Self-catalytic functional reaction monomer, self-catalytic polymerization and self-catalytic depolymerization functional copolymer and preparation method and application thereof
Through the autocatalytic functional reaction monomer, the catalyst residue and self-dispolymerization chemical recovery is achieved in the polymer, which solves the problems of catalyst residue and waste polymer recycling, and improves the environmental protection and resource utilization efficiency of the polymer.
Patent Information
- Application Number
- CN202110391482.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-04-13
AI Technical Summary
Catalyst residues in existing polymer synthesis lead to environmental protection and safety problems, and recycling of used polymers is difficult to achieve efficient chemical recycling, especially in the process of depolymerization, which has problems such as environmental pollution and performance degradation.
Develop an autocatalytic functional reaction monomer, which can be used as a polymerization catalyst and a third monomer, and can be connected to the polymer molecular chain during the polymerization process, so as to achieve no residue of small molecule catalysts, and no need for external depolymerization catalysts in chemical recycling. Self-depolymerization is used to repolymerize.
The synthesis of green polymers without catalyst residues is achieved, which improves the safety and environmental protection of the polymers, and improves resource utilization efficiency through self-depolymerization chemical recycling and reduces environmental pollution.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of functional reaction monomers, functionalized copolymers and their preparation, and specifically, the present invention relates to a new type of self-catalytic functional reaction monomers, self-catalytic polymerization and self-catalytic depolymerization functional copolymers and their preparation methods. That is to say, without adding a traditional catalyst, this type of compound can be used as a polymerization catalyst and a third reaction monomer at the same time, and can not only catalyze the melt copolymerization of itself with polymer raw material monomers such as polyester or polycarbonate, so as to synthesize copolymers such as copolyester or copolycarbonate without small molecule catalyst residue and with a preset monomer introduction amount, but also without adding an external depolymerization catalyst, the copolymer can undergo self-depolymerization reaction under suitable conditions, and the reaction monomer is obtained again, so as to realize the chemical recovery of the copolymer. At the same time, the introduction of the self-catalytic polymerization monomer can also give the polymer multifunctionality, thereby realizing the self-catalytic melt polymerization, multifunctionality and self-depolymerization chemical recovery of the copolymer. Background Art
[0002] As a conventional polymerization method, melt polycondensation has been widely used in the industrial production of various polymers, such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polybutylene succinate (PBS), polybutylene adipate / terephthalate (PBAT) and polyethylene furandicarboxylate (PEF). In recent years, the technology and products of melt polycondensation for the green preparation of polycarbonate (PC) without phosgene have also attracted more and more attention from the market. In the process of melt polycondensation, suitable catalysts can greatly improve the production efficiency of products, such as antimony catalysts used in polyester production and small molecule catalysts used in polycarbonate production. However, small molecule catalysts remaining in the polymer matrix often affect the safety and ecological safety of polymers, especially some heavy metal-based catalysts. With the enhancement of people's environmental awareness, green catalysts have become an important factor affecting the sustainable development of melt polycondensation polymer industry. However, some existing green catalysts with high catalytic activity and low toxicity still have many problems in terms of stability in storage and use, balance between polymerization activity and selectivity, and controllability of polymer production process and performance quality. For example, titanium catalysts developed for polyester generally have disadvantages such as poor stability and aggravated side reactions, which lead to poor hue and quality of synthesized PET; especially when titanium catalysts coexist with more phosphorus-containing compounds, it is easier to aggravate side reactions, so the phosphorus-containing copolymers synthesized by them are generally yellow in hue and have a particularly high b value, which cannot meet high-end applications and is not conducive to chemical recovery of polymers. In addition, the presence of residual small molecule catalysts in the resin will also have some adverse effects on the performance quality of the polymer, such as reduced thermal stability, and the application occasions will also be limited.
[0003] On the other hand, while polymer materials and their products bring convenience to people's lives, the generation and improper disposal of a large number of waste polymers also bring serious environmental pollution and resource waste problems. Therefore, the recovery and comprehensive utilization of waste polymers have become one of the major issues affecting the environment and human sustainable development worldwide. Existing waste polymer recovery methods mainly include physical methods, physical and chemical methods, and chemical methods. Among them, the chemical method can achieve closed-loop recovery from "polymer-monomer-polymer" to obtain high-value recycled products, which is particularly suitable for high-value recovery of polycondensation polymers such as polyester. However, in the process of chemical recovery of monomers, polymer depolymerization requires an external catalyst, which not only faces the problem of depolymerization efficiency, but also the residual catalyst also brings great difficulties to the separation and purification of monomers. Moreover, the original heavy metals or small molecule catalysts in the material also face the problem of environmental pollution or unstable properties during the recovery process, which has an adverse effect on the separation and purification of monomers. And the above are just the difficulties of chemical recovery of simple polymer systems. In the actual use of polymer materials, due to their own shortcomings or deficiencies in performance, they often need to be functionalized according to the requirements of the application. At present, the most common way to functionalize polymers is to add functional additives directly to the substrate by physical blending during polymer polymerization or processing. The chemical recycling of complex polymer material systems based on blended functional modification also requires solving the separation and purification problems of various functional additives and reactive monomers, which increases the difficulty of chemical recycling of materials, aggravates environmental pollution and resource consumption during the recycling process, and is not conducive to the recycling and sustainable development of polymer materials.
[0004] In view of this, the inventors hope to develop a copolymer having the following characteristics: the polymer uses a polymerizable compound with self-catalytic polymerization activity (i.e., a self-catalytic functional reaction monomer) as a polymerization catalyst and a third monomer, so that it can be connected to the molecular chain of the polymer during the polymerization process, so that there is no small molecule catalyst residue in the obtained resin; in the chemical recovery process of the polymer, no external depolymerization catalyst is required, and the obtained copolymer can undergo self-depolymerization reaction under suitable conditions to obtain the reaction monomer again, and the third monomer can be directly used for the repolymerization of the copolymer without separation and purification; the third monomer structure used in the polymer has specific functionality, and after being introduced into the polymer macromolecular chain, it can also give the obtained copolymer certain functionality. Therefore, the copolymer can simultaneously realize the self-catalytic melt polymerization, multifunctionality and self-depolymerization chemical recovery of multiple polymers. Summary of the invention
[0005] One of the purposes of the present invention is to provide a class of self-catalytic functional reaction monomers.
[0006] The second object of the present invention is to provide a functional copolymer of autocatalytic polymerization and autocatalytic depolymerization.
[0007] The third object of the present invention is to provide a method for preparing a functional copolymer of autocatalytic polymerization and autocatalytic depolymerization.
[0008] A fourth object of the present invention is to provide an application of a functional copolymer of autocatalytic polymerization and autocatalytic depolymerization.
[0009] The self-catalytic functional reaction monomer provided by the present invention is characterized in that the general structural formula of the reaction monomer is as follows:
[0010]
[0011]
[0012] In the formula, Z1 and Z2 are carboxyl, ester, amino, hydroxyl, acyloxy or hydroxyl groups having polycondensation activity, and a is an integer of 1 to 12. Z2 is the same or different; Z3 and Z4 are H atoms, C1-C12 alkyl groups, cyano groups, C1-C12 alkoxy groups, secondary amino groups, tertiary amino groups, amide groups, aryl groups or substituted aryl groups; Z3 and Z4 are the same or different; Z5 and Z6 are H atoms, C1-C12 alkyl groups, C1-C12 alkoxy groups, secondary amino groups, tertiary amino groups, amide groups, aryl groups, substituted aryl groups, ester groups, carboxyl groups, hydroxyl groups, amino groups, acyloxy groups or a is an integer of 1 to 12; X is an O atom, an S atom, a secondary amino group, a nitrogen methyl group or a nitrogen ethyl group; W is an O atom or an S atom; Y is an O atom, an S atom, a secondary amino group, a nitrogen methyl group, a nitrogen ethyl group or an amide group; when the reaction monomer structure is AS, M n+ is an organic cation; when the reaction monomer structure is TW, M n+ It is an organic cation or an alkali metal ion.
[0013] The ester group described in the general structural formula of the above self-catalytic functional reaction monomer is a methyl ester group, an ethyl ester group, a propyl ester group, a butyl ester group, a pentyl ester group or a hexyl ester group after esterification of a monohydric alcohol, or a phenyl ester group after esterification of a monohydric phenol, or any one of an ethylene glycol ester group, a propylene glycol ester group, a butylene glycol group, a neopentyl glycol ester group, a diethylene glycol ester group, a glycerol ester group or a pentaerythritol ester group after esterification of a polyhydric alcohol.
[0014] The organic cation M described in the general structural formula of the above self-catalytic functional reaction monomer n+ is any one of the cations having the following structural formula, and n is an integer of 1 to 2:
[0015]
[0016]
[0017] In the formula, Z7, Z8, Z9, Z 10 is a C2-C16 alkyl, aryl or substituted aryl, which may be the same or different; Z 11 is a C2-C16 alkylene or arylene group; Z 12 is a C1-C16 alkyl, aryl or substituted aryl; Z 13 is an H atom, a C1-C12 alkyl group, a cyano group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an amide group, an aryl group or a substituted aryl group; and X is an O atom, an S atom, a C1-C16 nitrogen alkyl group or a nitrogen aryl group.
[0018] The present invention provides a method for preparing the above-mentioned self-catalytic functional reaction monomer, which comprises conducting a neutralization reaction between a precursor containing a phosphonic acid group and an alkali metal ion or a hydroxide, bicarbonate or acetate containing a B1-B8 organic cation according to a conventional molar ratio to prepare a target reaction monomer; or conducting an ion exchange reaction between a sodium salt, potassium salt or silver salt of the corresponding phosphonic acid group-containing precursor and a chloride salt, bromide salt or p-toluenesulfonate containing a B1-B8 organic cation structure in an organic solvent according to a conventional molar ratio to prepare a target reaction monomer.
[0019] The phosphonic acid group-containing precursors and corresponding salts used in the above self-catalytic functional reaction monomer preparation method can be prepared by referring to the methods disclosed in Inorganic Chemistry 2016, 55, 7928-7943; Polymer Chemistry, 2014, 5, 1982-1991; Journal of the American Chemical Society, 2005, 127, 8, 2398-2399; Journal of Polymer Part A: Polymer Chemistry, 2012, 50, 4977-4982 and other literature.
[0020] The present invention provides a self-catalytic polymerization and self-depolymerization functional copolymer, which is a copolymer of a fully aromatic polyester, a semi-aromatic polyester, an aliphatic polyester, an aliphatic-aromatic polyester, a bio-based polyester, a polycarbonate, a polyester elastomer, a nylon elastomer or a modified polymer of the above polymers and a self-catalytic functional reaction monomer, and the self-catalytic functional reaction monomer is fully connected to the molecular chain of the copolymer, and is composed of the following structural units represented by Ⅰ, Ⅱ, Ⅲ or Ⅰ, Ⅱ, Ⅳ:
[0021]
[0022] In the formula, R1 represents a polyamide segment terminated with an arylene group, a darylene group, a C2-C12 alkylene group or dalkylene group, a 2,5-furanyl group, a carboxylic acid group or an ester group;
[0023]
[0024] In the formula, R2 represents an arylene group, a aryl group, an alkylene group or an alkylene group of C2 to C12, a 4,4'-isopropylidene diphenyl group (bisphenol A group), a 4,4'-diphenylmethane group (bisphenol F group), a 4,4'-diphenylsulfone group (bisphenol S group), an isosorbide group, a polyether segment (polyether polyol group) or an alcohol-terminated polyester segment (polyester polyol group);
[0025]
[0026]
[0027] In the formula, R3 and R4 are carbonyl, secondary amine, O atom or a is an integer of 1 to 12, R3 and R4 are the same or different; R5 and R6 are H atoms, C1 to C12 alkyl groups, cyano groups, C1 to C12 alkoxy groups, secondary amino groups, tertiary amino groups, amide groups, aryl groups or substituted aryl groups, R5 and R6 are the same or different; R7 is H atoms, C1 to C12 alkyl groups, hydroxyl groups, C1 to C12 alkoxy groups, secondary amino groups, tertiary amino groups, aryl groups or substituted aryl groups; X is an O atom, an S atom, a secondary amino group, a nitrogen methyl group or a nitrogen ethyl group, W is an O atom or an S atom, and Y is an O atom, an S atom, a secondary amino group, a nitrogen methyl group, a nitrogen ethyl group or an amide group; the cation M n+ It is any one of an alkali metal ion or an organic cation having the following general structural formula:
[0028]
[0029] In the formula, Z7, Z8, Z9, Z 10 is a C2-C16 alkyl, aryl or substituted aryl, which may be the same or different; Z 11 is a C2-C16 alkylene or arylene group; Z 12 is a C1-C16 alkyl, aryl or substituted aryl; Z 13 is an H atom, a C1-C12 alkyl group, a cyano group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an amide group, an aryl group or a substituted aryl group; and X is an O atom, an S atom, a C1-C16 nitrogen alkyl group or a nitrogen aryl group.
