Laminated sheet and method for manufacturing the same

By forming a controlled adhesive layer on the protective film of the laminated sheet and optimizing laser cutting technology, the problem of reducing adsorption force caused by laser cutting is solved, and the stable fit between the laminated sheet and the display panel is ensured.

CN115244439BActive Publication Date: 2024-11-15SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180019939.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-19
Filing Date
2021-02-12
Publication Date
2024-11-15
Estimated Expiration
2041-02-12

AI Technical Summary

Technical Problem

When the laminated sheet is cut by laser, burrs are easily generated on the surface, resulting in a decrease in adsorption force and affecting the bonding effect between the laminated sheet and the display panel.

Method used

By forming a highly controlled adhesive layer on the protective film of the laminated sheet, and optimizing the laser output and cutting method during the laser cutting process, it is ensured that the burrs height of the outer peripheral part of the protective film is less than 6.0 μm, thereby maintaining the adsorption force.

Benefits of technology

It effectively prevents the adsorption force from being lowered when the laminated sheet is bonded to the display panel, and improves the bonding quality and reliability of the laminated sheet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115244439B_ABST
    Figure CN115244439B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a laminated sheet whose adsorption force is not easily reduced when the laminated sheet is attached to a display panel. The laminated sheet is sequentially laminated with a first protective film, a front panel and a polarizing layer, the first protective film having a first adhesive layer on one surface of a first resin film, the first protective film being laminated to the front panel via the first adhesive layer, the first protective film being capable of being peeled off from the front panel, and the height of the burrs on the outer peripheral edge of the first protective film being 6.0 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminate and a method for producing the same. Background Art

[0002] The laminated sheet having the front panel and the polarizing layer is attached to the display panel via the adhesive layer formed on the polarizing layer side to form a display device. Before attaching the laminated sheet, in order to prevent the surface from being contaminated or scratched, an isolation film is laminated on the adhesive layer, and a surface protection film is laminated on the front panel. When attaching the laminated sheet to the display panel, the surface protection film side is first adsorbed to hold the laminated sheet. The isolation film is peeled off to expose the adhesive layer, and the laminate is attached to the display panel via the adhesive layer.

[0003] The laminated sheet having a front panel and a polarizing layer is manufactured by cutting a long laminated body into a single sheet of a specified shape using a laser. In particular, when the laminated sheet has a layer obtained by curing a polymerizable liquid crystal compound, laser-based cutting is more excellent than knife-based cutting in that it is not easy to produce tiny cracks (for example, the length of which is less than 200 μm) at the ends of the laminated sheet. In the case where the display device is bendable, if there are tiny cracks at the ends of the laminated sheet, the laminated sheet may be broken due to the tiny cracks when it is bent, so it is preferably cut with a laser.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: WO2016 / 158300 Summary of the invention

[0007] It is found that if cutting is performed by laser, burrs will be generated on the outer peripheral portion of the surface of the laminate. The burrs will reduce the adsorption force when the laminate is attached to the display panel, thereby causing the laminate to be unable to be held. The purpose of the present invention is to provide a laminate whose adsorption force is not easily reduced when the laminate is attached to the display panel.

[0008] [1] A laminated sheet comprising a first protective film and a polarizing layer laminated in this order,

[0009] The first protective film has a first adhesive layer on one surface of the first resin film.

[0010] The first protective film is laminated on the polarizing layer via the first adhesive layer.

[0011] The first protective film can be peeled off from the polarizing layer.

[0012] The height of the burrs on the outer peripheral edge of the first protective film is 6.0 μm or less.

[0013] [2] A laminated sheet comprising a first protective film, a front panel and a polarizing layer laminated in this order,

[0014] The first protective film has a first adhesive layer on one surface of the first resin film.

[0015] The first protective film is laminated on the front panel via the first adhesive layer.

[0016] The first protective film can be peeled off from the front panel.

[0017] The height of the burrs on the outer peripheral edge of the first protective film is 6.0 μm or less.

[0018] [3] The laminated sheet according to [1] or [2], wherein the height of the burrs is 0.1 μm or more.

[0019] [4] The laminated sheet according to any one of [1] to [3], wherein the polarizing layer comprises a layer obtained by curing a polymerizable liquid crystal compound.

[0020] [5] A method for manufacturing a laminated sheet, comprising:

[0021] Preparation step: preparing the laminated body,

[0022] The laminated body is sequentially laminated with a second protective film, a first protective film and a polarizing layer,

[0023] The first protective film has a first adhesive layer on one surface of the first resin film.

[0024] The first protective film is laminated on the polarizing layer via the first adhesive layer.

[0025] The second protective film has a second adhesive layer on one surface of the second resin film.

[0026] The second protective film is laminated on the first protective film via the second adhesive layer.

[0027] The first protective film can be peeled off from the polarizing layer.

[0028] The second protective film can be peeled off from the first protective film; and

[0029] The cutting step is to cut the laminate into a predetermined shape by irradiating the laminate with laser light from the polarizing layer side to obtain a laminate sheet.

[0030] [6] A method for manufacturing a laminated sheet, comprising:

[0031] Preparation step: preparing the laminated body,

[0032] The laminated body is sequentially laminated with a second protective film, a first protective film, a front panel and a polarizing layer.

[0033] The first protective film has a first adhesive layer on one surface of the first resin film.

