A method for restoring the performance of an electrochromic device

By heat-treating the electrochromic device, the problem of performance degradation was solved, the initial performance was restored, and the service life was extended.

CN115185134BActive Publication Date: 2024-11-29HARBIN INST OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210836491.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-15
Publication Date
2024-11-29
Estimated Expiration
2042-07-15

AI Technical Summary

Technical Problem

Existing methods for restoring the performance of electrochromic devices are not applicable to them, leading to performance degradation and limiting their commercial application.

Method used

By heat treatment, electrochromic devices with degraded performance are subjected to heat treatment at 40℃~800℃ to restore their initial performance.

Benefits of technology

It restores the initial performance of electrochromic devices, significantly extends their service life, and achieves a recovery efficiency of 95% to 100%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115185134B_ABST
    Figure CN115185134B_ABST
Patent Text Reader

Abstract

A method for restoring the performance of an electrochromic device relates to the field of electrochromic devices, and specifically to a method for restoring the performance of an electrochromic device. The purpose of the present invention is to solve the problem that the existing method for restoring the performance attenuation of electrochromic films is not suitable for electrochromic devices, and the performance attenuation of electrochromic devices limits their commercial applications. A method for restoring the performance of an electrochromic device is to use heat treatment to restore the initial performance of the electrochromic device with attenuated performance. The specific method is to heat treat the electrochromic device with attenuated performance at 40°C to 800°C to restore the initial performance of the electrochromic device with attenuated performance. The present invention proposes a simple and novel method, which can significantly extend the service life of the device by heating to regenerate the attenuated electrochromic device, and has important value; using the method for restoring the performance of an electrochromic device of the present invention, the initial performance can be restored to 95% to 100%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electrochromic devices, and in particular to a method for restoring the performance of an electrochromic device. Background Art

[0002] Electrochromism refers to the phenomenon that when a material is subjected to an external electric field, the optical properties (transmittance, absorptivity and reflectivity, etc.) change reversibly through the reversible insertion and extraction of cations such as hydrogen ions and lithium ions. Electrochromic devices are usually composed of five layers of thin films, including two transparent conductive layers, an electrochromic layer, an electrolyte layer and an ion storage layer. Electrochromic devices have shown great application potential in the fields of smart windows, anti-glare rearview mirrors, spacecraft thermal control systems and electronic tags.

[0003] The optical properties of electrochromic materials change due to the insertion and extraction of small cations. However, the insertion and extraction of ions are not balanced during the cycle because some ions will be trapped. This will lead to the attenuation of electrochromic materials and limit their commercial applications. In recent years, people have been committed to improving the cyclic stability of ECD on the one hand, and on the other hand, due to the inevitable existence of ion capture, can the attenuated electrochromic device restore its performance? It is reported that applying a constant current or voltage to the electrochromic film can release the trapped ions. Therefore, the attenuation of the performance of the electrochromic film caused by capture can be eliminated and its initial performance can be restored. However, this method is not suitable for devices because when a constant current or voltage is applied to the electrochromic layer to release the trapped ions, the ions will be over-embedded into the complementary layer. Summary of the invention

[0004] The purpose of the present invention is to solve the problem that the existing method for restoring the performance attenuation of electrochromic films is not suitable for electrochromic devices, and the performance attenuation of electrochromic devices limits their commercial applications, and to provide a method for restoring the performance of electrochromic devices.

[0005] A method for restoring the performance of an electrochromic device is applicable to various types of electrochromic devices, including liquid electrolyte, gel electrolyte and solid electrolyte devices. The electrochromic layer can be an organic material, such as polyaniline, polythiophene, polypyrrole, etc., or an inorganic material, such as tungsten oxide, nickel oxide, vanadium oxide.

[0006] The performance of electrochromic devices decays during the cycling process, which is manifested by a decrease in optical modulation amplitude, a slow response speed, and a decrease in coloring efficiency.

[0007] A method for restoring the performance of an electrochromic device is to use heat treatment to restore the initial performance of the electrochromic device with degraded performance.

[0008] Furthermore, the electrochromic device with performance degradation is heat-treated at 40° C. to 800° C. to restore the initial performance of the electrochromic device with performance degradation.

