A kind of lipoic acid hydrogel and its preparation method and application
By heating the specific molar ratio reaction between lipoic acid and sodium lipoate in water, a lipoic acid hydrogel rich in disulfide bonds and hydrogen bonds is formed, which solves the problem of depolymerization of polylipoic acid materials in concentrated alkalis and achieves high Stability and self-healing ability, suitable for a variety of applications.
Patent Information
- Application Number
- CN202210943867.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-04
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-08-04
AI Technical Summary
In the prior art, polylipoic acid materials need the participation of strong alkalis during the preparation process, resulting in the possibility of depolymerization in concentrated alkalis, and the use of volatile toxic substances or ionic liquids affects biosafety, and polylipoic acid hydrogels. The stability of the decomposition behavior is difficult to solve.
By heating the lipoic acid and sodium lipoate in water at a specific molar ratio, a hydrogel is formed, and the combination of disulfide bonds, hydrogen bonds and ion bonds is used to achieve efficient self-healing and stability, avoiding strong The use of alkali and the contamination of volatile substances.
The obtained lipoic acid hydrogel does not depolymerize under time and temperature changes, has high stability and self-healing ability, is suitable for binders, dressings and anti-counterfeiting materials, and has good injectability, reducing environmental pollution.
Smart Images

Figure CN115232329B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer hydrogels, and more specifically to a lipoic acid hydrogel and a preparation method and application thereof. Background Art
[0002] Lipoic acid is a vitamin-like disulfide compound and an important coenzyme in organisms. It also has antioxidant, anti-glycation, and anti-inflammatory effects. Its molecular structure mainly exists in the form of a five-membered ring containing a disulfide bond and an active carboxyl group. Nowadays, lipoic acid is increasingly used to prepare supramolecular polymer hydrogels by causing five-membered disulfide ring opening self-polymerization (ROP) through dynamic disulfide exchange, and is widely used in the fields of recyclable polymer materials, bioantibacterial materials, and adhesive materials. Since the disulfide free radicals at the active end of polylipoic acid will trigger reverse closed-loop depolymerization, polylipoic acid is in a metastable state, which greatly limits the application of polylipoic acid materials. At present, some studies have reported that the disulfide bonds in polylipoic acid are stabilized by adding vinyl monomers (1,3-diisopropenylbenzene, acrylic acid, and itaconic acid, etc.) to participate in the polymerization process of lipoic acid or by introducing ionic liquids, etc., to prevent its closed-loop depolymerization behavior. However, this involves the use of volatile toxic substances or the leakage of ionic liquids, which is easy to pollute the environment, and requires multi-step organic synthesis, and the preparation process is complicated.
[0003] The prior art discloses a lipoic acid-based hydrogel and a preparation method and application thereof. The lipoic acid monomer and an alkaline solution are mixed and heated to form a lipoic acid-based hydrogel through ring-opening polymerization and hydrogen bond cross-linking of the lipoic acid monomer, thereby solving the problem of threats to biosafety caused by the introduction of volatile toxic substances or ionic liquids. The preparation process is simple and can be applied to skin wound repair, spinal nerve injury repair and ultraviolet shielding. However, polylipoic acid will depolymerize in concentrated alkali, and the concentration of the alkali solution needs to be strictly controlled during the preparation process. The depolymerization behavior of polylipoic acid cannot be solved, and the prepared hydrogel is unstable. The residual alkali in the alkali solution will affect subsequent use, such as causing irritation to the skin. Summary of the invention
[0004] In view of the defects and shortcomings of the prior art, the present invention provides a method for preparing lipoic acid hydrogel, which does not require the participation of a strong base, and the obtained lipoic acid hydrogel will not depolymerize with the change of time or temperature. In the preparation process, the disulfide ring is fully opened to form a disulfide bond, and hydrogen bonds, ionic bonds and disulfide bonds exist in the gel, which can achieve efficient self-healing.
[0005] Another object of the present invention is to provide a lipoic acid hydrogel.
[0006] Another object of the present invention is to provide an application of lipoic acid hydrogel in a binder.
[0007] Another object of the present invention is to provide an application of lipoic acid hydrogel in dressings.
[0008] Another object of the present invention is to provide an application of lipoic acid hydrogel in anti-counterfeiting materials.
