Low melting point polyester chips for producing ground hot melt adhesive and preparation method thereof
Through step-by-step esterification and the combination of catalysts, low-melting polyester chips are prepared, which solves the problems of high melting range, high viscosity, and low melt index of polyester chips used in conventional hot fuse filaments, and achieves lower melting range and better performance. High melt index and better bonding strength improve production efficiency and reduce costs.
Patent Information
- Application Number
- CN202210854209.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-14
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-07-14
AI Technical Summary
The polyester chips used in conventional low-melting point thermal fuse wires have high melting range, high viscosity and low melt index, which leads to problems such as high ironing temperature, long time and low production efficiency during use.
By adding 1,3-propanediol and diethylene glycol to isophthalic acid, ethylene glycol and terephthalic acid in a beating kettle for a step-by-step esterification reaction, combining catalysts and stabilizers, and controlling the reaction temperature and vacuum degree, we prepared Low melting point polyester chips with low melting range, high melt index and high bonding strength.
The melting range of polyester chips is reduced to 85-105°C, the melt index is increased by more than three times, the bonding strength is increased by more than 30%, and the intrinsic viscosity is controlled at 0.400±0.005dl/g, which significantly shortens and reduces the ironing time and temperature.
Smart Images

Figure BDA0003745577300000071
Abstract
Description
Technical Field
[0001] The invention relates to a polyester chip and a preparation method thereof, in particular to a low melting point polyester chip used for producing ground hot melt adhesive and a preparation method thereof. Background Art
[0002] In recent years, conventional low-melting point hot-melt polyester chips have been widely used in the bonding of sportswear, shoe uppers and other fabrics. With the popularization of applications, the problems of the product itself have become increasingly prominent. The problems of conventional low-melting point hot-melt polyester chips, such as high melting range, high viscosity, and low melt index, have greatly restricted the continued promotion of the product. During the use of downstream customers, the disadvantages of conventional low-melting point hot-melt wires, such as high ironing temperature requirements, long ironing time, and low production efficiency, have become increasingly obvious. The product of the present invention aims to reduce the melting range of the grinding polyester chips and improve their fluidity through dual improvements in formula and process, so as to solve the problems existing in the use of the above-mentioned products to the greatest extent. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a low-melting point polyester chip for producing a powdered hot melt adhesive and a preparation method thereof. The polyester chip of the present invention is used to produce and process a powdered hot melt adhesive, which has the advantages of low melting range, high melt index, low bonding heat requirement, high bonding strength, etc., and can well solve the problem that the physical indicators of conventional low-melting point hot melt polyester chips are not ideal, such as high melting range, high viscosity, and low melt index.
[0004] In order to achieve the above excellent product characteristics and to make up for the defects of existing processing technology and materials, the technical solution adopted by the present invention is: a preparation method of low melting point polyester chips for producing ground hot melt adhesive, comprising the following steps:
[0005] ① Add a certain amount of 1,3-propylene glycol and diethylene glycol to a beating kettle, and then add a certain amount of isophthalic acid solid powder to prepare a viscous slurry, and then pump it into the esterification reaction kettle through a slurry pump to start the first step of esterification reaction, wherein the molar ratio of isophthalic acid to the total acid in the esterification reaction is 35%-50%, the molar ratio of 1,3-propylene glycol to the total alcohol in the esterification reaction is 2%-5%, and the molar ratio of diethylene glycol to the total alcohol in the esterification reaction is 8%-15%;
[0006] ② After the raw materials added in ① have reacted completely, a certain amount of ethylene glycol solution and a certain amount of terephthalic acid solid are added to the pulping kettle to prepare a uniform slurry, which is pumped into the esterification reaction kettle again through the slurry supply pump to carry out the second step of esterification reaction, wherein the molar ratio of terephthalic acid to the total acid in the esterification reaction is 50%-65%, the molar ratio of ethylene glycol to the total alcohol in the esterification reaction is 80%-90%, and the molar ratio of the total acid to the total alcohol in the two esterification reactions is 1: (1.25-1.45);
[0007] ③ When the reaction of step ② is completed and the slurry temperature is stabilized to 245-265°C, the materials in the esterification reactor are pressed into the polycondensation reactor by high-purity nitrogen through a 15-25μm stainless steel filter;
[0008] ④ After the mixed slurry enters the polycondensation kettle, add the catalyst, colorant and stabilizer, continue stirring for 10-30 minutes, start heating and draw low vacuum; control the reaction temperature at 275-285°C, carry out negative pressure polymerization reaction, require the vacuum degree ≤30Pa, at the final temperature of 275-285°C, control the stirring polycondensation current and power through the equipment, and synthesize the ultra-low viscosity polyester chip melt with a characteristic viscosity of 0.400-0.420dl / g, and then pass through the casting head, underwater pelletizer, dryer and vibrating screen to finally obtain the low melting point polyester chips for the production of ground hot melt adhesive.