[0030]
[0031]
[0032] In the formula, R3 is a carbonyl group, a secondary amine group, an O atom or a is an integer of 1 to 12; R5 and R6 are H atoms, C1 to C12 alkyl groups, cyano groups, C1 to C12 alkoxy groups, secondary amino groups, tertiary amino groups, amide groups, aryl groups or substituted aryl groups, and R5 and R6 are the same or different; R7 is an H atom, C1 to C12 alkyl groups, hydroxyl groups, C1 to C12 alkoxy groups, secondary amino groups, tertiary amino groups, aryl groups or substituted aryl groups; X is an O atom, an S atom, a secondary amino group, a nitrogen methyl group or a nitrogen ethyl group; W is an O atom or an S atom; and Y is an O atom, an S atom, a secondary amino group, a nitrogen methyl group, a nitrogen ethyl group or an amide group; the cation M n+ It is any one of an alkali metal ion or an organic cation having the following general structural formula:
[0033]
[0034] In the formula, Z7, Z8, Z9, Z 10 is a C2-C16 alkyl, aryl or substituted aryl, which may be the same or different; Z 11 is a C2-C16 alkylene or arylene group; Z 12 is a C1-C16 alkyl, aryl or substituted aryl; Z 13 is an H atom, a C1-C12 alkyl group, a cyano group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an amide group, an aryl group or a substituted aryl group; and X is an O atom, an S atom, a C1-C16 nitrogen alkyl group or a nitrogen aryl group.
[0035] The number of structural units of [III] is 0.05 to 99% of the number of structural units of [I]; the number of structural units of [IV] is 0.05 to 40% of the number of structural units of [I]. The intrinsic viscosity [η] of the copolymer is 0.16 to 2.10 dL / g, the limiting oxygen index is 22.5 to 57.0%, the vertical combustion grade is V-2 to V-0, the antibacterial rate against Staphylococcus aureus is 30% to 99.99%, and the antibacterial rate against Escherichia coli is 30% to 99.99%.
[0036] The functional copolymer of self-catalytic polymerization and self-catalytic depolymerization can undergo self-depolymerization chemical reaction in an alcohol reaction medium at normal pressure and heated to 120-280°C or in an alcohol reaction medium under pressure and heated to 120-280°C, and the target monomer can be recovered and directly used for the repolymerization of the copolymer without separation and purification.
[0037] The functional copolymer of the above-mentioned self-catalytic polymerization and self-catalytic depolymerization is preferably such that the number of structural units of [III] is 0.1 to 60% of the number of structural units of [I]; the number of structural units of [IV] is 0.1 to 30% of the number of structural units of [I], and the intrinsic viscosity [η] of the copolymer is 0.20 to 2.10 dL / g; the limiting oxygen index is 23.5 to 53.0%, the vertical combustion grade is V-2 to V-0, the antibacterial rate against Staphylococcus aureus is 40 to 99.99%, and the antibacterial rate against Escherichia coli is 40 to 99.99%.
[0038] The self-catalytic functional reaction monomer in the functional copolymer of the self-catalytic polymerization and self-catalytic depolymerization is at least one of the following structural formulas:
[0039]
[0040]
[0041] In the formula, Z1 and Z2 are carboxyl, ester, amino, hydroxyl, acyloxy or a is an integer of 1 to 12, Z1 and Z2 are the same or different; Z3 and Z4 are H atoms, C1 to C12 alkyl groups, cyano groups, C1 to C12 alkoxy groups, secondary amino groups, tertiary amino groups, amide groups, aryl groups or substituted aryl groups, Z3 and Z4 are the same or different; Z5 and Z6 are H atoms, C1 to C12 alkyl groups, C1 to C12 alkoxy groups, secondary amino groups, tertiary amino groups, amide groups, aryl groups or substituted aryl groups, ester groups, carboxyl groups, hydroxyl groups, amino groups, acyloxy groups or a is an integer of 1 to 12; X is an O atom, a S atom, a secondary amino group, a nitrogen methyl group or a nitrogen ethyl group; W is an O atom or a S atom; Y is an O atom, a S atom, a secondary amino group, a nitrogen methyl group, a nitrogen ethyl group or an amide group; M n+ is an alkali metal ion or an organic cation, and n is an integer of 1 to 3.
[0042] In the general structural formula of the above self-catalytic functional reaction monomer, the ester group is a methyl ester group, ethyl ester group, propyl ester group, butyl ester group, pentyl ester group or hexyl ester group after esterification of a monohydric alcohol, or a phenyl ester group after esterification of a monohydric phenol, or any one of an ethylene glycol ester group, propylene glycol ester group, butanediol group, neopentyl glycol ester group, diethylene glycol ester group, glycerol ester group or pentaerythritol ester group after esterification of a polyhydric alcohol.
[0043] The cation M in the above general structure of the self-catalytic functional reaction monomer n+ It is any one of an alkali metal ion or an organic cation having the following structural formula B1-B8:
[0044]
[0045] In the formula, Z7, Z8, Z9, Z 10 is a C2-C16 alkyl, aryl or substituted aryl, which may be the same or different; Z 11 is a C2-C16 alkylene or arylene group; Z 12 is a C1-C16 alkyl, aryl or substituted aryl; Z 13 is an H atom, a C1-C12 alkyl group, a cyano group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an amide group, an aryl group or a substituted aryl group; and X is an O atom, an S atom, a C1-C16 nitrogen alkyl group or a nitrogen aryl group.
[0046] The self-catalytic functional reaction monomers used above can be prepared by referring to the methods disclosed in Polymer Chemistry, 2014, 5, 1982-1991; Polymer, 2015, 60, 50-61; Journal of the American Chemical Society, 2005, 127, 8, 2398-2399 and other literatures.
[0047] The present invention provides a method for preparing a functional copolymer of self-catalytic polymerization and self-catalytic depolymerization. The method comprises the following steps: preparing a polymer monomer of dicarboxylic acid or dicarboxylic acid ester and a diol or phenol according to conventional proportions, esterifying or esterifying by conventional direct esterification method or ester exchange method, and then subjecting the polymer monomer to melt polycondensation reaction or further solid phase polycondensation reaction. The method is characterized in that before the esterification or ester exchange reaction or before the polycondensation after the esterification reaction, 0.05-99% of a dual polymerizable functional group or 0.05-40% of a single polymerizable functional group self-catalytic functional reaction monomer is added to the reaction system based on the molar number of the dicarboxylic acid or dicarboxylic acid ester in the polymer monomer; preferably 0.1-60% of a dual polymerizable functional group or 0.1-30% of a single polymerizable functional group self-catalytic functional reaction monomer.
[0048] The self-catalytic functional reaction monomers used in the above self-catalytic polymerization methods have obvious catalytic effects on esterification reactions, ester exchange reactions and polycondensation reactions, and are suitable for polymerization processes such as direct esterification-melt polycondensation, ester exchange-melt polycondensation, solid phase polycondensation and melt polycondensation-solid phase polycondensation.
[0049] The polymerization process steps and conditions of the conventional direct esterification method, ester exchange method melt polycondensation and solid phase polycondensation adopted by the present invention are specifically as follows:
[0050] Direct esterification method: Add polymer monomers (dicarboxylic acids, diols or phenols) and autocatalytic polymerization monomers in a conventional ratio into a reactor, pressurize and heat to 120-240°C for esterification for 0.5-8 hours; after the esterification is completed, pre-condense at 160-270°C for 0.5-2 hours under low vacuum, then condense at 200-300°C for 1-8 hours under high vacuum, press out the polymer melt with inert gas (preferably nitrogen), and water-cool the melt to obtain the target polymer. Among them, the autocatalytic polymerization functional reaction monomer can be added to the reactor before esterification or before condensation after esterification.
[0051] Ester exchange method: Add polymer monomers (esters of dicarboxylic acids, diols or phenols) and self-catalytic polymerization monomers in a conventional ratio into a reactor, and carry out ester exchange reaction at 120-240°C under normal pressure for 0.5-8 hours; after the ester exchange, pre-condense at 160-270°C for 0.5-2 hours under low vacuum, and then condense at 200-300°C for 1-8 hours under high vacuum, press out the polymer melt with an inert gas (preferably nitrogen), and water-cool the melt to obtain the target polymer.
[0052] Solid phase polycondensation: First, a relatively low molecular weight polymer is prepared by melt polycondensation through the above-mentioned ester exchange method or direct esterification method. After the obtained low molecular weight polymer is dried and pre-crystallized under nitrogen protection, the sample is placed in a solid phase polycondensation reaction device, and polycondensation is continued at 120-240°C under high vacuum for 0.5-15 hours, cooled and granulated to obtain the target polymer.
[0053] The self-catalytic functional reaction monomers used in the above self-catalytic polymerization method can be used not only as esterification, transesterification and polycondensation catalysts alone, but also as main catalysts in combination with co-catalysts, stabilizers, antioxidants, matting agents, toners and other auxiliary agents.
[0054] Since the introduced self-catalytic functional reaction groups also have the function of catalyzing transesterification, the self-catalytic depolymerization chemical recovery of the copolymer is suitable for recovery methods such as hydrolysis, alcohol (or phenol) hydrolysis, aminolysis and alcoholysis-esterification combined method using water, alcohols, phenols or amines as reaction media.
[0055] The application of the functional copolymer of self-catalytic polymerization and self-catalytic depolymerization provided by the present invention is to be used alone in the fields of fibers and their products, non-woven fabrics, engineering plastics, membrane materials, container materials, packaging materials, biomedical materials, shape memory materials or 3D printing materials, and to be used as a functional additive for the modification of polymer materials.
[0056] Compared with the prior art, the present invention has the following advantages:
[0057] 1. Since the functional copolymer of self-catalytic polymerization and self-catalytic depolymerization provided by the present invention utilizes the self-catalytic functional reaction monomer as the catalyst and the third monomer of melt polycondensation at the same time, it can be realized that the functional reaction monomer catalyzes the melt copolymerization of itself and the polymer raw material monomer without adding other catalysts, and is connected to the macromolecular chain of the copolymer to obtain the corresponding copolymer. Therefore, the copolymer eliminates the catalyst residue and migration in the corresponding polymer prepared by the existing method and the health and ecological environment problems that may be caused from the source, and provides a new solution for realizing the green synthesis and safe use of various polymers.
[0058] 2. Since the functional copolymers of self-catalytic polymerization and self-catalytic depolymerization provided by the present invention are designed with specific functional structures in mind, when a certain amount of functional reaction monomers are connected to the macromolecular chain of the copolymer, it will bring about changes in the performance of the copolymer. Therefore, while achieving self-catalytic polymerization, the polymer can be endowed with good flame retardancy, anti-drip, antistatic, antibacterial and easy-to-dye functionality. It has good application prospects and meets the huge development needs of the polyester industry.
[0059] 3. Since the self-catalytic functional reaction monomers used in the self-catalytic polymerization method provided by the present invention have obvious catalytic effects on transesterification reaction, esterification reaction, melt and solid phase polycondensation reaction, the self-catalytic polymerization method provided by the present invention is suitable for synthesizing all aromatic polyesters, semi-aromatic polyesters, aliphatic polyesters, aliphatic-aromatic polyesters, bio-based polyesters, polycarbonates, polyester elastomers, nylon elastomers and modified copolymers of the above polymers by direct esterification-melt polycondensation, transesterification-melt polycondensation, Solid phase polycondensation and melt polycondensation-solid phase polycondensation and other polymerization methods, such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polytrimethylene terephthalate (PTT), polybutylene terephthalate (PBT), aromatic polyester liquid crystal polymer (LCP), polybutylene succinate (PBS), polybutylene adipate / terephthalate (PBAT), polyethylene furandicarboxylate (PEF), polylactic acid (PLA), polycarbonate (PC), isosorbide modified copolyester or polycarbonate, thermoplastic polyester elastomer (TPEE) and thermoplastic nylon elastomer (TPAE).
[0060] 4. Since the self-catalytic functional reaction monomers used in the self-catalytic polymerization method provided by the present invention have stable chemical properties and good compatibility with the polymer reaction system, the self-catalytic functional reaction monomers used in this method have good storage stability, hydrolysis resistance, thermal stability, reaction activity and matrix compatibility.
[0061] 5. Since the self-catalytic functional reaction monomer used in the self-catalytic polymerization method provided by the present invention contains a phosphonate structure, it can not only act as a catalyst but also as a stabilizer, thereby inhibiting the occurrence of side reactions and improving the performance quality of the obtained copolymer (especially the b value of the polymer). Compared with the pure polymer and copolymer system using an added catalyst, the obtained copolymer has higher thermal stability and better hue.
[0062] 6. Since the functional copolymer of the self-catalytic polymerization and self-catalytic depolymerization provided by the present invention contains phosphonate ion groups similar to sulfonates, the copolymer also exhibits good antistatic properties and affinity with cationic dyes.
