A method for preparing porous Ni-Mn-Ga shape memory alloy
Through the preparation method of porous Ni-Mn-Ga alloy, the porosity and pore size are controlled by using NaCl porosity agent, the problems of twin motion resistance and low heat transfer efficiency of polycrystalline Ni-Mn-Ga alloy are solved, and high efficiency is achieved The magneto-thermal effect and cost reduction.
Patent Information
- Application Number
- CN202210718126.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-06-23
AI Technical Summary
In the polycrystal state, the existing Ni-Mn-Ga alloys have problems such as large twin motion resistance, low heat transfer efficiency, poor elastic and thermal magneto-thermal effect, high preparation cost and unstable tissue structure.
Using the Ni-Mn-Ga alloy preparation method with porous structure, NaCl is used as a pore-making agent to control porosity and pore size distribution, reduce the number of grain boundaries, and improve the material Specific surface area and heat transfer efficiency.
It effectively reduces the twin motion resistance, improves the heat transfer efficiency and elastic thermal magneto-thermal effect of porous alloys, reduces the preparation cost, and achieves the stability and adaptability of the material.
Smart Images

Figure CN115194152B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of shape memory effect, superelastic effect and elastocaloric effect alloys, and relates to a method for preparing a porous Ni-Mn-Ga shape memory alloy. Background Art
[0002] Ni-Mn-Ga alloy is an important alloy system in the field of metal functional materials. A large number of materials with practical value have been discovered in it, including magnetic shape memory alloys, semi-metals, topological insulators, etc., which makes the research of Ni-Mn-Ga alloy a hot topic. At present, researchers' research on Ni-Mn-Ga alloy is mainly focused on improving the thermal effect of materials under magnetic fields and force fields, improving the shape memory effect and superelastic effect of materials, and adjusting the temperature range of materials showing shape memory, superelastic effect, magnetocaloric effect and elastocaloric effect. The shape memory effect refers to the alloy being heated to the austenite transformation end temperature (A) after undergoing a certain amount of plastic deformation in the martensitic state. f ) above, the shape memory alloy returns to its shape before deformation. Superelasticity refers to when the thermoelastic martensite is above the phase transition temperature A f When the austenite phase appears above, stress-induced martensitic transformation will occur when external force is applied to it. When the stress is removed, the stress-induced martensite undergoes reverse transformation and completely returns to the parent phase. Magnetocaloric effect is the phenomenon that the temperature of ferromagnets or paramagnets changes with the change of magnetic field intensity during adiabatic process. Elastic caloric effect refers to the isothermal entropy change (ΔS) that occurs when uniaxial stress is applied or released in shape memory alloys. iso ) or adiabatic temperature change (ΔT ad ) phenomenon. Ni-Mn-Ga alloy has become one of the most promising choices for the new generation of solid magnetic refrigeration materials due to its high magnetocaloric effect and elastocaloric effect.
[0003] Currently, large strains of Ni-Mn-Ga alloys driven by temperature fields, force fields or magnetic fields are all obtained in single crystals (single-morph state).
[0004] The preparation process of single crystal Ni-Mn-Ga alloy is complicated, the production equipment is expensive, the production cost is high, and it is difficult to prepare large single crystal samples in industrial production.
[0005] Polycrystalline Ni-Mn-Ga alloy has the advantages of low production cost, simple process and wide application. However, in polycrystalline Ni-Mn-Ga alloy, the orientation distribution of martensitic twins is isotropic, which causes the twin stresses of the grains in the alloy to cancel each other out and cannot be released in the same macroscopic direction, resulting in the physical properties of polycrystalline materials being greatly reduced compared with single crystal materials.
[0006] Chinese patent CN108060330A discloses a method for preparing a Ni-Mn-Ga shape memory alloy by suppressing the γ phase ratio through powder sintering, wherein the powder sintering utilizes 57-59 parts of Ni powder, 25 parts of Mn powder and 16-18 parts of Ga powder instead of Ni-Mn-Ga alloy powder, and the prepared material is not a porous polycrystalline shape memory alloy.
[0007] Chinese patent CN103741003A discloses a novel high-temperature magnetic shape memory alloy and a preparation method thereof, wherein the preparation method is not powder sintering, but mixed melting and heat treatment of alloy single substance powder, and the prepared alloy is also not a porous polycrystalline shape memory alloy.
[0008] Chinese patent CN105316527A discloses a nickel-manganese-gallium superelastic shape memory alloy wire and a preparation method thereof, wherein the preparation method is not powder sintering, but a glass-coated spinning method is used to prepare two-dimensional shape memory alloy microwires.
[0009] In summary, the existing preparation methods of Ni-Mn-Ga shape memory alloys include smelting preparation, powder sintering and glass-coated spinning. Among them, the polycrystalline shape memory alloys prepared by smelting preparation and powder sintering have the problems of a large number of grain boundaries in the alloy and large obstacles to the movement of martensitic twins in the grains. At the same time, there are many problems such as the adaptability of elastic-caloric and magnetocaloric effects in engineering applications. In the above-mentioned patents, the alloy powder in powder metallurgy is a mixture of single metal powders of constituent components, and the raw material selection in smelting preparation is also single powder. The glass-coated spinning method can only produce two-dimensional shape memory alloy microwires, and it is impossible to produce bulk shape memory alloys. Summary of the invention
[0010] The technical problem to be solved by the present invention is how to overcome the large resistance to twin movement during the twin movement of polycrystalline Ni-Mn-Ga alloys in the prior art, the low internal and external heat exchange efficiency between the porous alloy and the heat transfer medium, the poor elastic-caloric and magnetocaloric effects, the high cost of preparing alloy powder, the difficulty in preparing porous materials of polycrystalline Ni-Mn-Ga alloys to match the solutions to the above-mentioned problems, and the unstable organizational structure and performance.
[0011] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0012] A method for preparing a porous Ni-Mn-Ga shape memory alloy, the method comprising the following steps:
[0013] S1, weighing raw alloy powder of porous Ni-Mn-Ga shape memory alloy and pore-forming agent according to a ratio, ball milling and mixing, and drying to obtain mixed alloy powder;
[0014] S2, pressing the mixed alloy powder in step S1 into a compact to obtain a green compact;
[0015] S3, sintering the compact in step S2 under vacuum conditions to obtain a sintered compact;
[0016] S4, furnace cooling and quenching the sintered blank in step S3 to obtain a primary porous Ni-Mn-Ga shape memory alloy;
[0017] S5. Ultrasonic treatment is performed on the primary porous Ni—Mn—Ga shape memory alloy in step S4, and the alloy is dried to obtain an ultimate porous Ni—Mn—Ga shape memory alloy.
