A polishing liquid for KDP crystal and a high-efficiency grinding and polishing process

CN115181498BInactive Publication Date: 2024-10-25DALIAN UNIV OF TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202210746930.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-29
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN115181498B_ABST
    Figure CN115181498B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of grinding and polishing processing, and provides a polishing liquid for KDP crystal and an efficient grinding and polishing process. The polishing liquid is a non-aqueous chemical mechanical polishing liquid composed of abrasive particles, reactants, additives, organic solvents, and deionized water. The efficient grinding and polishing process includes rough grinding, fine grinding, polishing, and cleaning. In the grinding stage, the present invention quickly removes the macroscopic processing texture and brittle damage caused by wire cutting through the micro-cutting action of the effective abrasive particles on the surface of the consolidated abrasive pad. The present invention divides the grinding into two stages, taking into account both the grinding efficiency and the surface quality; in the polishing stage, the chemical action of the reactants in the polishing liquid, the dissolving action of the deionized water, and the mechanical action of the abrasive particles are used to remove the material, and the surface roughness of the crystal can be quickly reduced to the nanometer level under low pressure; the consolidated abrasive grinding and polishing pad used is not easy to cause surface damage and has high processing efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of grinding and polishing processing, and relates to a high-efficiency processing method for soft, brittle and easily deliquescent crystals, and in particular to a fast processing method for the smooth surface of a KDP crystal. Background Art

[0002] Potassium dihydrogen phosphate (KDP) crystal, with the chemical formula KH2PO4, has excellent properties such as high laser damage threshold, low optical absorption coefficient, good optical uniformity, and large nonlinear coefficient. It is a key optical material in major national strategic equipment such as high-power laser weapons and inertial confinement nuclear fusion devices. However, due to the difficult processing characteristics of KDP crystal, such as soft and brittle, easy to deliquesce, poor thermal conductivity, and strong anisotropy, it is difficult to achieve efficient and high-quality processing.

[0003] At present, KDP crystal processing usually uses wire cutting technology to first divide the single crystal ingot into KDP crystal blanks, then single-point diamond flycutting is used to remove the macro-processing texture and brittle damage on the surface of the blank, and finally the KDP crystal surface is made to reach the target level through ultra-precision processing technology. However, there is a large bottleneck in the material removal rate of single-point diamond flycutting, and single-point diamond flycutting is easy to introduce small-scale ripples. In order to remove the small-scale ripples produced by single-point diamond flycutting, polishing technology is often used. There are many patents for KDP polishing, including magnetorheological polishing, ion beam polishing, polishing based on water dissolution, etc. Patent CN201410288335.8 discloses a deliquescent magnetorheological polishing method, but the magnetorheological polishing efficiency is low and is not suitable for polishing larger crystals. Patent 201610271922.5 discloses a surface polishing method for potassium dihydrogen phosphate crystals, including spin coating a flattening layer, heat treatment, ion beam etching and other steps, but this method requires sufficient vacuum, the machine tool structure is complex, and the processing efficiency is low. Patent 200810064046.4 discloses a deliquescent polishing method for potassium dihydrogen phosphate crystals, and Patent 200910010268.2 discloses a non-aqueous abrasive-free polishing liquid for soft, brittle, and easily deliquescent crystals. The above patents use water to dissolve KDP and remove materials, but this method requires strict control of the water content, resulting in a low material removal rate. In addition, Patent 202010992961.0 discloses a method for anhydrous polishing of KDP crystals. The polishing liquid consists of methyl oleate, silicon carbide / aluminum oxide abrasive mixed abrasives, and anhydrous sodium carbonate. However, due to the soft and brittle characteristics of KDP crystals, the silicon carbide and aluminum oxide abrasives used have high hardness and are prone to abrasive embedding and other problems. Patent 202110246315.4 discloses a consolidated abrasive polishing pad and a method for dry polishing of deliquescent KDP crystals. The consolidated abrasive polishing pad used for dry polishing of KDP crystals contains abrasives, reactants, catalysts, curing agents, and binders. However, the waste chips generated during polishing by this method cannot be discharged in time, which can easily damage the crystal surface and affect the processing quality. For the large-scale and large-volume application requirements of KDP crystals, the efficiency of existing KDP crystal ultra-precision processing technology is generally low, and it takes a lot of time to remove the macro-processing texture and damage on the surface of the crystal blank. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention develops a polishing liquid and an efficient grinding and polishing process for KDP crystals, which can realize efficient processing of KDP crystals after cutting and quickly reduce the surface roughness of KDP crystals to nanometer level.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A polishing liquid for KDP crystals is a non-aqueous chemical mechanical polishing liquid composed of abrasive particles, reactants, additives, organic solvents and deionized water.

