Softener for textiles, aqueous solution of softener for textiles and method for producing the same, textiles and method for producing the same
By reacting non-silicon-based compounds with crosslinking agents to generate functional groups, the problems of high combustion and low flame retardancy of existing softeners are solved, and efficient textile softness and washing durability are achieved.
Patent Information
- Application Number
- CN202111551877.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-11-23
- Filing Date
- 2021-12-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-12-17
AI Technical Summary
The conventional softener with detergent durability has problems such as high combustion and poor flame retardancy due to the silicone component.
Use a textile softener containing a specific compound (A) and a crosslinking agent (B), which is a non-silicon-based compound, and the ether, ester or nitrogen-containing compound functional group is formed by reaction with the crosslinking agent (B). , forming a polymer coating to improve the softness and flame retardancy of the fibers.
Without degrading flame retardancy, the washing durability of textiles is improved and excellent softness and cleaning performance are provided.
Smart Images

Figure BDA0003417935050000091 
Figure BDA0003417935050000102 
Figure BDA0003417935050000103
Abstract
Description
Technical Field
[0001] The present invention relates to a softener for textiles having washing durability, a first agent and a second agent of the softener for textiles, an aqueous liquid of the softener for textiles and a method for producing the same, and textiles and a method for producing the same. Background Art
[0002] Various methods for improving the touch or feel of fibers such as polyester are well known. Conventionally, softeners containing, for example, silicone components having washing durability as a main component have been used.
[0003] Patent document 1 discloses a method for imparting softness and hand feel to fibers, characterized in that the fibers are treated with a softener comprising (a) an amino-functional polymer and (b) a silicone polymer that can react with reactive groups of the amino-functional polymer and has washing durability.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: U.S. Patent No. 5,445,652 Summary of the invention
[0007] Problems to be solved by the invention
[0008] However, the conventional softener having washing durability disclosed in Patent Document 1 contains a silicone component as a main component and therefore has a problem of exhibiting high flammability and poor flame retardancy.
[0009] Means for solving problems
[0010] The present inventors have conducted studies to solve the above-mentioned problems and have found that a softening agent for textiles containing a specific compound (A) and a cross-linking agent (B) is exactly suitable.
[0011] In order to achieve the above-mentioned object, a softening agent for textiles which is one embodiment of the present invention mainly comprises the following compound (A) and a crosslinking agent (B).
[0012] Compound (A): A non-silicone compound having a polyoxyalkylene chain in the molecule, and having a functional group (R1) capable of generating an ether, an ester or a nitrogen-containing compound by reacting with the crosslinking agent (B).
[0013] In the softening agent for textiles, the compound (A) and the crosslinking agent (B) may not have a silicon atom in the molecule.
[0014] In the above-mentioned softening agent for textiles, the above-mentioned crosslinking agent (B) may have a functional group (R2) reactive with the above-mentioned functional group (R1), the number of functional groups (R1) in one molecule of the above-mentioned compound (A) is 2 or more, and the number of functional groups (R2) in one molecule of the above-mentioned crosslinking agent (B) is 2 or more, including a combination in which the total number of functional groups (R1) and the number of functional groups (R2) is 5 or more.
[0015] In the softening agent for textiles, the mass average molecular weight of the compound (A) may be 420 or more and 10,000,000 or less.
[0016] In the softening agent for textiles, the mass average molecular weight of the compound (A) may be 4,000 to 10,000.
[0017] In the softener for textiles, the functional group equivalent of the crosslinking agent (B) may be 10 to 2000.
[0018] In the softening agent for textiles, the crosslinking agent (B) may be a compound having a polyoxyalkylene chain in its molecule.
[0019] In the above-mentioned softening agent for textiles, the above-mentioned polyoxyalkylene chain can be a polyoxymethylene chain, a polyethylene oxide chain, a polyoxypropylene chain, a polyoxyisopropylene chain, a polyoxybutylene chain, or a polyoxyalkylene chain composed of two or more oxyalkylenes selected from formaldehyde, ethylene oxide, propylene oxide, oxyisopropylene and butylene oxide.
[0020] In the softener for textiles, the mass average molecular weight of the polyoxyalkylene chain may be 400 to 9000.
[0021] The softening agent for textiles may further optionally contain a silicone compound or a silane compound, and the total content of the silicone compound and the silane compound in the softening agent for textiles is 40% by mass or less.
[0022] In the softening agent for textiles, the total content of the silicone compound and the silane compound may be 1% by mass or less.
[0023] In order to achieve the above object, the first agent of the softening agent for textiles as another embodiment of the present invention comprises the following compound (A) and is used together with a crosslinking agent (B).
[0024] Compound (A): A non-silicone compound having a polyoxyalkylene chain in the molecule, and having a functional group (R1) capable of generating an ether, an ester or a nitrogen-containing compound by reacting with the crosslinking agent (B).