[0018] Preferably, the raw alloy powder of the porous Ni—Mn—Ga shape memory alloy in step S1 is firstly obtained by smelting the raw materials to obtain a Ni—Mn—Ga alloy ingot, and then grinding the Ni—Mn—Ga alloy ingot into powder.
[0019] Preferably, the raw alloy powder of the porous Ni-Mn-Ga shape memory alloy in step S1 needs to be mechanically ground and pulverized by a grinding machine on a Ni-Mn-Ga alloy ingot, and the Ni-Mn-Ga alloy powder is sieved to a target particle size grade that matches the NaCl powder particle size grade using standard sieves of different models.
[0020] Preferably, the raw materials in step S1 are melted in a non-consumable vacuum arc melting furnace, and ground into powder using a vibration mill.
[0021] Preferably, the Ni—Mn—Ga alloy ingot in step S1 is subjected to heat treatment and quenching treatment before being ground into powder.
[0022] Preferably, the heat treatment in step S1 is a homogenization heat treatment at 900° C. for 24 hours.
[0023] Preferably, the smelting raw materials in step S1 are Ni-Mn master alloy with a purity of 99.9%, 99.99% Ni, 99.99% Ga and other added elements with a purity not less than 99.9%.
[0024] Preferably, when preparing the ingredients in step S1, 5% of Mn element needs to be additionally added in the ingredient ratio as compensation.
[0025] Preferably, before the raw material is smelted in step S1, a mechanical pump and a molecular pump are used to evacuate the furnace to a vacuum degree of 5×10 -3 Pa, and then filled with high-purity argon gas to 2×10 -2 Pa, and then start smelting.
[0026] Preferably, in the raw material smelting in step S1, in order to make the ingot composition uniform, each sample is turned over and smelted four times during the smelting process and magnetically stirred.
[0027] Preferably, the Ni-Mn-Ga alloy ingot in step S1 has a composition of NixMnyGa(100-xyz)Rz(x=50-55, y=25-30, z=0-4), wherein R is the fourth element, such as Ti, Fe, Cu, Co, In, Sn, etc.
[0028] Preferably, the pore-forming agent in step S1 is NaCl powder.
[0029] Preferably, the NaCl powder in step S1 is sieved using different types of standard sieving sieves to obtain different powder particle sizes, such as 20-30 μm, 50-70 μm, 100-120 μm, etc.
[0030] Preferably, the raw alloy powder of the porous Ni—Mn—Ga shape memory alloy in step S1 is mixed with a mass ratio of Ni—Mn—Ga alloy powder to NaCl powder calculated according to the target porosity.
[0031] Preferably, the raw alloy powder of the porous Ni-Mn-Ga shape memory alloy in step S1 and the pore former NaCl powder have a particle size equivalent to the pore size of the target porous shape memory alloy, and the particle size of the Ni-Mn-Ga alloy powder does not exceed the particle size of the NaCl powder.
[0032] Preferably, the ball milling mixing in step S1 has a ball milling time of more than 5 hours and a rotation speed of 100-200 r / min.
[0033] Preferably, in the ball milling mixing in step S1, the ball-to-material ratio is 1:1-1:2, the material of the grinding balls is agate balls, and 1-2 ml of anhydrous ethanol is added for every 10 g of mixed powder.
[0034] Preferably, the mixed alloy powder in step S1 is dried at a temperature of 40-60° C. for 30-60 min.
[0035] Preferably, the mixed alloy powder in step S2 is compacted, the compacting pressure is not less than 100 MPa, and the holding time is 1-3 min.
[0036] Preferably, during the sintering process in step S3, the material is first heated from room temperature to 700-780°C and kept for 1-2 hours at a heating rate of 5-15°C / min, and then heated to 1100-1150°C and sintered for 2-3 hours at a heating rate of 5-15°C / min.
[0037] Preferably, the sintering in step S3 is performed by sequentially using a mechanical pump and a diffusion pump to evacuate the air, and the diffusion pump is kept working during the sintering process to make the vacuum degree in the quartz tube reach 5×10 -4 Pa.
[0038] Preferably, the furnace cooling and quenching treatment in step S4 is performed by cooling the furnace to 600-800° C. and then quenching.
[0039] Preferably, in the quenching treatment in step S4, the quenching liquid is water at 0-10°C.
[0040] Preferably, in the ultrasonic treatment in step S5, the primary porous Ni-Mn-Ga shape memory alloy is placed in a beaker filled with deionized water, and the beaker is placed in an ultrasonic cleaning machine for 0.3-0.8h to remove the residual NaCl on the surface and in the pores of the primary porous Ni-Mn-Ga shape memory alloy.
[0041] Preferably, the drying in step S5 is carried out at a temperature of 40-60° C. and for a time of 30-60 min.
[0042] Preferably, the porosity of the ultimate porous Ni-Mn-Ga shape memory alloy in step S5 is 30-60%; 50 Mn 30 Ga 20 The porous alloy has a recoverable strain of 8-11% at 100°C and 12MPa, and its superelastic effect recovery rate is 85-99%. 50 Mn 30 Ga 20-x Ti x The (x=1,2,3) porous alloy has a 2-5% recoverable strain upon heating at room temperature and a pressure of 23-45MPa, and its shape memory effect recovery rate is 85-98%.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] In the above scheme, the present invention proposes a method for preparing a Ni-Mn-Ga alloy with a porous structure, in order to reduce the resistance of twin movement during the twin movement of polycrystalline Ni-Mn-Ga alloy. And due to the introduction of the pore structure, on the one hand, the increase in the specific surface area of the material can improve the internal and external heat exchange efficiency between the porous alloy and the heat transfer medium, and on the other hand, the gap will be conducive to the transportation of the heat transfer medium, thereby improving the adaptability of the Ni-Mn-Ga alloy material in the elastic-caloric and magnetocaloric effects in engineering applications.
[0045] The porous structure of the present invention can effectively reduce the number of grain boundaries in the alloy, thereby reducing the obstacles to the movement of martensitic twins in the grains and improving the deformation and temperature change capabilities of the material when the temperature field, magnetic field or force field changes.
