A method for uniformly plating printed circuit boards

Through chemical oil removal, electroplating cleaning and water washing, combined with defoaming agent and recycling cleaning method, the problem of blackening and uneven coating of printed circuit boards caused by long plating time is solved, and the uniformity of copper plating and nickel plating is achieved and stability.

CN115182010BActive Publication Date: 2024-11-15GUANGDONG CHAMPION ASIA ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210427394.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-22
Publication Date
2024-11-15
Estimated Expiration
2042-04-22

AI Technical Summary

Technical Problem

During the electroplating process, the plating layer of printed circuit boards becomes black due to the long plating time, and the small current electroplating method is easily affected by the cleaning effect, resulting in uneven coating, which is prone to bubbles and flowering.

Method used

Using chemical oil removal, electroplating and cleaning, water washing, pre-impregnation, chemical copper plating, nickel plating, chromium plating and other steps, combined with defoaming by sodium hydroxide, sodium thiocyanate, cetyl trimethyl ammonium bromide and other components The agent and recycling cleaning method control the temperature and metal ion concentration during the electroplating process, and continuously flip to improve uniformity.

Benefits of technology

It effectively reduces the blackening of the plating, improves the uniformity and speed of electroplating, ensures that the copper and nickel plating surfaces are not easily discolored, and enhances the stability and wear resistance of electroplating.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an electroplating method for uniform electroplating of a printed circuit board, and relates to the technical field of electroplating. Aiming at the problem that the electroplating layer is blackened due to the long electroplating time of the existing printed circuit board and the small current electroplating method is easily affected by the cleaning effect, resulting in bubbling and floweriness of the plating layer, making the electroplating not uniform enough, the following scheme is proposed, which includes chemical degreasing: firstly, the workpiece to be electroplated is chemically degreased, and the main component in the chemical degreasing is sodium hydroxide, and the cleaning temperature of the workpiece is emulsified cleaning at 70-90°C; electroplating cleaning: then the emulsified workpiece is transferred to a cleaning tank for electroplating cleaning; water washing: the workpiece after the electroplating cleaning is transferred to water washing. The electroplating method for uniform electroplating of the present invention makes it difficult for the copper-plated and nickel-plated surfaces to change color, thereby effectively reducing the blackening of the workpiece electroplating layer during electroplating, and also effectively improving the uniformity of electroplating, which is convenient to use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electroplating, and in particular to an electroplating method for uniformly electroplating a printed circuit board. Background Art

[0002] In recent years, with the advent of the 5G era, the demand for printed circuit boards has increased, and the quality requirements have become higher and higher. When electroplating printed circuit boards, they are generally electroplated by a small current method, which reduces the deposition rate and performs electroplating for a long time to achieve uniform plating. The small current electroplating method causes the coating of the printed circuit board to turn black due to the long electroplating time, and reduces the work efficiency of electroplating. In addition, most manufacturers do not care much about cleaning the printed circuit boards before electroplating. The circuit boards are not cleaned properly, which makes the small current electroplating method susceptible to the cleaning effect, resulting in bubbling and blooming of the coating, making the plating uneven. Therefore, in order to solve such problems, we propose a plating method for uniform electroplating of printed circuit boards. Summary of the invention

[0003] The present invention provides a method for uniformly plating a printed circuit board, which solves the problem that the electroplating layer becomes black due to a long electroplating time of the printed circuit board and the small current electroplating method is easily affected by the cleaning effect, resulting in blistering and blooming of the plating layer, making the electroplating less uniform.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions:

[0005] A method for uniformly electroplating a printed circuit board comprises the following steps:

[0006] S1. Chemical degreasing: First, the workpiece to be electroplated is chemically degreased. The main component of chemical degreasing is sodium hydroxide, and the cleaning temperature of the workpiece is 70-90℃ for emulsification cleaning;

[0007] S2, electroplating cleaning: then the emulsified workpiece is transferred to the cleaning tank for electroplating cleaning;

[0008] S3, water washing: the workpiece after electroplating cleaning is transferred to water washing, and the defoaming agent in the water washing is used to reduce the bubbles generated by washing and improve the electroplating quality;

[0009] S4, pre-preg: after the workpiece is cleaned, the workpiece is transferred to the pre-preg process for immersion activation, so that the accelerator is attached to the surface of the workpiece;

[0010] S5. Chemical copper plating: After immersion, chemical copper plating is performed, using 3-15% sodium thiocyanate and 15-20% hexadecyltrimethylammonium bromide as a composite stabilizer to obtain a better deposition rate and greatly improve the stability of the chemical copper plating solution;

