A method for preparing a PERC battery
By using phosphorus doped oxide layer and laser windowing technology in the preparation of PERC cells, the tunnel oxide layer and poly-finger structure are formed, which solves the problems of complex process and underlying damage in the prior art, significantly improves the battery efficiency and Reduced costs and is suitable for mass production.
Patent Information
- Application Number
- CN202210764248.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-06-30
AI Technical Summary
The existing PERC battery preparation method is complex, and it is difficult to accurately control the figure size. Direct laser windowing can easily damage the bottom emitter, limiting the improvement of battery efficiency.
Using the phosphorus-doped oxide layer to grow on the front of the P-type silicon wafer as a mask, the tunnel oxide layer is formed by laser window opening and chemical oxidation treatment, and the phosphorus-doped amorphous silicon thin film is grown in situ and annealed to form a poly-finger Structure: Use laser to accurately open the window without damaging the bottom emitter, and removes the mask in the non-metalized area to improve battery efficiency.
It realizes simple process, accurate and controllable graphics, reduces under-metal composite, significantly improves battery efficiency, and reduces preparation costs, making it suitable for mass production applications.
Smart Images

Figure CN115207135B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photovoltaics and relates to a method for preparing a PERC cell. Background Art
[0002] PERC cells are the mainstream solar cells on the market. The efficiency of mass-produced PERC cells can reach 23.0-23.5%, but it is difficult to increase the efficiency of cells further, mainly due to the interface and passivation under the metal. At present, in PERC cells, the selective emitter technology is used to achieve heavy phosphorus doping under the metal, which can improve the efficiency of the cell. However, the recombination under the metal is still relatively high, which has become the main factor limiting the improvement of cell efficiency. In addition, by making a tunneling contact structure (poly-finger structure) on the front of the PERC cell, the cell efficiency can also be improved. However, the existing method for preparing PERC cells mainly adopts the following methods to prepare the poly-finger structure, such as preparing the poly-finger structure by first preparing the front poly-Si, mask, wet etching, phosphorus diffusion and annealing. This process still has the following defects: the process is complex, the cleaning process is increased, the yield is difficult to guarantee, the printing mask increases the risk of pollution, and the feasibility of mass production is small; the wet etching accuracy is poor, the width of the poly-Si under the patterned mask will be affected by the etching, and it cannot be made very fine, and the process window is small; because it is not a simple in-situ doping method, it is difficult to control the light and heavy doping formed by annealing and phosphorus diffusion at the same time, which is not conducive to reducing the composite under the metal, making it difficult to effectively improve the cell efficiency. For example, the poly-finger structure is prepared by direct laser windowing and secondary diffusion, which also has the defects of being difficult to control due to the complex process flow and small process window, and the direct laser windowing is easy to damage the underlying emitter, which also makes it difficult to effectively improve the cell efficiency. Therefore, obtaining a preparation method for PERC cells with simple process, easy operation, precise and controllable graphic size, and high efficiency is of great significance for the promotion and application of PERC cells. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a method for preparing a PERC battery with simple process, easy operation, precise and controllable graphic size and high efficiency.
[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions.
[0005] A method for preparing a PERC battery comprises the following steps:
[0006] S1, texturing the front side of the P-type silicon wafer;
[0007] S2, growing a phosphorus-doped oxide layer on the front side of the P-type silicon wafer as a mask;
[0008] S3, using laser to perform window processing on the metallized area;
[0009] S4, sequentially performing texturing and chemical oxidation treatment on the laser window opening area to form a tunneling oxide layer;
[0010] S5, growing a phosphorus-doped amorphous silicon film on the front side of the P-type silicon wafer;
[0011] S6, performing annealing treatment on the P-type silicon wafer with the phosphorus-doped amorphous silicon film grown on the front side, so as to simultaneously form a poly-finger structure and a lightly-doped phosphorus expansion region on the front side of the silicon wafer;
[0012] S7, using laser to perform window processing on the non-metallized area until the mask of the non-metallized area is exposed;
[0013] S8. Remove the mask of the non-metallized area to complete the preparation of the PERC cell.
[0014] The above preparation method is further improved, in step S2, a phosphorus-doped oxide layer is grown on the front side of the P-type silicon wafer by using a PECVD method or a PVD method; the thickness of the phosphorus-doped oxide layer is 20nm to 300nm; the phosphorus doping concentration of the phosphorus-doped oxide layer is 1E19 cm -3 ~1E21 cm -3 ; The phosphorus-doped oxide layer is a phosphorus-doped silicon oxide layer.
