Preparation method and application of PDI functionalized 3D g-C3N4 photocatalyst
By introducing PDI functionalization on 3D g-C3N4, the problems of low light energy utilization efficiency and poor CO2 adsorption capacity of photocatalytic materials are solved, the rate and selectivity of photocatalytic reduction of CO2 are significantly improved, and CO2 is realized to carbon hydrogen fuel efficient conversion.
Patent Information
- Application Number
- CN202210943339.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-08
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-08-08
AI Technical Summary
The existing photocatalytic materials have problems such as low photoenergy utilization efficiency, high photogenerating charge recombination rate, and slow charge transfer rate in terms of CO2 conversion to carbon and hydrogen fuel, which limit their catalytic activity, especially in the photocatalytic process of 3D g-C3N4. The photoresponse range is limited, the photogenerated electron-hole recombination rate is relatively high, the exciton binding energy is large, the redox potential is weak, and the carbon dioxide adsorption capacity is poor.
Through organic molecules functionalization, an intramolecular donor-acceptor (DA) structure was constructed, and 3D g-C3N4 was modified with perylene tetraacid dianhydride derivatives, and PDI was introduced to significantly improve the photoresponse range and reduce the photogenerated electron-hole recombination rate. , promote charge transfer efficiency, improve CO2 adsorption performance, and prepare PDI functionalized 3D g-C3N4 photocatalyst.
The rate and selectivity of photocatalytic reduction of CO2 are significantly improved, the ability of composite materials to capture CO2 is improved, and the efficient conversion of CO2 to carbon and hydrocarbon fuel is achieved, and the process is simple and easy to operate.
Smart Images

Figure CN115178294B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of organic molecular functionalized materials, and relates to a preparation method and application of a PDI functionalized 3D g-C3N4 photocatalyst. Background Art
[0002] Photocatalytic technology refers to a technology that uses photocatalysts under mild conditions to achieve chemical reactions that need to be carried out under severe conditions under the drive of light energy. Photocatalytic technology uses clean and pollution-free light energy as energy, is green and environmentally friendly, and does not require additional energy input. It is an ideal CO2 conversion technology. Using photocatalytic technology to convert CO2 into hydrocarbon fuels helps to reduce the concentration of CO2 in the atmosphere, alleviate the negative effects caused by the greenhouse effect, and also alleviate the energy crisis caused by the excessive consumption of fossil energy. In addition, photocatalytic reduction of CO2 technology constructs a new carbon cycle outside the carbon cycle in nature, which is conducive to achieving carbon balance. This technology is in line with the concept of sustainable development in today's society. However, existing photocatalytic materials still have disadvantages such as low light energy utilization efficiency, high recombination rate of photogenerated charges, and slow charge transfer rate, which are not conducive to the improvement of the activity of photocatalytic materials. Therefore, the development of a new type of photocatalytic material to achieve efficient and selective conversion of CO2 to hydrocarbon fuels has attracted widespread attention from scientific researchers.
[0003] Graphitic carbon nitride (g-C3N4) has the advantages of wide raw material sources, low cost, simple preparation, band gap structure suitable for CO2 reduction, and good stability, and has received widespread attention in the field of photocatalysis. However, defects such as low specific surface area, few active sites, limited light response range, and poor separation and transport performance of photogenerated charges in bulk g-C3N4 limit its catalytic activity. Preparing bulk g-C3N4 into a three-dimensional structure can significantly improve its light absorption performance by increasing the light absorption area, while shortening the transmission path from electrons to active sites, reducing photogenerated electron-hole recombination, and improving light energy utilization efficiency. In addition, the three-dimensional structure has a large specific surface area, many exposed active sites, and a fast substrate diffusion rate, which are all conducive to the improvement of the catalytic activity of 3D g-C3N4. However, 3D g-C3N4 still has problems such as limited light response range, high photogenerated electron-hole recombination rate, large exciton binding energy, weak redox potential, and poor carbon dioxide adsorption capacity in the photocatalytic process, which limits the further improvement of its catalytic activity. Summary of the invention
[0004] In view of the above problems, the present invention provides a preparation method and use of a PDI-functionalized 3D g-C3N4 photocatalyst.
