of the ark, and evenly place the discarded medical masks treated in step 1) on it, with the mass ratio of titanium sheet to treated discarded masks being 1:4. Place the ark in a tube furnace and evacuate it to 0.1 Pa, heat the tube furnace to 400°C at a heating rate of 5°C / min, and keep it warm for 2h to obtain the product.

[0053] Example 4

[0054] The method for preparing the carbon / nickel surface modified titanium-based metal bipolar plate of this embodiment comprises the following steps:

[0055] 1) Same as step 1) in Example 1.

[0056] 2) Place the pure titanium treated in step 1) in an electrodeposition tank and use a three-electrode system to uniformly electrodeposit a nickel layer on the surface of the titanium sheet. The plating solution used is 350 g / L nickel sulfate, 60 g / L nickel chloride, 35 g / L boric acid, 1 g / L sodium dodecyl sulfate, and the pH is 5. During electrodeposition, the auxiliary electrode is a Pt sheet, the reference electrode is a saturated calomel electrode (SCE), and the current density is 3×10 -4 A / cm 2 , potential is -0.9 V, and deposition time is 80 s.

[0057] 3) Take the titanium sheet obtained in step 2) and spread it on the bottom of the ark, and evenly place the discarded medical masks treated in step 1) on it, with the mass ratio of titanium sheet to treated discarded masks being 1:1.5. Place the ark in a tube furnace and evacuate it to 0.1 Pa, heat the tube furnace to 500°C at a heating rate of 5°C / min, and keep it warm for 2h to obtain the product.

[0058] Example 5

[0059] The method for preparing the carbon / nickel surface modified titanium-based metal bipolar plate of this embodiment comprises the following steps:

[0060] 1) Cut the commercial titanium alloy TC4 into 1×2cm size, prepare a mixed solution of 60g / L NaOH, 50g / L Na2CO3, 20g / LNa3PO4•12H2O, and 10g / L Na2SiO3, ultrasonicate for 10min, ultrasonicate with 3M hydrochloric acid solution for 3min, and wash with water for 10min. After the treatment, dry it in a drying oven at 70℃ for 12h for later use;

[0061] The other steps are the same as those in Example 4.

[0062] Example 6

[0063] The method for preparing the carbon / nickel surface modified titanium-based metal bipolar plate of this embodiment comprises the following steps:

[0064] 1) Same as step 1) in Example 1.

[0065] 2) Place the pure titanium treated in step 1) in an electrodeposition tank and use a three-electrode system to uniformly electrodeposit a nickel layer on the surface of the titanium sheet. The plating solution used is 350 g / L nickel sulfate, 60 g / L nickel chloride, 35 g / L boric acid, 1 g / L sodium dodecyl sulfate, and the pH is 5. During electrodeposition, the auxiliary electrode is a Pt sheet, the reference electrode is a saturated calomel electrode (SCE), and the current density is 6×10 -4 A / cm 2 , potential is -0.9 V, deposition time is 30 s.

[0066] 3) Take the titanium sheet obtained in step 2) and spread it on the bottom of the ark, and evenly place the discarded medical masks treated in step 1) on it, with the mass ratio of titanium sheet to treated discarded masks being 1:6. Place the ark in a tube furnace and evacuate it to 0.1 Pa, heat the tube furnace to 600°C at a heating rate of 5°C / min, and keep it warm for 2h to obtain the product.

[0067] Example 7

[0068] The method for preparing the carbon / nickel surface modified titanium-based metal bipolar plate of this embodiment comprises the following steps:

[0069] 1) Same as step 1) in Example 1.

[0070] 2) Place the pure titanium treated in step 1) in an electrodeposition tank and use a three-electrode system to uniformly electrodeposit a nickel layer on the surface of the titanium sheet. The plating solution used is 350 g / L nickel sulfate, 60 g / L nickel chloride, 35 g / L boric acid, 1 g / L sodium dodecyl sulfate, and the pH is 5. During electrodeposition, the auxiliary electrode is a Pt sheet, the reference electrode is a saturated calomel electrode (SCE), and the current density is 8×10 -4 A / cm 2 , potential is -0.9 V, deposition time is 20 s.