[0025] In order to achieve the above object, the second agent of the softening agent for textiles as another embodiment of the present invention is characterized in that it contains a crosslinking agent (B) and is used together with the following compound (A).
[0026] Compound (A): A non-silicone compound having a polyoxyalkylene chain in the molecule, and having a functional group (R1) capable of generating an ether, an ester or a nitrogen-containing compound by reacting with the crosslinking agent (B).
[0027] To achieve the above object, a method for producing an aqueous solution of a softener for textiles as another embodiment of the present invention comprises adding the first agent of the softener for textiles and the second agent of the softener for textiles to water for preparation.
[0028] In order to achieve the above object, an aqueous liquid softener for textiles as another embodiment of the present invention comprises the first softener for textiles, the second softener for textiles, and water.
[0029] In order to achieve the above object, a method for producing a textile product as another aspect of the present invention is characterized in that the aqueous liquid of the above-mentioned softening agent for textile products is applied to fibers.
[0030] In the method for producing a textile product, the softening agent for textile products may be added at a ratio of 0.1% by mass to 4.0% by mass based on the fiber.
[0031] In the method for producing the textile product, the fiber to which the softening agent for textile product is attached may be heated at a temperature of 100° C. to 250° C.
[0032] In order to achieve the above object, a textile product according to another embodiment of the present invention is characterized in that a polymer compound formed by a reaction between the compound (A) and a crosslinking agent (B) in the softener for textile products is attached thereto.
[0033] Effects of the Invention
[0034] According to the present invention, the washing durability of a softener for textiles can be improved without deteriorating the flame retardancy. DETAILED DESCRIPTION
[0035] <First Embodiment>
[0036] First, a first embodiment of the softening agent for textiles of the present invention (hereinafter also referred to as softening agent) will be described. The softening agent of this embodiment contains the following compound (A) and a crosslinking agent (B).
[0037] (Compound (A))
[0038] Compound (A) is a non-silicone compound having a polyoxyalkylene chain in the molecule, and is a compound having a functional group (R1) capable of generating an ether, an ester or a nitrogen-containing compound by reaction with a crosslinking agent (B). Compound (A) preferably has 2 or more functional groups (R1) in one molecule. By adopting this structure, a coating composed of a more durable polymer compound can be formed on the fiber by reaction with a crosslinking agent (B). From the aspect of improving flame retardancy, compound (A) preferably does not have a silicon atom in the molecule.
[0039] The functional group (R1) is not particularly limited as long as it can generate an ether, ester or nitrogen-containing compound by reaction with the crosslinking agent (B) as described above. Specific examples of the functional group (R1) include amino, carboxyl, hydroxyl, epoxy, isocyanate, ester, phosphoric acid, phosphate ester, sulfuric acid-containing group, sulfuric acid-containing ester group, etc.
[0040] Specific examples of the ester include compounds having, for example, carboxylate, phosphoric acid ester, thioester, and the like as an ester bond.
[0041] Specific examples of the ether include compounds having an ether bond and sulfides as compounds having a thioether bond.
[0042] Specific examples of the nitrogen-containing compound include amide compounds, phosphoramide compounds, sulfonamide compounds, imide compounds, carbamate compounds, amine compounds, and urea compounds.
[0043] The main chain of compound (A) contains a polyoxyalkylene chain. The polyoxyalkylene chain helps to improve the softness of the fiber. As the oxyalkylene unit constituting the polyoxyalkylene chain of compound (A), for example, an oxyalkylene unit having 1 to 4 carbon atoms can be mentioned. The polyoxyalkylene chain can be formed by one oxyalkylene unit, or it can be formed by combining two or more oxyalkylene units. When two or more oxyalkylene units are used, their addition method can be any method of block addition, random addition, and a combination of block addition and random addition, without particular limitation.
[0044] Specific examples of the polyoxyalkylene chain include a polyoxymethylene chain, a polyethylene oxide chain, a polyoxypropylene chain, a polyoxyisopropylene chain, a polyoxybutylene chain, or a polyoxyalkylene chain composed of two or more oxyalkylene units selected from the group consisting of formaldehyde, ethylene oxide, propylene oxide, isopropylene oxide and butylene oxide.
[0045] The lower limit of the mass average molecular weight of the polyoxyalkylene chain is not particularly limited, and is preferably 400 or more, and more preferably 1000 or more. The upper limit of the mass average molecular weight of the polyoxyalkylene chain is not particularly limited, and is preferably 9000 or less, and more preferably 7000 or less. It is also conceivable that the range formed by any combination of the above upper and lower limits. By using this numerical range, the softness of the fiber to which the softener is imparted can be improved. In addition, when compound (A) is dispersed in a solution, the stability of the solution can be improved. In addition, when an emulsifier is used, the stability can be further improved.