[0011] S6, secondary water washing: water washing is performed after the chemical copper plating is completed to clean the chemical residues and impurities attached to the chemical copper plating;

[0012] S7, nickel plating: nickel plating is performed after washing, and nickel is plated on metal or non-metal by electrolysis, and the electrolyte composition of nickel plating includes nickel salt 200-220g / L, conductive salt 80-120g / L, acid-base buffer 60-90mL / L and wetting agent 9-20mL / L;

[0013] S8, three water washing: After nickel plating, water washing is performed to defoam and remove impurities, reduce the impact of chemical reagents in nickel plating on the next process, and the metal ion concentration of the water in the washing process is controlled at 10mg / dm 3 , if it exceeds, it needs to be replaced;

[0014] S9, Chrome plating: Chrome plating is carried out after washing to improve the wear resistance of the workpiece. At the same time, chrome is not easy to change color and is not easy to react with most organic acids such as alkali and sulfide, and has chemical stability;

[0015] S10, washing, drying and inspection: After chrome plating, washing, drying and inspection are required. The metal ion concentration in the final washing is controlled at 20-50mg / dm 3 , once exceeded, it needs to be replaced.

[0016] Preferably, the defoaming agent can be directly dripped or sprayed into water for dilution, and the ratio of the defoaming agent to water is 1:15, and the added amount is 0.02-0.05% of the total product amount. At the same time, the water used to clean the workpiece by diluting the defoaming agent and water needs to be replaced when it is used up on the same day.

[0017] Preferably, the workpiece is continuously turned over during the chemical copper plating, nickel plating and chromium plating processes, so as to maintain the uniformity of electroplating through fluidity, and at the same time the current is increased to electroplate the workpiece, and the cathode current density of the electroplating is adjusted to 2.0ASD, so that the copper plating speed is faster and the electroplating uniformity is better.

[0018] Preferably, the chemical degreasing uses sodium hydroxide solution to saponify and emulsify the grease on the surface of the workpiece, and the chemical degreasing has a stronger emulsification cleaning ability at medium and high temperatures of 70-90°C. The sodium hydroxide solution and hot water are added in a ratio of 1:20, and cleaning is performed using a drum or ultrasonic cleaning machine.

[0019] Preferably, the pre-dip process contains 12-15% of the pre-dip agent mixed solution required for electroplating and 4-8% of the citric acid solution, so that the workpiece is activated in the pre-dip solution and the accelerator is attached to the surface of the workpiece.

[0020] Preferably, the electroplating cleaning includes water cleaning, gas cleaning, chemical cleaning, and solvent cleaning, and the cleaning method is a recovery cleaning method. The workpiece to be electroplated is first placed in a cleaning tank, and then the cleaning tank is replenished with cleaning water while the cleaned water is transported to a primary recovery tank for treatment. The primary recovery tank performs secondary treatment on the treated cleaning water, and the treated water is recycled or discharged.

[0021] Preferably, the recovery cleaning method must be equipped with a first or second recovery tank, and the recovery liquid in the recovery tank can be utilized, and the amount of cleaning water per unit area of ​​the plated piece in the recovery cleaning method should be less than 100dm 3 / m 2 .

[0022] Preferably, a water washing process is added before and after the electroplating, so that the electroplated workpiece can be effectively cleaned, and a defoaming agent is added to the water used for washing, which can effectively eliminate the foam generated when the electroplated product is cleaned, thereby reducing the impact of the foam generated by the workpiece cleaning on the electroplating.

[0023] The beneficial effects of the present invention are:

[0024] 1. By increasing the cathode current density, the electroplating speed of the workpiece is improved, and a layer of chromium is electroplated on the copper-plated surface, so that the copper-plated and nickel-plated surfaces are not easy to change color, thereby effectively reducing the blackening of the workpiece electroplating layer during electroplating.

[0025] 2. By adding a water washing process before and after electroplating, the chemical reagents produced by electroplating can be washed away, and the foaming caused by water washing can be eliminated by using a defoaming agent, and the surface can be turned over continuously during electroplating, thereby effectively improving the uniformity of electroplating.

[0026] In summary, the device makes the copper-plated and nickel-plated surfaces less likely to change color, thereby effectively reducing the blackening of the electroplating layer of the workpiece during electroplating, and can also effectively improve the uniformity of electroplating, making it easy to use. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments.