[0063] 7. Since the functional copolymer of self-catalytic polymerization and self-catalytic depolymerization provided by the present invention does not contain any additives that affect fiber preparation, the copolymer has good spinnability and can not only be directly used as a polymer raw material for fiber, but also can be processed by injection molding, blown film, cast film and other processing methods to obtain corresponding films, plates, packaging materials and engineering plastics.
[0064] 8. Since the self-catalytic functional groups in the self-catalytic polymerization and self-catalytic depolymerization functional copolymers provided by the present invention have the function of catalyzing transesterification, there is no need to add an external depolymerization catalyst. The obtained copolymers can undergo self-depolymerization reaction under appropriate conditions and completely depolymerize into reaction monomers.
[0065] 9. Since the functional copolymer of self-catalytic polymerization and self-catalytic depolymerization provided by the present invention can be completely self-depolymerized into reaction monomers, compared with the non-self-catalytic copolymer system, the chemical recovery of the copolymer not only has milder conditions and high depolymerization and conversion rates, but also can reduce the separation and purification problems caused by native small molecule catalysts and external depolymerization catalysts. The third monomer can remain in the recovered monomer without separation and purification and be reused in the synthesis of the copolymer. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] Figure 1 The nuclear magnetic hydrogen spectrum of the self-catalytic functional reaction monomer 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite prepared in Example 1 of the present invention. The peaks at 7.27, 7.92ppm and 8.25ppm in the hydrogen spectrum are attributed to the hydrogen on the anthracene oxacyclic ring, the peaks at 9.21, 7.79 and 7.70ppm are attributed to the hydrogen on the imidazole ring, the peak at 3.87ppm is attributed to the hydrogen of the methyl ester, the peaks at 4.42, 4.16 and 1.44ppm are attributed to the hydrogen of the methyl and methylene on the imidazole ring, and the remaining peaks are solvent peaks and water peaks. The results of the nuclear magnetic hydrogen spectrum show that the target monomer has been successfully prepared.
[0067] Figure 2This is the nuclear magnetic phosphorus spectrum of the self-catalytic functional reaction monomer 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite prepared in Example 1 of the present invention. The chemical shift of this spectrum has only one peak: -13.7ppm, indicating that there is only one phosphorus environment, and also indicating that the target monomer has been successfully prepared.
[0068] Figure 3 This is the nuclear magnetic hydrogen spectrum of the functional copolymer of self-catalytic polymerization and self-catalytic depolymerization prepared in Example 23 of the present invention. The peak near 8.22ppm in the hydrogen spectrum corresponds to the hydrogen on the benzene ring in the copolymer structural unit, the peak at 4.94ppm corresponds to the hydrogen on the ethylene glycol unit of the copolymer main chain, and the peaks at 9.10, 8.92 and 8.02ppm correspond to the hydrogen on the copolymer self-catalytic functional reaction monomer structural unit. This shows that the self-catalytic functional reaction monomer has been successfully introduced into the copolymer molecular chain.
[0069] Figure 4 This is the nuclear magnetic phosphorus spectrum of the functional copolymer of autocatalytic polymerization and autocatalytic depolymerization prepared in Example 23 of the present invention. The peak near 2.3 ppm in the phosphorus spectrum corresponds to the phosphorus element in the autocatalytic functional reaction monomer structural unit in the copolymer, and the result further proves that the autocatalytic functional reaction monomer is successfully introduced into the copolymer molecular chain.
[0070] Figure 5 This is a thermogravimetric curve of the self-catalytic functional reaction monomer prepared in Example 1 of the present invention. The figure shows that the prepared self-catalytic functional reaction monomer can maintain good thermal stability during the melt polycondensation process.
[0071] Figure 6 The thermogravimetric curves of the polymers prepared in Example 41 of the present invention and Comparative Examples 1 and 2 are shown. It can be seen that the thermal stability of the polymer obtained by the autocatalytic polymerization is significantly higher than that of the same polymers prepared by other catalysts.
[0072] Figure 7 The heat release curves of the copolymer prepared in Example 53 of the present invention and the PET prepared in Comparative Example 1 are shown. From the results, it can be seen that the functional copolymers of autocatalytic polymerization and autocatalytic depolymerization exhibit different combustion behaviors, with significantly reduced heat release rates, and their peak heat release rates are more than half lower than those of pure PET, showing excellent flame retardant properties.
[0073] Figure 8The smoke density curves of the functional copolymer of autocatalytic polymerization and autocatalytic depolymerization prepared in Example 53 of the present invention and the PET prepared in Comparative Example 1 are shown. From the results, it can be seen that with the introduction of the autocatalytic functional reaction monomer, the smoke density of the copolymer is significantly reduced, only about 30% of that of pure PET, showing extremely excellent smoke suppression performance. This shows that the introduction of the autocatalytic functional reaction monomer has well suppressed the smoke generation of the copolymer.
[0074] Fig. 9 The curves are the absorbance of the dye liquor of the functional copolymer fiber prepared by the self-catalytic polymerization and self-catalytic depolymerization of Example 56 of the present invention and the PET fiber prepared by Comparative Example 1 after dyeing. From the results, it can be seen that the absorbance of the dye liquor of the copolymer fiber obtained by Example 56 after dyeing is significantly lower than the absorbance of the dye liquor of the pure PET fiber after dyeing, indicating that more dye is adsorbed onto the surface of the copolymer fiber during the dyeing process. This result shows that the copolymer has excellent cationic dyeing ability. DETAILED DESCRIPTION
[0075] The following examples are given to further illustrate the present invention. It is necessary to point out that the following examples cannot be understood as limiting the scope of protection of the present invention. If a person skilled in the art makes some non-essential improvements and adjustments to the present invention based on the above content of the present invention, it still belongs to the scope of protection of the present invention.
[0076] In addition, it is worth noting that the intrinsic viscosity [η] of the copolymers obtained in the following examples and the comparative copolymers were prepared with phenol / 1,1,2,2-tetrachloroethane (1:1, v:v) as solvent to prepare a solution with a concentration of 5 g / dL, and tested at 25° C. using an Ubbelohde viscometer; the limiting oxygen index was measured in accordance with ASTM D2863-97; the vertical burning test was measured in accordance with UL-94 standard, and the sample size was 125×12.7×3.2 mm 3 The cone calorimeter test is carried out according to ISO 5660-1 standard and is made into 100×100×3mm 3 The standard sample was measured on an FTT cone calorimeter; the antibacterial test was carried out in accordance with QB-T2591-2018 standard; the fiber dyeing performance test used methylene blue as a cationic dye, 1g of fiber sample was weighed for dyeing test, and the dye solution absorbance test was carried out using a UV-visible spectrophotometer, and the absorbance at a wavelength of 665nm was taken as the maximum absorbance.
[0077] Example 1
[0078] In a reaction kettle, add 696g [2,8-di(methoxy)carbonyl] anthracene oxaphosphite and 3L ethanol, then stir to mix evenly and slowly heat to 50°C, then slowly drop 256g 1-ethyl-3-methylimidazole hydroxide (equimolar amount) and stir for 2 hours. Remove the solvent and dry to obtain 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite.
[0079] Example 2
[0080] In a reactor, 696g of [2,8-di(methoxy)carbonyl] anthracene oxaphosphite was dispersed in 3L of ethanol, 200g of potassium bicarbonate was added, the reaction was continued for 2 hours, and the solvent was removed to obtain [2,8-di(methoxy)carbonyl] anthracene oxaphosphite potassium. 386g of the product of the previous step was weighed and added to an ethanol solution containing 174.7g of 1-butyl-3-methylimidazole chloride, and stirred for 4 hours. Filter, remove the solvent from the filtrate, and recrystallize the obtained white solid with a mixed solution of ether and ethanol, and dry to obtain 1-butyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite.
[0081] Example 3
[0082] In a reactor, first disperse 696g of (2,8-dicarboxyl) anthracene oxaphosphite in 3L of ethanol, add 168g of sodium bicarbonate, react for 2 hours, remove the solvent, and obtain (2,8-dicarboxyl) anthracene oxaphosphite sodium. Weigh 370g of the product from the previous step and add it to an ethanol solution containing 216.1g of N-butylpyridinium bromide, stir for 4 hours, filter, remove the solvent from the filtrate, and recrystallize the obtained white solid with a mixed solution of ether and ethanol, and dry it to obtain N-butylpyridine (2,8-dicarboxyl) anthracene oxaphosphite.
[0083] Example 4
[0084] In a reaction kettle, 856.64 g of 2-carboxyethylphenyl hypophosphorous acid was first dissolved in 2 L of ethylene glycol, stirred, reacted at 190° C. for 4 hours, and cooled for use. Then, 512 g of 1-ethyl-3-methylimidazole hydroxide was added at room temperature for neutralization reaction, stirred for 4 hours, and the resulting solution was collected to obtain an ethylene glycol solution of 1-ethyl-3-methylimidazole 2-(2-hydroxyethoxycarbonyl)ethylphenyl hypophosphite, which was dried for use.
[0085] Example 5
[0086] In a reactor, first 856.64g 2-carboxyethylphenyl hypophosphorous acid and 20mL concentrated sulfuric acid were dissolved in 1L methanol, and refluxed for 6 hours. After the reaction was completed, sodium bicarbonate was added to neutralize sulfuric acid, filtered, and the filtrate was desolvated to obtain 2-(2-methoxycarbonyl)ethylphenyl hypophosphorous acid, which was dried for standby use. Weigh 228g of the previous step product, add it into an ethanol solution dissolved with 198g 1-butyl-3-methylimidazole acetate, stir for 6 hours, remove the solvent, and recrystallize to obtain 1-butyl-3-methylimidazole 2-(2-methoxycarbonyl)ethylphenyl hypophosphite.
[0087] Example 6
[0088] In a reaction kettle, first disperse 580g of 2,8-bis(5-methoxycarbonyl-1H-benzimidazole-2-yl) anthracene oxaphosphite in 3L ethanol, add 84g of sodium bicarbonate, react for 4 hours, remove the solvent, and obtain 2,8-bis(5-methoxycarbonyl-1H-benzimidazole-2-yl) anthracene oxaphosphite sodium. Weigh 301g of the product of the previous step and add it to a methanol solution containing 102.5g of 1,2-dimethyl-3-ethylimidazolium bromide, react for 6 hours, filter, remove the solvent from the filtrate, and recrystallize the obtained solid with ethanol and dry to obtain 1,2-dimethyl-3-ethylimidazolium 2,8-bis(5-methoxycarbonyl-1H-benzimidazole-2-yl) anthracene oxaphosphite.
[0089] Example 7
[0090] In a reaction kettle, first disperse 581g of 2,8-bis(5-methoxycarbonyl-benzoxazol-2-yl) anthracene oxaphosphite in 3L of ethanol, add 84g of sodium bicarbonate, react for 4 hours, remove the solvent, and obtain 2,8-bis(5-methoxycarbonyl-benzoxazol-2-yl) anthracene oxaphosphite sodium. Weigh 301.5g of the product of the previous step and add it to a methanol solution containing 102.5g of 1,2-dimethyl-3-ethylimidazolium bromide, react for 6 hours, filter, remove the solvent from the filtrate, and recrystallize the obtained solid with ethanol and dry to obtain 1,2-dimethyl-3-ethylimidazolium 2,8-bis(5-methoxycarbonyl-benzoxazol-2-yl) anthracene oxaphosphite.
[0091] Example 8
[0092] In a reaction kettle, first disperse 597g of 2,8-bis(5-methoxycarbonyl-benzothiazol-2-yl) anthracene oxaphosphite in 3L of ethanol, add 84g of sodium bicarbonate, react for 4 hours, remove the solvent, and obtain 2,8-bis(5-methoxycarbonyl-benzothiazol-2-yl) anthracene oxaphosphite sodium. Weigh 309.5g of the product of the previous step and add it to a methanol solution containing 102.5g of 1,2-dimethyl-3-ethylimidazolium bromide, react for 6 hours, filter, remove the solvent from the filtrate, and recrystallize the obtained solid with ethanol and dry to obtain 1,2-dimethyl-3-ethylimidazolium 2,8-bis(5-methoxycarbonyl-benzothiazol-2-yl) anthracene oxaphosphite.
[0093] Example 9
[0094] In a reaction kettle, add 246g 3,5-dicarboxyphenylphosphonic acid, 332g 3,4-diaminobenzoic acid methyl ester, 394g EDCI, 80g HOBT and 1000mL DMF, react at room temperature for 24 hours, remove the solvent, wash the product twice with water and dry it. The obtained solid is refluxed in 250ml glacial acetic acid for 12 hours, filtered to obtain 3,5-di(5-methoxycarbonyl-1H-benzimidazol-2-yl)phenylphosphonic acid. Weigh 101.2g of the product of the previous step and disperse it in ethanol, add 51.2g 1-ethyl-3-methylimidazole hydroxide, react at 60°C for 4 hours, remove the solvent, and dry to obtain di(1-ethyl-3-methylimidazole)3,5-di(5-methoxycarbonyl-1H-benzimidazol-2-yl)phenylphosphonate.