[0071] 3) Take the titanium sheet obtained in step 2) and spread it on the bottom of the ark, and evenly place the discarded medical masks treated in step 1) on it, with the mass ratio of titanium sheet to treated discarded masks being 1:8. Place the ark in a tube furnace and evacuate it to 0.1 Pa, heat the tube furnace to 600°C at a heating rate of 5°C / min, and keep it warm for 2h to obtain the product.

[0072] Example 8

[0073] The method for preparing the carbon / nickel surface modified titanium-based metal bipolar plate of this embodiment comprises the following steps:

[0074] 1) Same as step 1) in Example 1.

[0075] 2) Place the pure titanium treated in step 1) in an electrodeposition tank and use a three-electrode system to uniformly electrodeposit a nickel layer on the surface of the titanium sheet. The plating solution used is 350 g / L nickel sulfate, 60 g / L nickel chloride, 35 g / L boric acid, 1 g / L sodium dodecyl sulfate, and the pH is 5. During electrodeposition, the auxiliary electrode is a Pt sheet, the reference electrode is a saturated calomel electrode (SCE), and the current density is 1×10 -3 A / cm 2 , potential is -0.9 V, deposition time is 10 s.

[0076] 3) Take the titanium sheet obtained in step 2) and spread it on the bottom of the ark, and evenly place the discarded medical masks treated in step 1) on it, with the mass ratio of titanium sheet to treated discarded masks being 1:10. Place the ark in a tube furnace and evacuate it to 0.1 Pa, heat the tube furnace to 500°C at a heating rate of 5°C / min, and keep it warm for 2h to obtain the product.

[0077] Test example

[0078] 1) Physical phase test

[0079] The carbon / nickel surface modified pure titanium bipolar plate (denoted as: C / Ni-Ti) prepared in Example 4 was subjected to X-ray diffraction (XRD) analysis, and the results are as follows: Figure 1As shown in the figure, for comparison, the diffraction pattern of pure titanium matrix is ​​also listed. Figure 1 It can be seen that the carbon / nickel surface modified pure titanium bipolar plate prepared in Example 4 has obvious diffraction peaks, which are found to be diffraction peaks of Ti when compared with the substrate. A short and broadened diffraction peak can be observed near 21°, corresponding to amorphous carbon.

[0080] 2) Morphology test

[0081] The carbon / nickel surface modified pure titanium bipolar plate material prepared in Example 4 was tested by scanning electron microscope (SEM). Figure 2 , as shown in 3.

[0082] Figure 2 The surface SEM image of the pure titanium bipolar plate modified with carbon / nickel shows that the carbon particles are evenly distributed on the surface of the titanium plate, forming a dense protective film.

[0083] Figure 3 This is a cross-sectional SEM image of a pure titanium bipolar plate modified with carbon / nickel. It can be observed that the outermost layer is an amorphous carbon layer with a thickness of about 100nm. The carbon layer is dense and uniform. Connected to the carbon layer is a nickel layer with a thickness of about 1μm.

[0084] 3) Corrosion resistance test

[0085] The corrosion resistance of the carbon / nickel surface modified pure titanium bipolar plate prepared in Example 4 was tested by a three-electrode system, wherein the carbon / nickel surface modified pure titanium bipolar plate was the working electrode, the platinum electrode was the counter electrode, and the saturated calomel electrode was the reference electrode. The proton exchange membrane fuel cell environment was simulated by a 0.5 mol / L H2SO4+2ppm HF solution at 80°C. Figure 4 It is a Tafel curve. It can be seen that the corrosion potential of the pure titanium bipolar plate after carbon / nickel surface modification moves to the positive direction, and the passivation current density is significantly lower than that of the pure titanium substrate, indicating that the carbon / nickel surface modification layer improves the corrosion resistance of the substrate.

[0086] Figure 5 The time current line of the carbon / nickel surface modified pure titanium material prepared in Example 4 as a bipolar plate was tested at a constant potential of 0.6 V for 4 hours in a simulated proton exchange membrane fuel cell cathode environment (0.5 mol / L H2SO4+2ppm HF, 80°C, oxygen flow). After 4 hours of testing, the corrosion current density was still 3.5×10 -8 A / cm 2 , meeting DOE's requirements for cathode bipolar plate corrosion resistance (<1×10 -6 A / cm 2 ).