[0046] The porous Ni-Mn-Ga polycrystalline alloy prepared by the present invention has mostly pore structures, and the structure is uniform and stable, and the porosity and pore size distribution can be controlled by the volume fraction and particle size distribution of the pore former. The pores of the prepared porous alloy are mostly through holes, and the pore size of the through holes distributed between the metal skeletons is determined by the particle size of the pore former NaCl powder in the mixed powder, and a small part of the closed pores formed during the sintering process are distributed on the metal skeleton. Therefore, the pore size distribution, porosity, and pore shape of the prepared porous alloy can be controlled by adjusting the powder particle size distribution, mass ratio, and shape of the NaCl powder.
[0047] The pore size of the porous Ni-Mn-Ga shape memory alloy prepared by the preparation method of the present invention increases with the increase of the size of the added NaCl particles, the porosity increases with the increase of the added NaCl volume, and the pore shape is determined by the shape of the NaCl particles. Therefore, the pore size distribution, porosity, and pore shape of the prepared porous alloy can be controlled by adjusting the powder particle size, mass ratio, and shape of the NaCl powder. At the same time, the superelasticity and shape memory effect of the porous Ni-Mn-Ga shape memory alloy prepared by the present invention are improved with the increase of the powder pressing pressure and the holding time.
[0048] The present invention adopts NaCl as a pore-forming agent to prepare a porous Ni-Mn-Ga shape memory alloy. NaCl has the following advantages over other types of pore-forming agents: NaCl is a neutral reagent and will not corrode the alloy; NaCl is easy to remove and can be directly dissolved in water without pollution; NaCl has a high hardness and is not easily deformed during the pressing process, and can well maintain the pore structure.
[0049] In the preparation method of the present invention, the sintering process of the porous Ni-Mn-Ga shape memory alloy is first subjected to a low-temperature heat treatment at 700-780°C to order the alloy. As the vacuum system is continuously evacuated, most of the NaCl pore-forming agent is directly volatilized from the pores under the high-temperature heat treatment at 1100-1150°C, and the NaCl remaining in the pores can be dissolved by water infiltration and ultrasonic treatment.
[0050] The ultimate porous Ni-Mn-Ga shape memory alloy prepared by the present invention has a porosity of 30-60%. 50 Mn 30 Ga 20 The porous alloy has a recoverable strain of 8-11% at 100°C and 12MPa, and its superelastic effect recovery rate is 85-99%. 50Mn 30 Ga 20-x Ti x The (x=1,2,3) porous alloy has a 2-5% recoverable strain upon heating at room temperature and a pressure of 23-45MPa, and its shape memory effect recovery rate is 85-98%.
[0051] The overall preparation process of the present invention is simple, the production efficiency is high, the product quality is high, the product added value is high, the secondary pollution is low, the process is short and the cost is low. The prepared memory alloy has small resistance to twin movement during twin movement, the internal and external heat exchange efficiency between the porous alloy and the heat transfer medium is high, the elastic-caloric and magnetocaloric effects are good, the preparation cost of the alloy powder is low, and the preparation of polycrystalline Ni-Mn-Ga alloy porous materials can be well matched with the above-mentioned technical effects, the organizational structure and performance are stable, and it is suitable for large-scale industrial production and promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0053] Figure 1 A schematic diagram of a vacuum sintering system for a porous Ni-Mn-Ga shape memory alloy prepared in accordance with a specific embodiment of the present invention;
[0054] Figure 2 This is a physical picture of the porous Ni-Mn-Ga shape memory alloy prepared in Example 1 of the present invention;
[0055] Figure 3 This is a SEM microscopic morphology image of the porous Ni-Mn-Ga shape memory alloy prepared in Example 1 of the present invention;
[0056] Figure 4 This is a SEM microscopic morphology image of the porous Ni-Mn-Ga shape memory alloy prepared in Example 2 of the present invention;
[0057] Figure 5 The XRD spectrum of the porous Ni-Mn-Ga shape memory alloy prepared in Example 1 of the present invention;
[0058] Figure 6 The DSC spectrum of the porous Ni-Mn-Ga shape memory alloy prepared in Example 1 of the present invention;
[0059] Figure 7 This is the stress-strain curve of the porous Ni—Mn—Ga shape memory alloy prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0060] The following will describe the technical solutions and technical problems solved in the embodiments of the present invention in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them.
[0061] The following examples are described by Figure 1 The sintering system in the schematic diagram of the vacuum sintering system of the porous Ni-Mn-Ga shape memory alloy is used to sinter and prepare the porous Ni-Mn-Ga shape memory alloy.
[0062] Example 1
[0063] Porous Ni 50 Mn 30 Ga 20 A method for preparing a (at.%) shape memory alloy, the method comprising the following steps:
[0064] S1. Using 99.9% pure Ni-Mn master alloy, 99.99% Ni, and 99.99% Ga as raw materials, a non-consumable vacuum arc melting furnace is used to melt the ingot. Due to the strong volatility of Mn element, an additional 5% Mn element needs to be added to the ingredient ratio as compensation. Before melting, the vacuum degree in the furnace is adjusted to 5×10 -3 Pa, and then filled with high-purity argon gas to 2×10 -2 Pa, and then began to melt; in order to make the ingot composition uniform, each sample was turned over and melted four times during the melting process and magnetic stirring was performed, and finally button-shaped Ni 50 Mn 30 Ga 20 Alloy ingot; the prepared Ni 50 Mn 30 Ga 20 The alloy ingot was sealed in a quartz test tube filled with argon and heat treated at 900°C for 24 h, followed by quenching.