[0009] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0010] A method for preparing lipoic acid hydrogel comprises the following steps:
[0011] S1. dissolving a mixed monomer of lipoic acid and sodium lipoate in a molar ratio of 10:4 to 10:8 in water, wherein the mass of the water is 2 to 4 times the mass of the mixed monomer to obtain a mixed solution;
[0012] S2. The mixed solution is heated at 45-80°C and mixed evenly and reacted for more than 1 hour, and then kept at a constant temperature of 40-60°C to form a hydrogel. The resulting hydrogel is lipoic acid hydrogel.
[0013] The inventors found that when the molar ratio of lipoic acid to sodium lipoate is lower than 10:4, due to the low solubility of lipoic acid in water, the two will phase separate in water and cannot undergo ring-opening polymerization to form polylipoic acid; when the molar ratio of lipoic acid to sodium lipoate is higher than 10:8, the reaction product after the polymerization reaction is difficult to gel, i.e., a stable hydrogel cannot be formed. Therefore, it is necessary to control the molar ratio of lipoic acid to sodium lipoate to obtain a lipoic acid hydrogel with abundant disulfide bonds.
[0014] The amount of water added in S1 will also affect the ring-opening polymerization reaction of lipoic acid and sodium lipoate and the gelation of the solution. When the amount of water added is less than 2 times the mass of the mixed monomers described in S1, lipoic acid and sodium lipoate cannot be mixed evenly, resulting in the polymerization reaction failing to proceed smoothly. When the amount of water added is too high, the reaction product after the polymerization reaction is difficult to gel and a hydrogel product cannot be obtained.
[0015] The reaction temperature described in S2 is to induce thioctic acid and sodium thioctic acid to self-assemble in water to form polythioctic acid. When the temperature is too low, it is not enough to induce the disulfide ring in thioctic acid and sodium thioctic acid to undergo ring-opening polymerization. When the reaction temperature is too high, the evaporation of water is too fast, which affects the water content of the thioctic acid hydrogel of the present invention, and a stable hydrogel cannot be formed. The excessively high temperature can make the reaction product in a sol state, making the gelation process difficult to carry out. Since the disulfide ring-opening polymerization requires time, the reaction time described in S2 can also affect the occurrence of the polymerization reaction. When the reaction time is too short, thioctic acid and sodium thioctic acid cannot fully react, resulting in the disulfide ring being unable to completely react with the ring-opening reaction, which affects the degree of polymerization of the final thioctic acid hydrogel.
[0016] In addition, after the ring-opening polymerization reaction, the lipoic acid hydrogel of the present invention needs to be kept at a constant temperature for a period of time, as described in S2. This is because a viscous substance is obtained after the ring-opening reaction, and gelation is not achieved. In the gelation process, there is also the formation and stabilization of bonds, such as hydrogen bonds between carboxyl groups, hydrogen bonds between carboxyl groups and carboxyl anions, and ionic bonds between carboxyl anions and sodium ions. The formation of these chemical bonds requires energy, so it is necessary to be carried out under constant temperature conditions. When the constant temperature is too low, it is impossible to provide sufficient energy for various chemical bonds inside the gel during the gelation process, which is not conducive to the formation and stabilization of chemical bonds, thereby affecting the stability of the lipoic acid hydrogel; and when the temperature is too high, it will not only fail to further promote the stability of the formation of chemical bonds, but also be unfavorable for the gelation process.
[0017] Preferably, the molar ratio of lipoic acid to sodium lipoate in S1 is 10:4 to 10:6.
[0018] Preferably, the reaction time in S2 is 1 to 2 hours.
[0019] After the disulfide ring has fully undergone ring-opening polymerization, too long a reaction time will not bring better effects to the lipoic acid hydrogel but will reduce the preparation efficiency.
[0020] Preferably, the constant temperature time in S2 is 6 to 12 hours.
[0021] If the constant temperature time is too short, the chemical bonds in the gel are not completely formed and stabilized, which affects the stability of the final lipoic acid hydrogel. However, too long a constant temperature time will not bring better effects to the lipoic acid hydrogel, so the constant temperature time needs to be controlled.
[0022] The preparation method of the lipoic acid hydrogel of the invention is simple, and the raw materials used will not cause pollution to the environment. By controlling the molar ratio of lipoic acid and sodium lipoate, a uniform liquid can be formed after heating in water, and the polymerization reaction of lipoic acid and sodium lipoate is induced by temperature. The obtained lipoic acid hydrogel has high stability and will not depolymerize with changes in time and temperature.
[0023] The present invention specifically protects a lipoic acid hydrogel prepared by the preparation method of the lipoic acid hydrogel.