[0005] By functionalizing organic molecules and constructing an intramolecular donor-acceptor (DA) structure, the electron-hole separation efficiency can be significantly improved, the interfacial charge transfer can be promoted, the band gap structure of the catalytic material can be regulated, and a redox potential that is beneficial to the reduction of CO2 can be obtained. At the same time, organic molecule functionalization can also improve the adsorption performance of the composite material for CO2, thereby significantly improving the rate of photocatalytic reduction of CO2.
[0006] The present invention adopts perylenetetracarboxylic dianhydride derivatives as functional molecules to modify 3D g-C3N4, and prepares DA composite photocatalytic materials based on PDI and 3D g-C3N4. The introduction of PDI into the 3D g-C3N4 structure significantly improves the light response range of the composite material, reduces the photogenerated electron-hole recombination rate, and promotes the charge transfer efficiency. At the same time, the composite material's ability to capture CO2 is improved, and the efficient and selective conversion of CO2 to hydrocarbon fuels is achieved.
[0007] The present invention adopts a high-temperature calcination method to prepare 3D g-C3N4. First, melamine-cyanuric chloride supramolecular aggregates are prepared in a solvent, and then the supramolecular aggregates are calcined at a high temperature to obtain 3D g-C3N4; then, a perylene tetracarboxylic dianhydride derivative is used to react with 3D g-C3N4 at a certain temperature to obtain a 3D g-C3N4-PDI composite photocatalyst.
[0008] The present invention achieves the above technical objectives through the following technical means.
[0009] A method for preparing a PDI-functionalized 3D g-C3N4 photocatalyst comprises the following steps:
[0010] (1) Preparation of melamine-cyanuric chloride supramolecular aggregates:
[0011] Dissolving melamine and cyanuric chloride in dimethyl sulfoxide respectively, stirring and dissolving to obtain a melamine solution and a cyanuric chloride solution; then mixing the melamine solution and the cyanuric chloride solution under stirring conditions, reacting the mixture to form a white precipitate, collecting the precipitate by centrifugation, washing it several times with ethanol, and then vacuum drying the precipitate to obtain a melamine-cyanuric chloride supramolecular aggregate;
[0012] (2) Preparation of 3D g-C3N4:
[0013] The melamine-cyanuric chloride supramolecular aggregate obtained in step (1) is ground into powder, sealed and packaged, and then calcined in a tube furnace under an inert gas atmosphere at a specific heating rate to a target temperature, to obtain a khaki solid product after calcination, which is recorded as 3D g-C3N4;
[0014] (3) Preparation of 3D g-C3N4-PDI composite photocatalyst:
[0015] The 3D g-C3N4 obtained in step (2) is ground to obtain 3D g-C3N4 powder; the perylene tetracarboxylic acid dianhydride derivative is dispersed in a solvent, and a dispersion is obtained after stirring and ultrasonic dispersion;
[0016] Subsequently, 3D g-C3N4 powder was added to the dispersion and stirred evenly. The solvent was removed by rotary evaporation, and the obtained product was vacuum dried to obtain a dry product. The dry product was calcined at a certain temperature to obtain a PDI-functionalized 3D g-C3N4 photocatalyst, which was recorded as 3D g-C3N4-PDI.
[0017] Preferably, in step (1), the dosage of melamine and dimethyl sulfoxide is 1 g: 5-30 mL; the dosage of cyanuric chloride and dimethyl sulfoxide is 1 g: 5-30 mL; and the volume ratio of the melamine solution and the cyanuric chloride solution when mixed is 1:1.
[0018] Preferably, the temperature of the vacuum drying oven in step (1) is 60° C. and the drying time is 6-12 h.