[0065] Use NaCl analytical pure powder as pore-forming agent, grind NaCl in a grinding mortar. Use different types of standard sample sieves to sieve NaCl powder into 20-30μm powder particle size; 50 Mn 30 Ga 20 The shape memory alloy ingot was mechanically ground and pulverized using a grinding machine, and Ni 50 Mn 30 Ga 20 The alloy powder was sieved to a target particle size of 20-30 μm matching the particle size of the NaCl powder;
[0066] Ni 50 Mn 30 Ga 20 The alloy powder and the pore-forming agent NaCl powder were weighed according to the atomic ratio and put into the alloy ball mill, and 10g of agate grinding balls and 1ml of anhydrous ethanol were added to every 10g of the mixed powder. The ball mill was then put into a planetary ball mill for mixing the powders; the mixing time was 5h and the speed was 150r / min; the mixed powder was put into a drying oven and dried for 30min to remove the anhydrous ethanol to obtain a mixed alloy powder;
[0067] S2, putting the mixed alloy powder in step S1 into an alloy mold, placing the mold into a vertical compressor for powder compacting, the compacting pressure is 100 MPa, and taking out after holding the pressure for 1 min to obtain a compact;
[0068] S3, placing the compact in step S2 into a quartz tube with one end sealed, and evacuating the other end with a mechanical pump and a vacuum diffusion pump in turn; the vacuum degree in the quartz tube can reach 5×10 -4 Pa, and the diffusion pump is constantly evacuating during the sintering process to ensure a constant vacuum degree in the quartz tube;
[0069] Put the end of the quartz tube with the sample into the heating section of the heating furnace, add a water bath cooling system between the quartz tube and the vacuum system to cool the quartz tube, so that the Mn and NaCl volatilized by the sample during the heating process are solidified in the quartz tube, and ensure that the volatilized components during the heating process will not enter the vacuum system; during the sintering process, first heat from room temperature to 780℃ and keep it for 1h, the heating rate is 10℃ / min, and then heat to 1100℃ and sinter for 2h, the heating rate is 10℃ / min, and a sintered blank is obtained;
[0070] S4, cooling the sintered billet in step S3 to 600°C, and then spraying the quartz tube sample for 0.5h, and taking out the sample after it is completely cooled to obtain the primary porous Ni 50 Mn 30 Ga 20 Shape memory alloys;
[0071] S5, the primary porous Ni in step S4 50 Mn 30 Ga 20 The shape memory alloy was placed in a beaker filled with deionized water, and the beaker was placed in an ultrasonic cleaner for 0.3 h to remove the residual NaCl in the sample; the sample was then placed in a drying oven and dried at 40°C for 60 min to obtain the following: Figure 2 The ultimate porous Ni 50 Mn 30 Ga20 Shape memory alloy.
[0072] like Figure 3 and 5 As shown, a porous Ni with a porosity of 42% was obtained. 50 Mn 30 Ga 20 Polycrystalline shape memory alloy. The actual porosity is measured by relative density function method. Figure 6 As shown, the porous Ni prepared in this embodiment 50 Mn 30 Ga 20 The polycrystalline alloy can produce a recoverable strain of 10.6% at 100°C and a pressure of 12MPa, and has a superelastic effect with a recovery rate of 99.34%.
[0073] Example 2
[0074] Porous Ni 50 Mn 30 Ga 20 A method for preparing a (at.%) shape memory alloy, the method comprising the following steps:
[0075] S1. Using 99.9% pure Ni-Mn master alloy, 99.99% Ni, and 99.99% Ga as raw materials, a non-consumable vacuum arc melting furnace is used to melt the ingot. Due to the strong volatility of Mn element, an additional 5% Mn element needs to be added to the ingredient ratio as compensation. Before melting, the vacuum degree in the furnace is adjusted to 5×10 -3 Pa, and then filled with high-purity argon gas to 2×10 -2 Pa, and then began to melt; in order to make the ingot composition uniform, each sample was turned over and melted four times during the melting process and magnetic stirring was performed, and finally button-shaped Ni 50 Mn 30 Ga 20 Alloy ingot; the prepared Ni 50 Mn 30 Ga 20 The alloy ingot was sealed in a quartz test tube filled with argon and heat treated at 900°C for 24 h, followed by quenching.
[0076] Use NaCl analytical pure powder as pore-forming agent, grind NaCl in a grinding mortar. Use different types of standard sample sieves to sieve NaCl powder into 50-70μm powder particle size; 50 Mn 30 Ga 20 The shape memory alloy ingot was mechanically ground and pulverized using a grinding machine, and Ni50 Mn 30 Ga 20 The alloy powder was sieved to a target particle size of 20-30 μm matching the particle size of the NaCl powder;
[0077] Ni 50 Mn 30 Ga 20 The alloy powder and the pore-forming agent NaCl powder were weighed according to the atomic ratio and put into the alloy ball mill, and 10g of agate grinding balls and 1ml of anhydrous ethanol were added to every 10g of the mixed powder. The ball mill was then put into a planetary ball mill for mixing the powders; the mixing time was 5h and the speed was 150r / min; the mixed powder was put into a drying oven and dried for 30min to remove the anhydrous ethanol to obtain a mixed alloy powder;
[0078] S2, putting the mixed alloy powder in step S1 into an alloy mold, placing the mold into a vertical compressor for powder compacting, the compacting pressure is 150 MPa, and taking out after holding the pressure for 1 min to obtain a compact;
[0079] S3, placing the compact in step S2 into a quartz tube with one end sealed, and evacuating the other end with a mechanical pump and a vacuum diffusion pump in turn; the vacuum degree in the quartz tube can reach 5×10 -4 Pa, and the diffusion pump is constantly evacuating during the sintering process to ensure a constant vacuum degree in the quartz tube;
[0080] The end of the quartz tube with the sample is placed in the heating section of the heating furnace, and a water bath cooling system is added between the quartz tube and the vacuum system to cool the quartz tube, so that the Mn and NaCl volatilized by the sample during the heating process are solidified in the quartz tube, and it is ensured that the volatilized components during the heating process will not enter the vacuum system; during the sintering process, it is first heated from room temperature to 780℃ and kept for 1h, the heating rate is 15℃ / min, and then heated to 1100℃ and sintered for 2h, the heating rate is 15℃ / min, and a sintered blank is obtained;
[0081] S4, cooling the sintered billet in step S3 to 600°C, and then spraying the quartz tube sample for 0.5h, and taking out the sample after it is completely cooled to obtain the primary porous Ni 50 Mn 30 Ga 20 Shape memory alloys;
[0082] S5, the primary porous Ni in step S4 50 Mn 30 Ga 20The shape memory alloy was placed in a beaker filled with deionized water, and the beaker was placed in an ultrasonic cleaner for 0.3 h to remove the residual NaCl in the sample; the sample was then placed in a drying oven and dried at 50 ° C for 40 min to obtain the ultimate porous Ni 50 Mn 30 Ga 20 Shape memory alloy.