[0046] In the case where an alkylene oxide is added to form a polyoxyalkylene chain, the lower limit of the number of moles of alkylene oxide added is not particularly limited, and is preferably 10 moles or more, and more preferably 25 moles or more. The upper limit of the number of moles added is not particularly limited, and is preferably 200 moles or less, and more preferably 150 moles or less. It is also possible to conceive of a range in which the above upper and lower limits are arbitrarily combined. By using this numerical range, the softness of the fiber to which the softener is imparted can be improved. In addition, when compound (A) is dispersed in a solution, the stability of the solution can be improved. In addition, when an emulsifier is used, the stability can be further improved. It should be noted that the number of moles of alkylene oxide added represents the number of moles of alkylene oxide relative to 1 mole of the compound having a functional group (R1) put into the raw material.
[0047] Examples of the compound (A) include compounds having a polyoxyalkylene chain represented by the following formulae (1) to (3) as a main chain and two or more functional groups (R1) or a compound having a functional group (R1) added to the terminal, midway, or both of the terminal and midway of the polymer chain.
[0048] R1-(Oxidized alkyl) a -R1 (1)
[0049] [(Oxidized alkyl) b -R1-(Oxidized alkyl) c ] d (2)
[0050] R1-[(Oxidized alkyl) e -R1-(Oxidized alkyl) f ] g -R1 (3)
[0051] In formulae (1) to (3), a to g respectively represent the degree of polymerization.
[0052] In addition, examples of compound (A) include: a compound obtained by adding a polyoxyalkylene chain to a compound having a functional group (R1); a compound obtained by ether-bonding a polyoxyalkylene chain to a polyol and then adding a compound having a functional group (R1) to the polyoxyalkylene chain; etc. More specifically, examples include a compound obtained by capping both ends of polyoxyethylene with 1,2,4,5-benzenetetracarboxylic acid, glycerol polypropoxy triglycidyl ether, glycerol poly(oxypropylene) triamine, etc.
[0053] Among these, one compound (A) may be used alone, or two or more compounds (A) may be used in combination.
[0054] The lower limit of the mass average molecular weight of compound (A) is not particularly limited, preferably 420 or more, more preferably 4,000 or more. The upper limit of the mass average molecular weight of compound (A) is not particularly limited, preferably 10,000,000 or less, more preferably 10,000 or less. It is also conceivable that the range formed by any combination of the above upper and lower limits. By limiting to this range, softness can be effectively imparted to the fiber. It should be noted that the mass average molecular weight can be measured by gel permeation chromatography (GPC) based on polystyrene.
[0055] (Crosslinking agent (B))
[0056] Crosslinking agent (B) means a compound that can generate ether, ester or nitrogen-containing compound by reaction with the above-mentioned compound (A). Crosslinking agent (B) has a functional group (R2) that is reactive with the functional group (R1) of compound (A). Therefore, crosslinking agent (B) is suitably selected from a compound that is reactive with functional group (R1) and functional group (R2) according to the type of functional group (R1) of compound (A). As a specific example of functional group (R2), for example, amino, imino, carboxyl, carboxylic anhydride, halogenated acyl, carbonyl, hydroxyl, epoxy, ester, thioester, phosphoric acid, phosphate, phosphonate, thioisocyanate, blocked isocyanate, isocyanate etc. can be cited.
[0057] Specific examples of the combination of the functional group (R1) of the compound (A) and the functional group (R2) of the crosslinking agent (B) include, for example, a carboxyl group and an amino group, a carboxyl group and a hydroxyl group, an anhydride of a hydroxyl group and an amino group, an anhydride of a hydroxyl group and a hydroxyl group, an amino group and an epoxy group, a carboxyl group and an isocyanate group, an amino group and an isocyanate group, a carboxyl group and a blocked isocyanate group, an amino group and a blocked isocyanate group, an ester group and an amino group, a phosphoric acid group or a phosphoric acid ester group and an amino group, a phosphoric acid group and an epoxy group, a sulfuric acid group or a sulfuric acid-containing ester group and an amino group, a sulfuric acid group or a sulfuric acid-containing ester group and an epoxy group, and the like.
[0058] The number of functional groups (R2) in one molecule of the crosslinking agent (B) is preferably 2 or more. By adopting this structure, a more durable coating can be formed on the fiber by reacting with the compound (A). It is further more preferred that the number of functional groups (R1) and the number of functional groups (R2) in one molecule are respectively 2 or more, and the total number of functional groups (R1) and the number of functional groups (R2) is 5 or more. By adopting this structure, a three-dimensional network structure can be formed by reacting with the compound (A), forming a more durable coating on the fiber. From the aspect of improving flame retardancy, the crosslinking agent (B) preferably does not have a silicon atom in the molecule.