[0095] Example 10
[0096] In a reactor, first, 856g of 2-carboxyethylphenyl hypophosphorous acid and 608g of 3,4-diaminobenzoic acid are added to 2L of hydrochloric acid solution (4mol / L), refluxed for 8 hours, the solution is adjusted to neutrality with ammonia water, filtered, the filter cake is washed twice with hot water, and dried to obtain 2-(5-methoxycarbonyl-1H-benzimidazole-2-yl)ethylphenyl hypophosphorous acid. 330g of the previous step product and 84g of sodium bicarbonate are added to ethanol and reacted for 6 hours. 216.1g of N-butylpyridine bromide is added, reacted for 4 hours, filtered, the filtrate is freed from the solvent, the obtained white solid is recrystallized with ether, and dried to obtain N-butylpyridine 2-(5-methoxycarbonyl-1H-benzimidazole-2-yl)ethylphenyl hypophosphite.
[0097] Embodiment 11
[0098] In a reaction kettle, first, 865g of (4-aminophenyl)phosphonic acid was added to 3L of ethanol, and 530g of sodium carbonate was added, and the reaction was carried out for 8 hours. After removing the solvent, disodium (4-aminophenyl)phosphonate was obtained. 78g of the product of the previous step was weighed and added to an acetone solution containing 197.7g of 1-hexyl-3-methylimidazole bromide, and the reaction was carried out for 10 hours. The solution was filtered, and the solvent was removed from the filtrate. The obtained white solid was recrystallized from ethylene glycol ethyl ether and dried to obtain di(1-hexyl-3-methylimidazole) (4-aminophenyl)phosphonate.
[0099] Example 12
[0100] In a reactor, first 870g (4-hydroxyphenyl) phosphonic acid is dissolved in 2L of DMF, 392g of acetyl chloride is slowly dripped, reacted for 10 hours, and the solvent is removed to obtain [4-(acetoxy) phenyl] phosphonic acid. 648g of the previous step product and 504g of sodium bicarbonate are weighed and added to 1L of ethanol, reacted for 8 hours, filtered, the filtrate is desolvated, and dried to obtain [4-(acetoxy) phenyl] disodium phosphonate. 260g of the previous step product is weighed and added to the ethanol solution dissolved with 606g 1-decyl-3-methylimidazole bromide, reacted for 10 hours, filtered, the filtrate is desolvated, and the gained white solid is recrystallized from acetone, and dried to obtain di(1-decyl-3-methylimidazole)[4-(acetoxy) phenyl] phosphonate.
[0101] Example 13
[0102] In a reaction kettle, first add 864g (4-methoxycarbonylphenyl) phosphonic acid to 2L ethanol, add 672g sodium bicarbonate, react for 4 hours, remove the solvent, obtain disodium (4-methoxycarbonylphenyl) phosphonate, and dry for use. Weigh 780g of the product of the previous step and add it to an isopropanol solution containing 880g 1-ethyl-3-methylimidazole chloride, react for 10 hours, filter, remove the solvent from the filtrate, and recrystallize the obtained white solid with acetone and dry to obtain di(1-ethyl-3-methylimidazole) (4-methoxycarbonylphenyl) phosphonate.
[0103] Embodiment 14
[0104] In a reaction kettle, add 920g (4-methoxycarbonyl-3-methylphenyl)phosphonic acid to 2L ethanol, add 672g sodium bicarbonate, react for 4 hours, remove the solvent, obtain disodium (4-methoxycarbonyl-3-methylphenyl)phosphonate, and dry. Weigh 822g of the product of the previous step and add it to an isopropanol solution containing 1098g 1,1'-(1,3-trimethylene)bis-3-methylimidazole dibromide, react for 10 hours, filter, remove the solvent from the filtrate, and the obtained white solid is recrystallized with acetone and dried to obtain 1,1'-(1,3-trimethylene)bis-3-methylimidazole (4-methoxycarbonylphenyl)phosphonate.
[0105] Embodiment 15
[0106] In a reaction kettle, add 822g of 3,5-bis(methoxycarbonyl)phenylphosphonic acid to 2L of ethanol, add 504g of sodium bicarbonate, react for 4 hours, remove the solvent, obtain disodium 3,5-bis(methoxycarbonyl)phenylphosphonate, and dry for use. Weigh 636g of the product of the previous step and add it to an isopropanol solution containing 586.7g of 1-ethyl-3-methylimidazole chloride, react for 10 hours, filter, remove the solvent from the filtrate, and recrystallize the obtained white solid with ether and dry it to obtain di(1-ethyl-3-methylimidazole) 3,5-bis(methoxycarbonyl)phenylphosphonate.
[0107] Example 16
[0108] In a reaction kettle, add 822g of 3,5-bis(methoxycarbonyl)phenylphosphonic acid to 2L of ethanol, add 504g of sodium bicarbonate, react for 4 hours, remove the solvent, obtain disodium 3,5-bis(methoxycarbonyl)phenylphosphonate, and dry for use. Weigh 636g of the product of the previous step and add it to a n-butanol solution containing 1356g of tetra-n-butylphosphonium bromide, react for 10 hours, filter, remove the solvent from the filtrate, recrystallize the obtained solid with ethanol, and dry to obtain di(tetra-n-butylphosphine) 3,5-bis(methoxycarbonyl)phenylphosphonate.
[0109] Embodiment 17
[0110] In a reaction kettle, add 822g of 3,5-bis(methoxycarbonyl)phenylphosphonic acid to 2L of ethanol, add 600g of potassium bicarbonate, react for 4 hours, remove the solvent, obtain dipotassium 3,5-bis(methoxycarbonyl)phenylphosphonate, and dry for use. Weigh 700g of the product of the previous step and add it to a methanol solution containing 1581.8g of tributyl n-octylphosphine bromide, react for 10 hours, filter, remove the solvent from the filtrate, recrystallize the obtained white solid with ethanol, and dry to obtain di(tributyl n-octylphosphine) 3,5-bis(methoxycarbonyl)phenylphosphonate.
[0111] Embodiment 18
[0112] In a reaction kettle, add 822g of 3,5-bis(methoxycarbonyl)phenylphosphonic acid to 2L of ethanol, add 600g of potassium bicarbonate, react for 4 hours, remove the solvent, obtain dipotassium 3,5-bis(methoxycarbonyl)phenylphosphonate, and dry for use. Weigh 350g of the product of the previous step and add it to a methanol solution containing 360g of N,N'-(1,3-trimethylene)bipyridine, react for 10 hours, filter, remove the solvent from the filtrate, recrystallize the obtained white solid with acetone, and dry to obtain N,N'-(1,3-trimethylene)bipyridine 3,5-bis(methoxycarbonyl)phenylphosphonate.
[0113] Embodiment 19
[0114] In the reactor, add 264.95g 2,5-dibromo-p-xylene and 5g nickel bromide, under nitrogen protection, slowly drip 520g triethyl phosphite, reflux at 180°C for 10 hours, extract and separate with dichloromethane and water, remove the solvent, reflux and hydrolyze the obtained oil in concentrated hydrochloric acid for 10 hours, filter, and obtain a white solid. Weigh 216g of white solid and dissolve it in sodium hydroxide aqueous solution, add 345g potassium permanganate for oxidation, react at 80°C for 6 hours, filter, acidify the filtrate to obtain a white solid, and wash twice. The obtained product is placed in a methanol / concentrated sulfuric acid system for methyl esterification, and then potassium bicarbonate is added for neutralization, filtered, and the filtrate is recrystallized to obtain 1,4-dimethyl terephthalate-2,5-diphosphonic acid dipotassium.
[0115] Embodiment 20
[0116] In a reaction kettle, add 822g of 2,5-bis(methoxycarbonyl)phenylphosphonic acid to 2L of ethanol, add 504g of sodium bicarbonate, react for 4 hours, remove the solvent, obtain 3,5-bis(methoxycarbonyl)phenylphosphonic acid disodium, and dry. Weigh 318g of the product of the previous step and add it to an isopropanol solution containing 648.4g of 1,1'-(1,6-hexamethylene)bis(tributylphosphine) bromide, react for 10 hours, filter, remove the solvent from the filtrate, and recrystallize the obtained white solid with ethanol and dry to obtain 1,1'-(1,6-hexamethylene)bis(tributylphosphine)2,5-bis(methoxycarbonyl)phenylphosphonate.
[0117] Embodiment 21
[0118] 415g of terephthalic acid, 225mL of ethylene glycol and 11.45g of 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite are added to a reaction kettle, nitrogen is filled to remove the air in the kettle, and the pressure is increased to 0.1MPa; the temperature is raised to 240°C within 2 hours to start the esterification reaction, the pressure in the kettle is controlled to be 0.3-0.4MPa, maintained for 2 hours, and then the temperature is gradually raised to 260°C, and after the esterification reaction is completed, vacuum is drawn, and low vacuum polycondensation is carried out at 260-270°C for 0.5-2 hours, and then the temperature is raised to 270°C, and after high vacuum (pressure <80Pa) polycondensation reaction is carried out for 1-4 hours, the material is discharged.
[0119] The copolymer has an intrinsic viscosity [η] of 0.57 dL / g, a limiting oxygen index of 25.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 76%, and an antibacterial rate against Escherichia coli of 79%.
[0120] Embodiment 22
[0121] 415 g of terephthalic acid, 230 mL of ethylene glycol and 34.35 g of 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0122] The copolymer has an intrinsic viscosity [η] of 0.62 dL / g, a limiting oxygen index of 27.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 86%, and an antibacterial rate against Escherichia coli of 82%.
[0123] Embodiment 23
[0124] 415 g of terephthalic acid, 240 mL of ethylene glycol and 57.25 g of 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0125] The copolymer has an intrinsic viscosity [η] of 0.68 dL / g, a limiting oxygen index of 29.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 91%, and an antibacterial rate against Escherichia coli of 92%.
[0126] Embodiment 24
[0127] 415 g of terephthalic acid, 250 mL of ethylene glycol and 80.15 g of 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0128] The copolymer has an intrinsic viscosity [η] of 0.72 dL / g, a limiting oxygen index of 31.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 92%, and an antibacterial rate against Escherichia coli of 93%.
[0129] Embodiment 25
[0130] 415 g of terephthalic acid, 260 mL of ethylene glycol and 114.5 g of 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0131] The copolymer has an intrinsic viscosity [η] of 0.78 dL / g, a limiting oxygen index of 32.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 94%, and an antibacterial rate against Escherichia coli of 95%.
[0132] Embodiment 26
[0133] 415 g of terephthalic acid, 280 mL of ethylene glycol and 229 g of 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0134] The copolymer has an intrinsic viscosity [η] of 0.80 dL / g, a limiting oxygen index of 36.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 97%, and an antibacterial rate against Escherichia coli of 96%.
[0135] Embodiment 27
[0136] 415 g of terephthalic acid, 320 mL of ethylene glycol and 343.5 g of 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0137] The copolymer has an intrinsic viscosity [η] of 0.89 dL / g, a limiting oxygen index of 39.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 98%, and an antibacterial rate against Escherichia coli of 99%.
[0138] Embodiment 28
[0139] 415 g of terephthalic acid, 240 mL of ethylene glycol and 85.05 g of 1-butyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0140] The copolymer has an intrinsic viscosity [η] of 0.71 dL / g, a limiting oxygen index of 29.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 96%, and an antibacterial rate against Escherichia coli of 99%.
[0141] Embodiment 29
[0142] 415 g of terephthalic acid, 240 mL of ethylene glycol and 89.95 g of 1-hexyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0143] The copolymer has an intrinsic viscosity [η] of 0.69 dL / g, a limiting oxygen index of 29.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 99.1%, and an antibacterial rate against Escherichia coli of 99.2%.
[0144] Embodiment 30
[0145] 415 g of terephthalic acid, 250 mL of ethylene glycol and 99.75 g of 1-decyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0146] The copolymer has an intrinsic viscosity [η] of 0.65 dL / g, a limiting oxygen index of 29.0%, a vertical combustion grade of V-2, an antibacterial rate of 99.9% against Staphylococcus aureus, and an antibacterial rate of 99.9% against Escherichia coli.
[0147] Embodiment 31
[0148] 415 g of terephthalic acid, 220 mL of ethylene glycol and 0.1 g of trimethyl phosphate (stabilizer) were added to a reactor, and esterification was carried out according to the steps and conditions of Example 21. After the esterification was completed, an ethylene glycol solution containing 60.52 g of N-butylpyridine [2,8-di(methoxy)carbonyl] anthracene oxaphosphite was added to the reactor under nitrogen protection, and the temperature was controlled at 240°C. After the addition, the nitrogen was stopped and vacuum was started. The reaction mixture was polycondensed at 260-270°C in a low vacuum for 0.5 to 2 hours, and then the temperature was raised to 270°C in a high vacuum (pressure <100 Pa) for polycondensation reaction for 1 to 3 hours before discharging the mixture.