[0015] The above preparation method is further improved, in step S2, the thickness of the phosphorus-doped oxide layer is 50nm-150nm; the phosphorus doping concentration of the phosphorus-doped oxide layer is 5E19 cm -3 ~6E20 cm -3 .
[0016] The above-mentioned preparation method is further improved. In step S1, an alkaline solution is used to texture the front side of the P-type silicon wafer to form a pyramid texture surface; the size of the pyramid texture surface is 0.5μm to 3μm; the alkaline solution is at least one of potassium hydroxide solution, sodium hydroxide solution, and TMAH solution; the resistivity of the P-type silicon wafer is 0.3Ω·cm to 7Ω·cm.
[0017] The above preparation method is further improved, in step S3, the window width of the metallized area is 20 μm to 150 μm.
[0018] The above-mentioned preparation method is further improved. In step S4, an alkaline solution is used to texture the laser window opening area to remove laser damage and form a pyramid velvet surface; the size of the pyramid velvet surface is 0.5μm to 3μm; the alkaline solution is at least one of potassium hydroxide solution, sodium hydroxide solution, and TMAH solution.
[0019] The above-mentioned preparation method is further improved. In step S4, the texturing area is chemically oxidized using one of ozone, concentrated nitric acid, a mixed solution of concentrated hydrochloric acid and hydrogen peroxide, and a mixed solution of concentrated sulfuric acid and hydrogen peroxide to form a tunneling oxide layer on the texturing area; the thickness of the tunneling oxide layer is 0.5nm to 2.5nm; the tunneling oxide layer is a silicon oxide layer.
[0020] The above preparation method is further improved, in step S5, a phosphorus-doped amorphous silicon film is in-situ grown on the front side of the P-type silicon wafer by a PECVD method or a PVD method; the thickness of the phosphorus-doped amorphous silicon film is 20nm to 300nm; the phosphorus doping concentration of the phosphorus-doped oxide layer is 5E19 cm -3 ~1E21 cm -3 .
[0021] The above preparation method is further improved, in step S6, the annealing temperature is 800°C to 950°C; the sheet resistance of the poly-finger structure is 10Ω / sq to 80Ω / sq; the sheet resistance of the lightly doped phosphorus extension region is 120Ω / sq to 250Ω / sq.
[0022] The above preparation method is further improved, in step S8, a hydrofluoric acid solution is used to clean the mask in the non-metallized area to complete the removal of the mask.
[0023] The above preparation method is further improved, and in step S8, before removing the mask of the non-metallized area, it also includes: polishing the back side of the P-type silicon wafer by an etching method.
[0024] The above-mentioned preparation method is further improved. In step S8, after removing the mask of the non-metallized area, it also includes: growing a passivation layer on the front and back sides of the P-type silicon wafer, growing an anti-reflection layer on the front and back sides of the P-type silicon wafer, opening a window on the back side, metallization, sintering and post-processing.
[0025] The above preparation method is further improved by growing a passivation layer on the front side of the P-type silicon wafer by thermal oxidation; the passivation layer is a silicon oxide layer and / or a silicon nitride layer; the thickness of the passivation layer is 1nm to 5nm.
[0026] The above preparation method is further improved by using ALD or PEALD to grow a passivation layer on the back of the P-type silicon wafer; the passivation layer is an aluminum oxide layer; the thickness of the passivation layer is 3nm to 20nm.
[0027] The above-mentioned preparation method is further improved by using the PECVD method to grow anti-reflection layers on the front and back sides of the P-type silicon wafer respectively; the anti-reflection layer is a film layer or a plurality of stacked films selected from silicon nitride, silicon oxynitride, and silicon oxide; the thickness of the anti-reflection layer is 60nm to 150nm.
[0028] The above-mentioned preparation method is further improved by using laser to open a window on the back side of the P-type silicon wafer.
[0029] The above-mentioned preparation method is further improved by using screen printing or laser transfer to prepare front auxiliary gate lines and front main gate electrodes on the front side of the P-type silicon wafer, and to prepare back auxiliary gate lines and back main gate electrodes on the back side of the P-type silicon wafer, to complete the metallization treatment of the silicon wafer; the front auxiliary gate lines and front main gate electrodes are silver electrodes; the back auxiliary gate lines are aluminum electrodes; and the back main gate electrodes are silver electrodes.
[0030] The above-mentioned preparation method is further improved, wherein the post-processing includes processing the battery cell by light injection or electric injection.