[0059] The equivalent ratio of the functional group (R1) to the functional group (R2) in the softener is not particularly limited, but is preferably in the range of 1:0.1 to 20, and more preferably in the range of 1:0.5 to 10. A range formed by any combination of the upper and lower limits is also assumed. By first determining this range, a more durable coating can be formed on the fiber.
[0060] The lower limit of the functional group equivalent of the crosslinking agent (B) is not particularly limited, and is preferably 10 or more, more preferably 20 or more. The upper limit of the functional group equivalent of the crosslinking agent (B) is not particularly limited, and is preferably 2000 or less, and more preferably 1500 or less. It is also assumed that the range formed by any combination of the above upper and lower limits. By utilizing this configuration, a three-dimensional network structure can be formed by reaction with compound (A), forming a more durable coating on the fiber.
[0061] The crosslinking agent (B) is preferably a compound having a polyoxyalkylene chain in the molecule. The polyoxyalkylene chain may be a structure described in the column of compound (A). The polyoxyalkylene chain structure can further improve the softness of the fiber to which the softener is attached.
[0062] (Other ingredients)
[0063] In the softener of this embodiment, in addition to the compound (A) and the crosslinking agent (B), a silicone compound or a silane compound may be optionally included to the extent that the flame retardancy is not reduced. In the case of including a silicone compound or a silane compound, the total content ratio of the silicone compound and the silane compound in the softener excluding solvents such as water is 40% by mass or less, preferably 1% by mass or less.
[0064] In addition, the softener may be blended with known additives within a range that does not impair the effects of the present invention for the purpose of maintaining quality, improving reactivity, etc. Examples of the additives include water, emulsifiers, catalysts, solvents, stabilizers, flame retardants, and the like.
[0065] (Dosage Form)
[0066] The dosage form of the softener of the present embodiment during storage is not particularly limited. From the aspect of improving storage stability, it is preferably composed in the form of a multi-dose form comprising a first dose of a softener containing the above-mentioned compound (A) and a second dose of a softener containing the above-mentioned cross-linking agent (B). By adopting this structure, the stability of the mixed components can be improved during storage, and the reactivity of the compound (A) and the cross-linking agent (B) can be improved during use. In the case where the reactivity of the compound (A) and the cross-linking agent (B) at room temperature is sufficiently low, the softener can also be composed in the form of a softener containing a single dosage form of the compound (A) and the cross-linking agent (B).
[0067] <Second Embodiment>
[0068] Next, a second embodiment of the textile product of the present invention will be described.
[0069] The textile of the present embodiment is a textile to which a cross-linked polymer compound is attached, and the cross-linked polymer compound is formed by applying the compound (A) and the cross-linking agent (B) described in the first embodiment to the fiber and reacting the compound (A) and the cross-linking agent (B) on the fiber. By coating the fiber surface with the cross-linked polymer compound formed by the reaction of the compound (A) and the cross-linking agent (B), softness and washing durability can be imparted to the textile.
[0070] As the form in which the softener is applied to the fiber, it can be applied in the form of a diluted solution diluted with a diluting solvent, such as a low-viscosity mineral oil solution, an organic solvent solution, an aqueous liquid, etc. From the perspective of excellent stability, reactivity of compound (A) and crosslinking agent (B), and handleability, the softener is preferably prepared in the form of an aqueous liquid. The aqueous liquid can be prepared by adding a first dose of the softener and a second dose of the softener to a specific volume of water and mixing them. In addition, the aqueous liquid can also be prepared by first preparing an aqueous liquid of the first dose of the softener and an aqueous liquid of the second dose of the softener, respectively, and mixing them when used.
[0071] The fibers to which the softener is applied may be short fibers, woven fabrics, or nonwoven fabrics. In addition, they may be melt-spun yarns, drawn yarns, fiber bundles, etc., used to make woven fabrics or nonwoven fabrics. The fibers constituting the textile may be synthetic fibers or natural fibers. There is no particular limitation on the types of fibers, and examples thereof include: (1) polyester fibers such as polyethylene terephthalate (PET), polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polylactic acid, and composite fibers containing these polyester resins; (2) polyamide fibers such as nylon 6 and nylon 66; (3) polyacrylic acid fibers such as polyacrylic acid and modified acrylic acid; (4) polyolefin fibers such as polyethylene and polypropylene; (5) natural fibers such as cotton fibers, rayon fibers, and wool fibers; blends of two or more of these fibers; and the like.
[0072] The diluted softener solution such as an aqueous liquid obtained as described above is applied to the fiber by a known method. The method of applying the softener to the fiber is not particularly limited, and examples thereof include a roll oiling method, a guide oiling method, an immersion oiling method, and a spray oiling method.