[0034] The first protective film is laminated on the front panel via the first adhesive layer.

[0035] The second protective film has a second adhesive layer on one surface of the second resin film.

[0036] The second protective film is laminated on the first protective film via the second adhesive layer.

[0037] The first protective film can be peeled off from the front panel.

[0038] The second protective film can be peeled off from the first protective film; and

[0039] The cutting step is to cut the laminate into a predetermined shape by irradiating the laminate with laser light from the polarizing layer side to obtain a laminate sheet.

[0040] [7] The method for producing a laminated sheet according to [5] or [6], wherein in the cutting step, the output of the laser is 50 W to 200 W.

[0041] [8] The method for producing a laminated sheet according to any one of [5] to [7], wherein in the cutting step, the laminated body is cut into a predetermined shape by a full-cut method.

[0042] [9] The method for producing a laminated sheet according to any one of [5] to [8], wherein the second resin film has a thickness of 40 μm or more.

[0043]

[10] The method for producing a laminated sheet according to any one of [5] to [9], wherein the polarizing layer comprises a layer obtained by curing a polymerizable liquid crystal compound.

[0044] According to the present invention, it is possible to provide a laminate sheet in which the adsorption force is less likely to decrease when the laminate sheet is attached to a display panel. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a schematic cross-sectional view showing an example of the laminated sheet of the present invention.

[0046] Figure 2 This is a schematic cross-sectional view showing an example of the laminated sheet of the present invention.

[0047] Figure 3 This is a schematic cross-sectional view showing an example of a laminate used when producing the laminate sheet of the present invention.

[0048] Figure 4 This is a schematic cross-sectional view showing an example of the laminated sheet of the present invention.

[0049] Figure 5 This is a schematic cross-sectional view showing an example of the laminated sheet of the present invention. DETAILED DESCRIPTION

[0050] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings, but the present invention is not limited to the following embodiments. In all the following drawings, the scales are appropriately adjusted for easy understanding of each component, and the scales of each component shown in the drawings are not necessarily consistent with the scales of the actual components.

[0051] <Laminated sheet>

[0052] Figure 1 This is a schematic cross-sectional view showing an example of the laminated sheet of the present invention. Figure 1 The laminated sheet 300 shown is laminated with the first protective film 100, the front panel 1, and the polarizing layer 2 in this order. The front panel 1 and the polarizing layer 2 are laminated by the laminating layer 3. The polarizing layer 2 has a linear polarizing plate 20 and a phase difference film 22 from the front panel 1 side. The first protective film 100 corresponds to a so-called surface protective film, and has a first adhesive layer 102 on one surface of a first resin film 101. The first protective film 100 is laminated on the front panel 1 via the first adhesive layer 102. The first protective film 100 can be peeled off from the front panel 1, and the first adhesive layer 102 has its adhesive force adjusted so that it can be peeled off from the front panel 1.

[0053] Figure 4 This is a schematic cross-sectional view showing an example of the laminated sheet of the present invention. Figure 4 The laminated sheet 302 shown has the first protective film 100 and the polarizing layer 2 laminated in this order. The polarizing layer 2 has a linear polarizing plate 20 and a phase difference film 22 from the first protective film 100 side. The first protective film 100 corresponds to a so-called surface protective film, and has a first adhesive layer 102 on one surface of a first resin film 101. The first protective film 100 is laminated on the polarizing layer 2 via the first adhesive layer 102. The first protective film 100 can be peeled off from the polarizing layer 2, and the first adhesive layer 102 has its adhesive force adjusted so that it can be peeled off from the polarizing layer 2.

[0054] The laminated sheet may include a third pressure-sensitive adhesive layer and a third resin film on the side of the polarizing layer opposite to the front panel side (or the first protective film side). Figure 2 , Figure 5 This is a schematic cross-sectional view showing an example of the laminated sheet of the present invention. Figure 2The laminated sheet 301 shown is laminated with the first protective film 100, the front panel 1, the polarizing layer 2, the third adhesive layer 50, and the third resin film 51 in this order. The front panel 1 and the polarizing layer 2 are laminated by the laminating layer 3. The polarizing layer 2 has a linear polarizing plate 20 and a phase difference film 22 from the front panel 1 side. The third resin film 51 can be equivalent to a so-called isolation film, and the third adhesive layer 50 can be an adhesive layer for laminating the laminated sheet to the display panel. The third resin film 51 can be peeled off from the third adhesive layer 50, and the surface of the third resin film 51 can be subjected to a demolding treatment so that it can be peeled off from the third adhesive layer 50.

[0055] Figure 5 The laminated sheet 303 shown is laminated with the first protective film 100, the polarizing layer 2, the third adhesive layer 50, and the third resin film 51 in this order. The polarizing layer 2 has a linear polarizing plate 20 and a phase difference film 22 from the first protective film 100 side. The third resin film 51 can be equivalent to a so-called isolation film, and the third adhesive layer 50 can be an adhesive layer for attaching the laminated sheet to the display panel. The third resin film 51 can be peeled off from the third adhesive layer 50, and the surface of the third resin film 51 can be subjected to a demolding treatment so that it can be peeled off from the third adhesive layer 50.

[0056] The laminate can have Figures 1-2 , Figures 4-5 The laminated sheet may include, for example, a touch sensor layer, a coloring layer formed in a frame shape between the front panel 1 and the polarizing layer 2 in a plan view, an impact-resistant film disposed between the front panel 1 and the polarizing layer 2, and a resin film.