[0031] Compared with the prior art, the advantages of the present invention are:
[0032] In view of the defects of the preparation method of PERC cells, such as complex process, difficult operation, difficulty in accurately controlling the size of patterns, great damage to the underlying emitter and low efficiency caused by them, the present invention creatively proposes a preparation method of PERC cells, firstly growing a phosphorus-doped oxide layer on the front side of the silicon wafer after texturing as a mask; then using a laser to perform window opening, texturing and chemical oxidation on the metallized area on the front side of the silicon wafer, wherein texturing can remove the damaged layer caused by the first laser window opening and re-form a pyramid velvet surface on the surface of the metallized area of the silicon wafer, and chemical oxidation can form a tunneling oxide layer on the velvet surface of the metallized area on the front side of the silicon wafer; then in-situ growing a phosphorus-doped amorphous silicon film on the front side of the silicon wafer and performing annealing In principle, through annealing treatment, amorphous silicon is converted into poly-Si, that is, the phosphorus-doped amorphous silicon in the metallized area is converted into phosphorus-doped polysilicon, which forms a contact passivation structure (n+poly-finger structure) with the tunneling oxide layer. At the same time, a low-concentration n+ emitter is formed on the surface of the silicon wafer below the doped silicon oxide, which is the bottom emitter; further, a laser is used to open a window in the non-metallized area on the front side of the silicon wafer, and the phosphorus-doped polysilicon on the lightly phosphorus-doped area (non-metallized area) is removed under the protection of the phosphorus-doped oxide layer (mask) until the bottom doped oxide layer (mask) is exposed, so the bottom emitter will not be damaged when the laser is used to open the window. Finally, the mask is removed by cleaning to complete the preparation of the PERC battery. Compared with the conventional preparation method, in the preparation method of the present invention, a poly-finger structure is introduced on the front side of the silicon wafer by laser windowing, and the graphic size precision is controllable, which greatly reduces the process complexity and cost investment. At the same time, the poly-finger structure prepared thereby can not only ensure that the recombination under the metal is greatly reduced, but also greatly reduce the absorption of light on the front side, thereby effectively reducing the recombination under the front metal, greatly improving the open circuit voltage and fill factor of the battery, and thus significantly improving the battery efficiency. The preparation method of the PERC battery of the present invention has the advantages of simple process, easy operation, precise and controllable graphic size, and little damage to the bottom emitter, and the PERC battery prepared thereby has better efficiency. At the same time, the preparation method of the present invention is highly overlapped with the conventional PERC battery preparation route, and only CVD equipment needs to be added to prepare the poly-finger structure, so the existing production line can be effectively used to complete the production, which is conducive to further reducing the preparation cost and is more suitable for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0034] Figure 1 Schematic diagram of the preparation process of the PERC cell in Example 1 of the present invention.
[0035] Figure 2 Schematic diagram of the structure of the PERC cell in Example 1 of the present invention.
[0036] Legend:
[0037] 1. P-type silicon wafer; 2. n+ emitter; 3. front passivation layer; 4. front anti-reflection layer; 5. tunneling oxide layer; 6. phosphorus-doped polysilicon layer; 7. silver electrode; 8. back passivation layer; 9. back anti-reflection layer; 10. aluminum electrode. DETAILED DESCRIPTION
[0038] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby.
[0039] The materials and instruments used in the following examples are all commercially available.
[0040] Example:
[0041] A method for preparing a PERC battery comprises the following steps:
[0042] S1. Use an alkaline solution to texture the front side of a P-type silicon wafer to form a pyramid texture surface with a size of 0.5 μm to 3 μm, wherein the alkaline solution is at least one of a potassium hydroxide solution, a sodium hydroxide solution, and a TMAH solution, and the resistivity of the P-type silicon wafer is 0.3 Ω·cm to 7 Ω·cm. Preferably, the size of the pyramid texture surface is 1.0 μm to 2.5 μm; the resistivity of the P-type silicon wafer is 1 Ω·cm to 3 Ω·cm.
[0043] S2. Use PECVD or PVD to grow a phosphorus-doped oxide layer on the front of the P-type silicon wafer as a mask, where the phosphorus-doped oxide layer is a phosphorus-doped silicon oxide layer (n+SiOx layer) with a thickness of 20nm to 300nm and a phosphorus doping concentration of 1E19 cm -3 ~1E21 cm -3 Further preferably, the thickness of the phosphorus-doped oxide layer is 50nm to 150nm, and the phosphorus doping concentration is 5E19 cm -3 ~6E20 cm -3 More preferably, the thickness of the phosphorus-doped oxide layer is 50 nm to 80 nm, and the phosphorus doping concentration is 5E19 cm -3 ~5E20 cm -3 In the present invention, by controlling the doping concentration of the phosphorus-doped silicon oxide layer, it is beneficial to achieve accurate control of the doping curve. At the same time, compared with other masks (such as phosphorus-doped silicon nitride layer, phosphorus-doped silicon oxynitride film layer), the phosphorus-doped silicon oxide layer (n+SiOx layer) used as a mask in the present invention is easier to remove.