[0019] Preferably, in step (2), the mesh size of the powder is 100-150 mesh; the sealed packaging is specifically placing the powder in a porcelain boat and sealing it with tin foil; and the inert gas is argon.
[0020] Preferably, in step (2), the heating rate is 2.3° C. / min; the target temperature is 550° C., and the calcination time is 2 to 8 h.
[0021] Preferably, the mesh size of the 3D g-C3N4 powder in step (3) is 100-150 mesh.
[0022] Preferably, the perylenetetracarboxylic acid dianhydride derivative in step (3) is perylenetetracarboxylic acid dianhydride, 1,6,7,12-tetrachloro-3,4,9,10-perylenetetracarboxylic acid dianhydride or 1,6,7,12-tetrabromo-3,4,9,10-perylenetetracarboxylic acid dianhydride; the solvent is ethanol, acetone, dichloromethane, benzene, methanol, chloroform, tetrahydrofuran or acetonitrile; the amount of the perylenetetracarboxylic acid dianhydride derivative and the solvent is in the ratio of 0.1-1 g:10 mL.
[0023] Preferably, in step (3), the mass ratio of the 3D g-C3N4 powder to the perylene tetracarboxylic acid dianhydride derivative in the dispersion is 1 to 100:1.
[0024] Preferably, in step (3), the temperature of the vacuum drying oven is 60°C, and the drying time is 6-12h; the specific operation of calcining the dried product at a certain temperature is: placing the dried product in a porcelain boat and sealing it with tin foil; calcining it at a heating rate of 5°C / min to 250-550°C in an argon atmosphere, and the calcination time is 2-6h.
[0025] The PDI-functionalized 3D g-C3N4 photocatalyst prepared by the present invention is applied to the photocatalytic reduction of CO2 to prepare hydrocarbon fuels.
[0026] Beneficial effects of the present invention:
[0027] (1) The present invention uses perylene tetracarboxylic acid dianhydride derivatives and 3D g-C3N4 to react and construct a PDI-modified 3D g-C3N4-based intramolecular DA structure catalyst 3D g-C3N4-PDI, which significantly improves the visible light response range of 3D g-C3N4, improves the photogenerated electron-hole separation efficiency, and promotes the carrier transfer efficiency; in addition, the introduction of PDI functional groups is beneficial to improve the CO2 adsorption capacity of the composite material. Therefore, 3D g-C3N4-PDI exhibits efficient photocatalytic reduction of CO2 activity.
[0028] (2) The present invention prepares melamine-cyanuric chloride supramolecular aggregates by a simple solution reaction method, and then obtains 3D g-C3N4 by simple calcination, and obtains PDI-modified 3Dg-C3N4-based intramolecular DA composite photocatalytic material by reacting 3D g-C3N4 with a perylene tetracarboxylic dianhydride derivative. The process is simple, easy to operate, and convenient for large-scale production.
[0029] (3) The 3D g-C3N4-DA-PDI composite photocatalyst of the present invention catalyzes the reduction of CO2 in water under the drive of light energy. During this process, CO2 and H adsorbed on the catalyst surface + The reduction reaction occurs through interaction with photogenerated electrons to generate hydrocarbon fuels; the H2O adsorbed on the catalyst surface undergoes an oxidation reaction with the photogenerated holes and is oxidized to H + and oxygen; no additives are required during the reaction, making it a green and sustainable CO2 reduction technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Schematic diagram of the structure of the 3D g-C3N4-PDI photocatalytic material prepared by the present invention.
[0031] Figure 2 X-ray diffraction (XRD) spectrum of the photocatalytic material prepared in Example 1 of the present invention.
[0032] Figure 3Infrared spectrum of the 3D g-C3N4-PDI photocatalytic material prepared in Example 1 of the present invention.
[0033] Figure 4 Ultraviolet visible diffuse reflectance spectrum (UV-vis DRS) of the photocatalytic material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0034] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the protection scope of the present invention is not limited thereto. The PTCDA in the examples refers to 3,4,9,10-perylenetetracarboxylic dianhydride.