[0057] The height of the burrs on the outer peripheral portion of the first protective film of the laminate of the present invention is 6.0 μm or less. The burrs may be residues on the outside of the geometric shape of the corner edge of the laminate, or residues on the laminate after a machining or forming process. Specifically, the burrs may be melted and solidified objects of the material constituting the laminate (particularly the material of the first protective film) that exists on the surface of the first protective film on the side opposite to the first adhesive layer side and exists on its outer peripheral portion. The burrs may be generated by laser processing. The burrs may exist on at least a portion of the entire circumference of the outer peripheral portion of the first protective film when viewed from above, or may exist on the entire circumference of the outer peripheral portion.

[0058] Figure 1 In the figure, the burrs 40 are present on the surface of the first protective film 100 opposite to the first adhesive layer 102 side surface and on the outer peripheral portion thereof in a plan view. The height of the burrs corresponds to the height indicated by reference numeral 41 .

[0059] By making the height of the burrs on the outer peripheral portion of the first protective film 6.0 μm or less, the gap between the laminated sheet and the adsorption device can be reduced. Therefore, it is estimated that the force of adsorbing the laminated sheet becomes less likely to decrease. Therefore, the height of the burrs is preferably 2.0 μm or less, more preferably 1.5 μm or less, further preferably 1.0 μm or less, and may also be 0.7 μm or less.

[0060] The lower limit of the height of the burr is not particularly limited, and the height of the burr may be 0.01 μm or more, 0.1 μm or more, or 0.3 μm or more. If the height of the burr is within the above range, it is easy to prevent the undesirable situation (multiple extraction) of taking out multiple laminated sheets when taking out the top laminated sheet from a laminated body of laminated sheets formed by overlapping multiple laminated sheets.

[0061] The height of the burrs can be measured using a stylus film thickness meter. Examples of the stylus film thickness meter include DEKTAK32 (manufactured by VEECO).

[0062] The laminate may also have burrs on the surface on the side opposite to the first protective film side. Specifically, the burrs may exist on the surface of the third resin film on the side opposite to the third adhesive layer side and on its outer peripheral portion. The burrs may be a melted and solidified object of the material constituting the laminate (particularly the material of the third resin film). The height of the burrs that may exist on the surface on the side opposite to the first protective film side may be greater than 0 μm and less than 100 μm, or may be greater than the height of the burrs on the outer peripheral portion of the first protective film.

[0063] The laminated film having the front panel 1 and the polarizing layer 2 constituting the laminated sheet is preferably bendable at least in a direction with the front panel 1 being the inner side and the polarizing layer 2 being the outer side (so-called in-folding mode). Bendable means that it can be bent without breaking in a direction with the front panel 1 being the inner side and the polarizing layer 2 being the outer side.

[0064] In another embodiment, the laminated film constituting the laminated sheet and having the polarizing layer 2 is preferably bendable at least in a direction with the linear polarizing plate 20 as the inner side and the phase difference film 22 as the outer side (so-called in-folding mode). Bendable means that it can be bent without breaking in a direction with the linear polarizing plate 20 as the inner side and the phase difference film 22 as the outer side.

[0065] The shape of the surface direction of the laminated sheet can be, for example, a square shape, preferably a square shape with long sides and short sides, and more preferably a rectangle. When the shape of the surface direction of the laminated sheet is a rectangle, the length of the long side can be, for example, 10 mm to 1400 mm, preferably 50 mm to 600 mm. The length of the short side is, for example, 5 mm to 800 mm, preferably 30 mm to 500 mm, and more preferably 50 mm to 300 mm. Each layer constituting the laminated sheet can be R-processed at the corner, or the end can be notched, or the hole can be opened.

[0066] The thickness of the laminated sheet varies depending on the function required of the laminated sheet, the use of the laminated sheet, etc., and is not particularly limited, but is, for example, 20 μm to 1000 μm, and preferably 50 μm to 500 μm.

[0067] [1st protective film]

[0068] The first protective film is equivalent to a so-called surface protective film, and one surface of the first resin film has a first adhesive layer. The first protective film is laminated on the front panel via the first adhesive layer. Usually, for example, after the laminate is attached to the display panel or other optical components, the first protective film is peeled off together with the first adhesive layer it has. Therefore, the first protective film can be peeled off from the front panel, and the first adhesive layer adjusts its adhesive force in a manner that it can be peeled off from the front panel.

[0069] In another embodiment, the first protective film is laminated on the polarizing layer via the first adhesive layer. Usually, after laminating the laminated sheet on the display panel or other optical components, the first protective film is peeled off together with the first adhesive layer it has. Therefore, the first protective film can be peeled off from the polarizing layer, and the first adhesive layer adjusts its adhesive force in a manner that allows it to be peeled off from the polarizing layer.

[0070] The thickness of the first protective film may be, for example, 30 μm to 200 μm, or 50 μm to 150 μm. The thickness of the first protective film refers to the thickness of the central portion (not the outer peripheral portion) of the laminated sheet.