[0009] The molar ratio of acid to alcohol in the first step of esterification reaction is greater than 1 to ensure complete esterification of alcohol. The first step of esterification temperature is 200-220° C. The ratio of the molar number of esterification water produced in the first step of esterification reaction to the molar number of alcohol added is not less than 1.96.
[0010] The acid-alcohol molar ratio of the second step esterification reaction is less than 0.8 to ensure that the acid esterification is complete. The second step esterification temperature is 240-260°C, and the ratio of the molar number of esterification water produced in the second step esterification reaction to the molar number of the added acid is not less than 1.96.
[0011] The catalyst is one or a combination of ethylene glycol antimony, antimony trioxide, antimony acetate, butyl titanate, zinc sulfate, germanium oxide; the stabilizer is one or a combination of trimethyl phosphate and polyphosphate; the toner is one or a combination of red and blue dye, cobalt acetate, fluorescent whitening agent.
[0012] The compound catalyst is added in an amount of 200-500ppm of the theoretical polyester chip output, and is composed of 30%-50% of the total catalyst mass of antimony acetate, 20%-40% of butyl titanate, 10%-20% of zinc sulfate, and 1%-10% of germanium oxide.
[0013] The toner is a single toner. For example, if red and blue dye is used, the usage amount is 1-5ppm of the theoretical polyester chip output; if cobalt acetate is used, the usage amount is 30-100ppm of the theoretical polyester chip output; if fluorescent brightener is used, the usage amount is 50-300ppm of the theoretical polyester chip output; and if trimethyl phosphate or polyphosphate is used as a stabilizer, the usage amount is 100-500ppm of the theoretical polyester chip output.
[0014] The low melting point polyester chips prepared by the above preparation method are used for producing ground hot melt adhesive.