[0035] Embodiment 1:
[0036] (1) Preparation of melamine-cyanuric chloride supramolecular aggregates:
[0037] 1.0 g of melamine and 1.0 g of cyanuric chloride were dissolved in 20 mL of DMSO respectively, and stirred until fully dissolved to obtain two solutions; then the two solutions were mixed under stirring conditions to generate a white solid, and stirring was continued for 2 h. The precipitate after centrifugation was washed with 10 mL of ethanol, and the washing was repeated twice; the washed product was dried in a vacuum drying oven at 60°C for 8 h to obtain a white melamine-cyanuric chloride supramolecular aggregate.
[0038] (2) Preparation of 3D g-C3N4:
[0039] The melamine-cyanuric chloride supramolecular aggregate was ground into 100 mesh powder, then placed in a porcelain boat, sealed with tin foil, and then heated to 550°C at a rate of 2.3°C / min in an argon atmosphere in a tube furnace and calcined at this temperature for 4 h to obtain a khaki solid, which was recorded as 3D g-C3N4.
[0040] (3) Preparation of 3D g-C3N4-PDI composite photocatalyst:
[0041] The 3D g-C3N4 obtained in step (2) was ground to obtain 100 mesh 3D g-C3N4 powder for standby use. 0.2 g of perylene tetracarboxylic dianhydride was dispersed in 20 mL of ethanol and dispersed evenly by ultrasonic stirring. Then 1 g of 3D g-C3N4 powder was dispersed in the above solution and dispersed evenly by stirring. The solvent was removed by rotary evaporation and dried in a vacuum oven at 60°C for 8 h. The obtained solid was placed in a porcelain boat, sealed with tin foil, and heated to 325°C at a heating rate of 5°C / min in an argon atmosphere in a tube furnace, and calcined for 4 h to obtain a PDI-modified 3D g-C3N4 composite photocatalyst, which was recorded as 3D g-C3N4-PDI.
[0042] (4) 0.02 g of 3D g-C3N4-PDI was evenly dispersed on a 2×2 cm glass sheet and then placed in a quartz reactor. The gas in the reactor was evacuated using a vacuum pump, and then high-purity CO2 saturated with water vapor was filled into the reactor at a pressure of 1 atm. The reactor was then sealed and the entire reaction system was placed in a CO2 atmosphere. A 300 W xenon lamp was used as the light source, and samples were taken every 1 hour. The reaction products were analyzed using a gas chromatograph equipped with a methanogen. After 4 hours of reaction, the CO yield was calculated to be 10.34 μmol / g / h.
[0043] Embodiment 2:
[0044] (1) Preparation of melamine-cyanuric chloride supramolecular aggregates:
[0045] Dissolve 1.0 g of melamine and 1.0 g of cyanuric chloride in 20 mL of DMSO respectively, stir until fully dissolved, and obtain two solutions; then mix the two solutions under stirring conditions to generate a white solid, continue stirring for 2 h, wash the precipitate after centrifugation with 10 mL×2 ethanol, use 10 mL of ethanol for centrifugal washing, and repeat the washing twice; the washed product is dried in a vacuum drying oven at 60°C for 8 h to obtain a white melamine-cyanuric chloride supramolecular aggregate.
[0046] (2) Preparation of 3D g-C3N4:
[0047] The melamine-cyanuric chloride supramolecular aggregate was ground into 100 mesh powder, then placed in a porcelain boat, sealed with tin foil, and then heated to 550°C at a rate of 2.3°C / min in an argon atmosphere in a tube furnace and calcined at this temperature for 4 h to obtain a khaki solid, which was recorded as 3D g-C3N4.
