A Co-PiNiCoLDH@Nickel Foam electrode and preparation method thereof
By constructing the Co-PiNiCoLDH@Nickel Foam electrode on nickel foam, the problems of insufficient OER performance and high cost of precious metal catalysts in the existing technology are solved, and an efficient and stable water splitting electrode is achieved, which is suitable for large-scale water electrolysis and electrochemistry. industry.
Patent Information
- Application Number
- CN202210787476.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-07-06
AI Technical Summary
The high overpotential and sluggish reaction kinetics of existing electrocatalysts in oxygen evolution reaction (OER) limit water splitting efficiency, and the high cost and poor long-term stability of noble metal oxide catalysts limit industrial applications, especially in foams. Cobalt phosphate materials on nickel substrates lack sufficient stability.
Co-PiNiCoLDH@Nickel Foam electrode is used, nickel foam is activated through pretreatment, NiCoLDH intermediate layer is prepared by electrodeposition, and Co-Hopeite functional layer is formed by hydrothermal method to construct a three-layer structure electrode, using Co2( PO4)3 serves as a functional layer to improve the stability and electrochemical activity of the electrode.
It achieves excellent OER and HER electrode performance in large-scale water electrolysis processes, improves the stability and economic benefits of the electrode, avoids the cost problem of precious metal catalysts, and significantly improves the oxygen evolution and hydrogen evolution activities of the electrocatalyst.
Smart Images

Figure CN115181984B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrocatalytic electrodes, and in particular to a Co-PiNiCoLDH@Nickel Foam electrode and a preparation method thereof. Technical Background
[0002] In recent years, the continued consumption of fossil fuels and uncontrolled greenhouse gas emissions have driven intensive research on innovative technologies for generating clean energy through sustainable electrocatalytic water splitting. Using solar energy to split water to produce hydrogen is one of the most attractive routes to produce renewable fuels. In the process of water electrolysis, hydrogen and oxygen are usually generated through two half reactions, namely the hydrogen evolution reaction (HER) and the oxygen evolution reaction (OER). Compared with HER, the high overpotential and sluggish reaction kinetics of OER severely limit the efficiency of overall water splitting. So far, the most advanced OER electrocatalysts are usually noble metal oxides (such as IrO2 and RuO2). However, the high cost and poor long-term stability of these rare materials inevitably limit their industrial applications. Due to the large surface area of the catalyst in large-scale applications, abundant catalyst materials on the earth are required to avoid scarcity and cost issues. Nickel foam has a great cost advantage in this regard. Among the substrates prepared using nickel foam as catalysts, a lot of work is currently focused on the development of efficient non-precious metal-based electrocatalysts, including transition metal oxides, transition metal hydroxides, transition metal chalcogenides / carbides, transition metal borides / nitrides and carbon-based materials. Among the many promising materials, phosphate-based materials play an indispensable role. Cobalt phosphate is a well-known earth-abundant oxygen evolution reaction (OER) catalyst. It is self-assembled by cobalt and phosphate ions in a neutral pH environment. Its structure is a combination of cobalt hydroxide and phosphate ions, acting as a proton acceptor during water oxidation. Cobalt-based catalysts can work in both acidic and alkaline solutions. It has been found in many studies that cobalt phosphate materials have strong bifunctionality. However, it is difficult for related electrocatalysts to solve the stability of cobalt phosphate materials on nickel foam substrates. Because the electrocatalyst materials are not tightly bound, the stability performance in practical applications is not satisfactory. Summary of the invention
[0003] In view of this, the present invention proposes a Co-PiNiCoLDH@Nickel Foam electrode and a preparation method thereof to solve the above problems.
[0004] The technical solution of the present invention is achieved in this way:
[0005] A method for preparing a Co-PiNiCoLDH@Nickel Foam electrode comprises the following steps:
[0006] (1) Pretreatment: soak the nickel foam in an organic solvent, wash it with water after ultrasonication, soak it in an acid solution, wash it with water, and then dry it to obtain an activated nickel foam; pretreat the nickel foam to remove the grease layer and the oxide layer on the surface of the nickel foam.