[0015] The beneficial effects of the present invention are:
[0016] 1. Through the step-by-step esterification operation, the alternative alcohol of ethylene glycol and the alternative acid of terephthalic acid can participate in the esterification reaction to the maximum extent, thereby achieving a significant drop in the product melting range to 85-105°C. This melting range is more than 30°C lower than the conventional low-melting point hot fuse 117-137°C, which is a huge breakthrough in the melting range;
[0017] 2. At the same time, the introduction of diethylene glycol to replace traditional ethylene glycol can greatly improve the fluidity of polyester chips in semi-fluid and fluid states. The melting index of conventional low-melting point hot melt wire is more than three times higher than that of less than 10g / 10min (160℃ / 2160g), reaching more than 35g / 10min (160℃ / 2160g). Good fluidity provides a strong guarantee for increasing the contact area during ironing;
[0018] 3. By introducing an appropriate amount of 1,3-propylene glycol monomer, the bonding strength after grinding can be greatly improved. The bonding strength of the same quality of ground polyester chips and conventional low-melting point hot-melt polyester chips can be increased by more than 30%;
[0019] 4. During the polymerization process, precise control of the intrinsic viscosity can stabilize the intrinsic viscosity of polyester chips at 0.400±0.005dl / g. This intrinsic viscosity has greatly exceeded the control accuracy and range of 0.66±0.012dl / g of conventional polyester chips, creating a very favorable physical basis for reducing ironing time, lowering ironing temperature, improving production efficiency, and saving processing costs, and providing technical support for the reasonable substitution of products. DETAILED DESCRIPTION
[0020] The present invention is further described in detail below in conjunction with specific embodiments:
[0021] The present invention discloses a method for preparing a low melting point polyester chip for producing a ground hot melt adhesive, comprising the following steps:
[0022] ① Add a certain amount of 1,3-propylene glycol and diethylene glycol to a beating kettle, and then add a certain amount of isophthalic acid solid powder to prepare a viscous slurry, and then pump it into the esterification reaction kettle through a slurry pump to start the first step of esterification reaction, wherein the molar ratio of isophthalic acid to the total acid in the esterification reaction is 35%-50%, the molar ratio of 1,3-propylene glycol to the total alcohol in the esterification reaction is 2%-5%, and the molar ratio of diethylene glycol to the total alcohol in the esterification reaction is 8%-15%;
[0023] ② After the raw materials added in ① have reacted completely, a certain amount of ethylene glycol solution and a certain amount of terephthalic acid solid are added to the pulping kettle to prepare a uniform slurry, which is pumped into the esterification reaction kettle again through the slurry supply pump to carry out the second step of esterification reaction, wherein the molar ratio of terephthalic acid to the total acid in the esterification reaction is 50%-65%, the molar ratio of ethylene glycol to the total alcohol in the esterification reaction is 80%-90%, and the molar ratio of the total acid to the total alcohol in the two esterification reactions is 1: (1.25-1.45);
[0024] ③ When the reaction of step ② is completed and the slurry temperature is stabilized to 245-265°C, the materials in the esterification reactor are pressed into the polycondensation reactor by high-purity nitrogen through a 15-25μm stainless steel filter;
[0025] ④ After the mixed slurry enters the polycondensation kettle, add the catalyst, colorant and stabilizer, continue stirring for 10-30 minutes, start heating and draw low vacuum; control the reaction temperature at 275-285°C, carry out negative pressure polymerization reaction, require the vacuum degree ≤30Pa, at the final temperature of 275-285°C, control the stirring polycondensation current and power through the equipment, and synthesize the ultra-low viscosity polyester chip melt with a characteristic viscosity of 0.400-0.420dl / g, and then pass through the casting head, underwater pelletizer, dryer and vibrating screen to finally obtain the low melting point polyester chips for the production of ground hot melt adhesive.
[0026] The molar ratio of acid to alcohol in the first step of esterification reaction is greater than 1 to ensure complete esterification of alcohol. The first step of esterification temperature is 200-220° C. The ratio of the molar number of esterification water produced in the first step of esterification reaction to the molar number of alcohol added is not less than 1.96.
[0027] The acid-alcohol molar ratio of the second step esterification reaction is less than 0.8 to ensure that the acid esterification is complete. The second step esterification temperature is 240-260°C, and the ratio of the molar number of esterification water produced in the second step esterification reaction to the molar number of the added acid is not less than 1.96.
[0028] The catalyst is one or a combination of ethylene glycol antimony, antimony trioxide, antimony acetate, butyl titanate, zinc sulfate, germanium oxide; the stabilizer is one or a combination of trimethyl phosphate and polyphosphate; the toner is one or a combination of red and blue dye, cobalt acetate, fluorescent whitening agent.
[0029] The compound catalyst is added in an amount of 200-500ppm of the theoretical polyester chip output, and is composed of 30%-50% of the total catalyst mass of antimony acetate, 20%-40% of butyl titanate, 10%-20% of zinc sulfate, and 1%-10% of germanium oxide.