[0073] The attachment ratio of the softener to the fiber is not particularly limited, but preferably the softener is attached in a ratio of 0.1% by mass to 4.0% by mass relative to the fiber, based on the softener without diluting solvents such as water. By this configuration, the softness imparting effect can be effectively exerted.
[0074] Next, the fiber to which the softener is applied is subjected to a heat treatment preferably at a temperature of 100°C to 250°C. The heating time is appropriately set according to the treatment temperature, etc., and is preferably 1 to 20 minutes, and more preferably 5 to 10 minutes. This heat treatment can promote the reaction between the compound (A) and the crosslinking agent (B), and form a coating composed of a durable crosslinked polymer compound on the fiber. The fiber formed with the coating can be further subjected to a post-curing treatment by post-aging under a storage environment such as room temperature. With this configuration, a coating composed of a more durable crosslinked polymer compound can be formed. The period of post-aging is appropriately set according to temperature conditions, productivity, etc., and is preferably 1 to 30 days, and more preferably 7 to 14 days.
[0075] The functions and effects of the softener and textile product according to the above-mentioned embodiment will be described.
[0076] The softener of the above embodiment is constituted in a manner including a crosslinking agent (B) and a compound (A), wherein the compound (A) is a non-silicone compound having a polyoxyalkylene chain in the molecule and having a functional group (R1) that can generate an ether or the like by reacting with the crosslinking agent (B). Since the softener does not contain a silicone component as a main component, a textile with no deterioration in flame retardancy can be obtained. In addition, a textile with excellent softness and washing durability can be obtained.
[0077] Example
[0078] In order to more specifically explain the configuration and effects of the present invention, examples are given below, but the present invention is not limited to these examples. It should be noted that in the following examples and comparative examples, parts refer to parts by mass, and % refers to mass %.
[0079] Test Group 1 (Manufacture of Textiles)
[0080] Using the softeners shown in Table 4, polyester staple fibers of Examples and Comparative Examples were prepared in which a film of a cross-linked polymer compound was formed on polyester staple fibers corresponding to textiles.
[0081] Each softener shown in Table 4 is composed of compositions (P-1) to (P-31), (rP-1), and a silicone compound (rA-1) added as needed. Compositions (P-1) to (P-31) and composition (rP-1) contain compound (A), a crosslinking agent (B), and, if necessary, a catalyst (C) in the ratios shown in Table 3.
[0082] The method for preparing the polyester staple fibers of each example and comparative example is as follows.
[0083] (Example 1)
[0084] First, while stirring deionized water, slowly add the compound (A-1) shown in Table 1 to finally reach 1.2 parts (%) to prepare a dispersed dispersion treatment liquid A. Similarly, while stirring deionized water, slowly add the crosslinking agent (B-1) shown in Table 2 to finally reach 1.2 parts (%) to prepare a dispersed dispersion treatment liquid B. Before being applied to polyester staple fibers, 82.3 parts of the dispersion treatment liquid A of the compound (A-1) and 17.7 parts of the dispersion treatment liquid B of the crosslinking agent (B-1) are mixed in the ratio of the composition (P-1) shown in Table 3 to prepare a softener dispersion treatment liquid. Immerse polyester staple fibers (15 denier × 64 mm) in the softener dispersion treatment liquid. At this time, squeeze in such a manner that 10 parts of the softener dispersion treatment liquid are attached to 10 parts of the polyester staple fibers to remove excess softener dispersion treatment liquid. The softener (pure product) concentration in the softener dispersion treatment liquid was adjusted to 1.2% and the amount attached to the polyester staple fibers was adjusted to 1.2% owf.
[0085] The fiber sample was then naturally dried to prepare a fiber sample before heat curing. The fiber sample was placed in a hot air oven at 130° C. for 10 minutes to perform heat curing. The polyester staple fiber of Example 1 having a cross-linked polymer compound coating formed on the fiber was obtained.
[0086] (Examples 2 to 17, 19 to 21)
[0087] Compositions (P-2) to (P-16) and (P-20) shown in Tables 3 and 4 were used respectively. The concentration of the softener (pure product) in the softener dispersion treatment liquid and the amount of the softener attached to the polyester staple fibers were set to the amounts shown in Table 4. Polyester staple fibers were prepared in the same manner as in Example 1 except for the above.
[0088] (Example 18)
[0089] The composition (P-19) shown in Tables 3 and 4 was used. The amount of the softener attached to the polyester staple fibers was set to the amount shown in Table 4.