[0028] Embodiment 1:

[0029] A method for uniformly electroplating a printed circuit board comprises the following steps:

[0030] S1: First, the workpiece to be electroplated is chemically degreased, and the main component of the chemical degreasing is sodium hydroxide, and the cleaning temperature of the workpiece is emulsified cleaning at 50-60℃;

[0031] S2: The emulsified workpiece is then transferred to a cleaning tank for electroplating cleaning;

[0032] S3: The workpiece after electroplating cleaning is transferred to water washing, and the defoaming agent in the water washing is used to reduce the bubbles generated by washing and improve the electroplating quality;

[0033] S4: After the workpiece is cleaned, the workpiece is transferred to the pre-preg process for immersion activation, so that the accelerator is attached to the surface of the workpiece;

[0034] S5: After the immersion is completed, chemical copper plating is performed, using 5-11% sodium thiocyanate and 5-8% hexadecyltrimethylammonium bromide as a composite stabilizer, and the deposition rate is 50 μm / h, so that the chemical copper plating solution is not stable enough;

[0035] S6: After the chemical copper plating is completed, water washing is performed to clean the chemical residues and impurities attached to the chemical copper plating;

[0036] S7: After washing, nickel plating is performed, and nickel is plated on the metal or non-metal by electrolysis, and the electrolyte composition of the nickel plating includes 100-180g / L of nickel salt, 40-80g / L of conductive salt, 20-60mL / L of acid-base buffer and 3-8mL / L of wetting agent;

[0037] S8: After nickel plating, water washing is performed to defoam and remove impurities, reduce the impact of chemical reagents in nickel plating on the next process, and the metal ion concentration of water in the washing process is controlled at 10mg / dm 3 , if it exceeds, it needs to be replaced;

[0038] S9: After washing, chrome plating is performed to improve the wear resistance of the workpiece. At the same time, chrome is not easy to change color and is not easy to react with most organic acids such as alkali and sulfide, and has chemical stability;

[0039] S10: After chrome plating, it can be washed, dried and sent for inspection. The metal ion concentration in the final washing is controlled at 20-50mg / dm 3 , once exceeded, it needs to be replaced.

[0040] The defoaming agent can be directly added or sprayed into the water for dilution, and the ratio of defoaming agent to water is 1:10, and the added amount can be added according to 0.01-0.08% of the total product amount. At the same time, the water used to clean the workpiece with the defoaming agent and water needs to be replaced when it is used up on the same day.

[0041] During the process of chemical copper plating, nickel plating and chromium plating, the workpiece is constantly turned over to maintain the uniformity of electroplating through fluidity, while the current is increased to electroplate the workpiece, and the cathode current density of electroplating is adjusted to 1.0ASD, which makes the copper plating speed slower and the electroplating uniformity worse.

[0042] Chemical degreasing uses sodium hydroxide solution to saponify and emulsify the grease on the surface of the workpiece, and chemical degreasing has stronger emulsification cleaning ability at medium and high temperatures of 50-60°C. The ratio of sodium hydroxide solution to hot water is added in a ratio of 1:10, and cleaning is performed with a drum or ultrasonic cleaning machine, which makes the emulsification cleaning effect poor.

[0043] The pre-dip process includes a pre-dip agent mixed solution of 8-12% required for electroplating and a citric acid solution of 8-15%, so that the workpiece is activated in the pre-dip solution and the accelerator is attached to the surface of the workpiece.

[0044] Electroplating cleaning includes water cleaning, gas cleaning, chemical cleaning, and solvent cleaning, and the cleaning method is recovery cleaning. First, the workpiece to be electroplated is placed in the cleaning tank, and then the cleaning tank is replenished with cleaning water while the cleaned water is transported to the primary recovery tank for treatment. The primary recovery tank will perform secondary treatment on the treated cleaning water, and the treated water will be recycled or discharged.

[0045] The recovery cleaning method must have a one-stage or two-stage recovery tank, and the recovery liquid in the recovery tank can be used. The amount of cleaning water per unit area of ​​the plated part in the recovery cleaning method should be less than 150dm 3 / ㎡.

[0046] A water washing process is added before and after electroplating, so that the electroplated workpiece can be effectively cleaned, and defoaming agent is added to the water for washing, which can effectively eliminate the foam generated when the electroplated product is cleaned, and reduce the impact of the foam generated by the workpiece cleaning on electroplating.