[0007] (2) Preparation of NiCoLDH electrolyte: nickel salt and cobalt salt were dissolved in water, the pH value was adjusted to 6.5-7.5, and the NiCoLDH electrolyte was obtained after ultrasonic oscillation;
[0008] (3) Electrodeposition to prepare the intermediate layer NiCoLDH: The nickel foam activated in step (1) is cut into pieces and used as the cathode and anode in the three-electrode system respectively. The NiCoLDH electrolyte in step (2) is used as the electrolyte of the three-electrode system to perform an electrodeposition treatment, thereby obtaining NiCoLDH@NF containing a NiCoLDH intermediate layer on the cathode nickel foam;
[0009] (4) Preparation of Co-Hopeite functional layer by hydrothermal method: Add the NiCoLDH@NF prepared in step (3) to an aqueous solution containing (NH4)2HPO4 and cobalt salt, place in a high-pressure reactor for hydrothermal reaction, cool, wash and dry to obtain Co-PiNiCoLDH@Nickel Foam electrode.
[0010] Furthermore, in step (1), the organic solvent is ethanol or acetone; the pickling uses 2.5-3.5 mol / L hydrochloric acid or sulfuric acid solution; in step (1), the ultrasonic time is 25-35 min; the acid solution is immersed for 25-35 min; the drying is vacuum drying, the drying temperature is 65-75°C, and the drying time is 5-7h.
[0011] Furthermore, in step (2), the ratio of the sum of the nickel salt and the cobalt salt to water is 2mmol:30-40mL, and the molar ratio of the nickel salt to the cobalt salt is 1-5:5-1; sodium citrate and boric acid are used to adjust the pH value to 6.5-7.5; and the ultrasonic oscillation time is 8-12min.
[0012] Furthermore, in step (3), the size of the nickel foam cut is (2.5-3.5) cm×(1.2-1.8) cm.
[0013] Furthermore, in step (3), the electrodeposition is carried out by a fixed voltage method, the electrodeposition voltage is 1.2-1.4V, and the electrodeposition time is 180-360 seconds; or, the electrodeposition is carried out by a fixed current method, and an electrodeposition amount of 1-3 coulombs per square centimeter is input.
[0014] Furthermore, in step (4), the size of the NiCoLDH@NF is (1.8-2.2) cm×(1.2-1.8) cm.
[0015] Furthermore, in step (4), the molar ratio of (NH4)2HPO4 to cobalt salt is 1-5:1-5; and the ratio of the sum of (NH4)2HPO4 and cobalt salt to water is 2mmol:30-40mL.
[0016] Furthermore, in step (4), the hydrothermal reaction temperature is controlled between 160-200°C, the reaction time is 5-7h; the standing time is 5-7h; the drying is vacuum drying, the drying temperature is 55-65°C, and the drying time is 4-6h.
[0017] A Co-PiNiCoLDH@Nickel Foam electrode has a three-layer structure consisting of a support layer, an intermediate layer and a functional layer; the support layer is made of nickel foam, the NiCoLDH grown on the nickel foam is used as the intermediate layer, and Co2(PO4)3 with a phosphotinite structure is used as the functional layer.
[0018] A Co-PiNiCoLDH@Nickel Foam electrode is prepared according to any method described in the present invention.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (i) The Co-Hopeite / NiCoLDH@NF electrode prepared by the present invention has excellent OER and HER electrodes, and the special structural design makes the electrocatalyst have reliable stability, can be used in the process of full water electrolysis, can be applied to large-scale water electrolysis process, can be applicable to electrochemical fields such as water electrolysis for hydrogen production, chlor-alkali industry and seawater electrolysis, and has strong economic benefits.
[0021] (ii) The present invention adopts a special assembly structure design, with activated nickel foam as the support layer, NiCoLDH grown on nickel foam as the middle layer, and Co2(PO4)3 with a phosphotyrite structure as the functional layer, to form a three-layer assembly structure, which can greatly improve the stability of the electrode while simultaneously improving the electrochemical activities of OER and HER.
[0022] (III) The present invention optimizes the morphology of cobalt phosphate when constituting the catalyst functional layer, and designs its morphology into a "Hopeite" phosphorite structure to improve the electrochemical performance and stability of the electrode. Among them, the sea urchin-like surface morphology presented by the Hopeite phosphorite structure designed by the present invention can greatly increase the active area, expose more active sites, and greatly improve the oxygen and chlorine evolution activities of the electrocatalyst.