[0009] Advantages of the present invention:

[0010] First, after using the method of the present invention, the trapped ions can cross the energy barrier and be released again to restore vitality, so that the electrochromic device restores its initial performance;

[0011] Second, the present invention proposes a simple and novel method to regenerate the attenuated electrochromic device by heating, which can significantly extend the service life of the device and achieve green and sustainable development, which is of great value;

[0012] 3. Using a method of restoring the performance of an electrochromic device of the present invention, the initial performance can be restored to 95% to 100%. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 A recovery mechanism diagram for recovering the performance of an electrochromic device according to the present invention;

[0014] Figure 2 This is a transmittance regulation recovery performance diagram for restoring the performance of an electrochromic device in Example 1. DETAILED DESCRIPTION

[0015] The following examples further illustrate the content of the present invention, but should not be construed as limiting the present invention. Without departing from the essence of the present invention, modifications and substitutions made to the methods, steps or conditions of the present invention all fall within the scope of the present invention.

[0016] Specific implementation method 1: In this implementation method, a method for restoring the performance of an electrochromic device is to use heat treatment to restore the initial performance of the electrochromic device with degraded performance.

[0017] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the electrochromic device with degraded performance is heat treated at 40° C. to 800° C. to restore the initial performance of the electrochromic device with degraded performance. The other steps are the same as those of specific implementation method 1.

[0018] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the heat treatment time is 20 minutes to 300 minutes. The other steps are the same as those of specific implementation method 1 or 2.

[0019] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the heat treatment atmosphere is air, argon or vacuum atmosphere. The other steps are the same as those of specific embodiments 1 to 3.

[0020] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the electrochromic device with degraded performance is placed in a tube furnace, a muffle furnace or an oven for heat treatment. The other steps are the same as those of specific embodiments 1 to 4.

[0021] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the electrochromic device is a fully solid electrochromic device, which is prepared on a glass substrate by magnetron sputtering, the upper and lower electrodes are indium tin oxide, the electrochromic layer is tungsten oxide, the electrolyte layer is lithium tantalate, and the ion storage layer is nickel oxide. The prepared electrochromic device has performance degradation after cycling, and the attenuated electrochromic device is heat-treated at 300°C for 2h. The other steps are the same as those of specific embodiments 1 to 5.

[0022] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the electrochromic device is a fully solid electrochromic device, which is prepared on a glass substrate by vacuum evaporation coating, the upper and lower electrodes are indium tin oxide, the electrochromic layer is tungsten oxide, the electrolyte layer is tantalum oxide, the ion storage layer is nickel oxide, and the electrolyte ions are evaporated metallic lithium. The prepared electrochromic device has performance decay after cycling, and the decayed electrochromic device is heat treated at 350°C for 2h. The other steps are the same as those of specific embodiments 1 to 6.

[0023] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that the electrochromic device is a laminated electrochromic device, the electrochromic layer is tungsten oxide, the ion storage layer is nickel oxide, the substrate is ITO glass, the electrolyte layer is a mixture of lithium perchlorate dissolved in propylene carbonate and ultraviolet curing glue, the prepared electrochromic device has performance degradation after cycling, and the attenuated electrochromic device is heat-treated at 50°C for 50 minutes. The other steps are the same as those of specific embodiments one to seven.

[0024] Specific embodiment nine: The difference between this embodiment and specific embodiments one to eight is that the electrochromic device is a liquid electrolyte electrochromic device, the electrochromic layer and the ion storage layer are both polyaniline, the substrate is a gold-plated porous membrane, the electrolyte layer is lithium perchlorate dissolved in propylene carbonate, and the prepared electrochromic device shows performance degradation after cycling, and the attenuated electrochromic device is heat treated at 50°C for 30 minutes.

[0025] The other steps are the same as those in Specific Embodiments 1 to 8.

[0026] The following examples are used to verify the beneficial effects of the present invention:

[0027] Example 1: A method for restoring the performance of an electrochromic device is accomplished by the following steps:

[0028] The electrochromic device is an all-solid electrochromic device, which is prepared on a glass substrate by magnetron sputtering. The upper and lower electrodes are indium tin oxide, the electrochromic layer is tungsten oxide, the electrolyte layer is lithium tantalate, and the ion storage layer is nickel oxide. The prepared all-solid-state electrochromic device shows performance degradation after cycling, and the attenuated electrochromic device is heat treated at 300°C for 2 hours.

[0029] Using the method of Example 1, the attenuated electrochromic device recovered 97% of its initial performance, such as Figure 2 .

[0030] Figure 2 This is a transmittance regulation recovery performance diagram for restoring the performance of an electrochromic device in Example 1.

[0031] from Figure 2 It can be seen that: in the initial state, the transmittance modulation amplitude of the device at 550nm is 48.8%, and after the cycle, the transmittance modulation amplitude is greatly reduced to 18.8%, and the optical modulation range of the device at 550nm is restored to 47.5%, which is only 1.3% lower than the initial state, and the recovery efficiency can reach 97%.