[0044] S3. Use laser to open windows in the metallized area, wherein the window width of the metallized area is 20μm to 150μm (preferably, the width is 30μm to 80μm). Compared with conventional window opening methods (such as wet method, screen printing), in the present invention, the vault is higher by laser window opening, wherein the accuracy can be controlled within ±10μm, while the conventional screen printing method (printing accuracy ±25μm, screen accuracy ±20μm, plus the influence of wet etching), the patterning accuracy is >±50μm. At the same time, in the present invention, by laser window opening, a higher window opening accuracy can be controlled, which means that the subsequent efficiency improvement space is larger, the process window and stability are better. In addition, the laser process used in the present invention can save a lot of cleaning links, and the process is simpler.
[0045] S4. Use an alkaline solution to texture the laser window area to remove laser damage and form a pyramid velvet surface with a size of 0.5μm to 3μm (preferably, a size of 1.0μm to 1.5μm), the alkaline solution is at least one of potassium hydroxide solution, sodium hydroxide solution, and TMAH solution; then, use one of ozone, concentrated nitric acid, a mixed solution of concentrated hydrochloric acid and hydrogen peroxide, and a mixed solution of concentrated sulfuric acid and hydrogen peroxide to chemically oxidize the textured area to form a tunneling oxide layer, wherein the tunneling oxide layer is a silicon oxide layer with a thickness of 0.5nm to 2.5nm, and more preferably, a thickness of 1nm to 2nm.
[0046] S5. Use PECVD or PVD to grow a phosphorus-doped amorphous silicon film on the front of a P-type silicon wafer, where the thickness of the phosphorus-doped oxide layer is 20nm to 300nm and the phosphorus doping concentration is 5E19 cm -3 ~1E21 cm -3 Further preferably, the thickness of the phosphorus-doped amorphous silicon film is 50 nm to 150 nm, and the phosphorus doping concentration is 1E20 cm -3 ~7E20 cm -3 In the present invention, by controlling the doping concentration of the phosphorus-doped amorphous silicon film, it is beneficial to achieve accurate control of the doping curve.
[0047] S6. Annealing the P-type silicon wafer with phosphorus-doped amorphous silicon film grown on the front side at a temperature of 800°C to 950°C (preferably, 880°C to 930°C), and simultaneously forming a poly-finger structure and a lightly doped phosphorus expansion area on the front side of the silicon wafer. In the present invention, in the laser windowing area, there is only doped amorphous silicon, and the area without laser windowing is doped silicon oxide + doped amorphous silicon. Light and heavy doping can be achieved by controlling the amount of two sources, that is, light doping and heavy doping are formed simultaneously, wherein the square resistance of the heavily phosphorus-doped area (the metallized pattern area where the poly-finger structure is located) is 10 to 80Ω / sq, preferably, the square resistance is 40 to 60Ω / sq; the square resistance of the lightly doped phosphorus expansion area (non-metallized pattern area) is 120 to 250Ω / sq, preferably, the square resistance is 180 to 200Ω / sq.
[0048] S7, using laser to open the window of the non-metallized area until the mask of the non-metallized area is exposed. In the present invention, the phosphorus-doped polysilicon on the lightly phosphorus-expanded area (non-metallized area) is removed under the protection of the phosphorus-doped oxide layer (mask) until the bottom doped oxide layer (mask) is exposed, so that the bottom emitter will not be damaged when the laser is used to open the window, which is beneficial to improve the efficiency of the battery.
[0049] S8. Clean the mask in the non-metallized area with a hydrofluoric acid solution to remove the mask in the non-metallized area.
[0050] In the present invention, before removing the mask of the non-metallized area, the method further comprises: polishing the back side of the P-type silicon wafer by using an etching method.