[0030] The toner is a single toner. For example, if red and blue dye is used, the usage amount is 1-5ppm of the theoretical polyester chip output; if cobalt acetate is used, the usage amount is 30-100ppm of the theoretical polyester chip output; if fluorescent brightener is used, the usage amount is 50-300ppm of the theoretical polyester chip output; and if trimethyl phosphate or polyphosphate is used as a stabilizer, the usage amount is 100-500ppm of the theoretical polyester chip output.
[0031] The low melting point polyester chips prepared by the above preparation method are used for producing ground hot melt adhesive.
[0032] Compared with existing products, conventional polyester chips for low melting point hot melt wires have the following shortcomings:
[0033] 1. Conventional hot-melt polyester chips need to be processed into polyester yarns in downstream applications, which requires a complete set of spinning equipment. The equipment investment is large, and once the equipment is fixed, it is difficult to flexibly adjust the processing method;
[0034] 2. The lowest melting range that conventional polyester chips for hot-melt wire can reach is 117-137℃. It is very difficult to lower the melting range, and the later processing requires more heat and longer ironing time. However, the melting range of this product can be lowered to 85-105℃, which can greatly reduce the ironing heat consumption and ironing residence time;
[0035] 3. Comparing the same amount of conventional hot-melt yarn made of polyester chips and processed into yarn and powder, the bonding strength of the latter is increased by more than 30%;
[0036] 4. The melting index of conventional polyester chips for hot melt wire is less than 10g / 10min (160℃ / 2160g), while the melting index of this product can reach more than 35g / 10min (160℃ / 2160g). Good fluidity can combine with the material surface more quickly during ironing and increase the bonding contact area.
[0037] The polyester chips prepared by the present invention solve these pain points and difficulties in use, and it is necessary to implement synchronous control of various indicators in the synthesis of the product of the present invention:
[0038] 1. Melting range control technology solution:
[0039] Through the step-by-step esterification operation, the alternative alcohol of ethylene glycol and the alternative acid of terephthalic acid can participate in the esterification reaction to the maximum extent, thereby significantly reducing the melting range of the product to 85-105°C. This melting range is more than 30°C lower than the conventional low-melting point hot fuse of 117-137°C, which is a huge breakthrough in the melting range.
[0040] 2. Rong melt index control technology solution:
[0041] At the same time, the introduction of diethylene glycol to replace traditional ethylene glycol can greatly improve the fluidity of polyester chips in semi-fluid and fluid states. The melting index of conventional low-melting point hot melt wire is more than three times higher than that of less than 10g / 10min (160℃ / 2160g), reaching more than 35g / 10min (160℃ / 2160g). Good fluidity provides a strong guarantee for increasing the contact area during ironing.
[0042] 3. Technical solution for controlling bonding reliability:
[0043] By introducing an appropriate amount of 1,3-propylene glycol monomer, the bonding strength after grinding can be greatly improved. The bonding strength of the same quality of ground polyester chips and conventional low-melting point hot-melt polyester chips can be increased by more than 30%.
[0044] 4. Intrinsic viscosity control technology solution:
[0045] During the polymerization process, precise intrinsic viscosity control can stabilize the intrinsic viscosity of polyester chips at 0.400±0.05dl / g. This intrinsic viscosity has greatly exceeded the control accuracy and range of 0.66±0.012dl / g of conventional polyester chips, creating a very favorable physical basis for reducing ironing time, lowering ironing temperature, improving production efficiency, and saving processing costs, and providing technical support for the reasonable substitution of products. To achieve this effect, it is necessary to match and accurately control the stirring power, vacuum degree and reaction time. On the one hand, the sensor accuracy and stability of the control system are improved, and on the other hand, the pelletizing system of the discharging is improved to ensure stable pelletizing of ultra-low intrinsic viscosity polyester chips and reduce product degradation during the pelletizing process.