[0048] (3) Preparation of 3D g-C3N4-PDI-Cl composite photocatalyst:
[0049] The 3D g-C3N4 obtained in step (2) was ground to obtain 100 mesh 3D g-C3N4 powder for standby use; 0.2g 1,6,7,12-tetrachloro-3,4,9,10-perylenetetracarboxylic acid dianhydride was dispersed in 20mL ethanol, and ultrasonically dispersed uniformly under stirring, and then 1g 3Dg-C3N4 was dispersed in the above solution and dispersed uniformly under stirring, and the solvent was removed by rotary evaporation, and dried in a vacuum drying oven at 60°C for 8h. The obtained solid powder was placed in a porcelain boat, sealed with tin foil, and heated to 325°C at a heating rate of 5°C / min in an argon atmosphere in a tube furnace, and calcined at this temperature for 4h to obtain a PDI-modified 3D g-C3N4 composite photocatalyst, which was recorded as 3D g-C3N4-PDI-Cl.
[0050] (4) 0.02 g of 3D g-C3N4-PDI-Cl was evenly dispersed on a 2×2 cm glass sheet and then placed in a quartz reactor. The gas in the reactor was evacuated using a vacuum pump, and then high-purity CO2 saturated with water vapor was filled into the reactor at a pressure of 1 atm. The reactor was then sealed and the entire reaction system was placed in a CO2 atmosphere. A 300 W xenon lamp was used as the light source, and samples were taken every 1 hour. The reaction products were analyzed using a gas chromatograph equipped with a methanogen. After 4 hours of reaction, the CO yield was calculated to be 13.07 μmol / g / h.
[0051] Embodiment 3:
[0052] (1) Preparation of melamine-cyanuric chloride supramolecular aggregates:
[0053] 1.0 g of melamine and 1.0 g of cyanuric chloride were dissolved in 20 mL of DMSO respectively, and stirred until fully dissolved to obtain two solutions; then the two solutions were mixed under stirring conditions to generate a white solid, and stirring was continued for 2 h. The precipitate after centrifugation was washed with 10 mL of ethanol, and the washing was repeated twice; the washed product was dried in a vacuum drying oven at 60°C for 8 h to obtain a white melamine-cyanuric chloride supramolecular aggregate.
[0054] (2) Preparation of 3D g-C3N4:
[0055] The melamine-cyanuric chloride supramolecular aggregates were ground into 150 mesh powder, then placed in a porcelain boat, sealed with tin foil, and then heated to 550 °C at a rate of 2.3 °C / min in an argon atmosphere in a tube furnace and calcined at this temperature for 4 h to obtain a khaki 3D g-C3N4 solid.
[0056] (3) Preparation of 3D g-C3N4-PDI-Br composite photocatalyst:
[0057] The khaki 3D g-C3N4 solid obtained in step (2) was ground into 150 mesh 3D g-C3N4 powder for later use; 0.2 g of 1,6,7,12-tetrabromo-3,4,9,10-perylenetetracarboxylic acid dianhydride was dispersed in 20 mL of ethanol and uniformly dispersed by ultrasonication under stirring; then 1 g of 3D g-C3N4 was dispersed in the above solution and uniformly dispersed under stirring, the solvent was removed by rotary evaporation, and the powder was dried in a vacuum drying oven at 60°C for 8 h; the solid powder was placed in a porcelain boat, sealed with tin foil, and heated to 325°C at a heating rate of 5°C / min in an argon atmosphere in a tube furnace, and calcined at this temperature for 4 h to obtain a PDI-modified 3D g-C3N4 composite photocatalyst, which was recorded as 3D g-C3N4-PDI-Br.
[0058] (4) 0.02 g of 3D g-C3N4-PDI-Br was evenly dispersed on a 2×2 cm glass sheet and then placed in a quartz reactor. The gas in the reactor was evacuated using a vacuum pump, and then high-purity CO2 saturated with water vapor was filled into the reactor at a pressure of 1 atm. The reactor was then sealed and the entire reaction system was placed in a CO2 atmosphere. A 300 W xenon lamp was used as the light source, and samples were taken every 1 hour. The reaction products were analyzed using a gas chromatograph equipped with a methanogen. After 4 hours of reaction, the CO yield was calculated to be 12.55 μmol / g / h.