[0149] The copolymer has an intrinsic viscosity [η] of 0.76 dL / g, a limiting oxygen index of 31.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 94%, and an antibacterial rate against Escherichia coli of 98%.
[0150] Embodiment 32
[0151] 485 g of dimethyl terephthalate, 280 mL of ethylene glycol and 59.40 g of 1,2-dimethyl-3-ethylimidazole 2,8-bis(5-methoxycarbonyl-1H-benzimidazol-2-yl)anthracene oxaphosphite are added to a reaction kettle, nitrogen is filled to remove the air in the kettle, and an ester exchange reaction is carried out at 190-210° C. for 2-4 hours. After the ester exchange is completed, the temperature is raised to 240° C., vacuum is drawn, and a low vacuum polycondensation reaction is carried out at 240-260° C. for 0.5-2 hours. The temperature is then raised to 270° C. and a high vacuum (pressure <80 Pa) polycondensation reaction is carried out for 1-3 hours before discharging the material.
[0152] The copolymer has an intrinsic viscosity [η] of 0.67 dL / g, a limiting oxygen index of 28.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 88%, and an antibacterial rate against Escherichia coli of 91%.
[0153] Embodiment 33
[0154] 485 g of dimethyl terephthalate, 290 mL of ethylene glycol and 118.8 g of 1,2-dimethyl-3-ethylimidazole 2,8-di(5-methoxycarbonyl-1H-benzimidazol-2-yl)anthracene oxaphosphite were added to a reaction kettle, and ester exchange and polycondensation reactions were carried out according to the steps and conditions of Example 32, and then the material was discharged.
[0155] The copolymer has an intrinsic viscosity [η] of 0.74 dL / g, a limiting oxygen index of 32.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 94%, and an antibacterial rate against Escherichia coli of 96%.
[0156] Embodiment 34
[0157] 485 g of dimethyl terephthalate, 280 mL of ethylene glycol and 120.8 g of 1,2-dimethyl-3-ethylimidazole 2,8-di(5-methoxycarbonyl-1H-benzoxazol-2-yl)anthracene oxaphosphite were added to a reaction kettle, and ester exchange and polycondensation reactions were carried out according to the steps and conditions of Example 32, and then the material was discharged.
[0158] The copolymer has an intrinsic viscosity [η] of 0.72 dL / g, a limiting oxygen index of 31.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 95%, and an antibacterial rate against Escherichia coli of 95%.
[0159] Embodiment 35
[0160] 485 g of dimethyl terephthalate, 280 mL of ethylene glycol and 6.08 g of 1-butyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and after ester exchange and polycondensation reactions were carried out according to the steps and conditions of Example 32, the material was discharged.
[0161] The copolymer has an intrinsic viscosity [η] of 0.45 dL / g, a limiting oxygen index of 24.5%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 75%, and an antibacterial rate against Escherichia coli of 74%.
[0162] Embodiment 36
[0163] 415 g of terephthalic acid, 220 mL of ethylene glycol and 1.27 g of disodium 1,4-dimethyl terephthalate-2,5-diphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0164] The intrinsic viscosity [η] of the copolymer is 0.45 dL / g; the antibacterial rate against Staphylococcus aureus is 40%, and the antibacterial rate against Escherichia coli is 40%.
[0165] Embodiment 37
[0166] 415 g of terephthalic acid, 220 mL of ethylene glycol and 0.63 g of disodium 1,4-dimethyl terephthalate-2,5-diphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0167] The intrinsic viscosity [η] of the copolymer is 0.31 dL / g; the antibacterial rate against Staphylococcus aureus is 30%, and the antibacterial rate against Escherichia coli is 30%.
[0168] Embodiment 38
[0169] After the polymer obtained in Example 35 is dried under nitrogen protection, the sample is pre-crystallized at 80-180°C for 0.25-4 hours under nitrogen protection at normal pressure, and then the sample is placed in a solid phase polycondensation reaction device and continued to be polycondensed at 180-240°C under high vacuum for 2-8 hours to obtain the target polymer.
[0170] The copolymer has an intrinsic viscosity [η] of 1.12 dL / g, a limiting oxygen index of 24.5%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 75%, and an antibacterial rate against Escherichia coli of 74%.
[0171] Embodiment 39
[0172] After the polymer obtained in Example 36 is dried under nitrogen protection, the sample is pre-crystallized at 80-180°C for 0.25-4 hours under nitrogen protection at normal pressure, and then the sample is placed in a solid phase polycondensation reaction device and continued to be polycondensed at 180-240°C under high vacuum for 2-8 hours to obtain the target polymer.
[0173] The copolymer has an intrinsic viscosity [η] of 0.90 dL / g, a limiting oxygen index of 23.5%, a vertical combustion grade of V-2, an antibacterial rate of 40% for Staphylococcus aureus, and an antibacterial rate of 40% for Escherichia coli.
[0174] Embodiment 40
[0175] After the polymer obtained in Example 37 is dried under nitrogen protection, the sample is pre-crystallized at 80-180°C for 0.25-4 hours under nitrogen protection at normal pressure, and then the sample is placed in a solid phase polycondensation reaction device and continued to be polycondensed at 180-240°C under high vacuum for 2-8 hours to obtain the target polymer.
[0176] The copolymer has an intrinsic viscosity [η] of 0.72 dL / g, a limiting oxygen index of 22.5%, a vertical combustion grade of V-2, an antibacterial rate of 30% for Staphylococcus aureus, and an antibacterial rate of 30% for Escherichia coli.
[0177] Embodiment 41
[0178] 415 g of terephthalic acid, 230 mL of ethylene glycol and 18.98 g of dipotassium 1,4-dimethyl terephthalate-2,5-diphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0179] The copolymer has an intrinsic viscosity [η] of 0.74 dL / g, a limiting oxygen index of 25.0%, a vertical combustion grade of V-2, an antibacterial rate of 40% for Staphylococcus aureus, and an antibacterial rate of 40% for Escherichia coli.
[0180] Embodiment 42
[0181] 485 g of dimethyl terephthalate, 240 mL of ethylene glycol and 25.30 g of dipotassium 1,4-dimethyl terephthalate-2,5-diphosphonate were added to a reaction kettle, and ester exchange and polycondensation reactions were carried out according to the steps and conditions of Example 32 to discharge the material.
[0182] The copolymer has an intrinsic viscosity [η] of 0.82 dL / g, a limiting oxygen index of 28%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 42%, and an antibacterial rate against Escherichia coli of 43%.
[0183] Embodiment 43
[0184] 485 g of dimethyl terephthalate, 240 mL of ethylene glycol and 63.25 g of dipotassium 1,4-dimethyl terephthalate-2,5-diphosphonate were added to a reaction kettle, and ester exchange and polycondensation reactions were carried out according to the process of Example 32 to discharge the material.
[0185] The copolymer has an intrinsic viscosity [η] of 0.89 dL / g, a limiting oxygen index of 31%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 48%, and an antibacterial rate against Escherichia coli of 47%.
[0186] Embodiment 44
[0187] 485 g of dimethyl terephthalate, 280 mL of ethylene glycol and 75.80 g of tetra-n-butylphosphino[2,8-di(methoxy)carbonyl]anthracene oxaphosphite were added to a reaction kettle, and ester exchange and polycondensation reactions were carried out according to the process of Example 32 to discharge the material.
[0188] The copolymer has an intrinsic viscosity [η] of 0.70 dL / g, a limiting oxygen index of 31%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 96%, and an antibacterial rate against Escherichia coli of 97%.
[0189] Embodiment 45
[0190] 415 g of terephthalic acid, 225 mL of ethylene glycol and 25.35 g of 1-ethyl-3-methylimidazole 2-(2-methoxycarbonyl)ethylphenyl hypophosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 21, and then the material was discharged.
[0191] The copolymer has an intrinsic viscosity [η] of 0.70 dL / g, a limiting oxygen index of 30.0%, a vertical combustion grade of V-2, an antibacterial rate of 79% against Staphylococcus aureus, and an antibacterial rate of 90% against Escherichia coli.
[0192] Embodiment 46
[0193] 415 g of terephthalic acid, 230 mL of ethylene glycol and 42.25 g of 1-ethyl-3-methylimidazole 2-(2-methoxycarbonyl)ethylphenyl hypophosphorous acid were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 21 to discharge the material.
[0194] The copolymer has an intrinsic viscosity [η] of 0.65 dL / g, a limiting oxygen index of 32.0%, a vertical combustion grade of V-0, an antibacterial rate of 90% for Staphylococcus aureus, and an antibacterial rate of 94% for Escherichia coli.
[0195] Embodiment 47
[0196] 415 g of terephthalic acid, 220 mL of ethylene glycol and 0.4225 g of 1-ethyl-3-methylimidazole 2-(2-methoxycarbonyl)ethylphenyl hypophosphorous acid were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 21, and then the material was discharged.
[0197] The copolymer has an intrinsic viscosity [η] of 0.16 dL / g, a limiting oxygen index of 22.5%, a vertical combustion grade of V-2, an antibacterial rate of 30% for Staphylococcus aureus, and an antibacterial rate of 30% for Escherichia coli.
[0198] Embodiment 48
[0199] 415 g of terephthalic acid, 290 mL of ethylene glycol and 338 g of 1-ethyl-3-methylimidazole 2-(2-methoxycarbonyl)ethylphenyl hypophosphorous acid were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 21, and then the material was discharged.
[0200] The copolymer has an intrinsic viscosity [η] of 0.35 dL / g, a limiting oxygen index of 57%, a vertical combustion grade of V-0, an antibacterial rate of 99.9% for Staphylococcus aureus, and an antibacterial rate of 99.9% for Escherichia coli.
[0201] Embodiment 49
[0202] 415 g of terephthalic acid, 225 mL of ethylene glycol and 19.95 g of 2-(2-methoxycarbonyl)ethylphenyl potassium hypophosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 21, and then the material was discharged.
[0203] The copolymer has an intrinsic viscosity [η] of 0.71 dL / g, a limiting oxygen index of 27.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 45%, and an antibacterial rate against Escherichia coli of 45%.
[0204] Embodiment 50
[0205] 415 g of terephthalic acid, 225 mL of ethylene glycol, 0.1 g of trimethyl phosphate (stabilizer) and 38.96 g of dipotassium 1,4-dimethyl terephthalate-2,5-diphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 21, and then the material was discharged.
[0206] The copolymer has an intrinsic viscosity [η] of 0.84 dL / g, a limiting oxygen index of 29.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 99%, and an antibacterial rate against Escherichia coli of 99.1%.
[0207] Embodiment 51
[0208] 415 g of terephthalic acid, 220 mL of ethylene glycol, 0.1 g of triphenyl phosphate (stabilizer) and an ethylene glycol solution containing 49.5 g of 1-butyl-3-methylimidazole 2-(2-hydroxyethoxycarbonyl)ethylphenyl hypophosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 21, and then the material was discharged.
[0209] The copolymer has an intrinsic viscosity [η] of 0.62 dL / g, a limiting oxygen index of 30.0%, a vertical combustion grade of V-0, an antibacterial rate against Staphylococcus aureus of 98%, and an antibacterial rate against Escherichia coli of 96%.
[0210] Embodiment 52
[0211] 415 g of terephthalic acid, 230 mL of ethylene glycol and 55.5 g of 1-hexyl-3-methylimidazole 2,8-di(5-methoxycarbonyl-1H-benzimidazol-2-yl)anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0212] The copolymer has an intrinsic viscosity [η] of 0.64 dL / g, a limiting oxygen index of 32.0%, a vertical combustion grade of V-0, an antibacterial rate against Staphylococcus aureus of 96%, and an antibacterial rate against Escherichia coli of 97%.
[0213] Embodiment 53
[0214] 415 g of terephthalic acid, 260 mL of ethylene glycol and 174 g of 1-ethyl-3-methylimidazole 2,8-di(5-methoxycarbonyl-1H-benzimidazol-2-yl)anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0215] The copolymer has an intrinsic viscosity [η] of 0.72 dL / g, a limiting oxygen index of 51.0%, a vertical combustion grade of V-0, an antibacterial rate against Staphylococcus aureus of 98%, and an antibacterial rate against Escherichia coli of 98.5%.
[0216] Embodiment 54
[0217] 415 g of terephthalic acid, 225 mL of ethylene glycol and 32.7 g of di(1-ethyl-3-methylimidazole)(4-methoxycarbonylphenyl)phosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 21, and then the material was discharged.
[0218] The copolymer has an intrinsic viscosity [η] of 0.82 dL / g, a limiting oxygen index of 26.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 90%, and an antibacterial rate against Escherichia coli of 92%.