[0032] Example 2: A method for restoring the performance of an electrochromic device is accomplished by the following steps:

[0033] The electrochromic device is a fully solid electrochromic device, which is prepared on a glass substrate by vacuum evaporation coating. The upper and lower electrodes are indium tin oxide, the electrochromic layer is tungsten oxide, the electrolyte layer is tantalum oxide, the ion storage layer is nickel oxide, and the electrolyte ions are evaporated metallic lithium. The prepared electrochromic device shows performance degradation after cycling, and the attenuated electrochromic device is heat treated at 350°C for 2h.

[0034] Using the method of Example 2, the degraded electrochromic device recovered 95% of the initial performance.

[0035] Example 3: A method for restoring the performance of an electrochromic device is accomplished by the following steps:

[0036] The electrochromic device is a laminated electrochromic device, the electrochromic layer is tungsten oxide, the ion storage layer is nickel oxide, the substrate is ITO glass, and the electrolyte layer is a mixture of lithium perchlorate dissolved in propylene carbonate and ultraviolet curing glue. The prepared electrochromic device shows performance degradation after cycling, and the attenuated electrochromic device is heat-treated at 50°C for 50 minutes;

[0037] Using the method of Example 3, the degraded electrochromic device recovered 100% of the initial performance.

[0038] Example 4: A method for restoring the performance of an electrochromic device is accomplished by the following steps:

[0039] The electrochromic device is a liquid electrolyte electrochromic device, the electrochromic layer and the ion storage layer are both polyaniline, the substrate is a gold-plated porous film, the electrolyte layer is lithium perchlorate dissolved in propylene carbonate, and the prepared electrochromic device shows performance degradation after cycling. The attenuated electrochromic device is heat-treated at 50°C for 30 minutes;

[0040] Using the method of Example 4, the degraded electrochromic device recovered 98% of the initial performance.

Claims

1. A method for restoring the performance of an electrochromic device, characterized in that A method for restoring the performance of an electrochromic device is to use heat treatment to restore the performance of the electrochromic device with attenuated performance to its initial performance. The specific method is: placing the electrochromic device with attenuated performance in a tube furnace, a muffle furnace or an oven, and heat treating the electrochromic device with attenuated performance at 40° C. to 800° C. for 20 min to 300 min in air, argon or vacuum atmosphere; When the electrochromic device is a fully solid electrochromic device, it is prepared on a glass substrate by magnetron sputtering, the upper and lower electrodes are indium tin oxide, the electrochromic layer is tungsten oxide, the electrolyte layer is lithium tantalate, and the ion storage layer is nickel oxide. The prepared electrochromic device shows performance degradation after cycling, and the attenuated electrochromic device is heat treated at 300°C for 2h; When the electrochromic device is a fully solid electrochromic device, it is prepared on a glass substrate by vacuum evaporation coating, the upper and lower electrodes are indium tin oxide, the electrochromic layer is tungsten oxide, the electrolyte layer is tantalum oxide, the ion storage layer is nickel oxide, and the electrolyte ions are evaporated metallic lithium. The prepared electrochromic device shows performance degradation after cycling, and the attenuated electrochromic device is heat treated at 350°C for 2h; When the electrochromic device is a laminated electrochromic device, the electrochromic layer is tungsten oxide, the ion storage layer is nickel oxide, the substrate is ITO glass, and the electrolyte layer is a mixture of lithium perchlorate dissolved in propylene carbonate and ultraviolet curing glue, the prepared electrochromic device shows performance degradation after cycling, and the attenuated electrochromic device is heat-treated at 50°C for 50 minutes; When the electrochromic device is a liquid electrolyte electrochromic device, the electrochromic layer and the ion storage layer are both polyaniline, the substrate is a gold-plated porous membrane, and the electrolyte layer is lithium perchlorate dissolved in propylene carbonate. The prepared electrochromic device shows performance degradation after cycling, and the attenuated electrochromic device is heat treated at 50°C for 30 minutes.

Citation Information

Patent Citations

  • Electrochromic devices

    CN104364707A

  • Electrochromic glass automatic repairing method and system

    CN107065372A

  • Repairable inorganic full-film electrochromic device taking water vapor as electrolyte and preparation method thereof

    CN113204146A

  • Electrochromic devices having improved ion conducting layers

    US20070097481A1

  • System and method for detecting and repairing defects in an electrochromic device using thermal imaging

    US20150097944A1