[0083] like Figure 4 As shown in Figure 2, a porous Ni with a porosity of 48% was obtained. 50 Mn 30 Ga 20 Polycrystalline shape memory alloy. The actual porosity is measured by relative density function method. 50 Mn 30 Ga 20 The polycrystalline alloy can produce 8.17% recoverable strain at 100°C and 12MPa pressure, and has a superelastic effect with a recovery rate of 88.6%.
[0084] Example 3
[0085] Porous Ni 50 Mn 30 Ga 20 A method for preparing a (at.%) shape memory alloy, the method comprising the following steps:
[0086] S1. Using 99.9% pure Ni-Mn master alloy, 99.99% Ni, and 99.99% Ga as raw materials, a non-consumable vacuum arc melting furnace is used to melt the ingot. Due to the strong volatility of Mn element, an additional 5% Mn element needs to be added to the ingredient ratio as compensation. Before melting, the vacuum degree in the furnace is adjusted to 5×10 -3 Pa, and then filled with high-purity argon gas to 2×10 -2 Pa, and then began to melt; in order to make the ingot composition uniform, each sample was turned over and melted four times during the melting process and magnetic stirring was performed, and finally button-shaped Ni 50 Mn 30 Ga 20 Alloy ingot; the prepared Ni 50 Mn 30 Ga 20 The alloy ingot was sealed in a quartz test tube filled with argon and heat treated at 900°C for 24 h, followed by quenching.
[0087] Use NaCl analytical pure powder as pore-forming agent, grind NaCl in a grinding mortar. Use different types of standard sample sieves to sieve NaCl powder into powder particles of 110-120μm; 50 Mn 30 Ga 20 The shape memory alloy ingot was mechanically ground and pulverized using a grinding machine, and Ni 50 Mn 30 Ga 20 The alloy powder was sieved to a target particle size of 20-30 μm matching the particle size of the NaCl powder;
[0088] Ni 50 Mn 30 Ga 20 The alloy powder and the pore-forming agent NaCl powder were weighed according to the atomic ratio and put into the alloy ball mill, and 10g of agate grinding balls and 1ml of anhydrous ethanol were added to every 10g of the mixed powder. The ball mill was then put into a planetary ball mill for mixing the powders; the mixing time was 5h and the speed was 150r / min; the mixed powder was put into a drying oven and dried for 30min to remove the anhydrous ethanol to obtain a mixed alloy powder;
[0089] S2, putting the mixed alloy powder in step S1 into an alloy mold, placing the mold into a vertical compressor for powder compacting, the compacting pressure is 150 MPa, and the compact is taken out after holding the pressure for 2 minutes to obtain a compact;
[0090] S3, placing the compact in step S2 into a quartz tube with one end sealed, and evacuating the other end with a mechanical pump and a vacuum diffusion pump in turn; the vacuum degree in the quartz tube can reach 5×10 -4 Pa, and the diffusion pump is constantly evacuating during the sintering process to ensure a constant vacuum degree in the quartz tube;
[0091] Put the end of the quartz tube with the sample into the heating section of the heating furnace, add a water bath cooling system between the quartz tube and the vacuum system to cool the quartz tube, so that the Mn and NaCl volatilized by the sample during the heating process are solidified in the quartz tube, and ensure that the volatilized components during the heating process will not enter the vacuum system; during the sintering process, first heat from room temperature to 780℃ and keep it for 1h, the heating rate is 10℃ / min, and then heat to 1100℃ and sinter for 2h, the heating rate is 10℃ / min, and a sintered blank is obtained;
[0092] S4, cooling the sintered billet in step S3 to 600°C, and then spraying the quartz tube sample for 0.5h, and taking out the sample after it is completely cooled to obtain the primary porous Ni 50 Mn 30 Ga 20 Shape memory alloys;
[0093] S5, the primary porous Ni in step S4 50 Mn 30 Ga 20 The shape memory alloy was placed in a beaker filled with deionized water, and the beaker was placed in an ultrasonic cleaner for 0.5 h to remove the residual NaCl in the sample; then the sample was placed in a drying oven and dried at 50 ° C for 40 min to obtain the ultimate porous Ni 50 Mn 30 Ga 20 Shape memory alloy.
[0094] The porous Ni with a porosity of 49% was obtained. 50 Mn 30 Ga 20 Polycrystalline shape memory alloy. The actual porosity is measured by relative density function method. Figure 7 As shown, the porous Ni prepared in this embodiment 50 Mn 30 Ga 20 The polycrystalline alloy can produce a recoverable strain of 10.53% at 100°C and a pressure of 12MPa, and has a superelastic effect with a recovery rate of 99.24%.
[0095] Example 4
[0096] Porous Ni 50 Mn 30 Ga 19 Ti 1 A method for preparing a (at.%) shape memory alloy, the method comprising the following steps:
[0097] S1. Using 99.9% pure Ni-Mn master alloy, 99.99% Ni, 99.99% Ga and 99.9% pure Ti as raw materials, a non-consumable vacuum arc melting furnace is used to melt the ingot. Due to the strong volatility of Mn element, an additional 5% Mn element needs to be added to the ingredient ratio as compensation. Before smelting, the vacuum degree in the furnace is adjusted to 5×10 -3 Pa, and then filled with high-purity argon gas to 2×10 -2 Pa, and then began to melt; in order to make the ingot composition uniform, each sample was turned over and melted four times during the melting process and magnetic stirring was performed, and finally button-shaped Ni 50 Mn 30 Ga 19 Ti 1 Alloy ingot; the prepared Ni 50 Mn 30 Ga 19 Ti1 The alloy ingot was sealed in a quartz test tube filled with argon and heat treated at 900°C for 24 h, followed by quenching.