[0071] [First resin film]

[0072] The resin constituting the first resin film may be, for example, a polyethylene resin such as polyethylene, a polypropylene resin such as polypropylene, a polyester resin such as polyethylene terephthalate or polyethylene naphthalate, a thermoplastic resin such as a polycarbonate resin, etc. Polyester resins such as polyethylene terephthalate are preferred. The first resin film may be a single-layer structure or a multi-layer structure, but is preferably a single-layer structure from the viewpoints of ease of manufacture and manufacturing cost.

[0073] The thickness of the first resin film may be, for example, 20 μm to 200 μm, or 30 μm to 150 μm. The thickness of the first resin film refers to the thickness of the central portion (not the outer peripheral portion) of the laminated sheet.

[0074] [First adhesive layer]

[0075] The first adhesive layer can be composed of an adhesive composition with a resin such as (meth) acrylic acid, rubber, polyurethane, ester, silicone, and polyvinyl ether as the main component. Among them, an adhesive composition with a (meth) acrylic resin having excellent transparency, weather resistance, heat resistance, etc. as the base polymer is preferred. The adhesive composition can be an active energy ray curable type or a heat curable type.

[0076] As the (meth)acrylic resin (base polymer) used in the adhesive composition, for example, a polymer or copolymer using one or more of (meth)acrylates such as butyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate as monomers is preferably used. The base polymer may be copolymerized with a polar monomer. As the polar monomer, for example, monomers having a carboxyl group, a hydroxyl group, an amide group, an amino group, an epoxy group, and the like such as (meth)acrylic acid, 2-hydroxypropyl (meth)acrylate, hydroxyethyl (meth)acrylate, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, and glycidyl (meth)acrylate may be cited.

[0077] The adhesive composition may contain a crosslinking agent. Examples of the crosslinking agent include metal ions having a valence of more than two and forming metal carboxylates with carboxyl groups, polyamine compounds forming amide bonds with carboxyl groups, polyepoxide compounds or polyols forming ester bonds with carboxyl groups, and polyisocyanate compounds forming amide bonds with carboxyl groups. Among them, polyisocyanate compounds are preferred.

[0078] The adhesive composition may contain additives such as microparticles, beads (resin beads, glass beads, etc.), glass fibers, resins other than base polymers, adhesion-imparting agents, fillers (metal powder, other inorganic powders, etc.), antioxidants, ultraviolet absorbers, dyes, pigments, colorants, defoaming agents, corrosion inhibitors, photopolymerization initiators, etc., for imparting light scattering properties.

[0079] The adhesive composition can be formed by applying a liquid diluted in an organic solvent onto a substrate and drying the liquid.

[0080] The thickness of the first adhesive layer is preferably 5 μm or more, and more preferably 10 μm or more. The upper limit of the thickness of the first adhesive layer is not particularly limited, and may be 50 μm or less, or 40 μm or less.

[0081] [Front panel]

[0082] The front panel 1 can be the outermost layer of the display device observed from the visual side. As long as the front panel 1 is a plate-like body that can transmit light, the material and thickness are not limited, and it can be composed of only one layer or more than two layers. As examples thereof, resin films, glass films, etc. can be cited. The front panel preferably has a resin film. The front panel 1 can be a laminate of a resin film and a glass film.

[0083] The thickness of the front panel 1 may be, for example, 30 to 200 μm, preferably 50 to 150 μm, and more preferably 50 to 100 μm.

[0084] When the front panel 1 has a resin film, as its material, for example, acrylic resins such as poly(methyl)acrylate and poly(ethyl)acrylate; polyolefin resins such as polyethylene, polypropylene, polymethylpentene and polystyrene; cellulose resins such as triacetyl cellulose, acetyl cellulose butyrate, propionyl cellulose, butyryl cellulose and acetyl propionyl cellulose; polyvinyl resins such as ethylene-vinyl acetate copolymer, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol and polyvinyl acetal; sulfone resins such as polysulfone and polyether sulfone; ketone resins such as polyether ketone and polyether ether ketone; polyether imide; polycarbonate resin; polyester resin; polyimide resin; polyamide-imide resin; and polyamide resin. These polymers can be used alone or in combination of two or more. Among them, from the viewpoint of improving strength and transparency, it is preferred to use polycarbonate resin, polyester resin, polyimide resin, polyamide-imide resin, or polyamide resin.

[0085] The thickness of the resin film may be, for example, 10 to 100 μm, preferably 20 to 70 μm, and more preferably 30 to 60 μm.

[0086] The front panel 1 can be a film in which a hard coating is provided on at least one surface of the resin film to further improve the hardness. The hard coating can be formed on one surface of the resin film or on both surfaces. A front panel with improved hardness and scratch resistance can be produced by providing a hard coating. The hard coating is, for example, a cured layer of an ultraviolet curing resin. As the ultraviolet curing resin, for example, acrylic resins, silicone resins, polyester resins, polyurethane resins, amide resins, epoxy resins, etc. can be cited. The hard coating can contain additives for improving hardness. The additives are not limited, and inorganic particles, organic particles, or mixtures thereof can be cited.