[0219] Embodiment 55
[0220] 415 g of terephthalic acid, 225 mL of ethylene glycol, 0.1 g of trimethyl phosphate (stabilizer), 21.9 g of dipotassium (4-methoxycarbonylphenyl)phosphonate and 10.1 g of di(tributyl-n-octylphosphine) 3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0221] The copolymer has an intrinsic viscosity [η] of 0.79 dL / g, a limiting oxygen index of 26.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 95%, and an antibacterial rate against Escherichia coli of 96%.
[0222] Embodiment 56
[0223] 415 g of terephthalic acid, 230 mL of ethylene glycol and 37.05 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0224] The copolymer has an intrinsic viscosity [η] of 0.72 dL / g, a limiting oxygen index of 26.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 90%, and an antibacterial rate against Escherichia coli of 92%.
[0225] Embodiment 57
[0226] 415 g of terephthalic acid, 220 mL of ethylene glycol, 0.1 g of trimethyl phosphate (stabilizer) and 1222.7 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0227] The copolymer has an intrinsic viscosity [η] of 0.69 dL / g, a limiting oxygen index of 57.0%, a vertical combustion grade of V-0, an antibacterial rate of 99.9% for Staphylococcus aureus, and an antibacterial rate of 99.9% for Escherichia coli.
[0228] Embodiment 58
[0229] 415 g of terephthalic acid, 300 mL of ethylene glycol, 0.1 g of trimethyl phosphate (stabilizer) and 370.5 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0230] The copolymer has an intrinsic viscosity [η] of 0.74 dL / g, a limiting oxygen index of 43.0%, a vertical combustion grade of V-0, an antibacterial rate of 99% for Staphylococcus aureus, and an antibacterial rate of 99% for Escherichia coli.
[0231] Embodiment 59
[0232] 415 g of terephthalic acid, 400 mL of ethylene glycol, 0.1 g of trimethyl phosphate (stabilizer) and 741 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0233] The copolymer has an intrinsic viscosity [η] of 0.74 dL / g, a limiting oxygen index of 53.0%, a vertical combustion grade of V-0, an antibacterial rate of 99.99% against Staphylococcus aureus, and an antibacterial rate of 99.99% against Escherichia coli.
[0234] Embodiment 60
[0235] 415 g of terephthalic acid, 230 mL of ethylene glycol, 15.3 g of sodium dimethyl isophthalate-5-sulfonate and 18.98 g of dipotassium 1,4-dimethyl terephthalate-2,5-diphosphonate were added to a reaction kettle, and after esterification and polycondensation reactions were carried out according to the process of Example 21, the semi-dull copolyester was obtained.
[0236] The copolymer has an intrinsic viscosity [η] of 0.78 dL / g, a limiting oxygen index of 26.0%, a vertical combustion grade of V-2, an antibacterial rate of 30% for Staphylococcus aureus, and an antibacterial rate of 30% for Escherichia coli.
[0237] Embodiment 61
[0238] 415 g of terephthalic acid, 230 mL of ethylene glycol, 12.31 g of titanium dioxide (matting agent) and 17.5 g of 3,5-bis(methoxycarbonyl)phenylphosphonic acid dipotassium salt were added to a reaction kettle, and after esterification and polycondensation reactions were carried out according to the process of Example 21, the material was discharged to obtain a fully matting copolyester.
[0239] The copolymer has an intrinsic viscosity [η] of 0.77 dL / g, a limiting oxygen index of 25.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 40%, and an antibacterial rate against Escherichia coli of 45%.
[0240] Embodiment 62
[0241] 415 g of terephthalic acid, 240 mL of ethylene glycol, 0.1 g of trimethyl phosphate (stabilizer), 0.55 g of titanium dioxide (matting agent) and 59.3 g of di(tetra-n-butylphosphine) 3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and after esterification and polycondensation reactions were carried out according to the process of Example 21, the material was discharged to obtain a bright copolyester.
[0242] The copolymer has an intrinsic viscosity [η] of 0.88 dL / g, a limiting oxygen index of 28.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 96%, and an antibacterial rate against Escherichia coli of 96%.
[0243] Embodiment 63
[0244] 415 g of terephthalic acid, 400 mL of ethylene glycol, 262.5 g of dipotassium 3,5-bis(methoxycarbonyl)benzenephosphonate and 427.5 g of 1-decyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0245] The copolymer has an intrinsic viscosity [η] of 0.69 dL / g, a limiting oxygen index of 53.0%, a vertical combustion grade of V-0, an antibacterial rate of 99.99% against Staphylococcus aureus, and an antibacterial rate of 99.99% against Escherichia coli.
[0246] Embodiment 64
[0247] 415 g of terephthalic acid, 590 mL of ethylene glycol, 700 g of dipotassium 3,5-bis(methoxycarbonyl)benzenephosphonate and 270.75 g of 1-decyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0248] The copolymer has an intrinsic viscosity [η] of 0.61 dL / g, a limiting oxygen index of 57.0%, a vertical combustion grade of V-0, an antibacterial rate of 99.99% against Staphylococcus aureus, and an antibacterial rate of 99.99% against Escherichia coli.
[0249] Embodiment 65
[0250] 200 g of the copolymer obtained in Example 24 was weighed and placed in a reactor containing 240 mL of ethylene glycol. The reaction was carried out at 180° C. for 3 hours under nitrogen protection. The copolymer was completely depolymerized, no solid residue was left, and the solution system was clear and transparent without discoloration. Excess ethylene glycol was removed, and the resulting product was a mixture of 1,4-ethylene terephthalate-2,5-diphosphonic acid dipotassium and ethylene terephthalate. The mixture could be used for repolymerization without further separation and purification.
[0251] Embodiment 66
[0252] 200 g of the copolymer obtained in Example 42 was weighed and placed in a reactor containing 240 mL of ethylene glycol. The mixture was reacted at 180° C. for 2 hours under nitrogen protection. The copolymer was completely depolymerized, no solid residue was left, and the solution system was clear and transparent without discoloration. Excess ethylene glycol was removed, and the resulting product was a mixture of 1,4-ethylene glycol terephthalate-2,5-diphosphonic acid dipotassium and ethylene glycol terephthalate. The mixture could be used for repolymerization without further separation and purification.
[0253] Embodiment 67
[0254] 415 g of terephthalic acid, 230 mL of propylene glycol and 57.25 g of 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0255] The copolymer has an intrinsic viscosity [η] of 0.71 dL / g, a limiting oxygen index of 24.5.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 71%, and an antibacterial rate against Escherichia coli of 75%.
[0256] Embodiment 68
[0257] 415 g of terephthalic acid, 240 mL of propylene glycol, 26.25 g of dipotassium 3,5-bis(methoxycarbonyl)phenylphosphonate and 57.25 g of 1-ethyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0258] The copolymer has an intrinsic viscosity [η] of 0.80 dL / g, a limiting oxygen index of 26.5%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 74%, and an antibacterial rate against Escherichia coli of 78%.
[0259] Embodiment 69
[0260] 415 g of terephthalic acid, 245 mL of 1,4-butanediol and 61.75 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0261] The copolymer has an intrinsic viscosity [η] of 0.89 dL / g, a limiting oxygen index of 25.5.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 78%, and an antibacterial rate against Escherichia coli of 81%.
[0262] Embodiment 70
[0263] 415 g of terephthalic acid, 245 mL of 1,4-butanediol and 60.9 g of [2,8-di(methoxy)carbonyl]anthracene oxaphosphite potassium salt were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0264] The copolymer has an intrinsic viscosity [η] of 0.84 dL / g, a limiting oxygen index of 24.5.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 45%, and an antibacterial rate against Escherichia coli of 40%.
[0265] Embodiment 71
[0266] 415 g of terephthalic acid, 250 mL of 1,4-butanediol, 9.25 g of sodium [2,8-di(methoxy)carbonyl]anthracene oxaphosphite and 68.75 g of di(1-butyl-3-methylimidazole) 3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0267] The copolymer has an intrinsic viscosity [η] of 0.89 dL / g, a limiting oxygen index of 25.5.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 80%, and an antibacterial rate against Escherichia coli of 85%.
[0268] Embodiment 72
[0269] 540 g of 2,6-naphthalene dicarboxylic acid, 260 mL of ethylene glycol, and 96.05 g of di(1-butyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 21 to discharge the product.
[0270] The copolymer has an intrinsic viscosity [η] of 0.86 dL / g, a limiting oxygen index of 27.5.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 90%, and an antibacterial rate against Escherichia coli of 87%.
[0271] Embodiment 73
[0272] 540 g of 2,6-naphthalene dicarboxylic acid, 270 mL of 1,4-butanediol, 39.75 g of disodium 3,5-bis(methoxycarbonyl)phenylphosphonate and 37.05 g of di(1-hexyl-3-methylimidazole) 3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21 to discharge the material.
[0273] The copolymer has an intrinsic viscosity [η] of 0.81 dL / g, a limiting oxygen index of 27.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 92%, and an antibacterial rate against Escherichia coli of 88%.
[0274] Embodiment 74
[0275] 415 g of terephthalic acid, 395 g of 1,4-cyclohexanedimethanol and 86.5 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 21.
[0276] The copolymer has an intrinsic viscosity [η] of 0.64 dL / g, a limiting oxygen index of 25.5.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 90%, and an antibacterial rate against Escherichia coli of 87%.
[0277] Embodiment 75
[0278] Add 468g of 2,5-furandicarboxylic acid, 270mL of ethylene glycol and 86.45g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate into the reaction kettle, and pressurize it to 0.1MPa under nitrogen protection; react at 160-210°C for 2-5 hours, control the pressure in the kettle to be 0.3-0.4MPa, evacuate after esterification is complete, perform low vacuum polycondensation at 220-240°C for 1-2 hours, then raise the temperature to 250°C, perform high vacuum polycondensation (pressure <80Pa) for 1-8 hours, and discharge the material.
[0279] The copolymer has an intrinsic viscosity [η] of 0.87 dL / g, a limiting oxygen index of 27.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 76%, and an antibacterial rate against Escherichia coli of 79%.
[0280] Embodiment 76
[0281] 552.3 g of furan-2,5-dicarboxylic acid dimethyl ester, 520 mL of ethylene glycol and 52.5 g of 3,5-bis(methoxycarbonyl)phenylphosphonic acid dipotassium were added to the reactor, and reacted at 160-210° C. for 2-5 hours under nitrogen protection. After the ester exchange was complete, the reaction was evacuated and polycondensed at 220-240° C. under low vacuum for 1-2 hours. The temperature was then raised to 250° C. and polycondensed under high vacuum (pressure <80 Pa) for 1-8 hours before discharging the material.
[0282] The copolymer has an intrinsic viscosity [η] of 0.77 dL / g, a limiting oxygen index of 26.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 45%, and an antibacterial rate against Escherichia coli of 40%.
[0283] Embodiment 77
[0284] 552.3 g of furan-2,5-dicarboxylic acid dimethyl ester, 520 mL of ethylene glycol, 0.05 g of trimethyl phosphate (stabilizer) and 76 g of 1-hexyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to the reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 76 to discharge the material.
[0285] The copolymer has an intrinsic viscosity [η] of 0.73 dL / g, a limiting oxygen index of 26.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 99%, and an antibacterial rate against Escherichia coli of 99%.
[0286] Embodiment 78
[0287] 552.3 g of furan-2,5-dicarboxylic acid dimethyl ester, 540 mL of ethylene glycol and 135 g of di(tributyl-n-octylphosphine)-3,5-bis(methoxycarbonyl)phenylphosphonate were added to the reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 76.
[0288] The copolymer has an intrinsic viscosity [η] of 0.87 dL / g, a limiting oxygen index of 31.0%, a vertical combustion grade of V-2, an antibacterial rate of 99.9% against Staphylococcus aureus, and an antibacterial rate of 99.9% against Escherichia coli.
[0289] Embodiment 79
[0290] First, add 552.3 g of furan-2,5-dicarboxylic acid dimethyl ester, 600 mL of 1,4-butanediol and 135 g of di(tributyl-n-octylphosphine)-3,5-bis(methoxycarbonyl)phenylphosphonate into the reaction kettle, and carry out esterification and polycondensation reactions according to the steps and conditions of Example 76 to discharge the material.
[0291] The copolymer has an intrinsic viscosity [η] of 0.93 dL / g, a limiting oxygen index of 26.0%, a vertical combustion grade of V-2, an antibacterial rate of 99.9% against Staphylococcus aureus, and an antibacterial rate of 99.9% against Escherichia coli.
[0292] Embodiment 80
[0293] 241 g of adipic acid, 224 g of terephthalic acid, 600 mL of 1,4-butanediol, 0.05 g of trimethyl phosphate (stabilizer) and 44.5 g of di(1-ethyl-3-methylimidazole) 3,5-bis(methoxycarbonyl)phenylphosphonate were added into a reaction kettle, and reacted at 140-220° C. for 2-5 hours under nitrogen protection. After esterification was complete, vacuum was evacuated, and low-vacuum polycondensation was performed at 220-250° C. for 1-2 hours. The temperature was raised to 255° C., and polycondensation was performed at high vacuum (pressure <50 Pa) for 1.5-3 hours before discharging the material.