[0023] (IV) The present invention adopts a method for preparing a Co-Hopeite / NiCoLDH@Nickel Foam electrode with high-efficiency hydrogen evolution performance and excellent current stability by electrodeposition and hydrothermal growth on the surface of nickel foam. The inexpensive nickel foam material is used as the raw material. On the basis of improving the electrocatalytic performance, the cost increase caused by precious metals is avoided. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a morphology diagram of the surface of the Co-Hopeite / NiCoLDH@NF electrode of Example 1 of the present invention. Figure 2 This is a diagram showing the voltage change of the electrode Co-Hopeite / NiCoLDH@NF in Example 1 of the present invention during the stability experiment; in the figure, at the current density of -500mA cm -2 Chinese meaning: at 500mA cm -2 at a current density of .
[0025] Figure 3 This is a diagram of the HER performance of the electrode Co-Hopeite / NiCoLDH@NF in Example 1 of the present invention in a linear voltammetry test.
[0026] Figure 4 This is the OER performance diagram of the electrode Co-Hopeite / NiCoLDH@NF in Example 1 of the present invention in the linear voltammetry test.
[0027] Figure 5 It is a schematic diagram of the electrode pre-assembly planar structure of Example 1 of the present invention.
[0028] Figure 6 is a schematic diagram of the electrode pre-assembly 3D structure of Example 1 of the present invention,
[0029] In the figure, Electro-Deposition: electrodeposition; Hydrotehrmal: hydrothermal reaction. DETAILED DESCRIPTION
[0030] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.
[0031] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.
[0032] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.
[0033] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.
[0034] RO water: reverse osmosis water
[0035] Example 1
[0036] A method for preparing a Co-Hopeite / NiCoLDH@Nickel Foam electrode is implemented by the following steps:
[0037] 1. Completely immerse the fresh nickel foam in acetone, then seal it in a large beaker and put it into an ultrasonic cleaner for cleaning for 30 minutes, then take it out and clean it with RO water; then soak it in hydrochloric acid (3M) for 30 minutes to remove the oxide on the surface of the nickel foam, and then use deionized water to remove the residue on the surface of the nickel foam; the obtained nickel foam is placed in a vacuum drying oven and vacuum dried at 70°C for 6 hours to obtain the activated nickel foam, which is then sealed for storage.
[0038] 2. Preparation of NiCoLDH electrolyte: Add 0.1mmol Ni(NO3)2, 0.1mmol Co(NO3)2, 0.2mmol sodium citrate and appropriate amount of boric acid (adjust pH to 7) into 35mL RO water, and obtain the desired electrolyte after ultrasonic oscillation for 10 minutes.
[0039] 3. Preparation of intermediate layer NiCoLDH by electrodeposition: The activated nickel foam was cut into 3cm×1.5cm size and used as cathode and anode in a three-electrode system respectively (with saturated calomel electrode as reference electrode). A voltage of 1.2V was input to the three-electrode system in the electrochemical workstation and maintained for 180s, and NiCoLDH@NF containing an intermediate layer of NiCoLDH was obtained on the cathode nickel foam.
[0040] 4. The prepared NiCoLDH@NF (2cm×1.5cm) was added to a solution containing 1mmol(NH4)2HPO4, 0.2mmolCo(NO3)2 and 35mL deionized water, and then transferred to a stainless steel autoclave lined with Teflon material, hydrothermally reacted at 180℃ for 6h, and then allowed to stand for 6h. After the sample cooled to room temperature, it was thoroughly washed with deionized water and ethanol, and dried in a vacuum drying oven at 60℃ for 5 hours. After drying, the target Co-Hopeite / NiCoLDH@Nickel Foam electrode was obtained.
[0041] like Figure 1 As shown, the surface of the catalyst grown with needle-shaped CoPi material forms a sword cluster-like morphology. This special morphology can expose more active sites, promote mass transfer, and thus greatly improve the electrochemical performance of the catalyst.