[0007] The polishing liquid reactant is one or more of the neutral alkaline substances such as KOH, K2CO3, KHCO3, etc., and the mass ratio of the neutral alkaline substances in the polishing liquid is 0.02%-0.10%. Its function is to chemically react with the KDP crystal as an acid salt to form a product layer of K2HPO4 and K3PO4 on the surface of the crystal.

[0008] The polishing liquid abrasive particles are selected from one or more soft abrasive particles such as SiO2, CeO2, TiO2, CuO, etc. with a particle size of 20-100nm. The mass ratio in the polishing liquid is 0.25%-2.00%. Compared with abrasive particles such as SiO2, Al2O3, MgO, etc., the above abrasive particles are softer, with a Mohs hardness of 3-6, and are more suitable for polishing soft and brittle materials.

[0009] The polishing liquid additive is graphene oxide, and the mass ratio in the polishing liquid is 0.02%-0.20%. The graphene oxide plays an interfacial lubricating role, helps to reduce the friction between the abrasive grains and the substrate interface, and can improve the surface quality after polishing.

[0010] The function of the deionized water in the polishing liquid is to dissolve the salts soluble in water but insoluble in alcohol generated after the chemical reaction in time, so as to prevent the products from remaining on the workpiece surface and gradually accumulating to affect the polishing quality. The mass ratio of deionized water in the polishing liquid is 5%-30%.

[0011] The organic solvent in the polishing liquid is selected from one or more of anhydrous ethanol, glycerol, polyethylene glycol, low-viscosity silicone oil, methyl laurate, and methyl oleate. KDP crystals are easily soluble in water and easily deliquesce in the air. If a traditional water-based polishing liquid is used, the dissolution rate is too high to be controlled. A non-toxic organic solvent is selected to replace the role of water in a conventional polishing liquid as a dispersed phase to avoid the KDP crystal dissolving too fast to form a deliquescent layer.

[0012] The polishing liquid is stirred by a magnetic stirrer and fully mixed by ultrasonic vibration.

[0013] An efficient grinding and polishing process for KDP crystals comprises the following steps:

[0014] 1) Rough grinding

[0015] An organic solvent is selected as the grinding liquid, and a diamond-consolidated abrasive pad is selected as the grinding pad. The KDP crystal sample after wire cutting is ground for 5-30 minutes, the grinding pressure is 1-5 kPa, and the grinding disk speed is 50-100 rpm.

[0016] The purpose of the rough grinding process is to quickly remove the damage and processing texture generated by the cutting stage. The fixed abrasive pad is a 15-20 μm fixed diamond abrasive pad.

[0017] The organic solvent includes one or a combination of anhydrous ethanol, low-viscosity silicone oil, polyethylene glycol, ethylene glycol, methyl laurate, and methyl oleate.

[0018] 2) Research

[0019] An organic solvent is selected as the grinding liquid, and a diamond-consolidated abrasive pad is used as the grinding pad. The KDP crystal sample after rough grinding in step 1 is ground for 5-20 minutes, the grinding pressure is 1-4 kPa, and the grinding disk speed is 40-80 rpm.

[0020] The purpose of the fine grinding process is to remove the pits and scratches generated in the rough grinding stage and quickly reduce the roughness to facilitate the next stage of polishing. The fixed abrasive pad is a 3-5 μm fixed diamond abrasive pad.

[0021] The organic solvent includes one or a combination of anhydrous ethanol, low-viscosity silicone oil, polyethylene glycol, ethylene glycol, methyl laurate, and methyl oleate.

[0022] 3) Polishing

[0023] An IC1000 polishing pad is selected and the non-aqueous chemical mechanical polishing liquid configured in the present invention is used to polish the KDP crystal after the fine grinding in step 2. The polishing time is 5-30 minutes, the polishing pressure is 1-3 kPa, and the polishing disk speed is 40-80 rpm.