[0051] At the same time, after removing the mask of the non-metallized area, it also includes: growing a passivation layer on the front and back of the P-type silicon wafer, growing an anti-reflection layer on the front and back of the P-type silicon wafer, opening a window on the back, metallization, sintering and post-processing, as follows:
[0052] A passivation layer is grown on the front of a P-type silicon wafer by thermal oxidation, wherein the passivation layer is a silicon oxide layer and / or a silicon nitride layer, and the thickness of the passivation layer is 1nm to 5nm, preferably, the thickness is 2nm to 3nm. In the present invention, silicon nitride is both an anti-reflection layer and a passivation layer, so a silicon oxide layer is used as a bottom layer and a silicon nitride layer is deposited on the silicon oxide layer, so that a better cross-sectional passivation effect can be obtained, because silicon oxide has a very good passivation effect, and together with silicon nitride, it plays a dual passivation role, and silicon nitride has a very low hydrogen passivation and silicon oxide interface state density, and has a good interface passivation effect. If a silicon nitride layer is used alone as a passivation layer and an anti-reflection layer, it can be prepared by chemical vapor deposition (such as PECVD method), and the thickness of the silicon nitride layer is 60nm to 100nm, preferably, the thickness is 70nm to 80nm.
[0053] A passivation layer is grown on the back of a P-type silicon wafer by using an ALD method or a PEALD method, wherein the passivation layer is an aluminum oxide layer with a thickness of 3nm to 20nm, preferably, a thickness of 8nm to 15nm.
[0054] The PECVD method is used to grow anti-reflection layers on the front and back sides of the P-type silicon wafer, wherein the anti-reflection layer is a film layer or a plurality of stacked films selected from silicon nitride, silicon oxynitride, and silicon oxide, and the thickness of the anti-reflection layer is 60nm to 150nm, preferably, the thickness is 60nm to 130nm, further preferably, the thickness is 60nm to 100nm, and further preferably, the thickness is 80nm to 100nm.
[0055] A laser is used to open windows on the back of the P-type silicon wafer to form a patterned area for subsequent aluminum paste printing to form ohmic contact with the silicon substrate.
[0056] The front sub-grid and the front main gate electrode are patterned on the front of the P-type silicon wafer by screen printing for current collection. The sub-grid and the n+Poly-Si need to be overprinted, and the back-printed aluminum paste and the back laser window area need to be overprinted (burn-through aluminum paste can also be used without overprinting), and the back sub-grid and the back main gate electrode are prepared on the back of the P-type silicon wafer. In this step, the front metal electrode (main gate and sub-grid) is a silver electrode, and the silver electrode needs to burn through the anti-reflection layer, but cannot burn through the doped poly-Si. The back sub-grid is aluminum plasma, and the aluminum electrode needs to burn through the aluminum oxide to form an ohmic contact with silicon. The back main gate is a silver electrode, which is mainly used for subsequent welding of the battery. Generally, the main gate is printed on the back first and then the sub-grid, and there is no requirement on the front.
[0057] Post-processing includes processing the cell using light injection or electrical injection.
[0058] Embodiment 1:
[0059] A method for preparing a PERC battery, the preparation process flow chart of which is as follows Figure 1 As shown, the following steps are included:
[0060] S1. Texturing the front side of the P-type silicon wafer, specifically: using a KOH solution with a mass fraction of 1.5% to texturing the front side of the P-type silicon wafer (first time) to form a pyramid texture surface with a size of 1.5μm; in this step, the resistivity of the P-type silicon wafer used is 1.5Ω·cm.
[0061] S2. Growing a phosphorus-doped oxide layer on the front of the P-type silicon wafer as a mask, specifically: using PECVD to grow a phosphorus-doped silicon oxide layer (n+SiOx layer) on the front of the P-type silicon wafer, wherein the thickness of the phosphorus-doped silicon oxide layer is 70 nm and the phosphorus doping concentration is 2E20 cm -3 .
[0062] S3. Use laser to perform window opening treatment on the metallized area (first laser window opening), specifically: use laser to perform patterned laser window opening treatment on the phosphorus-doped silicon oxide layer (the window opening area corresponds to the subsequent metallized area), and the width of the laser window opening area is 50μm.
[0063] S4. The laser windowing area is sequentially textured and chemically oxidized to form a tunneling oxide layer. Specifically, a KOH solution with a mass fraction of 1.5% is used to texture the front laser windowing area (for the second time) to remove the laser damaged layer and form a pyramid texture surface with a size of 1.5 μm. Then, a mixed solution of concentrated sulfuric acid and hydrogen peroxide (the mixed solution is made of concentrated sulfuric acid with a mass fraction of 98% and hydrogen peroxide with a mass fraction of 30%, and the volume ratio of the two is 7:3) is used for chemical oxidation treatment to form a tunneling oxide layer in the secondary textured area after the windowing, wherein the tunneling oxide layer is a silicon oxide layer with a thickness of 1.5 nm.
[0064] S5. Grow a phosphorus-doped amorphous silicon film on the front side of the P-type silicon wafer. Specifically, grow a phosphorus-doped amorphous silicon film on the front side using the PECVD method. The thickness of the film is 100 nm, and the phosphorus doping concentration is 5E20 cm -3 .