[0047] Embodiment 2:

[0048] A method for uniformly electroplating a printed circuit board comprises the following steps:

[0049] S1. Chemical degreasing: First, the workpiece to be electroplated is chemically degreased. The main component of chemical degreasing is sodium hydroxide, and the cleaning temperature of the workpiece is 70-90℃ for emulsification cleaning;

[0050] S2, electroplating cleaning: then the emulsified workpiece is transferred to the cleaning tank for electroplating cleaning;

[0051] S3, water washing: the workpiece after electroplating cleaning is transferred to water washing, and the defoaming agent in the water washing is used to reduce the bubbles generated by washing and improve the electroplating quality;

[0052] S4, pre-preg: after the workpiece is cleaned, the workpiece is transferred to the pre-preg process for immersion activation, so that the accelerator is attached to the surface of the workpiece;

[0053] S5. Chemical copper plating: After immersion, chemical copper plating is performed, using 3-15% sodium thiocyanate and 15-20% hexadecyltrimethylammonium bromide as a composite stabilizer to obtain a better deposition rate and greatly improve the stability of the chemical copper plating solution;

[0054] S6, secondary water washing: water washing is performed after the chemical copper plating is completed to clean the chemical residues and impurities attached to the chemical copper plating;

[0055] S7, nickel plating: nickel plating is performed after washing, and nickel is plated on metal or non-metal by electrolysis, and the electrolyte composition of nickel plating includes nickel salt 200-220g / L, conductive salt 80-120g / L, acid-base buffer 60-90mL / L and wetting agent 9-20mL / L;

[0056] S8, three water washing: After nickel plating, water washing is performed to defoam and remove impurities, reduce the impact of chemical reagents in nickel plating on the next process, and the metal ion concentration of the water in the washing process is controlled at 10mg / dm 3 , if it exceeds, it needs to be replaced;

[0057] S9, Chrome plating: Chrome plating is carried out after washing to improve the wear resistance of the workpiece. At the same time, chrome is not easy to change color and is not easy to react with most organic acids such as alkali and sulfide, and has chemical stability;

[0058] S10, washing, drying and inspection: After chrome plating, washing, drying and inspection are required. The metal ion concentration in the final washing is controlled at 20-50mg / dm 3 , once exceeded, it needs to be replaced.

[0059] The defoaming agent can be directly added or sprayed into the water for dilution, and the ratio of defoaming agent to water is 1:15, and the added amount can be added according to 0.02-0.05% of the total product amount. At the same time, the water used to clean the workpiece with the defoaming agent and water needs to be replaced when it is used up on the same day.

[0060] During the process of chemical copper plating, nickel plating and chromium plating, the workpiece is constantly turned over to maintain the uniformity of electroplating through fluidity, while the current is increased to electroplate the workpiece, and the cathode current density of electroplating is adjusted to 2.0ASD, which makes the copper plating speed faster and the electroplating uniformity better.

[0061] Chemical degreasing uses sodium hydroxide solution to saponify and emulsify the grease on the surface of the workpiece. Chemical degreasing has stronger emulsification and cleaning ability at medium and high temperatures of 70-90°C. The ratio of sodium hydroxide solution to hot water is 1:20, and cleaning is carried out with a drum or ultrasonic cleaner.

[0062] The pre-dip process includes a pre-dip agent mixed solution of 12-15% required for electroplating and a citric acid solution of 4-8%, so that the workpiece is activated in the pre-dip solution and the accelerator is attached to the surface of the workpiece.

[0063] Electroplating cleaning includes water cleaning, gas cleaning, chemical cleaning, and solvent cleaning, and the cleaning method is recovery cleaning. First, the workpiece to be electroplated is placed in the cleaning tank, and then the cleaning tank is replenished with cleaning water while the cleaned water is transported to the primary recovery tank for treatment. The primary recovery tank will perform secondary treatment on the treated cleaning water, and the treated water will be recycled or discharged.

[0064] The recovery cleaning method must have a one-stage or two-stage recovery tank, and the recovery liquid in the recovery tank can be used. The amount of cleaning water per unit area of ​​the plated part in the recovery cleaning method should be less than 100dm 3 / m 2 .

[0065] A water washing process is added before and after electroplating, so that the electroplated workpiece can be effectively cleaned, and defoaming agent is added to the water for washing, which can effectively eliminate the foam generated when the electroplated product is cleaned, and reduce the impact of the foam generated by the workpiece cleaning on electroplating.

[0066] In summary: the solution ratio and temperature requirements in Example 1 and Example 2 are different, and the ratio and temperature in Example 2 are more reasonable, so that the electroplating uniformity is higher.