[0098] Use NaCl analytical pure powder as pore-forming agent, grind NaCl in a grinding mortar. Use different types of standard sample sieves to sieve NaCl powder into 20-30μm powder particle size; 50 Mn 30 Ga 20 The shape memory alloy ingot was mechanically ground and pulverized using a grinding machine, and Ni 50 Mn 30 Ga 20 The alloy powder was sieved to a target particle size of 20-30 μm matching the particle size of the NaCl powder;
[0099] Ni 50 Mn 30 Ga 20 The alloy powder and the pore-forming agent NaCl powder were weighed according to the atomic ratio and put into the alloy ball mill, and 10g of agate grinding balls and 1ml of anhydrous ethanol were added to every 10g of the mixed powder. The ball mill was then put into a planetary ball mill for mixing the powders; the mixing time was 5h and the speed was 150r / min; the mixed powder was put into a drying oven and dried for 30min to remove the anhydrous ethanol to obtain a mixed alloy powder;
[0100] S2, putting the mixed alloy powder in step S1 into an alloy mold, placing the mold into a vertical compressor for powder compacting, the compacting pressure is 100 MPa, and taking out after holding the pressure for 1 min to obtain a compact;
[0101] S3, placing the compact in step S2 into a quartz tube with one end sealed, and evacuating the other end with a mechanical pump and a vacuum diffusion pump in turn; the vacuum degree in the quartz tube can reach 5×10 -4 Pa, and the diffusion pump is constantly evacuating during the sintering process to ensure a constant vacuum degree in the quartz tube;
[0102] The end of the quartz tube with the sample is placed in the heating section of the heating furnace, and a water bath cooling system is added between the quartz tube and the vacuum system to cool the quartz tube, so that the Mn and NaCl volatilized by the sample during the heating process are solidified in the quartz tube, and it is ensured that the volatilized components during the heating process will not enter the vacuum system; during the sintering process, it is first heated from room temperature to 780℃ and kept for 1h, the heating rate is 15℃ / min, and then heated to 1100℃ and sintered for 2h, the heating rate is 15℃ / min, and a sintered blank is obtained;
[0103] S4, cooling the sintered billet in step S3 to 600°C, and then spraying the quartz tube sample for 0.5h, and taking out the sample after it is completely cooled to obtain the primary porous Ni 50 Mn 30 Ga 20 Shape memory alloys;
[0104] S5, the primary porous Ni in step S4 50 Mn 30 Ga 20 The shape memory alloy was placed in a beaker filled with deionized water, and the beaker was placed in an ultrasonic cleaner for 0.3 h to remove the residual NaCl in the sample; the sample was then placed in a drying oven and dried at 40 ° C for 40 min to obtain the ultimate porous Ni 50 Mn 30 Ga 20 Shape memory alloy.
[0105] The porous Ni with a porosity of 46% was obtained. 50 Mn 30 Ga 19 Ti 1 Polycrystalline shape memory alloy. The actual porosity is measured by relative density function method. 50 Mn 30 Ga 19 Ti 1 The polycrystalline alloy can produce a strain of 2.5% at 200°C and a pressure of 23MPa, and has a shape memory effect with a recovery rate of 93.41% after being kept at 200°C for 10 minutes.
[0106] Example 5
[0107] Porous Ni 50 Mn 30 Ga 18 Ti 2 A method for preparing a (at.%) shape memory alloy, the method comprising the following steps:
[0108] S1. Using 99.9% pure Ni-Mn master alloy, 99.99% Ni, 99.99% Ga and 99.9% pure Ti as raw materials, a non-consumable vacuum arc melting furnace is used to melt the ingot. Due to the strong volatility of Mn element, an additional 5% Mn element needs to be added to the ingredient ratio as compensation. Before smelting, the vacuum degree in the furnace is adjusted to 5×10 -3 Pa, and then filled with high-purity argon gas to 2×10 -2Pa, and then began to melt; in order to make the ingot composition uniform, each sample was turned over and melted four times during the melting process and magnetic stirring was performed, and finally button-shaped Ni 50 Mn 30 Ga 18 Ti 2 Alloy ingot; the prepared Ni 50 Mn 30 Ga 18 Ti 2 The alloy ingot was sealed in a quartz test tube filled with argon and heat treated at 900℃ for 24h, followed by quenching. NaCl analytical pure powder was used as a pore-forming agent and ground in a grinding mortar. Different types of standard sample sieves were used to sieve the NaCl powder into a powder particle size of 20-30μm. The quenched Ni 50 Mn 30 Ga 18 Ti 2 The shape memory alloy ingot was mechanically ground and pulverized using a grinding machine, and Ni 50 Mn 30 Ga 18 Ti 2 The alloy powder was sieved to the target particle size of 20-30 μm, which matched the particle size of NaCl powder. 50 Mn 30 Ga 18 Ti 2 The alloy powder and the pore-forming agent NaCl powder were weighed according to the atomic ratio and put into the alloy ball mill, and 10g of agate grinding balls and 1ml of anhydrous ethanol were added to every 10g of the mixed powder. The ball mill was then placed in a planetary ball mill for mixing the powders; the mixing time was 6h and the speed was 200r / min; the mixed powder was placed in a drying oven and dried for 30min to remove the anhydrous ethanol, thereby obtaining a mixed alloy powder;
[0109] S2, putting the mixed alloy powder in step S1 into an alloy mold, placing the mold into a vertical compressor for powder compacting, the compacting pressure is 100 MPa, and taking out after holding the pressure for 1 min to obtain a compact;
[0110] S3, placing the compact in step S2 into a quartz tube with one end sealed, and evacuating the other end with a mechanical pump and a vacuum diffusion pump in turn; the vacuum degree in the quartz tube can reach 5×10 -4Pa, and the diffusion pump is always evacuating during the sintering process to ensure that the vacuum degree in the quartz tube is constant; the end of the quartz tube with the sample is placed in the heating section of the heating furnace, and a water bath cooling system is added between the quartz tube and the vacuum system to cool the quartz tube, so that the Mn and NaCl volatilized from the sample during the heating process are solidified in the quartz tube, ensuring that the volatilized components during the heating process will not enter the vacuum system; during the sintering process, it is first heated from room temperature to 780℃ for 1h, the heating rate is 10℃ / min, and then heated to 1100℃ for sintering for 2h, the heating rate is 10℃ / min, and a sintered blank is obtained;
[0111] S4, cooling the sintered billet in step S3 to 800°C, and then spraying the quartz tube sample for 0.5h, and taking out the sample after it is completely cooled to obtain the primary porous Ni 50 Mn 30 Ga 18 Ti 2 Shape memory alloys;
[0112] S5, the primary porous Ni in step S4 50 Mn 30 Ga 18 Ti 2 The shape memory alloy was placed in a beaker filled with deionized water, and the beaker was placed in an ultrasonic cleaner for 1 hour to remove the residual NaCl in the sample; then the sample was placed in a drying oven and dried at 40°C for 60 minutes to obtain the ultimate porous Ni 50 Mn 30 Ga 18 Ti 2 Shape memory alloy.