[0046] Example 1
[0047] ① The first step of esterification reaction: add 24 kg of 1,3-propylene glycol and 100 kg of diethylene glycol into the pulping kettle, and then add 305 kg of isophthalic acid solid powder to prepare a viscous slurry, and then pump it into the esterification reactor through the slurry supply pump to start the first step of esterification reaction. The reaction temperature is controlled at 220 ° C. When the reaction water reaches more than 45 kg, the first step of esterification reaction is completed;
[0048] ② Second step esterification reaction: After the reaction of the raw materials added in ① is completed, 330 kg of ethylene glycol solution and 560 kg of terephthalic acid solid are added to the pulping kettle to prepare a uniform slurry, which is pumped into the esterification reaction kettle again through the slurry supply pump to carry out the second step esterification reaction. The temperature of the second step esterification reaction is controlled at 255°C. When the esterification water reaches more than 138 kg, the second step esterification reaction is completed;
[0049] ③ When the reaction of step ② is completed and the slurry temperature is stabilized to 245-265°C, the materials in the esterification reactor are pressed into the polycondensation reactor by high-purity nitrogen through three 25μm stainless steel filters;
[0050] ④ After the mixed slurry enters the polycondensation reactor, add 175g of catalyst antimony acetate, 150g of butyl titanate, 65g of zinc sulfate, 10g of germanium oxide, 50g of toner cobalt acetate, and 150g of stabilizer trimethyl phosphate, continue stirring for 10-30 minutes, and start heating to draw a low vacuum. Control the reaction temperature to 275-285℃, carry out negative pressure polymerization, and require the vacuum degree ≤30Pa. At the final temperature of 275-285℃, control the stirring polycondensation current and power through the equipment to synthesize an ultra-low viscosity polyester chip melt with a characteristic viscosity of 0.400±0.005dl / g, and then pass through a casting head, an underwater pelletizer, a dryer, and a vibrating screen to finally obtain a low melting point polyester chip for the production of ground hot melt adhesive.
[0051] According to the methods of steps ① to ④, implement other 2-4 examples. The specific data are shown in Table 1.
[0052] Table 1
[0053] Parameters Example 1 Example 2 Example 3 Example 4 1,3-Propanediol / Kg 24 28 10 20 Diethylene glycol / Kg 100 120 60 80 Ethylene glycol / Kg 330 380 400 390 Isophthalic acid / Kg 305 430 350 400 Terephthalic acid / Kg 560 435 515 465 Total amount of catalyst / g 500 400 300 500
[0054] The low-melting-point polyester chips used in the present invention for producing ground hot-melt adhesives have a high melting index, a low melting range, and a low intrinsic viscosity compared to conventional low-melting-point hot-melt polyester chips. During use, customers can experience better fluidity and better bonding reliability in the product, and the ironing time and ironing temperature are significantly shortened and reduced.
[0055] The following is explained in conjunction with specific embodiments:
[0056] The low melting point polyester chips used for producing the ground hot melt adhesive in the above Examples 1-4 were tested for a number of physical and chemical indicators, and the test results are summarized in Table 2 below.
[0057] Table 2
[0058]
[0059] The embodiments described above are only used to illustrate the technical ideas and features of the present invention, and their purpose is to enable those skilled in the art to understand the contents of the present invention and implement them accordingly. The patent scope of the present invention cannot be limited only by this embodiment, that is, any equivalent changes or modifications made to the spirit disclosed by the present invention still fall within the patent scope of the present invention.