[0090] While stirring deionized water, the compound (A-3) shown in Table 1 was slowly added to a final amount of 0.7 parts (%) to prepare a dispersed dispersion treatment liquid A. Similarly, while stirring deionized water, the crosslinking agent (B-1) shown in Table 2 was slowly added to a final amount of 0.7 parts (%) to prepare a dispersed dispersion treatment liquid B. Furthermore, while stirring deionized water, the catalyst (C-1) shown in Table 3 was slowly added to a final amount of 0.7 parts (%) to prepare a dispersed dispersion treatment liquid C. Immediately before applying to polyester staple fibers, 70 parts of the dispersion treatment liquid A of the compound (A-3), 28 parts of the dispersion treatment liquid B of the crosslinking agent (B-1), and 2 parts of the dispersion treatment liquid C of the catalyst (C-1) were mixed in a ratio of the composition (P-19) shown in Table 3 to prepare a softener dispersion treatment liquid. The concentration of the softener (pure product) in the obtained softener dispersion treatment liquid was 0.7%. Polyester staple fibers were prepared in the same manner as in Example 1 except for the above.
[0091] (Example 22)
[0092] The composition (P-23) and the silicone compound (rA-1) shown in Tables 3 and 4 were used. The amount of the softener attached to the polyester staple fibers was set to the amount shown in Table 4.
[0093] First, 0.0929 parts (%) of compound (A-3), 0.0066 parts (%) of crosslinking agent (B-7), and 0.00125 parts (%) of a solution containing 40% of silicone compound (rA-1) were slowly added to deionized water at 25°C to prepare a dispersed softener dispersion treatment liquid. The concentration of the softener (pure product) in the obtained softener dispersion treatment liquid was 0.1%. Except for this, polyester staple fibers were prepared in the same manner as in Example 1.
[0094] (Examples 23 to 30)
[0095] Compositions (P-23) and (P-29) to (P-31) shown in Tables 3 and 4 were used, respectively. The concentration of the softener (pure product) in the softener dispersion treatment liquid and the amount of the softener attached to the polyester staple fibers were set to the amounts shown in Table 4. Polyester staple fibers were prepared in the same manner as in Example 22 except for the above.
[0096] (Comparative Example 1)
[0097] The composition (rP-1) shown in Tables 3 and 4 was used. In addition, the amount of softener attached to the polyester staple fiber was set to the amount shown in Table 4. That is, 0.95 parts (%) of a solution containing 40% silicone compound (rA-1) and 0.02 parts (%) of a crosslinking agent (rB-1) were slowly added to deionized water at 25°C to prepare a dispersed softener dispersion treatment liquid. The concentration of the softener (pure product) in the obtained softener dispersion treatment liquid was 0.4%. In addition, the polyester staple fiber was prepared using the same method as in Example 22.
[0098] For the compound (A) used in the preparation of the polyester staple fibers of each example, the type and mass average molecular weight of the polyoxyalkylene chain in the compound (A), the type and number of the functional group (R1) in the compound (A), and the mass average molecular weight of the compound (A) are shown in the "Polyoxyalkylene chain" column, the "Functional group (R1)" column, and the "Mass average molecular weight" column of Table 1, respectively.
[0099] In addition, for the cross-linking agent (B) used in the preparation of the polyester staple fiber of each example, the type of functional group (R2) and the number in the cross-linking agent (B), the type and mass average molecular weight of the polyoxyalkylene chain in the cross-linking agent (B), the functional group equivalent, and the mass average molecular weight of the cross-linking agent (B) are respectively shown in the "Functional group (R2)" column, the "Polyoxyalkylene chain" column, the "Functional group equivalent" column, and the "Mass average molecular weight" column of Table 2.
[0100] In addition, for the composition (P) used in the preparation of the polyester staple fiber of each example, the type of compound (A) and the proportion in the composition (P), the type of crosslinking agent (B) and the proportion in the composition (P), the equivalent ratio of the functional group (R1) to the functional group (R2) in the composition (P), and the type of catalyst (C) and the proportion in the composition (P) are shown in the "Compound (A)" column, "Crosslinking agent (B)" column, "Functional group" column, and "Catalyst (C)" column of Table 3, respectively.
[0101] In addition, regarding the softener used in the preparation of the polyester staple fibers of each example, the type of composition (P) and the ratio in the softener, the type of silicone compound and the ratio in the softener, the amount of softener (pure product excluding water as a solvent) attached to the polyester staple fibers (%owf), and the concentration (%) of the softener (pure product excluding water as a solvent) in the softener dispersion treatment liquid are shown in the "Composition (P)" column, "Silicone compound" column, "Softener attachment amount" column, and "Softener concentration" column of Table 4, respectively. It should be noted that the ratio of the composition (P) and the silicone compound in the softener is expressed as the pure amount excluding water.
[0102] [Table 1]
[0103]
[0104]
[0105] [Table 2]
[0106]
[0107] [Table 3]
[0108]
[0109] [Table 4]
[0110]
[0111] The details of the compound (A), the crosslinking agent (B), the catalyst (C), and other components described in Tables 1 to 4 are as follows.