[0024] The disulfide bonds in the lipoic acid hydrogel are dynamic disulfide bonds, which can be re-crosslinked by exchanging between the disulfide bonds after being damaged to restore the original state, and the lipoic acid hydrogel prepared by the present invention also contains hydrogen bonds between carboxyl groups, hydrogen bonds between carboxyl groups and carboxyl anions, and ionic bonds between carboxyl anions and sodium ions, and the effects between these chemical bonds make it self-healing faster. In addition, the lipoic acid hydrogel prepared by the present invention is also injectable, providing a good implementation method for the application of various lipoic acid hydrogels.
[0025] The present invention particularly protects the use of lipoic acid hydrogel in adhesives.
[0026] Preferably, the adhesive is used as an adhesive for wood or metal bonding.
[0027] Thioctic acid hydrogel of the present invention has cohesiveness, by coating thioctic acid hydrogel on dry wood or metal surface, can realize the bonding of dry wood or metal, also has adhesion to polytetrafluoroethylene, rubber, wood board, stone, metal, plastic, glass, leaf surface and pigskin.And the thioctic acid hydrogel prepared by the present invention has injectability, can also adhere to the surface of object by injection.In addition, because the disulfide bond in polylipoic acid can be decomposed by the enzyme of organism, degraded into small molecule thioctic acid, and then absorbed and utilized by organism.Therefore, thioctic acid hydrogel of the present invention can realize microbial degradability as binding agent, reduces the pollution of binding agent to environment.
[0028] More preferably, the molar ratio of lipoic acid to sodium lipoate in the lipoic acid hydrogel as a binder is 10:6.
[0029] When the molar ratio of lipoic acid to sodium lipoate is 10:6, the shear strength of the adhesive when adhering to wood reaches 1.927 MPa, and the peel strength when adhering to metal zinc reaches 329 N / m.
[0030] Another object of the present invention is to protect the use of lipoic acid hydrogel in dressings.
[0031] The lipoic acid hydrogel of the present invention has the characteristics of efficient self-healing, can be quickly restored to the original state after being damaged by the outside world, therefore when used as a wound dressing, the gel can be injected into the wound by a needle tube injection to promote wound healing. In addition, because disulfide bonds in polylipoic acid can produce sulfhydryl radicals, react with the surface of bacteria, the bacteria are inactivated, so the lipoic acid hydrogel of the present invention can also be used as a biological anti-inflammatory agent, and no additional anti-inflammatory agent is needed, based on this, the lipoic acid hydrogel when used as a wound dressing, in addition to promoting wound healing, can also play the role of inhibiting wound inflammation, and the lipoic acid hydrogel of the present invention has efficient healing properties, can better maintain the integrity of the gel, so that it can better play an anti-inflammatory effect.
[0032] Another object of the present invention is to protect the use of a lipoic acid hydrogel in anti-counterfeiting materials, wherein the lipoic acid hydrogel is prepared by the preparation method of the present invention, and the molar ratio of lipoic acid to sodium lipoate in S1 is 10:4.
[0033] When the molar ratio of lipoic acid and sodium lipoate is 10:4, the prepared lipoic acid hydrogel is thermosensitive and will undergo a phase change from a transparent state to an opaque state as the temperature changes. This temperature change is reversible and this property can be used to make anti-counterfeiting materials such as anti-counterfeiting labels.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] The present invention prepares thioctic acid hydrogel by self-assembly of thioctic acid and sodium thioctic acid in water and ring-opening polymerization occurs. Due to sufficient reaction time, reverse closed-loop depolymerization behavior will not occur, so the thioctic acid hydrogel obtained has abundant disulfide bonds, and thioctic acid and sodium thioctic acid are used as raw materials, and hydrogen bonds and ionic bonds are also contained in the obtained gel, so that the gel can be self-healed within 30 minutes after being damaged, and return to the original state. Since hydrogen bonds between stable carboxyl groups, hydrogen bonds between carboxyl groups and carboxyl anions, and ionic bonds between carboxyl anions and sodium ions are formed inside the gel during the gelation process, the thioctic acid hydrogel prepared by the present invention has high stability, and depolymerization behavior will not occur even if placed at room temperature for 60 days.