[0294] The copolymer has an intrinsic viscosity [η] of 1.37 dL / g, a limiting oxygen index of 25.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 85%, and an antibacterial rate against Escherichia coli of 87%.
[0295] Embodiment 81
[0296] 241 g of adipic acid, 224 g of terephthalic acid, 600 mL of 1,4-butanediol, 31.5 g of dipotassium 3,5-bis(methoxycarbonyl)benzenephosphonate and 15.5 g of 1-hexyl-3-methylimidazole [2,8-di(methoxy)carbonyl] anthracene oxaphosphite were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 80 to discharge the material.
[0297] The copolymer has an intrinsic viscosity [η] of 1.31 dL / g, a limiting oxygen index of 24%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 89%, and an antibacterial rate against Escherichia coli of 90%.
[0298] Embodiment 82
[0299] 472 g of succinic acid, 430 mL of 1,4-butanediol, 0.05 g of trimethyl phosphate (stabilizer) and 47.2 g of di(1-ethyl-3-methylimidazole) 3,5-bis(methoxycarbonyl)phenylphosphonate are added to a reaction kettle, and reacted at 120-180° C. for 2-5 hours under nitrogen protection. After esterification is complete, vacuum is evacuated, and low-vacuum polycondensation is performed at 200-220° C. for 1-2 hours. Then the temperature is raised to 230° C., and the polycondensation reaction is performed under high vacuum (pressure <50 Pa) for 1.5-8 hours before discharging the material.
[0300] The copolymer has an intrinsic viscosity [η] of 1.97 dL / g, a limiting oxygen index of 24%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 86%, and an antibacterial rate against Escherichia coli of 88%.
[0301] Embodiment 83
[0302] 472 g of succinic acid, 430 mL of 1,4-butanediol, 0.05 g of trimethyl phosphate (stabilizer), 42 g of dipotassium 3,5-bis(methoxycarbonyl)phenylphosphonate and 19.76 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 82 to discharge the material.
[0303] The copolymer has an intrinsic viscosity [η] of 2.10 dL / g, a limiting oxygen index of 24.5%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 75%, and an antibacterial rate against Escherichia coli of 78%.
[0304] Embodiment 84
[0305] 415 g of isophthalic acid, 230 mL of ethylene glycol and 26.25 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the process of Example 21, and then the material was discharged.
[0306] The copolymer has an intrinsic viscosity [η] of 0.84 dL / g, a limiting oxygen index of 24.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 76%, and an antibacterial rate against Escherichia coli of 78%.
[0307] Embodiment 85
[0308] 382 g of terephthalic acid, 33 g of isophthalic acid, 230 mL of ethylene glycol, and 34.25 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0309] The copolymer has an intrinsic viscosity [η] of 0.81 dL / g, a limiting oxygen index of 25.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 81%, and an antibacterial rate against Escherichia coli of 83%.
[0310] Embodiment 86
[0311] 415 g of terephthalic acid, 182 g of isosorbide, 180 mL of ethylene glycol, and 37.05 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0312] The copolymer has an intrinsic viscosity [η] of 0.78 dL / g, a limiting oxygen index of 27.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 79%, and an antibacterial rate against Escherichia coli of 86%.
[0313] Embodiment 87
[0314] 354 g of succinic acid, 177 g of isosorbide, 140 mL of 1,4-butanediol and 37.05 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to the reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 82, and then the material was discharged.
[0315] The copolymer has an intrinsic viscosity [η] of 1.08 dL / g, a limiting oxygen index of 23.5%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 79%, and an antibacterial rate against Escherichia coli of 86%.
[0316] Embodiment 88
[0317] 485 g of dimethyl terephthalate, 300 mL of 1,4-butanediol, 520 g of polytetramethylene ether glycol (polytetrahydrofuran diol, PTMEG, Mn=1000), 0.2 g of Irganox1098 (antioxidant) and 68.05 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate are added to a reaction kettle, and reacted at 160-220° C. for 2-5 hours under nitrogen protection. After the ester exchange is complete, vacuum is drawn, and low-vacuum polycondensation is carried out at 220-240° C. for 0.5-2 hours. The temperature is then raised to 250° C., and polycondensation is carried out under high vacuum (pressure <50 Pa) for 1.5-4 hours before discharging.
[0318] The copolymer has an intrinsic viscosity [η] of 1.28 dL / g, a limiting oxygen index of 24.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 76%, and an antibacterial rate against Escherichia coli of 78%.
[0319] Embodiment 89
[0320] 485 g of dimethyl terephthalate, 300 mL of 1,4-butanediol, 150 g of polytetramethylene ether glycol (polytetrahydrofuran, PTMEG, Mn=1000), 0.2 g of Irganox1098 (antioxidant), 49.55 g of 2,8-bis(5-methoxycarbonyl-1H-benzimidazol-2-yl) anthracene oxaphosphite potassium and 12.3 g of di(1-hexyl-3-methylimidazole) 3,5-bis(methoxycarbonyl) benzenephosphonate were added to the reaction kettle. After transesterification and polycondensation reaction were carried out according to the process of Example 82, the material was discharged.
[0321] The copolymer has an intrinsic viscosity [η] of 1.18 dL / g, a limiting oxygen index of 24.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 97%, and an antibacterial rate against Escherichia coli of 98%.
[0322] Embodiment 90
[0323] 600g of caprolactam, 47g of adipic acid and 16mL of water were added to the reactor, and the ring-opening polymerization of caprolactam was carried out at 240°C under nitrogen protection. After 4 hours of reaction, a carboxyl-terminated polyamide prepolymer was obtained and dried. 300g of the obtained polyamide prepolymer, 140g of polyethylene glycol (Mn=1000), 0.2g of Irganox1098 (antioxidant), and 20.55g of di(1-hexyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were weighed and added to the reactor, and reacted at 240-260°C for 2-3 hours under nitrogen protection, and then vacuuming was started, and low vacuum polycondensation was carried out at 260°C for 0.5 hour, and then the temperature was raised to 280°C, and polycondensation was carried out under high vacuum (pressure <100Pa) for 1.5-4 hours, and then the material was discharged.
[0324] The copolymer has an intrinsic viscosity [η] of 1.09 dL / g, a limiting oxygen index of 28.0%, a vertical combustion grade of V-2, an antibacterial rate of 81% for Staphylococcus aureus, and an antibacterial rate of 86% for Escherichia coli.
[0325] Embodiment 91
[0326] A polyamide prepolymer was prepared according to the steps and conditions of Example 90. Then 300 g of the polyamide prepolymer, 140 g of polytetramethylene ether glycol (Mn=1000), 0.2 g of Irganox1098 (antioxidant), 18.55 g of 2,8-bis(5-methoxycarbonyl-1H-benzimidazol-2-yl) anthracene oxaphosphite potassium and 16.3 g of di(1-hexyl-3-methylimidazole) 3,5-bis(methoxycarbonyl) benzenephosphonate were weighed and added to a reaction kettle. After transesterification and polycondensation reactions were carried out according to the steps and conditions of Example 90, the material was discharged.
[0327] The copolymer has an intrinsic viscosity [η] of 1.14 dL / g, a limiting oxygen index of 27.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 96%, and an antibacterial rate against Escherichia coli of 97%.
[0328] Embodiment 92
[0329] 600g of lauryl lactam, 36g of adipic acid and 16mL of water were added to a reactor. Under nitrogen protection, ring-opening polymerization of caprolactam was carried out at 240°C. After 4 hours of reaction, a carboxyl-terminated polyamide prepolymer was obtained and dried. 300g of the obtained polyamide prepolymer, 140g of polypropylene glycol (Mn=1000), 0.2g of Irganox1098 (antioxidant) and 20.55g of di(1-butyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were weighed and added to the reactor. After transesterification and polycondensation reaction were carried out according to the steps and conditions of Example 90, the material was discharged.
[0330] The copolymer has an intrinsic viscosity [η] of 1.03 dL / g, a limiting oxygen index of 26.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 87%, and an antibacterial rate against Escherichia coli of 84%.
[0331] Embodiment 93
[0332] 300 g PA66 polyamide prepolymer (Mn=1000), 140 g polypropylene glycol (Mn=1000), 0.2 g Irganox 1098 (antioxidant), and 20.55 g di(1-butyl-3-methylimidazole) 3,5-bis(methoxycarbonyl)phenylphosphonate were added to the reaction kettle. After transesterification and polycondensation reaction were carried out according to the steps and conditions of Example 90, the material was discharged.
[0333] The copolymer has an intrinsic viscosity [η] of 1.23 dL / g, a limiting oxygen index of 29.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 86%, and an antibacterial rate against Escherichia coli of 85%.
[0334] Embodiment 94
[0335] 457g of bisphenol A, 450g of diphenyl carbonate and 29.6g of di(1-ethyl-3-methylimidazole) 3,5-bis(methoxycarbonyl)phenylphosphonate were added to the reaction kettle. Under nitrogen protection, the ester exchange reaction was carried out at 160-180°C for 0.5-3 hours; then vacuum was started, and low vacuum polycondensation was carried out at 210-260°C for 0.5-2 hours, and then the temperature was raised, and the polycondensation reaction was carried out at 270-300°C under high vacuum (pressure <50Pa) for 1-3 hours, and then the material was discharged.
[0336] The copolymer has an intrinsic viscosity [η] of 0.62 dL / g, a limiting oxygen index of 37.0%, a vertical combustion grade of V-0, an antibacterial rate of 79% against Staphylococcus aureus, and an antibacterial rate of 85% against Escherichia coli.
[0337] Embodiment 95
[0338] 457 g of bisphenol A, 450 g of diphenyl carbonate and 7.4 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to the reaction kettle, and the ester exchange and polycondensation reactions were carried out according to the process of Example 94, and the material was discharged.
[0339] The copolymer has an intrinsic viscosity [η] of 0.58 dL / g, a limiting oxygen index of 32.0%, a vertical combustion grade of V-1, an antibacterial rate against Staphylococcus aureus of 74%, and an antibacterial rate against Escherichia coli of 81%.
[0340] Embodiment 96
[0341] 457 g of bisphenol A, 450 g of diphenyl carbonate and 11.1 g of sodium 2,8-bis(5-methoxycarbonyl-1H-benzimidazol-2-yl)anthracene oxaphosphite were added to the reaction kettle, and the ester exchange and polycondensation reaction were carried out according to the process of Example 94, and the material was discharged.
[0342] The copolymer has an intrinsic viscosity [η] of 0.58 dL / g, a limiting oxygen index of 33.0%, a vertical combustion grade of V-0, an antibacterial rate against Staphylococcus aureus of 45%, and an antibacterial rate against Escherichia coli of 55%.
[0343] Embodiment 97
[0344] 457 g of bisphenol A, 450 g of diphenyl carbonate, 3.5 g of dipotassium 3,5-bis(methoxycarbonyl)phenylphosphonate and 4.9 g of di(1-decyl-3-methylimidazole) 3,5-bis(methoxycarbonyl)phenylphosphonate were added to the reaction kettle, and transesterification and polycondensation were carried out according to the steps and conditions of Example 94 to discharge the product.
[0345] The copolymer has an intrinsic viscosity [η] of 0.55 dL / g, a limiting oxygen index of 31.0%, a vertical combustion grade of V-1, an antibacterial rate against Staphylococcus aureus of 98%, and an antibacterial rate against Escherichia coli of 99%.
[0346] Embodiment 98
[0347] 445 g of bisphenol A, 450 g of diphenyl carbonate and 1.6 g of di(tetra-n-butylphosphine)3,5-bis(methoxycarbonyl)phenylphosphonate were added to the reaction kettle, and transesterification and polycondensation were carried out according to the steps and conditions of Example 94 to discharge the product.
[0348] The copolymer has an intrinsic viscosity [η] of 0.59 dL / g, a limiting oxygen index of 30.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 82%, and an antibacterial rate against Escherichia coli of 90%.
[0349] Embodiment 99
[0350] 401 g of bisphenol F, 450 g of diphenyl carbonate and 7.4 g of di(1-ethyl-3-methylimidazole)3,5-bis(methoxycarbonyl)phenylphosphonate were added to the reaction kettle, and the ester exchange and polycondensation reactions were carried out according to the process of Example 94, and the materials were discharged.
[0351] The copolymer has an intrinsic viscosity [η] of 0.63 dL / g, a limiting oxygen index of 29.0%, a vertical combustion grade of V-2, an antibacterial rate against Staphylococcus aureus of 72%, and an antibacterial rate against Escherichia coli of 80%.
[0352] Embodiment 100
[0353] 501 g of bisphenol S, 450 g of diphenyl carbonate and 15.8 g of di(tetra-n-butylphosphine)3,5-bis(methoxycarbonyl)phenylphosphonate were added to the reaction kettle, and transesterification and polycondensation were carried out according to the steps and conditions of Example 95 to discharge the material.