[0059] Figure 1 This is a schematic diagram of the structure of the 3D g-C3N4-PDI composite photocatalytic material prepared in Example 1 of the present invention. As can be seen from the figure, 3D g-C3N4 is a polymer with regular repeating units. When reacting with an organic molecule PTCDA derivative, the amino group at the edge of 3D g-C3N4 and the anhydride group of the PTCDA derivative undergo a ring-opening reaction, and the PTCDA derivative is introduced into the structure of 3D g-C3N4 in the form of an amide bond, forming a 3D g-C3N4-PDI composite photocatalyst with an intramolecular DA structure.
[0060] Figure 2 This is the XRD spectrum of the photocatalytic material prepared in Example 1. It can be seen that before and after the organic molecule PTCDA derivative is introduced into 3D g-C3N4, the positions of the (100) and (002) diffraction peaks of the catalytic material are almost unchanged, and no new diffraction peaks are found, indicating that the introduction of the PTCDA derivative does not change the main structure of 3D g-C3N4. However, with the introduction of the PTCDA derivative, the (100) and (002) diffraction peaks of 3D g-C3N4 become wider and the intensity becomes smaller, indicating that the crystallinity of 3D g-C3N4 deteriorates after the introduction of the PTCDA derivative, and the stacking mode of the 3D g-C3N4 molecules is partially changed.
[0061] Figure 3 This is the infrared spectrum of the catalyst prepared in Example 1, in which the PTCDA derivative has an infrared spectrum of about 1760 cm -1 The broad absorption band around 1672 cm is the vibration absorption of C=O in the anhydride. After reacting with 3D g-C3N4, the absorption band basically disappears. -1 The characteristic absorption band of amide appeared nearby, indicating that a chemical reaction occurred between the PTCDA derivative and 3D g-C3N4, proving that 3Dg-C3N4-PDI was successfully synthesized.
[0062] Figure 4This is the UV-Vis DRS spectrum of the sample prepared in Example 1. It can be seen from the figure that after the PTCDA derivative is introduced into the structure of 3D g-C3N4, 3D g-C3N4-PDI shows a strong absorption band in the range of 400 to 600 nm. This absorption band is due to the reaction of the PTCDA derivative and 3D g-C3N4 to generate new substances, which changes the band gap structure of the two substances and significantly increases the light response range of the composite material, thereby improving the light energy utilization efficiency, which is beneficial to the improvement of the photocatalytic activity of the 3D g-C3N4-PDI composite material.
[0063] The photocatalytic activity evaluation of the photocatalyst prepared in the present invention was carried out in a custom-made 300mL photochemical quartz reactor, using a 300W xenon lamp to simulate visible light irradiation. The specific reaction process was as follows: 0.02g of the catalyst was evenly dispersed on a 2×2cm glass sheet, and then placed in a quartz reactor. The gas in the reactor was removed by a vacuum pump, and then high-purity CO2 saturated with water vapor was filled into the reactor at a pressure of 1atm, and then the reactor was sealed, and the entire reaction system was in a CO2 atmosphere. Samples were taken every 1 hour, and the reaction products were analyzed using a gas chromatograph equipped with a methanogenization device.
[0064] The CO generation rate is calculated as follows:
[0065] Y CO =CO generation / (catalyst dosage × reaction time);
[0066] The experimental results show that the photocatalytic activity of 3D g-C3N4 can be significantly improved by introducing PTCDA derivatives into 3D g-C3N4 to construct 3D g-C3N4-PDI DA composites. For example, when 3D g-C3N4 is used as a catalyst alone, the CO generation rate is 1.03 μmol g -1 h -1 .
[0067] The photocatalytic CO generation rate of 3D g-C3N4-PDI prepared in Example 1 was 10.34 μmol g -1 h -1 Its photocatalytic reduction of CO2 to produce CO activity is increased by 10.04 times compared with 3D g-C3N4.