[0036] The lipoic acid hydrogel prepared by the present invention has the properties of adhesion, injectability, temperature sensitivity and efficient self-healing, and is suitable for the adhesion of adhesives, especially dry wood and metal. When adhering to dry wood, the shear strength can reach 1.927MPa, and when adhering to metal zinc, the peel strength can reach 329N / m. In addition, the lipoic acid hydrogel of the present invention is also suitable for dressings and anti-counterfeiting materials. When used as a dressing, it can promote wound healing. After being damaged by the external environment, the dressing can quickly return to its original state, and the anti-inflammatory effect of the gel can be better exerted; when used as an anti-counterfeiting material, the visibility of information can be controlled by temperature changes. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The ultraviolet absorption spectra of lipoic acid hydrogel with a molar ratio of 10:5 at different reaction times;
[0038] Figure 2 IR spectra of the lipoic acid hydrogels of Example 1, Example 2 and Example 3;
[0039] Figure 3 XRD spectra of thioctic acid, sodium thioctic acid and the thioctic acid hydrogel of Example 2;
[0040] Figure 4 This is a comparison diagram of the appearance of the lipoic acid hydrogels of Example 1 and Example 2 as the temperature changes;
[0041] Figure 5The adhesion of the hydrogel prepared by the present invention as a binder on the surfaces of different materials;
[0042] Figure 6 This is a diagram showing the injectability of the lipoic acid hydrogel of Example 2;
[0043] Figure 7 These are the self-healing pictures of the lipoic acid hydrogel of Example 2 at different times. DETAILED DESCRIPTION
[0044] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0045] Example 1
[0046] A method for preparing lipoic acid hydrogel comprises the following steps:
[0047] S1. dissolving lipoic acid and sodium lipoate in a molar ratio of 10:5 (mass ratio of 1.29 g:0.71 g) in deionized water, wherein the amount of deionized water added is 4 g to obtain a mixed solution;
[0048] S2. The mixed solution in S1 was heated at 60°C and stirred for reaction for 1.5 h. After stopping the stirring, the mixture was kept at 50°C for 6 h and cooled to room temperature to obtain lipoic acid hydrogel.
[0049] Examples 2 to 14 and Comparative Examples 1 to 8
[0050] A method for preparing a lipoic acid hydrogel, wherein the preparation steps are the same as those in Example 1, and the differences are shown in Table 1.
[0051] Table 1. Preparation parameters of lipoic acid hydrogels of Examples 1 to 14 and Comparative Examples 1 to 8
[0052]
[0053]
[0054] Comparative Example 9
[0055] A lipoic acid-based hydrogel, the preparation method comprising the following steps:
[0056] Under heating conditions at 45° C., 1 mmol of lipoic acid was evenly mixed with 1 mL of 0.4 M sodium bicarbonate solution, stirred to dissolve, and then reacted in a 60° C. water bath for 6 hours to obtain a lipoic acid polymer hydrogel material.
[0057] Performance Testing
[0058] The infrared spectrum testing method of the lipoic acid hydrogel of the present invention is as follows:
[0059] The lipoic acid hydrogel samples were analyzed using the Fourier transform infrared spectrometer iS50R in total reflection mode. Lipoic acid and sodium lipoate were tested using potassium bromide tablets with a wave number range of 4000-400cm -1 , the scanning times are 32 times, and the infrared spectrum data of lipoic acid, sodium lipoate and lipoic acid hydrogel samples with various ratios can be obtained.
[0060] The ultraviolet spectrum test method of the lipoic acid hydrogel is as follows:
[0061] The test was performed using an ultraviolet spectrophotometer (UV-Vis Spectrophotometer), with a wavelength accuracy of ±0.3 nm and a resolution of 0.1 nm. The test wavelength range was 230-500 nm, and the ultraviolet absorption spectra of lipoic acid hydrogels at the same solubility and different reaction times were tested.
[0062] The healing speed of the lipoic acid hydrogel was tested in the following manner:
[0063] A cross was made on the surface of the gel with a blade to a depth of 3 mm. The gel was placed at room temperature and the time required for complete healing was recorded and observed.
[0064] The depolymerization behavior of the lipoic acid hydrogel was tested in the following manner:
[0065] XRD characterization was performed on the lipoic acid hydrogels placed at room temperature for different periods of time, and whether reverse ring-closing depolymerization occurred was determined by testing whether there were diffraction peaks of lipoic acid or sodium lipoate crystals.