[0024] The polishing process removes material from the crystal surface by balancing the chemical action of reactants, the dissolving action of deionized water, and the mechanical action of abrasive particles. It can remove scratches generated by the grinding process and quickly reduce the surface to nanometer-level roughness, thereby achieving ultra-precision processing of the crystal.

[0025] 4) Cleaning

[0026] Select IC1000 polishing pad, mix anhydrous ethanol and 2%-5% deionized water to make polishing cleaning solution. Polish the KDP crystal polished in step 3 on the polishing machine with the prepared cleaning solution for 2-10 minutes, with a pressure of 1-4kPa and a grinding disc speed of 40-80rpm.

[0027] Finally, immerse the KDP crystal in anhydrous ethanol and clean it with an ultrasonic cleaner for 2-10 minutes. After cleaning, quickly wipe the surface with a dust-free cloth.

[0028] The cleaning process is to ensure that there is no chemical reaction product or polishing liquid residue on the crystal surface after polishing.

[0029] The beneficial effects of the present invention are:

[0030] (1) The present invention uses the micro-cutting action of the effective abrasive particles on the surface of the fixed abrasive pad to quickly remove the macro-processing texture and brittle damage caused by wire cutting during the grinding stage. The present invention divides the grinding into two stages, taking into account both grinding efficiency and surface quality. Compared with the single-point diamond flycutting technology commonly used in existing KDP crystals, it is more efficient and has more prominent advantages for the demand for large-scale and large-size KDP crystals.

[0031] (2) In the polishing stage, the present invention utilizes the chemical action of the reactants in the polishing liquid, the dissolving action of deionized water, and the mechanical action of the abrasive particles to achieve material removal. Compared with existing abrasive-free hydrolytic polishing, magnetorheological polishing, and ion beam polishing, the chemical mechanical polishing of the present invention is highly efficient and can quickly reduce the surface roughness of the crystal to the nanometer level under low pressure.

[0032] (3) The fixed abrasive polishing pad used in the present invention mainly removes materials by two-body wear, and most of them are uniform plastic removal. The abrasive grains and KDP crystals are mainly in sliding contact, which is not easy to cause surface damage and has high processing efficiency. The abrasive grains are fixed on the polishing pad, with high utilization rate, making the preparation of the polishing liquid simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The invention discloses a high-efficiency grinding and polishing process and a polishing liquid preparation process.

[0034] Figure 2 These are microscopic photographs obtained in the embodiments of the present invention, wherein (a) is after grinding, and (b) is after polishing.

[0035] Figure 3 The grinding removal rate measured by the grooving method in the embodiment of the present invention. Figure (a) is a schematic diagram of the principle of measuring the material removal rate by the grooving method, Figure (b) is the rough grinding and fine grinding efficiency measured by the embodiment and the efficiency of comparative example 1, and Figure (c) is the polishing efficiency measured by the embodiment and the efficiency of comparative example 2. DETAILED DESCRIPTION

[0036] The present invention is further described below in conjunction with specific embodiments.

[0037] Comparative Example 1:

[0038] Chen et al. [1] The fly cutting technology is used to process KDP. The specific processing parameters are: cutting depth of 40nm, feed rate of 150μm / s, and spindle speed of 1000rpm. If the KDP crystal of the same size (50×50mm) is processed, the efficiency is calculated to be about 0.17μm / min. Figure 3 (b) as shown.

[0039] [1]Chen D, Li S, Fan J.Effect of KDP-Crystal Material Properties onSurface Morphology in Ultra-Precision Fly Cutting[J].Micromachines,2020,11(9):802.

[0040] Comparative Example 2:

[0041] Wang et al. [2] Using oil-in-water non-abrasive polishing, the material removal efficiency is 0.70μm / min at a pressure of 40kPa and a rotation speed of 150rpm. Figure 3 (c) as shown.

[0042] [2]Gao H, Wang B, Guo D, et al. Experimental Study on Abrasive-FreePolishing for KDP Crystal[J]. Journal of the Electrochemical Society, 2010, 157(9): H853.

[0043] Embodiment 1:

[0044] The present invention will be further described below in conjunction with specific implementation examples.