[0087] The visual side of the hard coating preferably forms a wear-resistant layer to improve wear resistance, or prevent contamination by sebum, etc. The front panel may have a wear-resistant layer, and the wear-resistant layer may be a layer constituting the visual side surface of the front panel. The wear-resistant layer contains a structure from a fluorine compound. As a fluorine compound, a compound having a silicon atom and a hydrolyzable group such as an alkoxy group or a halogen on the silicon atom is preferred. A coating film can be formed by a dehydration condensation reaction of a hydrolyzable group, and the adhesion of the wear-resistant layer can be improved by reacting with active hydrogen on the substrate surface. In addition, when the fluorine compound has a perfluoroalkyl or perfluoropolyether structure, water repellency can be imparted, and thus it is preferred. Particularly preferred is a fluorine-containing polyorganosiloxane compound having a perfluoropolyether structure and a long-chain alkyl group with more than 4 carbon atoms. As a fluorine compound, it is also preferred to use more than two compounds. As a fluorine compound preferably further included, a fluorine-containing organosiloxane compound containing an alkylene group with more than 2 carbon atoms and a perfluoroalkylene group.

[0088] The thickness of the wear-resistant layer is, for example, 1 nm to 20 nm. In addition, the wear-resistant layer is water-repellent, and the water contact angle is, for example, about 110 to 125°. The contact angle hysteresis and the slide angle measured by the slide method are about 3 to 20° and about 2 to 55°, respectively. In addition, the wear-resistant layer may also contain various additives such as silanol condensation catalysts, antioxidants, rust inhibitors, ultraviolet absorbers, light stabilizers, mildew inhibitors, antibacterial agents, biological adhesion inhibitors, deodorants, pigments, flame retardants, antistatic agents, etc., within the range that does not impair the effects of the present invention.

[0089] A primer layer may also be provided between the wear-resistant layer and the hard coating layer. As the primer, for example, there are primers such as ultraviolet curing type, heat curing type, moisture curing type or two-component curing type epoxy compounds. In addition, as the primer, polyamic acid may be used, and a silane coupling agent is also preferably used. The thickness of the primer layer is, for example, 0.001 to 2 μm.

[0090] As the method for obtaining the front panel comprising the wear-resistant layer and hardcoat, it can be formed in the following manner, that is, as required, primer is coated on the hardcoat and dried, solidified and after forming the primer layer, the composition (wear-resistant layer coating composition) comprising fluorine compound is coated and dried. As the method for coating, for example, dip coating, roller coating, rod coating, spin coating, spray coating, die coating, gravure coating etc. can be enumerated. In addition, it is also preferred that before applying primer or wear-resistant layer coating composition, the coating surface is implemented to hydrophilic treatments such as plasma treatment, corona treatment or ultraviolet treatment. This laminated body can both be directly laminated on the front panel, and it is also possible to use adhesive, bonding agent that the laminated body laminated on another transparent substrate is attached to the front panel.

[0091] When the front panel 1 has a glass film, the glass film is preferably a tempered glass for display. The thickness of the glass film may be, for example, 10 μm to 500 μm, or 20 μm to 100 μm. The use of the glass film can provide the front panel 1 with excellent mechanical strength and surface hardness.

[0092] When the laminated sheet is used in a display device, the front panel 1 can function as a window film of the display device. The front panel 1 can also further function as a touch sensor, a blue light cutoff function, a viewing angle adjustment function, and the like.

[0093] [Polarization layer]

[0094] The polarizing layer may have a linear polarizer and a phase difference film from the side close to the front panel. The polarizing layer may be a circular polarizer (including an elliptical polarizer). The circular polarizer can absorb external light reflected in the display device, so it can give the laminated sheet a function as an anti-reflection film. The polarizing layer preferably has a layer obtained by curing a polymerizable liquid crystal compound. According to the present invention, although there is a layer obtained by curing a polymerizable liquid crystal compound, the height of the burr can be reduced and the bending property can be improved.

[0095] [Linear polarizing plate]

[0096] The linear polarizer has the function of selectively transmitting linear polarized light in a certain direction among non-polarized light such as natural light. The linear polarizer may include a stretched film or stretched layer adsorbed with a dichroic dye, a solidified product of a polymerizable liquid crystal compound and a dichroic dye, and a liquid crystal layer in which the dichroic dye is dispersed and oriented in a layer obtained by curing the polymerizable liquid crystal compound, etc. as a polarizer. Compared with a stretched film or stretched layer adsorbed with a dichroic dye, a linear polarizer using a liquid crystal layer as a polarizer has no restrictions on the bending direction, and is therefore preferred.

[0097] (As a polarizer for a stretched film or stretched layer having a dichroic dye adsorbed thereon)

[0098] A polarizer as a stretched film with adsorbed dichroic dye can generally be manufactured through the following steps, namely, a step of uniaxially stretching a polyvinyl alcohol resin film, a step of adsorbing the dichroic dye by dyeing the polyvinyl alcohol resin film with a dichroic dye such as iodine, a step of treating the polyvinyl alcohol resin film with adsorbed dichroic dye with an aqueous boric acid solution, and a step of washing with water after the treatment with the aqueous boric acid solution.

[0099] The thickness of the polarizer is usually 30 μm or less, preferably 18 μm or less, and more preferably 15 μm or less. Reducing the thickness of the polarizer is advantageous for thinning the laminate. The thickness of the polarizer is usually 1 μm or more, for example, 5 μm or more.

[0100] The polyvinyl alcohol resin is obtained by saponifying a polyvinyl acetate resin. As the polyvinyl acetate resin, in addition to polyvinyl acetate which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other monomers copolymerizable therewith can also be used. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acid compounds, olefin compounds, vinyl ether compounds, unsaturated sulfone compounds, and (meth)acrylamide compounds having an ammonium group.