[0087] Figure 6The time current line of the bipolar plate of the carbon / nickel surface modified pure titanium material prepared in Example 4 was tested at a constant potential of -0.1V for 4h in a simulated proton exchange membrane fuel cell anode environment (0.5 mol / L H2SO4+2ppm HF, 80℃, hydrogen flow). After 4h of testing, the corrosion current density was -0.8×10 -6 A / cm 2 , meeting DOE's requirements for corrosion resistance of anode bipolar plates (<1×10 -6 A / cm 2 ).

[0088] 4) Interface contact resistance test

[0089] The carbon / nickel surface modified pure titanium bipolar plate prepared in Example 4 was tested with reference to the test method and requirements for contact resistance of proton exchange membrane fuel cells in GB / T20042.6-2011 to obtain the contact resistance of the implementation sample and the substrate. Figure 7 As shown. The titanium bipolar plate modified with surface carbon / nickel has lower interface contact resistance at 140 N / cm 2 Under the assembly pressure, the contact resistance value is 8 mΩ·cm 2 , which is much lower than the interface contact resistance of the substrate at this pressure, 89 mΩ·cm 2 .

[0090] The above disclosure is only the preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made within the scope of the present invention still belong to the scope covered by the present invention.

Claims

1. A method for preparing a carbon / nickel surface-modified titanium-based metal bipolar plate, characterized in that: The steps include: 1) Place the titanium-based metal in an alkaline solution to remove oil, then place it in a hydrochloric acid solution for pickling, then wash it with distilled water, and dry it for later use; 2) Disinfect, disassemble, dry and crush the discarded medical masks to obtain powder for later use; 3) placing the titanium-based metal treated in step 1) in an electrodeposition tank, and using a three-electrode system to uniformly electrodeposit a nickel layer on the surface of the titanium sheet; 4) The powder obtained in step 2) and the titanium-based metal after the surface nickel electrodeposition in step 3) are placed together in an ark, and then placed in a tube furnace and the tube furnace is evacuated; 5) heating the vacuumized tubular furnace in step 4) to obtain a carbon / nickel surface-modified titanium-based metal bipolar plate; In step 3), the composition of the plating solution used for the nickel electrodeposition is as follows: 300-400 g / L nickel sulfate, 50-80 g / L nickel chloride, 30-40 g / L boric acid, 0.05-2 g / L sodium dodecyl sulfate, pH 5-6; Step 3) During the electrodeposition, the auxiliary electrode is a Pt sheet, the reference electrode is a saturated calomel electrode, and the current density is 1~100×10 -5 A / cm 2 , the potential is -1.0~-0.5V, and the deposition time is 10~1000s.

2. The method for preparing a carbon / nickel surface-modified titanium-based metal bipolar plate according to claim 1, characterized in that: The titanium-based metal in step 1) is one or more of pure titanium and titanium alloy.

3. The method for preparing the carbon / nickel surface-modified titanium-based metal bipolar plate according to claim 1, characterized in that: The size of the powder in step 2) is 1-10 μm.

4. The method for preparing a carbon / nickel surface-modified titanium-based metal bipolar plate according to claim 1, characterized in that: In step 3), the mass ratio of the powder to the titanium-based metal after nickel electrodeposition is 1:(1-10).

5. The method for preparing a carbon / nickel surface-modified titanium-based metal bipolar plate according to claim 1, characterized in that: The vacuum degree of the vacuum pump in step 4) is 0.01~1Pa.

6. The method for preparing a carbon / nickel surface-modified titanium-based metal bipolar plate according to claim 1, characterized in that: The heat preservation heating in step 5) is to increase the temperature to 200~600℃ at a rate of 1~10℃ / min and keep it at this temperature for 1~10h.

7. A titanium-based metal bipolar plate with carbon / nickel surface modification prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the surface-modified titanium-based metal bipolar plate according to claim 7 in the preparation of a fuel cell.