[0066] When the lipoic acid hydrogel is used as a binder, its shear strength is tested in the following manner:
[0067] The prepared gel was evenly coated on a rectangular pine board of 100*25*2mm, with a coating size of 25*25mm. After both boards were coated, the front of the board containing the gel was glued, placed on a press machine at 80℃ and 8Mpa for 12 hours to dry and solidify, and then the shear strength was tested using a universal tensile machine at a tensile speed of 5mm / min. Five parallel samples were used in each group and the average value was taken. The test results are shown in Table 2.
[0068] Table 2. Shear strength of lipoic acid hydrogels of Examples 1, 2 and 3 adhered to dry wood
[0069] Shear strength(MPa) Example 1 1.25878 Example 2 1.19843 Example 3 1.92725
[0070] The peel strength of the bond with the metal surface is tested in the following way:
[0071] The gel was evenly coated on different metal surfaces using a coating machine with a coating thickness of 0.15 mm, placed in a 60-degree Celsius oven for drying for 12 hours, and then adhered to the metal surface containing the sample using 3M tape, and rolled with a roller to make it adhere tightly. Finally, the peel strength was tested using a universal tensile machine with a speed of 100 mm / min, a peeling distance of 100 mm, and a tape width of 20 mm. Three parallel samples were tested in each group, and the average value was taken. The test results are shown in Table 3.
[0072] Table 3. Peel strength of lipoic acid hydrogels of Examples 1, 2 and 3 on different metals
[0073] Example 1 Peel Strength Example 2 Peel Strength Example 3 Peel Strength aluminum 105N / m 79.3 N / m 144N / m copper 199N / m 182N / m 215N / m Zinc 265N / m 251N / m 329N / m
[0074] Table 4. Test results of lipoic acid hydrogels of Examples 1 to 14 and Comparative Examples 1 to 9
[0075]
[0076]
[0077] From the test results of Table 4, it can be seen that when the molar ratio of thioctic acid and sodium thioctic acid is lower than 10:4, solid-liquid separation occurs, and polymerization reaction cannot occur. When the molar ratio is 10:9, the product obtained by the polymerization reaction cannot form a hydrogel, and when the reaction temperature exceeds 80°C, the reaction product is a sol, which cannot be gelled, and polymerization reaction cannot occur when it is lower than 45°C. When the constant temperature is lower than 40°C, due to insufficient energy provided to the gelation process, the gelation is not thorough, and the final reaction product exists in a sol state. Although the healing speed of the thioctic acid hydrogel obtained in Comparative Example 4 is fast, due to the short reaction time, thioctic acid and sodium thioctic acid cannot fully undergo ring-opening polymerization, so depolymerization is very easy to occur. In addition, the healing speed in Comparative Example 9 is significantly lower than the healing speed of the thioctic acid hydrogel prepared in Examples 1 to 12, because the types and contents of chemical bonds in the hydrogel of Comparative Example 9 are not as rich as those in Examples 1 to 14, and because there are fewer stable chemical bonds in the gel, the preparation conditions are alkaline, and closed-loop depolymerization is easy to occur.
[0078] Figure 1When the molar ratio of thioctic acid to sodium thioctic acid is 10:5, the ultraviolet absorption spectra under different reaction times show that when the reaction time is too short, there is an obvious ultraviolet absorption peak of the disulfide bond in the five-membered disulfide ring at 330 nm, and as the reaction time increases, the five-membered disulfide ring in thioctic acid and sodium thioctic acid gradually undergoes ring-opening polymerization. After 1 hour of reaction, the ultraviolet absorption peak almost completely disappears, which is consistent with the results of Example 11 and Comparative Example 4, and further illustrates that when the reaction time is too short, the five-membered disulfide ring in thioctic acid and sodium thioctic acid cannot fully undergo ring-opening polymerization, the content of disulfide bonds after ring opening in the obtained product is low, and the self-healing speed is also slow.
[0079] Figure 2 The infrared spectra of the lipoic acid hydrogels prepared in Examples 1, 2 and 3, wherein PTA1, PTA2 and PTA3 correspond to the lipoic acid hydrogels of Example 2, Example 1 and Example 3, respectively. As can be seen from the figure, the polylipoic acid product has a wavelength of 1702 cm -1 、1590cm -1 The stretching vibration peaks of carboxyl groups and carboxyl anions appear at the positions, indicating that carboxyl groups and carboxyl anions exist in the product, which further proves that the lipoic acid hydrogel of the present invention contains multiple chemical bonds, which enhances its stability and will not depolymerize over time.