[0101] The saponification degree of the polyvinyl alcohol resin is usually about 85 mol% to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and polyvinyl formal, polyvinyl acetal, etc. modified with aldehydes may be used. The polymerization degree of the polyvinyl alcohol resin is usually 1000 to 10000, preferably 1500 to 5000.

[0102] The polarizer as a stretched layer adsorbed with a dichroic pigment can usually be manufactured via the following steps, that is, a step of applying a coating liquid containing the above-mentioned polyvinyl alcohol resin to a substrate film, a step of uniaxially stretching the obtained laminated film, a step of dyeing the polyvinyl alcohol resin layer of the laminated film after uniaxial stretching with a dichroic pigment so that it adsorbs the dichroic pigment to make a polarizer, a step of treating the film adsorbed with the dichroic pigment with an aqueous boric acid solution, and a step of washing with water after the treatment based on the aqueous boric acid solution. The substrate film used to form the polarizer can also be used as a protective layer of the polarizer. The substrate film can also be peeled off and removed from the polarizer as needed. The material and thickness of the substrate film can be the same as the material and thickness of the resin film described later.

[0103] The polarizer as a stretched film or stretched layer to which the dichroic dye is adsorbed may be used as a linear polarizing plate as it is, or a resin film may be laminated on one or both sides thereof to use as a linear polarizing plate. The thickness of the linear polarizing plate is preferably 2 μm to 40 μm.

[0104] As for the resin film, for example, cyclic polyolefin resin film; cellulose acetate resin film composed of resins such as triacetyl cellulose and diacetyl cellulose; polyester resin film composed of resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polycarbonate resin film; (meth) acrylic resin film; polypropylene resin film and other films known in the art can be cited. The polarizer and the protective layer can be laminated via a laminating layer described later.

[0105] The thickness of the resin film is, for example, 100 μm or less, preferably 80 μm or less, more preferably 60 μm or less, further preferably 40 μm or less, further preferably 30 μm or less, and is usually 10 μm or more, and is preferably 15 μm or more from the viewpoint of improving the absorptivity of laser light.

[0106] A hard coating layer may also be formed on the resin film. The hard coating layer may be formed on one side of the resin film or on both sides. By providing the hard coating layer, a thermoplastic resin film having improved hardness and scratch resistance may be produced. The hard coating layer may be formed in the same manner as the hard coating layer formed on the above-mentioned resin film.

[0107] (as a polarizer for the liquid crystal layer)

[0108] The polymerizable liquid crystal compound used to form the liquid crystal layer is a compound having a polymerizable reaction group and exhibiting liquid crystal properties. The polymerizable reaction group is a group that participates in the polymerization reaction, preferably a photopolymerizable reaction group. The photopolymerizable reaction group refers to a group that can participate in the polymerization reaction through active free radicals, acids, etc. generated by a photopolymerization initiator. As photopolymerizable functional groups, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, oxetane, etc. can be cited. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxirane and oxetane are preferred, and acryloyloxy is more preferred. The type of polymerizable liquid crystal compound is not particularly limited, and rod-shaped liquid crystal compounds, disc-shaped liquid crystal compounds and mixtures thereof can be used. The liquid crystal properties of the polymerizable liquid crystal compound can be thermotropic liquid crystal or lyotropic liquid crystal, and as a phase sequence structure, it can be a nematic liquid crystal or a smectic liquid crystal.

[0109] The dichroic dye used as the polarizer of the liquid crystal layer preferably has a maximum absorption wavelength (λMAX) in the range of 300 to 700 nm. Examples of such dichroic dyes include acridine dyes, The present invention can be used for the preparation of the present invention. ...

[0110] The polarizer as a liquid crystal layer can be formed by, for example, applying a composition for forming a polarizer comprising a polymerizable liquid crystal compound and a dichroic pigment on an orientation film formed on a substrate film, polymerizing and curing the polymerizable liquid crystal compound. The substrate film used to form the polarizer can also be used as a protective layer of the polarizer. The material and thickness of the substrate film can be the same as those of the above-mentioned resin film.

[0111] As a composition for forming a polarizer including a polymerizable liquid crystal compound and a dichroic pigment and a method for manufacturing a polarizer using the composition, the technical solutions described in Japanese Patent Publication No. 2013-37353, Japanese Patent Publication No. 2013-33249, Japanese Patent Publication No. 2017-83843, etc. can be exemplified. In addition to the polymerizable liquid crystal compound and the dichroic pigment, the composition for forming a polarizer may further include additives such as a solvent, a polymerization initiator, a crosslinking agent, a leveling agent, an antioxidant, a plasticizer, and a sensitizer. These components can be used only one type, or two or more types can be used in combination.

[0112] The polymerization initiator that the polarizer-forming composition may contain is a compound that can initiate the polymerization reaction of a polymerizable liquid crystal compound. In terms of being able to initiate the polymerization reaction under lower temperature conditions, a photopolymerization initiator is preferred. Specifically, a photopolymerization initiator that can generate active free radicals or acids by the action of light can be cited, wherein a photopolymerization initiator that generates free radicals by the action of light is preferred. The content of the polymerization initiator is preferably 1 to 10 parts by mass, more preferably 3 to 8 parts by mass, relative to the total amount of 100 parts by weight of the polymerizable liquid crystal compound. Within this range, the reaction of the polymerizable group is fully carried out, and it is easy to stabilize the orientation state of the liquid crystal compound.