[0113] The porous Ni with a porosity of 42% was obtained. 50 Mn 30 Ga 18 Ti 2 Polycrystalline shape memory alloy. The actual porosity is measured by relative density function method. 50 Mn 30 Ga 18 Ti 2 The polycrystalline alloy can produce a strain of 4.5% under a pressure of 42MPa at room temperature, and has a shape memory effect with a recovery rate of 90.22% after being kept at 200°C for 10 minutes.
[0114] Example 6
[0115] Porous Ni 50 Mn 30 Ga 17 Ti 3A method for preparing a (at.%) shape memory alloy, the method comprising the following steps:
[0116] S1. Using 99.9% pure Ni-Mn master alloy, 99.99% Ni, 99.99% Ga and 99.9% pure Ti as raw materials, a non-consumable vacuum arc melting furnace is used to melt the ingot. Due to the strong volatility of Mn element, an additional 5% Mn element needs to be added to the ingredient ratio as compensation. Before smelting, the vacuum degree in the furnace is adjusted to 5×10 -3 Pa, and then filled with high-purity argon gas to 2×10 -2 Pa, and then began to melt; in order to make the ingot composition uniform, each sample was turned over and melted four times during the melting process and magnetic stirring was performed, and finally button-shaped Ni 50 Mn 30 Ga 17 Ti 3 Alloy ingot; the prepared Ni 50 Mn 30 Ga 17 Ti 3 The alloy ingot was sealed in a quartz test tube filled with argon and heat treated at 900°C for 24 h, followed by quenching.
[0117] Use NaCl analytical pure powder as pore-forming agent, grind NaCl in a grinding mortar. Use different types of standard sample sieves to sieve NaCl powder into 20-30μm powder particle size; 50 Mn 30 Ga 17 Ti 3 The shape memory alloy ingot was mechanically ground and pulverized using a grinding machine, and Ni 50 Mn 30 Ga 17 Ti 3 The alloy powder was sieved to the target particle size of 20-30 μm, which matched the particle size of NaCl powder. 50 Mn 30 Ga 17 Ti 3 The alloy powder and the pore-forming agent NaCl powder were weighed according to the atomic ratio and put into the alloy ball mill, and 10g of agate grinding balls and 1ml of anhydrous ethanol were added to every 10g of the mixed powder. The ball mill was then placed in a planetary ball mill for mixing the powders; the mixing time was 6h and the speed was 200r / min; the mixed powder was placed in a drying oven and dried for 30min to remove the anhydrous ethanol, thereby obtaining a mixed alloy powder;
[0118] S2, putting the mixed alloy powder in step S1 into an alloy mold, placing the mold into a vertical compressor for powder compacting, the compacting pressure is 100 MPa, and taking out after holding the pressure for 2 minutes to obtain a compact;
[0119] S3, placing the compact in step S2 into a quartz tube with one end sealed, and evacuating the other end with a mechanical pump and a vacuum diffusion pump in turn; the vacuum degree in the quartz tube can reach 5×10 -4 Pa, and the diffusion pump is always evacuating during the sintering process to ensure that the vacuum degree in the quartz tube is constant; the end of the quartz tube with the sample is placed in the heating section of the heating furnace, and a water bath cooling system is added between the quartz tube and the vacuum system to cool the quartz tube, so that the Mn and NaCl volatilized from the sample during the heating process are solidified in the quartz tube, ensuring that the volatilized components during the heating process will not enter the vacuum system; during the sintering process, it is first heated from room temperature to 780℃ for 1h, the heating rate is 15℃ / min, and then heated to 1100℃ for sintering for 2h, the heating rate is 15℃ / min, and a sintered blank is obtained;
[0120] S4, cooling the sintered billet in step S3 to 800°C, and then spraying the quartz tube sample for 0.5h, and taking out the sample after it is completely cooled to obtain the primary porous Ni 50 Mn 30 Ga 17 Ti 3 Shape memory alloys;
[0121] S5, the primary porous Ni in step S4 50 Mn 30 Ga 17 Ti 3 The shape memory alloy was placed in a beaker filled with deionized water, and the beaker was placed in an ultrasonic cleaner for 0.5 h to remove the residual NaCl in the sample; the sample was then placed in a drying oven and dried at 40 ° C for 60 min to obtain the ultimate porous Ni 50 Mn 30 Ga 17 Ti 3 Shape memory alloy.
[0122] The porous Ni with a porosity of 49% was obtained. 50 Mn 30 Ga 17 Ti 3 Polycrystalline shape memory alloy. The actual porosity is measured by relative density function method. 50 Mn 30 Ga 17 Ti 3The polycrystalline alloy can produce a strain of 2.5% under a pressure of 45MPa at room temperature, and has a shape memory effect with a recovery rate of 98.22% after being kept at 200°C for 10 minutes.
[0123] In the above scheme, the present invention proposes a method for preparing a Ni-Mn-Ga alloy with a porous structure, in order to reduce the resistance of twin movement during the twin movement of polycrystalline Ni-Mn-Ga alloy. And due to the introduction of the pore structure, on the one hand, the increase in the specific surface area of the material can improve the internal and external heat exchange efficiency between the porous alloy and the heat transfer medium, and on the other hand, the gap will be conducive to the transportation of the heat transfer medium, thereby improving the adaptability of the Ni-Mn-Ga alloy material in the elastic-caloric and magnetocaloric effects in engineering applications.
[0124] The porous structure of the present invention can effectively reduce the number of grain boundaries in the alloy, thereby reducing the obstacles to the movement of martensitic twins in the grains and improving the deformation and temperature change capabilities of the material when the temperature field, magnetic field or force field changes.
[0125] The porous Ni-Mn-Ga polycrystalline alloy prepared by the present invention has mostly pore structures, and the structure is uniform and stable, and the porosity and pore size distribution can be controlled by the volume fraction and particle size distribution of the pore former. The pores of the prepared porous alloy are mostly through holes, and the pore size of the through holes distributed between the metal skeletons is determined by the particle size of the pore former NaCl powder in the mixed powder, and a small part of the closed pores formed during the sintering process are distributed on the metal skeleton. Therefore, the pore size distribution, porosity, and pore shape of the prepared porous alloy can be controlled by adjusting the powder particle size distribution, mass ratio, and shape of the NaCl powder.