[0065] S6. Annealing the P-type silicon wafer with a phosphorus-doped amorphous silicon film grown on the front side, and simultaneously forming a poly-finger structure and a lightly doped phosphorus expansion area on the front side of the silicon wafer. Specifically, annealing the silicon wafer at an annealing temperature of 920°C, and simultaneously forming an n+poly-Si tunneling passivation structure (subsequent metallization pattern area, where the square resistance is 50Ω / sq) and a lightly doped phosphorus expansion area (subsequent non-metallization pattern area, light diffusion square resistance is 180Ω / sq) on the front side of the silicon wafer.
[0066] S7. Use laser to perform window opening processing on the non-metallized area (second laser window opening) until the mask of the non-metallized area is exposed. Specifically: on the front side of the silicon wafer, use laser to perform patterned window opening processing to remove the phosphorus-doped poly-Si (polycrystalline silicon) on the lightly phosphorus-expanded area to expose the underlying mask layer (n+SiOx layer). At the same time, the phosphorus-doped poly-Si on the n+poly-Si tunnel passivation structure is retained on the front side. In addition, since there is a silicon oxide mask on the lower layer, the lightly doped phosphorus-expanded silicon emitter underneath will not be damaged during laser window opening.
[0067] S8. Remove the mask of the non-metallized area, specifically: use hydrofluoric acid solution to clean and etch away the phosphorus-doped silicon oxide exposed after the laser window opening. To ensure the cleaning effect of the silicon wafer, RCA cleaning can also be performed.
[0068] In this embodiment, before removing the mask of the non-metallized area, the process further includes: polishing the back side of the P-type silicon wafer by using an etching method.
[0069] In this embodiment, after removing the mask of the non-metallized area, the process further includes: growing a passivation layer on the front and back sides of the P-type silicon wafer, growing an anti-reflection layer on the front and back sides of the P-type silicon wafer, opening windows on the back side, metallization, sintering, and post-processing, specifically:
[0070] (1) A passivation layer is grown on the front side of a P-type silicon wafer by thermal oxidation, wherein the passivation layer is a silicon oxide layer with a thickness of 3 nm.
[0071] (2) A passivation layer is grown on the back of a P-type silicon wafer using the ALD method, wherein the passivation layer is an aluminum oxide layer with a thickness of 10 nm.
[0072] (3) The PECVD method is used to grow anti-reflection layers on the front and back sides of the P-type silicon wafer, respectively. Specifically, a silicon nitride layer and a silicon oxide layer are sequentially deposited on the front and back sides, respectively. The thickness of the silicon nitride layer is 60 nm, the thickness of the silicon oxide layer is 30 nm, and the total thickness is 90 nm.
[0073] (4) A laser is used to open a window on the back of the P-type silicon wafer to form a patterned area for subsequent aluminum paste printing to form an ohmic contact with the silicon substrate.
[0074] (5) A patterned front sub-grid and front main-grid electrode are formed on the front of the P-type silicon wafer by screen printing for current collection. The sub-grid and n+Poly-Si need to be overprinted, and the back-printed aluminum paste and the back laser window area need to be overprinted (burn-through aluminum paste can also be used without overprinting), and the back sub-grid and back main-grid electrode are prepared on the back of the P-type silicon wafer. In this step, the front metal electrode (main grid and sub-grid) is a silver electrode, and the silver electrode needs to burn through the anti-reflection layer, but cannot burn through the doped poly-Si. The back sub-grid is aluminum plasma, and the aluminum electrode needs to burn through the aluminum oxide to form an ohmic contact with silicon. The back main grid is a silver electrode, which is mainly used for subsequent welding of the battery. Generally, the main grid is printed on the back first and then the sub-grid, and there is no requirement on the front.
[0075] (6) Sintering the screen-printed cell to form an ohmic contact between the metal electrode and the silicon wafer, and then post-processing the cell by electrical injection to obtain a PERC cell.
[0076] like Figure 2As shown, in this embodiment, the prepared PERC cell includes: a P-type silicon wafer 1 as a substrate, wherein the front side of the P-type silicon wafer 1 is provided with an n+ emitter 2, a front passivation layer 3 and a front anti-reflection layer 4 in sequence from the inside to the outside, and the front side of the P-type silicon wafer 1 is also provided with a silver electrode 7 penetrating the n+ emitter 2, the front passivation layer 3 and the front anti-reflection layer 4, and the front side of the P-type silicon wafer 1 and located below the silver electrode 7 are provided with a tunneling oxide layer 5 and a phosphorus-doped polysilicon layer 6 in sequence from the inside to the outside; the back side of the P-type silicon wafer 1 is provided with a back passivation layer 8 and a back anti-reflection layer 9 in sequence from the inside to the outside, and the back side of the P-type silicon wafer 1 is also provided with an aluminum electrode 10 penetrating the back passivation layer 8 and the back anti-reflection layer 9.