[0113] The thickness of the polarizer as the liquid crystal layer is usually 10 μm or less, preferably 0.5 μm to 8 μm, and more preferably 1 μm to 5 μm.

[0114] The polarizer used as the liquid crystal layer can be used as a linear polarizer without peeling off the substrate film, or the substrate film can be peeled off from the polarizer layer and used as a linear polarizer. The polarizer used as the liquid crystal layer can also be used as a linear polarizer by forming a protective layer on one or both sides thereof. As the protective layer, the above-mentioned resin film can be used.

[0115] The polarizer as the liquid crystal layer may have a cover layer on one or both sides of the polarizer for the purpose of protecting the polarizer. The cover layer may be formed, for example, by coating a material (composition) for forming the cover layer on the polarizer. As the material constituting the cover layer, for example, a photocurable resin, a water-soluble polymer, etc. may be cited. As the material constituting the cover layer, a (meth) acrylic resin, a polyvinyl alcohol resin, etc. may be used.

[0116] [Phase difference film]

[0117] The phase difference film included in the polarizing layer may be composed of a phase difference layer of one layer, or may be a laminate of more than two phase difference layers. The phase difference film preferably has a phase difference layer comprising a layer obtained by curing a polymerizable liquid crystal compound. In the case where the phase difference film is a laminate of two phase difference layers, it is preferred that any phase difference layer is a phase difference layer comprising a layer obtained by curing a polymerizable liquid crystal compound. The phase difference film is laminated on the side of the polarizer opposite to the front panel side (or the first protective film side). The phase difference film may have a cover layer for protecting its surface, a substrate film for supporting the phase difference film, and the like.

[0118] The phase difference film preferably has a λ / 4 layer as a phase difference layer, and may further have at least one of a λ / 2 layer or a positive C layer. The phase difference layer may have an oriented film. In the case where the phase difference film has a phase difference layer as a λ / 2 layer, the λ / 2 layer and the λ / 4 layer may be stacked in sequence from the polarizer side. In the case where the phase difference film includes a phase difference layer as a positive C layer, the λ / 4 layer and the positive C layer may be stacked in sequence from the polarizer side, or the positive C layer and the λ / 4 layer may be stacked in sequence from the polarizer side.

[0119] The thickness of the retardation layer is, for example, 0.1 μm to 10 μm, preferably 0.5 μm to 8 μm, and more preferably 1 μm to 6 μm.

[0120] The phase difference layer may be formed of a resin film exemplified as a material for the protective layer, or may be formed of a layer cured by a polymerizable liquid crystal compound. The phase difference layer may further include an orientation film. The phase difference film may have a laminating layer for laminating the λ / 4 layer to the λ / 2 layer and the positive C layer. As described later, the laminating layer may be formed of an adhesive layer or an adhesive layer.

[0121] When the polymerizable liquid crystal compound is cured to form a phase difference layer, the phase difference layer can be formed by applying a composition containing a polymerizable liquid crystal compound to a substrate film and curing it. An orientation film can be formed between the substrate film and the coating layer. The material and thickness of the substrate film can be the same as the material and thickness of the above-mentioned resin film. When the phase difference layer is formed by curing the polymerizable liquid crystal compound, the phase difference layer can be assembled in a laminated sheet in the form of an orientation film and a substrate film. The phase difference layer can be bonded to the linear polarizer via a bonding layer.

[0122] [Touch sensor layer]

[0123] The touch sensor layer has at least a transparent conductive layer and may further have a resin film. The touch sensor layer may have a transparent conductive layer and a resin film in order from the front panel side (or the first protective film side). The touch sensor layer may also have a resin film and a transparent conductive layer in order from the front panel side (or the first protective film side). The touch sensor layer may also not have a resin film. In addition to the transparent conductive layer and the resin film, the touch sensor layer may also have a separation layer, a lamination layer, and a protective layer.

[0124] As a touch sensor layer, as long as it is a sensor that can detect the position touched on the surface of the display device and has a transparent conductive layer, the detection method is not limited. As the detection method of the touch sensor layer, there can be cited a resistive film method, an electrostatic capacitance method, an optical sensor method, an ultrasonic method, an electromagnetic induction coupling method, a surface elastic wave method, etc. Among them, a touch sensor layer of an electrostatic capacitance method is preferably used in terms of low cost, fast response speed, and thin film.

[0125] The transparent conductive layer may be a transparent conductive layer composed of a metal oxide such as ITO, or may be a metal layer composed of a metal such as aluminum, copper, silver, gold, or an alloy thereof.

[0126] The separation layer may be a layer formed on a substrate such as glass and used to separate the transparent conductive layer formed on the separation layer from the substrate together with the separation layer. The separation layer is preferably an inorganic layer or an organic layer. As a material for forming the inorganic layer, for example, silicon oxide can be cited. As a material for forming the organic layer, for example, a (meth) acrylic resin composition, an epoxy resin composition, a polyimide resin composition, etc. can be used.

[0127] [Third adhesive layer]

[0128] The third adhesive layer may be an adhesive layer for attaching the laminated sheet to a display panel or the like. The third adhesive layer may be composed of the same adhesive composition as the first adhesive layer. The thickness of the third adhesive layer is preferably 10 μm or more, more preferably 20 μm or more. The upper limit of the thickness of the first adhesive layer is not particularly limited, and may be 50 μm or less, or 40 μm or less.