Claims
1. A method for preparing low melting point polyester chips for producing ground hot melt adhesive, characterized in that: The following steps are involved: ① Add a certain amount of 1,3-propylene glycol and diethylene glycol to a beating kettle, and then add a certain amount of isophthalic acid solid powder to prepare a viscous slurry, and then pump it into the esterification reaction kettle through a slurry pump to start the first step of esterification reaction, wherein the molar ratio of isophthalic acid to the total acid in the esterification reaction is 35%-50%, the molar ratio of 1,3-propylene glycol to the total alcohol in the esterification reaction is 2%-5%, and the molar ratio of diethylene glycol to the total alcohol in the esterification reaction is 8%-15%; ② After the raw materials added in ① have reacted completely, a certain amount of ethylene glycol solution and a certain amount of terephthalic acid solid are added to the pulping kettle to prepare a uniform slurry, which is pumped into the esterification reaction kettle again through the slurry supply pump to carry out the second step of esterification reaction, wherein the molar ratio of terephthalic acid to the total acid in the esterification reaction is 50%-65%, the molar ratio of ethylene glycol to the total alcohol in the esterification reaction is 80%-90%, and the molar ratio of the total acid to the total alcohol in the two esterification reactions is 1: (1.25-1.45); ③ When the reaction of step ② is completed and the slurry temperature is stabilized to 245-265°C, the materials in the esterification reactor are pressed into the polycondensation reactor by high-purity nitrogen through a 15-25μm stainless steel filter; ④ After the mixed slurry enters the polycondensation kettle, add the catalyst, colorant and stabilizer, continue stirring for 10-30 minutes, start heating and draw low vacuum; control the reaction temperature at 275-285°C, carry out negative pressure polymerization reaction, require the vacuum degree ≤30Pa, at the final temperature of 275-285°C, control the stirring polycondensation current and power through the equipment, and synthesize the ultra-low viscosity polyester chip melt with a characteristic viscosity of 0.400-0.420dl / g, and then pass through the casting head, underwater pelletizer, dryer and vibrating screen to finally obtain the low melting point polyester chips for the production of ground hot melt adhesive.
2. The method for preparing low melting point polyester chips for producing ground hot melt adhesive according to claim 1, characterized in that: The molar ratio of acid to alcohol in the first step of esterification reaction is greater than 1 to ensure complete esterification of alcohol. The first step of esterification temperature is 200-220° C. The ratio of the molar number of esterification water produced in the first step of esterification reaction to the molar number of alcohol added is not less than 1.
96.
3. The method for preparing low melting point polyester chips for producing ground hot melt adhesive according to claim 1, characterized in that: The acid-alcohol molar ratio of the second step esterification reaction is less than 0.8 to ensure that the acid esterification is complete. The second step esterification temperature is 240-260°C, and the ratio of the molar number of esterification water produced in the second step esterification reaction to the molar number of the added acid is not less than 1.
96.
4. The method for preparing low melting point polyester chips for producing ground hot melt adhesive according to claim 1, characterized in that: The catalyst is one or a combination of ethylene glycol antimony, antimony trioxide, antimony acetate, butyl titanate, zinc sulfate, germanium oxide; the stabilizer is one or a combination of trimethyl phosphate and polyphosphate; the toner is one or a combination of red and blue dye, cobalt acetate, fluorescent whitening agent.
5. The method for preparing low melting point polyester chips for producing ground hot melt adhesive according to claim 4, characterized in that: The compound catalyst is added in an amount of 200-500ppm of the theoretical polyester chip output, and is composed of 30%-50% of the total catalyst mass of antimony acetate, 20%-40% of butyl titanate, 10%-20% of zinc sulfate, and 1%-10% of germanium oxide.
6. The method for preparing low melting point polyester chips for producing ground hot melt adhesive according to claim 4, characterized in that: The toner is a single toner. For example, if red and blue dye is used, the usage amount is 1-5ppm of the theoretical polyester chip output; if cobalt acetate is used, the usage amount is 30-100ppm of the theoretical polyester chip output; if fluorescent brightener is used, the usage amount is 50-300ppm of the theoretical polyester chip output; and if trimethyl phosphate or polyphosphate is used as a stabilizer, the usage amount is 100-500ppm of the theoretical polyester chip output.
7. Low melting point polyester chips for producing ground hot melt adhesive obtained by the preparation method according to any one of claims 1 to 6.