[0077] In this embodiment, the p-type silicon wafer 1 has a resistivity of 1.5Ω·cm; the surface phosphorus doping concentration of the n+ emitter 2 is 2E20cm -3 , the diffusion square resistance is 180Ω / sq; the front passivation layer 3 is a silicon oxide layer with a thickness of 3nm; the front anti-reflection layer 4 is a stacked film of silicon nitride and silicon oxide, wherein the thickness of the silicon nitride layer is 60nm, the thickness of the silicon oxide layer is 30nm, and the total thickness is 90nm; the tunneling oxide layer 5 is a tunneling silicon oxide layer with a thickness of 1.5nm; the thickness of the phosphorus-doped polysilicon layer 6 is 100nm, and the phosphorus doping concentration is 5E20cm -3 , with a width of 50μm; the silver electrode 7 needs to burn through the anti-reflection layer, but cannot burn through the doped poly-Si; the back passivation layer 8 is an aluminum oxide layer with a thickness of 10nm; the back anti-reflection layer 9 is a stacked film of silicon nitride and silicon oxide, in which the thickness of the silicon nitride layer is 60nm, the thickness of the silicon oxide layer is 30nm, and the total thickness is 90nm; the aluminum electrode 10 needs to burn through the aluminum oxide to form an ohmic contact with the silicon.
[0078] The electrical performance of the PERC cell prepared in Example 1 of the present invention was tested, and the results are shown in Table 1.
[0079] Table 1 Electrical performance data of the PERC cell prepared in Example 1 of the present invention
[0080]
[0081] It can be seen from Table 1 that, compared with the PERC battery (without poly-finger structure on the front) prepared by the conventional method, the efficiency of the PERC battery (with poly-finger structure on the front) prepared by the preparation method of the present invention is greatly improved, with an increase of up to 0.57%; at the same time, compared with the conventional process, the preparation process of the present invention has outstanding advantages in improving the efficiency of the PERC battery (with poly-finger structure on the front), and can more significantly improve the efficiency of the battery.
[0082] In summary, the preparation method of the PERC battery of the present invention has the advantages of simple process, easy operation, precise and controllable graphic size, and little damage to the underlying emitter, and the PERC battery prepared thereby has better efficiency. At the same time, the preparation method of the present invention highly overlaps with the conventional PERC battery preparation route, and only needs to add CVD equipment to prepare the poly-finger structure, so that the existing production line can be effectively utilized to complete production, which is conducive to further reducing the preparation cost and is more suitable for promotion and application.
[0083] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as above in the preferred embodiment, it is not used to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention, still fall within the scope of protection of the technical solution of the present invention.
Claims
1. A method for preparing a PERC battery, characterized in that: The following steps are involved: S1, texturing the front side of the P-type silicon wafer; S2, growing a phosphorus-doped oxide layer on the front side of the P-type silicon wafer as a mask; S3, using laser to perform window processing on the metallized area; S4, sequentially performing texturing and chemical oxidation treatment on the laser window opening area to form a tunneling oxide layer; S5, growing a phosphorus-doped amorphous silicon film on the front side of the P-type silicon wafer; S6, annealing the P-type silicon wafer with the phosphorus-doped amorphous silicon film grown on the front side, wherein the phosphorus-doped amorphous silicon in the metallization area is converted into phosphorus-doped polysilicon through the annealing process, and a poly-finger structure is formed with the tunneling oxide layer, and a poly-finger structure and a lightly-doped phosphorus expansion area are simultaneously formed on the front side of the silicon wafer; S7, using laser to perform window processing on the non-metallized area until the mask of the non-metallized area is exposed; S8. Remove the mask of the non-metallized area to complete the preparation of the PERC cell.
2. The preparation method according to claim 1, characterized in that In step S2, a phosphorus-doped oxide layer is grown on the front side of the P-type silicon wafer by using a PECVD method or a PVD method; the thickness of the phosphorus-doped oxide layer is 20 nm to 300 nm; and the phosphorus doping concentration of the phosphorus-doped oxide layer is 1E19 cm -3 ~1E21 cm -3 ; The phosphorus-doped oxide layer is a phosphorus-doped silicon oxide layer.