[0068] The photocatalytic CO generation rate of 3D g-C3N4-PDI-Cl prepared in Example 2 was 13.07 μmol g -1 h -1 Its photocatalytic reduction of CO2 to produce CO activity is 12.69 times higher than that of 3D g-C3N4.
[0069] The photocatalytic CO generation rate of 3D g-C3N4-PDI-Br prepared in Example 3 was 12.55 μmol g -1 h -1 Its photocatalytic reduction of CO2 to produce CO activity is increased by 12.18 times compared with 3D g-C3N4.
[0070] In summary, the activity of the photocatalyst prepared by the present invention in photocatalytic reduction of CO2 to produce CO is more than 10 times higher than that of 3D g-C3N4, indicating that the introduction of PDI into 3D g-C3N4 to construct a DA structure can significantly improve the activity of 3D g-C3N4 in photocatalytic reduction of CO2.
[0071] It is noted that the above-mentioned specific implementation methods can enable those skilled in the art to understand the present invention more comprehensively, but they do not limit the present invention in any way. Therefore, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents; and all technical solutions and improvements that do not deviate from the spirit and technical essence of the present invention should be included in the protection scope of the patent of the present invention.
Claims
1. A PDI-functionalized 3D g-C3N4 photocatalyst for improving the activity of photocatalytic reduction of CO2 to produce hydrocarbon fuels, characterized in that: The preparation of the PDI functionalized 3D g-C3N4 photocatalyst comprises the following steps: (1) Melamine and cyanuric chloride are dissolved in dimethyl sulfoxide respectively, and stirred to dissolve to obtain a melamine solution and a cyanuric chloride solution; then the melamine solution and the cyanuric chloride solution are mixed under stirring conditions, and a white precipitate is formed by a mixing reaction, the precipitate is collected by centrifugation, and washed with ethanol for several times, and then the precipitate is vacuum dried to obtain a melamine-cyanuric chloride supramolecular aggregate; wherein the amount of melamine and dimethyl sulfoxide is 1 g:20 mL; the amount of cyanuric chloride and dimethyl sulfoxide is 1 g:20 mL; and the volume ratio of the melamine solution and the cyanuric chloride solution when mixed is 1:1; (2) grinding the melamine-cyanuric chloride supramolecular aggregate obtained in step (1) into powder, sealing and packaging, and calcining the powder in a tube furnace under an inert gas atmosphere at a heating rate of 2.3°C / min to a target temperature, to obtain a yellowish brown solid product, which is recorded as 3D g-C3N4; (3) Grinding the 3D g-C3N4 obtained in step (2) to obtain 3D g-C3N4 powder with a mesh size of 100 mesh; dispersing perylenetetracarboxylic acid dianhydride in ethanol, stirring and ultrasonically dispersing to obtain a dispersion; the amount of perylenetetracarboxylic acid dianhydride and ethanol is 0.1-1g:10 mL, and the mass ratio of the 3D g-C3N4 powder to the perylenetetracarboxylic acid dianhydride in the dispersion is 5:1; Subsequently, 3D g-C3N4 powder is added to the dispersion and stirred evenly. The solvent is removed by rotary evaporation, and the obtained product is then vacuum dried to obtain a dry product. The dry product is calcined at a certain temperature to obtain a PDI-functionalized 3D g-C3N4 photocatalyst. The calcination operation is as follows: the dry product is placed in a porcelain boat and sealed with tin foil; the temperature is increased to 325°C at a heating rate of 5°C / min in an argon atmosphere for 4 hours.
2. The use according to claim 1, characterized in that: The vacuum drying temperature in step (1) is 60° C. and the drying time is 6-12 h.
3. The use according to claim 1, characterized in that: In step (2), the sealed package is specifically placed in a porcelain boat and sealed with tin foil; the inert gas is argon.
4. The use according to claim 1, characterized in that: In step (2), the target temperature is 550°C and the calcination time is 4 h.