[0045] A polishing liquid for KDP crystal and an efficient grinding and polishing process, comprising the following steps:

[0046] The first step is rough research

[0047] The grinding liquid is anhydrous ethanol, and the grinding pad is a 15-20μm consolidated diamond grinding pad. The cut 50×50mm KDP crystal is roughly ground on a ZYP230 swing gravity grinding and polishing machine. The grinding pressure is 2kPa, the speed is set to 70rpm, and the grinding time is 20min. The surface roughness of the KDP crystal before grinding is measured by the Zygo surface profiler as Sa2415.7nm, and the surface roughness of the KDP crystal after grinding is Sa504.9nm. The material removal rate is measured by the grooving method. The schematic diagram is shown in the material Figure 3 As shown in (a), the depth of the same position is measured by Mitaka non-contact topography before and after grinding. The depth difference before and after grinding divided by the processing time is the material removal rate. The rough grinding material removal efficiency is measured to be 3.00μm / min. Figure 3 (b) as shown.

[0048] Step 2: intensive research

[0049] The grinding liquid was anhydrous ethanol, and the grinding pad was replaced with a 3-5μm consolidated diamond grinding pad. The 50×50mm KDP crystal after rough grinding was finely ground. The grinding pressure was 2kPa, the speed was set to 60rpm, and the grinding time was 15min. The surface roughness of the KDP crystal after grinding was measured using a Zygo surface profiler, and the measured Sa was 17.9nm. The material removal efficiency was measured by the groove method and was 0.80μm / min. Figure 3 (b) As shown. The surface after lapping was observed using an OLYMPUS metallographic microscope. Figure 2 (a) shown.

[0050] Step 3: Polishing

[0051] Anhydrous ethanol was used as the dispersed phase, and 0.5% CeO2, 0.06% KOH, 0.02% graphene oxide, and 17% deionized water were added to prepare the polishing liquid. The IC1000 polishing pad was selected, the polishing pressure was 2kPa, the speed was set to 60rpm, and the grinding time was 10min. The KDP crystal after fine grinding was polished. The proportion of each substance in the polishing liquid refers to the mass percentage of each substance in the total mass of the polishing liquid. The material removal efficiency in the polishing stage was measured by the grooving method to be 1.00μm / min, such as Figure 3 As shown in (c), compared with Comparative Example 2, under low pressure, the material removal efficiency is higher than that of the existing polishing technology.

[0052] Step 4: Cleaning

[0053] Mix anhydrous ethanol and 2% deionized water to make a polishing cleaning solution. Use an IC1000 pad with a pressure of 2kPa and a speed of 60rpm to continue polishing for 3 minutes. Immerse the polished KDP crystal in anhydrous ethanol for ultrasonic cleaning for 3 minutes. After cleaning, quickly wipe the crystal surface with a dust-free cloth. The surface roughness of the KDP crystal after polishing and cleaning is measured to be Sa 1.8nm. The cleaned surface is observed using an Olympus OLYMPUS metallographic microscope, such as Figure 2 (b) as shown.

[0054] Analysis of the results of the present invention and comparative examples:

[0055] The existing KDP crystal ultra-precision processing technology generally uses fly cutting technology to remove the damage after cutting after cutting, and then uses ultra-precision polishing technology to further improve the surface quality. In the grinding stage, the rough grinding material removal efficiency of the present invention is 3.00μm / min, and the fine grinding material removal efficiency is 0.80μm / min, which is better than the existing fly cutting technology. In the polishing stage, the material removal efficiency is 1.00μm / min under a pressure of 2kPa, which is better than the existing oil-in-water polishing technology.