3. The preparation method according to claim 2, characterized in that In step S2, the thickness of the phosphorus-doped oxide layer is 50 nm to 150 nm; the phosphorus doping concentration of the phosphorus-doped oxide layer is 5E19 cm -3 ~6E20 cm -3 .
4. The preparation method according to any one of claims 1 to 3, characterized in that: In step S1, an alkaline solution is used to texture the front side of a P-type silicon wafer to form a pyramid texture surface; the size of the pyramid texture surface is 0.5 μm to 3 μm; the alkaline solution is at least one of a potassium hydroxide solution, a sodium hydroxide solution, and a TMAH solution; the resistivity of the P-type silicon wafer is 0.3 Ω·cm to 7 Ω·cm.
5. The preparation method according to any one of claims 1 to 3, characterized in that In step S3, the window width of the metallized area is 20 μm to 150 μm.
6. The preparation method according to any one of claims 1 to 3, characterized in that: In step S4, an alkaline solution is used to texture the laser window area to remove laser damage and form a pyramid velvet surface; the size of the pyramid velvet surface is 0.5μm to 3μm; the alkaline solution is at least one of potassium hydroxide solution, sodium hydroxide solution, and TMAH solution; the textured area is chemically oxidized by one of ozone, concentrated nitric acid, a mixed solution of concentrated hydrochloric acid and hydrogen peroxide, and a mixed solution of concentrated sulfuric acid and hydrogen peroxide to form a tunneling oxide layer on the textured area; the thickness of the tunneling oxide layer is 0.5nm to 2.5 nm; the tunneling oxide layer is a silicon oxide layer.
7. The preparation method according to any one of claims 1 to 3, characterized in that: In step S5, a phosphorus-doped amorphous silicon film is in-situ grown on the front side of the P-type silicon wafer by a PECVD method or a PVD method; the thickness of the phosphorus-doped amorphous silicon film is 20 nm to 300 nm; the phosphorus doping concentration of the phosphorus-doped oxide layer is 5E19 cm -3 ~1E21 cm -3 ; In step S6, the temperature of the annealing treatment is 800°C to 950°C; the sheet resistance of the poly-finger structure is 10Ω / sq to 80Ω / sq; the sheet resistance of the lightly doped phosphorus extension region is 120Ω / sq to 250Ω / sq; In step S8, the mask in the non-metallized area is cleaned with a hydrofluoric acid solution to complete the removal of the mask.
8. The preparation method according to any one of claims 1 to 3, characterized in that In step S8, before removing the mask of the non-metallized area, the step further includes: polishing the back side of the P-type silicon wafer by an etching method; After removing the mask of the non-metallized area, the process also includes: growing a passivation layer on the front and back sides of the P-type silicon wafer, growing an anti-reflection layer on the front and back sides of the P-type silicon wafer, opening windows on the back side, metallization, sintering and post-processing.
9. The preparation method according to claim 8, characterized in that: A passivation layer is grown on the front side of a P-type silicon wafer by thermal oxidation; the passivation layer is a silicon oxide layer and / or a silicon nitride layer; the thickness of the passivation layer is 1 nm to 5 nm; A passivation layer is grown on the back of a P-type silicon wafer by using an ALD method or a PEALD method; the passivation layer is an aluminum oxide layer; the thickness of the passivation layer is 3nm to 20nm; The PECVD method is used to grow anti-reflection layers on the front and back of the P-type silicon wafer respectively; the anti-reflection layer is a film layer or a plurality of laminated films selected from silicon nitride, silicon oxynitride, and silicon oxide; the thickness of the anti-reflection layer is 60nm to 150nm; Use laser to open windows on the back of P-type silicon wafers; The front auxiliary grid line and the front main grid electrode are prepared on the front of the P-type silicon wafer by screen printing or laser transfer, and the back auxiliary grid line and the back main grid electrode are prepared on the back of the P-type silicon wafer to complete the metallization treatment of the silicon wafer; the front auxiliary grid line and the front main grid electrode are silver electrodes; the back auxiliary grid line is an aluminum electrode; The back main grid electrode is a silver electrode; The post-processing includes processing the battery cell by light injection or electricity injection.
Citation Information
Patent Citations
IBC cell manufacturing method
CN106340568A
Fabrication method of frontal emitter junction tunneling oxidation passivation battery base on single crystal PERC
CN109216499A
Local contact passivation solar cell and preparation method thereof
CN110581198A
Preparation method of P-type passivation contact battery
CN110993744A
Preparation method of tunneling oxidation passivation battery
CN111524999A