[0126] The pore size of the porous Ni-Mn-Ga shape memory alloy prepared by the preparation method of the present invention increases with the increase of the size of the added NaCl particles, the porosity increases with the increase of the added NaCl volume, and the pore shape is determined by the shape of the NaCl particles. Therefore, the pore size distribution, porosity, and pore shape of the prepared porous alloy can be controlled by adjusting the powder particle size, mass ratio, and shape of the NaCl powder. At the same time, the superelasticity and shape memory effect of the porous Ni-Mn-Ga shape memory alloy prepared by the present invention are improved with the increase of the powder pressing pressure and the holding time.
[0127] The present invention adopts NaCl as a pore-forming agent to prepare a porous Ni-Mn-Ga shape memory alloy. NaCl has the following advantages over other types of pore-forming agents: NaCl is a neutral reagent and will not corrode the alloy; NaCl is easy to remove and can be directly dissolved in water without pollution; NaCl has a high hardness and is not easily deformed during the pressing process, and can well maintain the pore structure.
[0128] In the preparation method of the present invention, the sintering process of the porous Ni-Mn-Ga shape memory alloy is first subjected to a low-temperature heat treatment at 700-780°C to order the alloy. As the vacuum system is continuously evacuated, most of the NaCl pore-forming agent is directly volatilized from the pores under the high-temperature heat treatment at 1100-1150°C, and the NaCl remaining in the pores can be dissolved by water infiltration and ultrasonic treatment.
[0129] The ultimate porous Ni-Mn-Ga shape memory alloy prepared by the present invention has a porosity of 30-60%. 50 Mn 30 Ga 20 The porous alloy has a recoverable strain of 8-11% at 100°C and 12MPa, and its superelastic effect recovery rate is 85-99%. 50 Mn 30 Ga 20-x Ti x The (x=1,2,3) porous alloy has a 2-5% recoverable strain upon heating at room temperature and a pressure of 23-45MPa, and its shape memory effect recovery rate is 85-98%.
[0130] The overall preparation process of the present invention is simple, the production efficiency is high, the product quality is high, the product added value is high, the secondary pollution is low, the process is short and the cost is low. The prepared memory alloy has small resistance to twin movement during twin movement, the internal and external heat exchange efficiency between the porous alloy and the heat transfer medium is high, the elastic-caloric and magnetocaloric effects are good, the preparation cost of the alloy powder is low, and the preparation of polycrystalline Ni-Mn-Ga alloy porous materials can be well matched with the above-mentioned technical effects, the organizational structure and performance are stable, and it is suitable for large-scale industrial production and promotion.
[0131] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a porous Ni-Mn-Ga shape memory alloy, characterized in that: The method comprises the following steps: S1. The raw alloy powder of the porous Ni-Mn-Ga shape memory alloy and the pore-forming agent are weighed according to a ratio, ball-milled and mixed, and dried to obtain a mixed alloy powder; the pore-forming agent is NaCl powder; the Ni-Mn-Ga alloy ingot has a composition of NixMnyGa(100-xyz)Rz, x=50-55, y=25-30, z=0-4, wherein R is a fourth element selected from Ti, Fe, Cu, Co, In or Sn; S2, pressing the mixed alloy powder in step S1 into a compact to obtain a compact; S3, sintering the compact in step S2 under vacuum conditions to obtain a sintered compact; S4, furnace cooling and quenching the sintered blank in step S3, furnace cooling to 600-800° C. and then quenching to obtain a primary porous Ni-Mn-Ga shape memory alloy; S5, subjecting the primary porous Ni-Mn-Ga shape memory alloy in step S4 to ultrasonic treatment and drying to obtain an ultimate porous Ni-Mn-Ga shape memory alloy; The raw material alloy powder of the porous Ni-Mn-Ga shape memory alloy in step S1 is firstly smelted to obtain a Ni-Mn-Ga alloy ingot, and then the Ni-Mn-Ga alloy ingot is ground into powder; The porosity of the ultimate porous Ni-Mn-Ga shape memory alloy is 30-49%.
2. The method for preparing the porous Ni-Mn-Ga shape memory alloy according to claim 1, characterized in that: Prepared Ni 50 Mn 30 Ga 20 The porous alloy has a recoverable strain of 8-11% at 100°C and 12MPa, and its superelastic effect recovery rate is 85-99%. 50 Mn 30 Ga 20-x Ti x , x=1,2,3, the porous alloy undergoes a 2-5% heating recoverable strain at room temperature and a pressure of 23-45MPa, and its shape memory effect recovery rate is 85-98%.
3. The method for preparing the porous Ni-Mn-Ga shape memory alloy according to claim 1, characterized in that: The raw alloy powder of the porous Ni-Mn-Ga shape memory alloy in step S1 is mixed with the mass ratio of Ni-Mn-Ga alloy powder and NaCl powder calculated according to the target porosity.
4. The method for preparing the porous Ni-Mn-Ga shape memory alloy according to claim 2, characterized in that: The raw materials in step S1 are melted in a non-consumable vacuum arc melting furnace, and ground into powder using a vibration mill.
5. The method for preparing the porous Ni-Mn-Ga shape memory alloy according to claim 2, characterized in that: The Ni—Mn—Ga alloy ingot in step S1 is subjected to homogenization heat treatment before being ground into powder.
6. The method for preparing the porous Ni-Mn-Ga shape memory alloy according to claim 2, characterized in that: The ball milling mixing in step S1 has a ball milling time of more than 5 hours and a rotation speed of 100-200 r / min.
7. The method for preparing the porous Ni-Mn-Ga shape memory alloy according to claim 1, characterized in that: In the pressing process in step S2, the pressing pressure is not less than 100 MPa, and the holding time is 1-3 min.
8. The method for preparing the porous Ni-Mn-Ga shape memory alloy according to claim 1, characterized in that: The sintering in step S3 is firstly heated from room temperature to 700-780° C. and kept at this temperature for 1-2 hours, and then heated to 1100-1150° C. and sintered for 2-3 hours.
9. The method for preparing the porous Ni-Mn-Ga shape memory alloy according to claim 1, characterized in that: The sintering in step S3 is performed by using a mechanical pump and a diffusion pump to evacuate the quartz tube in turn, and the diffusion pump is kept working during the sintering process to make the vacuum degree in the quartz tube reach 5×10 -4 Pa.
10. The method for preparing the porous Ni-Mn-Ga shape memory alloy according to claim 1, characterized in that: In the furnace cooling and quenching treatment in step S4, the quenching liquid is water at 0-10°C.