[0080] Figure 3 The XRD patterns of lipoic acid, sodium lipoate and the lipoic acid hydrogel prepared in Example 2 after being placed for 1 day, 3 days, 7 days and 15 days are given; wherein TA is lipoic acid, TA-Na is sodium lipoate, and PTA1 is the lipoic acid hydrogel prepared in Example 2. It can be seen that after the lipoic acid hydrogel has been placed for 15 days, no diffraction peaks of lipoic acid and sodium lipoate crystals appear, indicating that the lipoic acid hydrogel does not depolymerize over time and has stable properties.
[0081] Figure 4 The following is a comparison of the appearance of the lipoic acid hydrogels of Examples 1 and 2 as they change with temperature. At 25°C, PTA1 is in an opaque state due to the low temperature, while PTA2 is transparent. As the temperature rises, at 45°C, both PTA1 and PTA2 can observe the obscured information. The above changes are reversible for PTA1. The reason for this phenomenon is that when the ambient temperature is low, the solubility of the chain segments formed by the ring-opening polymerization of lipoic acid is low due to the high lipoic acid content. This property can be used to apply the lipoic acid hydrogel prepared by the present invention to anti-counterfeiting materials.
[0082] Figure 5The adhesion of lipoic acid hydrogel PTA2 on polytetrafluoroethylene, rubber, wood, stone, metal, plastic, glass, leaf surface, pigskin and finger surface is shown, proving that the lipoic acid hydrogel prepared by the present invention can be used as a bonding agent to adhere to various materials. When adhering to dry wood, its shear strength is a minimum of 1.198MPa and a maximum of 1.927MPa (Table 2); when adhering to metal zinc, its peel strength is a minimum of 251N / m and a maximum of 329N / m (Table 3); when adhering to metal copper, its peel strength is a minimum of 182N / m and a maximum of 215N / m (Table 3); when adhering to metal aluminum, its peel strength is a minimum of 79.3N / m and a maximum of 144N / m (Table 3).
[0083] Figure 6 The figure shows the injectable state of the hydrogel prepared by the present invention as an injectable material, indicating that the present invention can be injected into the surface of the corresponding substrate through a syringe when in use.
[0084] Figure 7 These are the self-healing pictures of the lipoic acid hydrogel of Example 2 at different times, which further prove that the lipoic acid hydrogel prepared by the present invention can achieve efficient self-healing, and can better exert anti-inflammatory effects when used as a wound dressing to further protect the wound.
[0085] It should be noted that although the remaining embodiments do not provide the ultraviolet absorption spectrum diagram, infrared spectrum diagram, adhesion diagram and injectability diagram, their properties are equivalent to the results shown in the accompanying drawings.
[0086] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a lipoic acid hydrogel, characterized in that: The steps include: S1. dissolving a mixed monomer of lipoic acid and sodium lipoate in a molar ratio of 10:4 to 10:8 in water, wherein the mass of the water is 2 to 4 times the mass of the mixed monomer to obtain a mixed solution; S2. The mixed solution is heated at 45-80°C and mixed evenly and reacted for more than 1 hour, and then kept at a constant temperature of 40-60°C to form a hydrogel. The resulting hydrogel is lipoic acid hydrogel.
2. The preparation method of lipoic acid hydrogel as claimed in claim 1, characterized in that, The molar ratio of lipoic acid to sodium lipoate in S1 is 10:4 to 10:
6.
3. The preparation method of lipoic acid hydrogel as claimed in claim 1, characterized in that, The reaction time in S2 is 1 to 2 hours.
4. The preparation method of lipoic acid hydrogel as claimed in claim 1, characterized in that, The constant temperature time in S2 is 6 to 12 hours.
5. The lipoic acid hydrogel prepared by the method for preparing the lipoic acid hydrogel according to any one of claims 1 to 4.
6. Use of the lipoic acid hydrogel according to claim 5 as a binding agent.
7. The use according to claim 6, characterized in that The adhesive is an adhesive used for bonding wood or metal.
8. The use according to claim 6, characterized in that The molar ratio of lipoic acid to sodium lipoate in the lipoic acid hydrogel is 10:
6.
9. Use of the lipoic acid hydrogel according to claim 5 as a dressing.
10. The use of lipoic acid hydrogel as an anti-counterfeiting material, characterized in that: The lipoic acid hydrogel is prepared by the preparation method according to claim 1, and the molar ratio of lipoic acid to sodium lipoate in S1 is 10:4.