[0354] The copolymer has an intrinsic viscosity [η] of 0.60 dL / g, a limiting oxygen index of 32.0%, a vertical combustion grade of V-0, an antibacterial rate against Staphylococcus aureus of 92%, and an antibacterial rate against Escherichia coli of 90%.
[0355] Embodiment 101
[0356] 438 g of isosorbide, 675 g of diphenyl carbonate and 26.1 g of di(tributyl-n-octylphosphine)-3,5-bis(methoxycarbonyl)phenylphosphonate were added to the reaction kettle, and the ester exchange and polycondensation reaction were carried out according to the process of Example 95, and the material was discharged.
[0357] The copolymer has an intrinsic viscosity [η] of 0.64 dL / g, a limiting oxygen index of 33.0%, a vertical combustion grade of V-0, an antibacterial rate of 99% for Staphylococcus aureus, and an antibacterial rate of 99% for Escherichia coli.
[0358] Comparative Example 1
[0359] 415 g of terephthalic acid, 250 mL of ethylene glycol and 0.2 g of ethylene glycol antimony were added to the reaction kettle, and the esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0360] The copolymer has an intrinsic viscosity [η] of 0.65 dL / g, a limiting oxygen index of 21.0%, a vertical combustion grade of no grade, an antibacterial rate for Staphylococcus aureus of 20%, and an antibacterial rate for Escherichia coli of 19%.
[0361] Comparative Example 2
[0362] 415 g of terephthalic acid, 250 mL of ethylene glycol and 0.1 g of tetrabutyl titanate were added to a reaction kettle, and esterification and polycondensation reactions were carried out according to the steps and conditions of Example 21, and then the material was discharged.
[0363] The copolymer has an intrinsic viscosity [η] of 0.72 dL / g, a limiting oxygen index of 21.0%, a vertical combustion grade of no grade, an antibacterial rate of Staphylococcus aureus of 20%, and an antibacterial rate of Escherichia coli of 19%.
Claims
1. A self-catalytic functional reaction monomer, Features The general structural formula of the self-catalytic functional reaction monomer is as follows: In the formula, Z 1 , Z 2 is a carboxyl group, ester group, amino group, hydroxyl group, acyloxy group or a is an integer from 1 to 12, Z 1 , Z 2 Same or different; Z 3 , Z 4 is a hydrogen atom, a C1-C12 alkyl group, a cyano group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an amide group, an aryl group or a substituted aryl group, and Z 3 , Z 4 Same or different; Z 6 is an H atom, a C1-C12 alkyl group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an amide group, an aryl group, a substituted aryl group, an ester group, a carboxyl group, a hydroxyl group, an amino group, an acyloxy group, or a is an integer of 1 to 12; W is an O atom or an S atom, and Y is an O atom, an S atom, a secondary amino group, a nitrogen methyl group, a nitrogen ethyl group or an amide group; when the reaction monomer structure is BCDGRS, M n+ is an organic cation; when the reaction monomer structure is TU, M n+ is an organic cation or an alkali metal ion; the organic cation M n+ For the following B 3 -B 5 Any of the cations of the general structural formula, wherein n is an integer of 1 to 2: In the formula, Z 7 is a C2-C16 alkyl, aryl or substituted aryl; Z 11 is a C2-C16 alkylene or arylene group; Z 12 is a C1-C16 alkyl, aryl or substituted aryl group; X is an O atom, a S atom, a C1-C16 nitrogen alkyl or nitrogen aryl group.
2. The self-catalytic functional reaction monomer according to claim 1, Features In the general structural formula of the self-catalytic functional reaction monomer, the ester group is a methyl ester group, an ethyl ester group, a propyl ester group, a butyl ester group, a pentyl ester group or a hexyl ester group after esterification of a monohydric alcohol, or a phenyl ester group after esterification of a monohydric phenol, or any one of an ethylene glycol ester group, a propylene glycol ester group, a butylene glycol group, a neopentyl glycol ester group, a diethylene glycol ester group, a glycerol ester group or a pentaerythritol ester group after esterification of a polyhydric alcohol.
3. A functional copolymer of autocatalytic polymerization and autocatalytic depolymerization, Features The copolymer is a copolymer of a wholly aromatic polyester, a semi-aromatic polyester, an aliphatic polyester, an aliphatic-aromatic polyester, a bio-based polyester, a polycarbonate, a polyester elastomer, a nylon elastomer or a modified polymer of the above polymers and a self-catalytic functional reaction monomer, and the self-catalytic functional reaction monomer is fully connected to the molecular chain of the copolymer, and is composed of the following structural units represented by Ⅰ, Ⅱ, Ⅲ or Ⅰ, Ⅱ, Ⅳ: In the formula, R 1 It represents a polyamide segment terminated by an arylene group, a darylene group, a C2-C12 alkylene group or dalkylene group, a 2,5-furyl group, a carboxylic acid group or an ester group; In the formula, R 2 represents an arylene group, a dylene group, a C2-C12 alkylene group or dylene group, a 4,4'-isopropylidene diphenyl group, a 4,4'-diphenylmethane group, a 4,4'-diphenyl sulfone group, an isosorbide group, a polyether polyol group or a polyester polyol group; In the formula, R 3 , R 4 is a carbonyl group, a secondary amine group, an O atom or a is an integer from 1 to 12, R 3 , R 4 Same or different; R 5 , R 6 is a hydrogen atom, a C1-C12 alkyl group, a cyano group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an amide group, an aryl group or a substituted aryl group, and R 5 , R 6 Same or different; R 7 is an H atom, a C1-C12 alkyl group, a hydroxyl group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an aryl group or a substituted aryl group; W is an O atom or an S atom, and Y is an O atom, an S atom, a secondary amino group, a nitrogen methyl group, a nitrogen ethyl group or an amide group; the cation M n+ is an alkali metal ion or has the following B 3 -B 5 Any of the organic cations of the general structural formula: In the formula, Z 7 is a C2-C16 alkyl, aryl or substituted aryl; Z 11 is a C2-C16 alkylene or arylene group; Z 12 is a C1-C16 alkyl, aryl or substituted aryl group; X is an O atom, a S atom, a C1-C16 nitrogen alkyl or nitrogen aryl group; In the formula, R 3 is a carbonyl group, a secondary amine group, an O atom or a is an integer from 1 to 12; R 5 is a hydrogen atom, a C1-C12 alkyl group, a cyano group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an amide group, an aryl group, or a substituted aryl group; R 7 is an H atom, a C1-C12 alkyl group, a hydroxyl group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an aryl group or a substituted aryl group; W is an O atom or a S atom; the cation M n+ is an alkali metal ion or has the following B 3 -B 5 Any of the organic cations of the general structural formula: In the formula, Z 7 is a C2-C16 alkyl, aryl or substituted aryl; Z 11 is a C2-C16 alkylene or arylene group; Z 12 is a C1-C16 alkyl, aryl or substituted aryl group; X is an O atom, a S atom, a C1-C16 nitrogen alkyl or nitrogen aryl group; The number of structural units of [III] is 0.05 to 99% of the number of structural units of [I]; the number of structural units of [IV] is 0.05 to 40% of the number of structural units of [I]. The intrinsic viscosity [η] of the copolymer is 0.16 to 2.10 dL / g, the limiting oxygen index is 22.5 to 57.0%, the vertical combustion grade is V-2 to V-0, the antibacterial rate of Staphylococcus aureus is 30 to 99.99%, and the antibacterial rate of Escherichia coli is 30 to 99.99%.
4. The functional copolymer of self-catalytic polymerization and self-catalytic depolymerization according to claim 3, Features The copolymer can undergo a self-depolymerization chemical reaction when the temperature is raised to 120-280° C. in an alcohol reaction medium at normal pressure or when the temperature is raised to 120-280° C. in an alcohol reaction medium under pressure, and the target monomer can be recovered again, and the target monomer can be directly used for the repolymerization of the copolymer without separation and purification.
5. The functional copolymer of self-catalytic polymerization and self-catalytic depolymerization according to claim 3, Features The number of structural units of the copolymer [III] is 0.1 to 60% of the number of structural units of [I]; the number of structural units of [IV] is 0.1 to 30% of the number of structural units of [I]; the intrinsic viscosity [η] of the copolymer is 0.20 to 2.10 dL / g; the limiting oxygen index is 23.5 to 53.0%, the vertical combustion grade is V-2 to V-0, the antibacterial rate of Staphylococcus aureus is 40 to 99.99%, and the antibacterial rate of Escherichia coli is 40 to 99.99%.
6. A method for preparing the functional copolymer of self-catalytic polymerization and self-catalytic depolymerization as claimed in claim 3, wherein the method comprises preparing the functional copolymer of self-catalytic polymerization and self-catalytic depolymerization by melt polycondensation or further solid phase polycondensation by mixing dicarboxylic acid or dicarboxylic acid ester and diol or phenol polymer monomers in conventional proportions, performing esterification or ester exchange by conventional direct esterification or transesterification, Features Before esterification or transesterification reaction or before polycondensation after esterification reaction, 0.05-99% of dipolymerization functional group autocatalytic functional reaction monomer or 0.05-40% of monopolymerization functional group autocatalytic functional reaction monomer is added into the reaction system based on the molar number of dibasic acid or dibasic acid ester in the polymer monomer.
7. The method for preparing a functional copolymer of autocatalytic polymerization and autocatalytic depolymerization according to claim 6, Features In the method, the molar number of the dibasic acid or dibasic acid ester added to the polymer monomer is 0.1-60% of the dipolymerization functional group self-catalytic functional reaction monomer or 0.1-30% of the monopolymerization functional group self-catalytic functional reaction monomer.
8. The method for preparing a functional copolymer of autocatalytic polymerization and autocatalytic depolymerization according to claim 6 or 7, Features The self-catalytic functional reaction monomer used in the method is at least one of the following structural formulas: In the formula, Z 1 , Z 2 is a carboxyl group, ester group, amino group, hydroxyl group, acyloxy group or a is an integer from 1 to 12, Z 1 , Z 2 Same or different; Z 3 , Z 4 is a hydrogen atom, a C1-C12 alkyl group, a cyano group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an amide group, an aryl group or a substituted aryl group, and Z 3 , Z 4 Same or different; Z 6 is an H atom, a C1-C12 alkyl group, a C1-C12 alkoxy group, a secondary amino group, a tertiary amino group, an amide group, an aryl group, a substituted aryl group, an ester group, a carboxyl group, a hydroxyl group, an amino group, an acyloxy group, or a is an integer of 1 to 12; W is an O atom or a S atom, Y is an O atom, a S atom, a secondary amino group, a nitrogen methyl group, a nitrogen ethyl group or an amide group; the cation M n+ is an alkali metal ion or has the following B 3 -B 5 Any one of the organic cations of the general structural formula, wherein n is an integer of 1 to 2: In the formula, Z 7 is a C2-C16 alkyl, aryl or substituted aryl; Z 11 is a C2-C16 alkylene or arylene group; Z 12 is a C1-C16 alkyl, aryl or substituted aryl group; X is an O atom, a S atom, a C1-C16 nitrogen alkyl or nitrogen aryl group.
9. The method for preparing a functional copolymer of autocatalytic polymerization and autocatalytic depolymerization according to claim 8, Features The ester group in the structure of the self-catalytic functional reaction monomer used in the method is a methyl ester group, an ethyl ester group, a propyl ester group, a butyl ester group, a pentyl ester group or a hexyl ester group after esterification of a monohydric alcohol, or a phenyl ester group after esterification of a monohydric phenol, or any one of an ethylene glycol ester group, a propylene glycol ester group, a butylene glycol group, a neopentyl glycol ester group, a diethylene glycol ester group, a glycerol ester group or a pentaerythritol ester group after esterification of a polyhydric alcohol.
10. Use of the functional copolymer of self-catalytic polymerization and self-catalytic depolymerization according to claim 3, Features The functional copolymer is used in the fields of fibers and their products, non-woven fabrics, engineering plastics, membrane materials, container materials, packaging materials, biomedical materials, shape memory materials or 3D printing materials, or as a functional additive for the modification of polymer materials.
Citation Information
Patent Citations
Phosphoric flame-proof copolyester ionomer and preparation method thereof
CN101225158A
High-temperature self-crosslinking flame-retardant anti-dripping copolyester and preparation method thereof
CN102174183A
Flame retardant anti-droplet copolyester based on benzimidazole structure, and preparation method thereof
CN108395526A
Ionic monomer of benzo-heterocycle structure containing phosphorus and nitrogen, copolyester-type ionomer utilizing ionic monomer for flame retarding, and preparation methods and application of ionic monomer and copolyester-type ionomer
CN110016054A
Ionic monomer containing benzo heterocyclic sulfonate structure, ionomer using same for flame resistance and molten resistance, and preparation method and application thereof
CN110066389A