[0067] The above are only preferred specific implementation modes of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for uniform electroplating of a printed circuit board, characterized in that: The steps include: S1. Chemical degreasing: First, the workpiece to be electroplated is chemically degreased, and the chemical degreasing contains sodium hydroxide, and the cleaning temperature of the workpiece is 70-90℃ for emulsification cleaning; S2, electroplating cleaning: then the emulsified workpiece is transferred to the cleaning tank for electroplating cleaning; S3, water washing: the workpiece after electroplating cleaning is transferred to water washing, and the defoaming agent in the water washing is used to reduce the bubbles generated by washing and improve the electroplating quality; S4, pre-impregnation: After the workpiece is cleaned, the workpiece is transferred to the pre-impregnation process for immersion activation, so that the accelerator is attached to the surface of the workpiece; S5, chemical copper plating: after immersion, chemical copper plating is performed, using 3-15% sodium thiocyanate and 15-20% hexadecyltrimethylammonium bromide as a composite stabilizer to improve the stability of the chemical copper plating solution; S6, secondary water washing: water washing is performed after the chemical copper plating is completed to clean the chemical residues and impurities attached to the chemical copper plating; S7, nickel plating: nickel plating is performed after washing, and nickel is plated on metal or non-metal by electrolysis, and the electrolyte composition of nickel plating includes nickel salt 200-220g / L, conductive salt 80-120g / L, acid-base buffer 60-90mL / L and wetting agent 9-20mL / L; S8, three water washings: After nickel plating, water washing is performed to defoam and remove impurities, reduce the impact of chemical reagents in nickel plating on the next process, and the metal ion concentration of the water in the washing process is controlled at 10mg / dm 3 , if it exceeds, it needs to be replaced; S9, Chrome plating: Chrome plating is carried out after washing to improve the wear resistance of the workpiece. At the same time, chrome is not easy to change color and is not easy to react with alkali, sulfide and most organic acids, and has chemical stability; S10, washing, drying and inspection: After chrome plating, washing, drying and inspection are required. The metal ion concentration in the final washing is controlled at 20-50mg / dm 3 , once exceeded, it needs to be replaced; During the chemical copper plating, nickel plating and chromium plating processes, the workpiece is constantly turned over to maintain the uniformity of electroplating through fluidity, while the current is increased to electroplate the workpiece, and the cathode current density of the electroplating is adjusted to 2.0ASD to increase the copper plating speed and the uniformity of the electroplating.

2. The electroplating method for uniform electroplating of a printed circuit board according to claim 1, characterized in that: The defoaming agent can be directly dripped or sprayed into water for dilution, and the ratio of the defoaming agent to water is 1:15, and the added amount can be added according to 0.02-0.05% of the total amount of the product. At the same time, the water used for cleaning the workpiece by diluting the defoaming agent and water needs to be replaced when it is used up on the same day.

3. The electroplating method for uniform electroplating of a printed circuit board according to claim 1, characterized in that: The chemical degreasing uses sodium hydroxide solution to saponify and emulsify the grease on the surface of the workpiece, and the chemical degreasing has a stronger emulsification and cleaning ability at medium and high temperatures of 70-90°C. The sodium hydroxide solution and hot water are added in a ratio of 1:20, and cleaning is performed using a drum or ultrasonic cleaning machine.

4. The electroplating method for uniform electroplating of a printed circuit board according to claim 1, characterized in that: The pre-dip process contains 12-15% of the pre-dip agent mixed solution required for electroplating and 4-8% of the citric acid solution, so that the workpiece is activated in the pre-dip solution, and the accelerator is attached to the surface of the workpiece.

5. The electroplating method for uniform electroplating of a printed circuit board according to claim 1, characterized in that: The electroplating cleaning includes water cleaning, gas cleaning, chemical cleaning, and solvent cleaning, and the cleaning method is a recovery cleaning method. First, the workpiece to be electroplated is placed in a cleaning tank, and then the cleaning tank is replenished with cleaning water while the cleaned water is transported to a primary recovery tank for treatment. The primary recovery tank performs a secondary treatment on the treated cleaning water, and the treated water is recycled or discharged.

6. The electroplating method for uniform electroplating of a printed circuit board according to claim 5, characterized in that: The recovery cleaning method is provided with a first-stage or a second-stage recovery tank, and the recovery liquid in the recovery tank can be utilized. The amount of cleaning water per unit area of ​​the plated piece in the recovery cleaning method should be less than 100 dm 3 / m 2 .

7. The electroplating method for uniform electroplating of a printed circuit board according to claim 1, characterized in that: A water washing process is added before and after the electroplating to clean the electroplated workpiece, and a defoaming agent is added to the water for washing to eliminate the foam generated when the electroplated product is washed, thereby reducing the impact of the foam generated by the workpiece cleaning on the electroplating.