[0112] (Compound (A))
[0113] A-1: Compound in which both ends of polyoxyethylene are capped with 1,2,4,5-benzenetetracarboxylic acid
[0114] A-2: Glyceryl polypropoxy triglycidyl ether
[0115] A-3: Glycerol poly(oxypropylene) triamine
[0116] (Crosslinking agent (B))
[0117] B-1: polyglycerol polyglycidyl ether, the repeating unit of polyglycerol is 3
[0118] B-2: Branched polyethyleneimine (repeating unit: -(CH2-CH2-NH)n-(10 <n<10 5 ))
[0119] B-3: Branched polyethyleneimine
[0120] B-4: Branched polyethyleneimine
[0121] B-5: Poly(allylamine)
[0122] B-6: Sorbitol polyglycidyl ether
[0123] B-7: (5-ethyl-2-methyl-1,3,2-dioxalate-5-yl)methyl dimethylphosphonate P-oxide and bis[(5-ethyl-2-methyl-1,3,2-dioxalate-5-yl)methyl]methylphosphonate P,P'-dioxide (2:1 mass ratio)
[0124] B-8: Blocked polyisocyanate (NCO content = 12.5 mass %)
[0125] rB-1: Silane-based crosslinking agent (manufactured by Goulston Technologies Inc., product name Lurol PS-662)
[0126] (Catalyst (C))
[0127] C-1: 2-Piperazin-1-yl-ethylamine
[0128] (Other ingredients)
[0129] rA-1: Silicone compound (manufactured by Goulston Technologies Inc., product name Lurol PS-12186)
[0130] Test group 2 (post-curing treatment (post-aging))
[0131] The polyester staple fibers obtained by performing oiling and heat curing treatment in the production line were further left to stand at room temperature for 2 weeks.
[0132] In the column “Post-curing treatment” in Table 4, the case where the post-curing treatment was performed is indicated as “Yes”, and the case where the post-curing treatment was not performed is indicated as “No”.
[0133] Test group 3 (softness before washing)
[0134] Using the obtained samples of the polyester staple fibers of each example, evaluations of softness before washing (feel) and softness before washing (SPF) were performed.
[0135] Softness before washing (touch)
[0136] Regarding the touch, three evaluators evaluated the touch by hand according to the following criteria with respect to the surface state of the polyester staple fibers, thereby judging whether the touch was excellent or not. The touch was scored on the following 5-level scale: 5 points for very excellent touch, 4 points for excellent touch, 3 points for good touch, 2 points for slightly poor touch, and 1 point for poor touch.
[0137] The average value of the scoring results of each evaluator was calculated. An average value of 4.6 points or more was recorded as "excellent: 5", 3.6 points or more and less than 4.6 points was recorded as "good: 4", 2.6 points or more and less than 3.6 points was recorded as "pass: 3", 1.6 points or more and less than 2.6 points was recorded as "slightly poor: 2", and less than 1.6 points was recorded as "poor: 1" as the evaluation result. The results are shown in the "touch" column of softness before washing in Table 4.
[0138] Softness before washing (SPF)
[0139] The softness of the polyester staple fibers was evaluated by a staple pad friction test using an INSTRON tester. The test was conducted in accordance with BS Gupta, Friction in Textile Materials, Chapter 5, pages 216-217, published by Woodhead Publishing Limited, Year 2008.
[0140] First, the obtained polyester staple fiber sample is opened and made into a mat shape, and then placed on a sample stand. A friction body with a load is placed on the sample, and the friction generated by stretching the friction body is measured, and the friction coefficient obtained (i.e., staple pad friction (SPF)) is measured. It should be noted that a high SPF value indicates a poor hand feel, and a low SPF value indicates that the staple fiber is soft. The measured values are shown in the "SPF" column of the softness before washing in Table 4.
[0141] Test group 4 (softness after washing)
[0142] After the softness of the test group 3 was evaluated, washing was performed as shown below, and the softness after washing was evaluated.
[0143] The cleaning method was carried out according to the AATCC-61 standard. Each sample of polyester staple fiber to which a softener was applied was cleaned using a Launder-Ometer at the cleaning temperature (40°C, 60°C or 90°C) shown in the "Cleaning Temperature" column of Table 4 using an accelerated cleaning method. The ratio of the mass of the sample to the volume of the cleaning water was 100:1.
[0144] The 45-minute cleaning time was divided into five cycles of 9 minutes each, and the cleaning solution to which 0.15 mass % of AATCC standard detergent 1993 deionized water was added was used in the first cycle.
[0145] After the first cycle, the sample was removed from the barrel and squeezed to remove as much liquid as possible. The second cycle was treated in the same way as the first cycle. The remaining three cycles were treated in the same way using only deionized water. After washing, the sample was dried by air drying.