[0042] like Figure 2 As shown in the catalytic stability test, it can be seen that at 500mA cm-2 Under high current density, the catalyst can operate stably for more than 55 hours without more than 5% performance degradation, indicating its excellent stability.
[0043] like Figure 3 As shown in the LSV linear voltammetric polarization curve of hydrogen evolution, it can be seen that the catalyst still exhibits a smaller overpotential when compared with other excellent catalysts. Under the condition of hydrogen evolution, 10 mA cm -2 The overpotential is only 45mV at 100mA cm -2 The overpotential is only 180mV, and the performance is very excellent.
[0044] like Figure 4 As shown in the LSV linear voltammetric polarization curve of oxygen evolution, it can be seen that the catalyst also shows a smaller overpotential when compared with other excellent catalysts. Under the condition of oxygen evolution, 100mA cm -2 The voltage is 1.58V (equivalent to an overpotential of only 350mV), and the performance is also very excellent.
[0045] The results show that the prepared Co-Hopeite / NiCoLDH@Nickel Foam electrode has both efficient hydrogen evolution and oxygen evolution properties and excellent high current density stability, so it is very suitable for large-scale industrial applications.
[0046] Example 2: This example is different from Example 1 in that the organic solvent acetone in step 1 is replaced with ethanol, and the pickling solvent hydrochloric acid is replaced with sulfuric acid (3M). Step 1 is specifically as follows:
[0047] The fresh nickel foam was completely immersed in ethanol, and then sealed in a large beaker and placed in an ultrasonic cleaner for cleaning for 30 minutes, then taken out and cleaned with RO water; then placed in sulfuric acid (3M) and soaked for 30 minutes to remove the oxide on the surface of the nickel foam, and then deionized water was used to remove the residual on the surface of the nickel foam. The obtained nickel foam was placed in a vacuum drying oven and vacuum dried at 70°C for 6 hours to obtain the activated nickel foam, which was then sealed and stored. The other steps and parameters were the same as those in Example 1.
[0048] The results show that the nickel foam obtained after activation by this method can be more conducive to the subsequent electrodeposition process and hydrothermal growth process, and improve the electrochemical performance of the catalyst and the stability under high current density.
[0049] Example 3: This embodiment differs from Example 1 in that the solutes in step 2 are replaced with Co(NO3)2 and Ni(NO3)2 in turn with CoSO4 and NiSO4. The other steps and parameters are the same as those in Example 1. Step 2 is specifically as follows:
[0050] Preparation of NiCoLDH electrolyte: Add 0.1mmol NiSO4, 0.1mmol CoSO4, 0.2mmol sodium citrate and appropriate amount of boric acid (to adjust the pH to neutral) to 35mL RO water, and obtain the desired electrolyte after ultrasonic oscillation for 10 minutes.
[0051] The results show that this method of electrodeposition can also obtain NiCoLDH@NF with excellent performance. Linear voltammetry electrochemical testing found that the NiCoLDH@NF prepared by this method is slightly inferior to the original catalyst in the starting point, but the change is not large, and it is still a catalyst with excellent performance.
[0052] Example 4: This embodiment is different from Example 1 in that the electrodeposition method in step 3 is changed from a fixed voltage method to a fixed current method, and the surface morphology of the catalyst intermediate layer is controlled by the standard of "1.5 coulombs of electrodeposition per square centimeter". Step 3 is specifically as follows:
[0053] Preparation of intermediate layer NiCoLDH by electrodeposition: The activated nickel foam was cut into 3 cm × 1.5 cm size and used as cathode and anode in the three-electrode system (saturated calomel electrode was used as reference electrode), and the electrodeposition amount of 1.5 coulombs per square centimeter was input into the three-electrode system in the electrochemical workstation and maintained for 180 seconds, and NiCoLDH@NF containing the intermediate layer of NiCoLDH was obtained on the cathode nickel foam. Other steps and parameters were the same as those in Example 1.
[0054] The results show that the electrochemical performance of the Co-Hopeite / NiCoLDH@Nickel Foam electrode prepared in Example 5 is slightly worse than that in Example 1, but the difference in electrochemical performance with the electrode in Example 1 is not significant.