[0056] The above-described embodiments merely express the implementation methods of the present invention, but they cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A polishing liquid for KDP crystal, characterized in that: The polishing liquid is a non-aqueous chemical mechanical polishing liquid composed of abrasive particles, reactants, additives, organic solvents and deionized water; The polishing liquid reactant is one or a combination of KOH, K2CO3, and KHCO3, and its mass ratio in the polishing liquid is 0.02%-0.10%; its function is to chemically react with KDP crystals as acid salts to form product layers K2HPO4 and K3PO4 on the surface of the crystals; The polishing liquid abrasive particles are one or a combination of SiO2, CeO2, TiO2, CuO; the mass ratio in the polishing liquid is 0.25%-2.00%; The polishing liquid additive is graphene oxide, and the mass ratio in the polishing liquid is 0.02%-0.20%; The role of deionized water in the polishing liquid is to dissolve the salts that are soluble in water but insoluble in alcohol generated after the chemical reaction in time, so as to prevent the products from remaining on the surface of the workpiece and gradually accumulating to affect the polishing quality. The mass ratio of deionized water in the polishing liquid is 5%-30%; The non-toxic organic solvent in the polishing liquid is used as a dispersed phase to prevent the KDP crystal from dissolving too quickly to form a deliquescent layer.

2. The polishing liquid for KDP crystal according to claim 1, characterized in that: The abrasive grain size of the polishing liquid is 20-100nm.

3. The polishing liquid for KDP crystal according to claim 1, characterized in that: The organic solvent includes one or a combination of anhydrous ethanol, glycerol, polyethylene glycol, low-viscosity silicone oil, methyl laurate, and methyl oleate.

4. An efficient grinding and polishing process for KDP crystals, characterized in that: The non-aqueous chemical mechanical polishing solution according to any one of claims 1 to 3 is implemented, specifically comprising the following steps: 1) Rough grinding to quickly remove damage and processing textures caused by the cutting stage An organic solvent is used as the grinding liquid, and a diamond-consolidated abrasive pad is used as the grinding pad. The KDP crystal sample after wire cutting is ground for 5-30 minutes, the grinding pressure is 1-5 kPa, and the grinding disc speed is 50-100 rpm; 2) Fine grinding to remove pits and scratches produced during the rough grinding stage An organic solvent is selected as the grinding liquid, and a diamond-bonded abrasive pad is used as the grinding pad. The KDP crystal sample after the rough grinding in step 1 is ground for 5-20 minutes, the grinding pressure is 1-4 kPa, and the grinding disc speed is 40-80 rpm; 3) Polishing Select IC1000 polishing pad and non-aqueous chemical mechanical polishing liquid to polish the KDP crystal after fine grinding in step 2, the polishing time is 8-30min, the polishing pressure is 1-3kPa, and the polishing disk speed is 40-80rpm; the polishing process removes materials from the crystal surface by balancing the chemical action of the reactants, the dissolution action of deionized water, and the mechanical action of the abrasive particles, removes the scratches generated by the grinding process, and quickly reduces the surface to nanometer-level roughness, thereby realizing ultra-precision processing of the crystal; 4) Cleaning After the KDP crystal polished in step 3 is further polished on a polishing machine using a polishing cleaning solution, the KDP crystal is immersed in anhydrous ethanol for ultrasonic cleaning.

5. A high-efficiency grinding and polishing process for KDP crystal according to claim 4, characterized in that: The fixed abrasive pad in step 1) is a fixed diamond abrasive pad of 15-20 μm.

6. A high-efficiency grinding and polishing process for KDP crystal according to claim 4, characterized in that: The organic solvent described in step 1) includes one or a combination of anhydrous ethanol, low-viscosity silicone oil, polyethylene glycol, ethylene glycol, methyl laurate, and methyl oleate.

7. The high-efficiency grinding and polishing process for KDP crystal according to claim 4, characterized in that: The fixed abrasive pad in step 2) is a fixed diamond abrasive pad of 3-5 μm.

8. The high-efficiency grinding and polishing process for KDP crystal according to claim 4, characterized in that: The organic solvent described in step 2) includes one or a combination of anhydrous ethanol, low-viscosity silicone oil, polyethylene glycol, ethylene glycol, methyl laurate, and methyl oleate.

9. The high-efficiency grinding and polishing process for KDP crystal according to claim 4, characterized in that: The polishing cleaning solution in step 4) is a mixed solution of anhydrous ethanol and 2%-5% deionized water by volume.

10. The high-efficiency grinding and polishing process for KDP crystal according to claim 4, characterized in that: In the polishing process described in step 4), an IC1000 polishing pad is selected, the polishing time is 2-10 min, the polishing pressure is 1-4 kPa, and the grinding disc speed is 40-80 rpm.

Citation Information

Cited By

  • Scintillation crystal polishing solution and preparation method thereof

    CN120310439A