[0146] The touch and SPF of each sample after washing were evaluated by the same methods as those for softness before washing (touch) and softness before washing (SPF). The results are shown in the "touch" column and "SPF" column of softness after washing 5 times in Table 4, respectively.
[0147] Test group 5 (flame retardancy)
[0148] The flame retardancy test was conducted based on BS-5852. Each sample of polyester staple fiber was burned for 40 seconds at an ambient temperature of 25°C using an ignition source with a gas flow rate of 160 mL / min. The ignition source was then removed and the duration of continuous burning of the sample was measured. The flame retardancy was evaluated based on the following criteria.
[0149] Evaluation criteria for flame retardancy
[0150] Pass: The sample continues to burn for less than 120 seconds
[0151] Failure: The sample continues to burn for more than 120 seconds
[0152] (other)
[0153] In the above-mentioned Example 1, the compound (A) and the crosslinking agent (B) were first prepared in the form of separate aqueous liquids, and then mixed immediately before use to prepare a softener dispersion treatment liquid.
[0154] On the other hand, even when the softener dispersion treatment liquid was prepared by simultaneously adding the compound (A) and the crosslinking agent (B) into water in the same container, when the softener dispersion treatment liquid was immediately attached to the fibers, the same evaluation as in Example 1 was confirmed.
[0155] As can be seen from the evaluation results of each example with respect to the comparative example in Table 4, according to the present invention, a softener having excellent flame retardancy can be obtained. In addition, a coating having excellent washing durability and excellent flexibility can be formed.
Claims
1. A softener for textiles, characterized in that: It comprises the following compound (A) and a cross-linking agent (B), Compound (A): a non-silicone compound having a polyoxyalkylene chain in the molecule, and having a functional group (R1) capable of generating an ether, an ester or a nitrogen-containing compound by reacting with the crosslinking agent (B), wherein the number of functional groups (R1) in one molecule is 3 or more, and the mass average molecular weight of the compound (A) is 420 or more and 10,000,000 or less; The crosslinking agent (B) has a functional group (R2) reactive with the functional group (R1), The combination of the functional group (R1) and the functional group (R2) is at least one combination selected from a combination of a carboxyl group and an imino group, an amino group and an epoxy group, a carboxyl group and an epoxy group, an epoxy group and an imino group, an amino group and an isocyanate group, an amino group and a blocked isocyanate group, and a phosphoric acid group or a phosphoric acid ester group and an amino group, The equivalent ratio of the functional group (R1) to the functional group (R2) is 1:0.1-20.
2. The softener for textiles according to claim 1, wherein The compound (A) and the cross-linking agent (B) do not have a silicon atom in the molecule.
3. The softener for textiles according to claim 1 or 2, wherein The number of functional groups (R2) in one molecule of the crosslinking agent (B) is 2 or more, and includes combinations in which the total number of functional groups (R1) and the number of functional groups (R2) is 5 or more.
4. The softener for textiles according to claim 1 or 2, wherein The mass average molecular weight of the compound (A) is 4,000 to 10,000.
5. The softener for textiles according to claim 1 or 2, wherein The functional group equivalent of the crosslinking agent (B) is 10 to 2000.
6. The softener for textiles according to claim 1 or 2, wherein The crosslinking agent (B) is a compound having a polyoxyalkylene chain in the molecule.
7. The softener for textiles according to claim 1 or 2, wherein The polyoxyalkylene chain is a polyoxymethylene chain, a polyethylene oxide chain, a polyoxypropylene chain, a polyoxyisopropylene chain, a polyoxybutylene chain, or a polyoxyalkylene chain composed of two or more oxyalkylenes selected from formaldehyde, ethylene oxide, propylene oxide, oxyisopropylene and butylene oxide.
8. The softener for textiles according to claim 1 or 2, wherein The mass average molecular weight of the polyoxyalkylene chain is 400 to 9000.
9. The softener for textiles according to claim 1 or 2, wherein: The softening agent may further contain a silicone compound or a silane compound, and the total content of the silicone compound and the silane compound in the softening agent for textiles is 40% by mass or less.
10. The softener for textiles according to claim 9, wherein The total content of the silicone compound and the silane compound is 1% by mass or less.
11. The softener for textiles according to claim 1 or 2, wherein: The softener for textiles is imparted to the short fibers.
12. The softener for textiles according to claim 11, wherein The softener for textiles is imparted to cotton fibers.
13. A textile, characterized in that: A polymer compound formed by the reaction of the compound (A) in the softening agent for textiles according to any one of claims 1 to 10 with the crosslinking agent (B) is attached thereto.
Citation Information
Patent Citations
Method for the treatment of cellulosic fibres with amino functional and silicone polymers
US5445652A
Fabric softener composition
CN1220694A
Liquid softener composition
JP2009155739A
Concentrated softener
US5242607A