[0055] Example 5: Based on Example 1, the molar ratio of the nickel salt and the cobalt salt in step 2 is adjusted to 1-5:5-1, and the specific dosage is as follows:
[0056] Group <![CDATA[Ni(NO3)2]]> <![CDATA[Co(NO3)2]]> 1 (Example 1) 0.1mmol 0.1mmol 2 0.2mmol 0.1mmol 3 0.3mmol 0.1mmol 4 0.4mmol 0.1mmol 5 0.5mmol 0.1mmol 6 0.1mmol 0.1mmol 7 0.1mmol 0.2mmol 8 0.1mmol 0.3mmol 9 0.1mmol 0.4mmol 10 0.1mmol 0.5mmol
[0057] The results show that the electrochemical performance of the Co-Hopeite / NiCoLDH@Nickel Foam electrode prepared in Groups 2-10 is slightly worse than that of Example 1, but the difference in electrochemical performance with the electrode in Example 1 is not significant.
[0058] Comparative Example 1: The difference from Example 1 is that the nickel foam is cut directly without activation to proceed to step 3. The results show that the catalyst cannot be effectively grown in situ due to the presence of the grease protective layer and the oxide layer on the surface of the unactivated nickel foam, and ultimately a dense microstructure cannot be obtained, resulting in poor performance.
[0059] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a Co-PiNiCoLDH@Nickel Foam electrode, characterized in that: The following steps are involved: Taking the nickel foam and soaking it in an organic solvent, washing it with water after ultrasonication, and then soaking it in an acid solution, washing it with water and drying it to obtain an activated nickel foam; Dissolving nickel salt and cobalt salt in water, adjusting the pH value to 6.5-7.5, and obtaining NiCoLDH electrolyte after ultrasonic oscillation; The nickel foam activated in step (1) is cut into pieces and used as the cathode and anode in the three-electrode system respectively. The NiCoLDH electrolyte in step (2) is used as the electrolyte of the three-electrode system to perform an electrodeposition treatment, thereby obtaining NiCoLDH@NF containing a NiCoLDH intermediate layer on the cathode nickel foam; The NiCoLDH@NF prepared in step (3) is added to an aqueous solution containing (NH4)2HPO4 and a cobalt salt, placed in a high-pressure reactor for hydrothermal reaction, cooled, washed, and dried to obtain a Co-PiNiCoLDH@Nickel Foam electrode.
2. The preparation method according to claim 1, characterized in that: In step (1), the organic solvent is ethanol or acetone; the acid solution is 2.5-3.5 mol / L hydrochloric acid or sulfuric acid solution; in step (1), the ultrasonic time is 25-35 min; the acid solution is immersed for 25-35 min; the drying is vacuum drying, the drying temperature is 65-75° C., and the drying time is 5-7 h.
3. The preparation method according to claim 1, characterized in that: In step (2), the molar ratio of the nickel salt to the cobalt salt is 1-5:5-1; sodium citrate and boric acid are used to adjust the pH value to 6.5-7.5; and the ultrasonic oscillation time is 8-12 min.
4. The preparation method according to claim 1, characterized in that: In step (3), the size of the nickel foam cut is (2.5-3.5) cm×(1.2-1.8) cm.
5. The preparation method according to claim 1, characterized in that: In step (3), the electrodeposition is carried out by a fixed voltage method, the electrodeposition voltage is 1.2-1.4 V, and the electrodeposition time is 180-360 seconds; or, the electrodeposition is carried out by a fixed current method, and an electrodeposition amount of 1-3 coulombs per square centimeter is input.
6. The preparation method according to claim 1, characterized in that: In step (4), the size of the NiCoLDH@NF is (1.8-2.2) cm×(1.2-1.8) cm.
7. The preparation method according to claim 1, characterized in that: In step (4), the molar ratio of (NH4)2HPO4 to cobalt salt is 1-5:1-5.
8. The preparation method according to claim 1, characterized in that: In step (4), the hydrothermal reaction temperature is controlled between 160-200°C, the reaction time is 5-7h; the standing time is 5-7h; the drying is vacuum drying, the drying temperature is 55-65°C, and the drying time is 4-6h.
9. A Co-PiNiCoLDH@Nickel Foam electrode, characterized in that: Prepared according to the method described in any one of claims 1 to 8.