[0129] [Third resin film]

[0130] The third resin film is a film used to temporarily adhere to the surface of the third adhesive layer to protect the display panel or other optical components before the third adhesive layer is attached to the display panel or other optical components. The third resin film can be a so-called isolation film. The third resin film is usually composed of a resin film subjected to a mold release treatment on one side with a silicone-based, fluorine-based or other mold release agent, and the mold release treatment surface is attached to the third adhesive layer.

[0131] As the resin constituting the third resin film, the same resin as the resin constituting the first resin film can be cited. The resin constituting the third resin film is preferably a polyester resin such as polyethylene terephthalate. The third resin film may be a single-layer structure or a multi-layer structure, and is preferably a single-layer structure from the viewpoints of ease of manufacture and manufacturing cost. The thickness of the third resin film may be, for example, 20 μm to 100 μm, or 30 μm to 80 μm.

[0132] [Lamination layer]

[0133] The laminating layer may be a layer for laminating the layers, and may be a layer composed of an adhesive or a bonding agent. Each laminating layer may be a layer composed of the same material, or a layer composed of different materials. When the phase difference film has a plurality of phase difference layers, the phase difference layers may be laminated to each other by an adhesive layer, or may be laminated to each other by an adhesive layer. Preferably, the linear polarizer and the phase difference film are laminated by an adhesive layer.

[0134] As the adhesive layer constituting the laminating layer, an adhesive layer similar to the above-mentioned first adhesive layer or third adhesive layer can be used.

[0135] As the adhesive, for example, one or more of water-based adhesives, active energy ray-curable adhesives, etc. can be combined to form. As the water-based adhesive, for example, polyvinyl alcohol resin aqueous solution, water-based two-component polyurethane emulsion adhesive, etc. can be cited. Active energy ray-curable adhesives are adhesives that are cured by irradiating active energy rays such as ultraviolet rays, and for example, adhesives containing polymerizable compounds and photopolymerization initiators, adhesives containing photoreactive resins, adhesives containing binder resins and photoreactive crosslinking agents can be cited. As the above-mentioned polymerizable compounds, photopolymerizable monomers such as photocurable epoxy monomers, photocurable acrylic monomers, photocurable urethane monomers, and oligomers from these monomers can be cited. As the above-mentioned photopolymerization initiator, compounds containing active species such as neutral free radicals, anionic free radicals, and cationic free radicals generated by irradiating active energy rays such as ultraviolet rays can be cited.

[0136] When the laminating layer is a pressure-sensitive adhesive layer, the thickness of the pressure-sensitive adhesive layer is preferably 1 to 30 μm, more preferably 2 to 20 μm, 3 to 10 μm. When the laminating layer is an adhesive layer, the thickness of the adhesive layer is preferably 0.01 to 5 μm, more preferably 0.1 to 3 μm.

[0137] <Method for producing laminated sheet>

[0138] The method for producing a laminated sheet includes a preparation step of preparing a laminated body and a cutting step of obtaining a laminated sheet from the laminated body. The method for producing a laminated sheet may include a peeling step of peeling off the second protective film.

[0139] The laminate prepared by the preparation process is sequentially laminated with the second protective film, the first protective film, the front panel and the polarizing layer. The first protective film has a first adhesive layer on one surface of the first resin film, and the first protective film is laminated on the front panel via the first adhesive layer. The second protective film has a second adhesive layer on one surface of the second resin film, and the second protective film is laminated on the first protective film via the second adhesive layer. The first protective film can be peeled off from the front panel, and the second protective film can be peeled off from the first protective film. The laminate can have layers (third adhesive layer, third resin film, touch sensor layer, coloring layer, impact-resistant film, resin film, etc.) that can be possessed by the laminate. The laminate can be in the shape of a long strip or a monolithic body of a specified size. The first protective film, the front panel and the polarizing layer can use the above-mentioned first protective film, the front panel and the polarizing layer.

[0140] In another embodiment, the laminate prepared by the preparation process is sequentially laminated with a second protective film, a first protective film and a polarizing layer. The first protective film has a first adhesive layer on one surface of the first resin film, and the first protective film is laminated on the polarizing layer via the first adhesive layer. The second protective film has a second adhesive layer on one surface of the second resin film, and the second protective film is laminated on the first protective film via the second adhesive layer. The first protective film can be peeled off from the polarizing layer, and the second protective film can be peeled off from the first protective film. The laminate can have layers that a laminate sheet can have (a third adhesive layer, a third resin film, a touch sensor layer, a coloring layer, an impact-resistant film, a resin film, etc.). The laminate can be in the form of a long strip or a monolithic body of a specified size. The first protective film and the polarizing layer can use the above-mentioned first protective film and polarizing layer.

[0141] Figure 3 The laminated body 400 shown is laminated with the second protective film 200, the first protective film 100, the front panel 1, and the polarizing layer 2 in this order. The first protective film 100 has a first adhesive layer 102 on one surface of the first resin film 101. The first protective film 100 is laminated on the front panel 1 via the first adhesive layer 102. The second protective film 200 has a second adhesive layer 202 on one surface of the second resin film 201. The second protective film 200 is laminated on the first protective film 100 via the second adhesive layer 202. The first protective film 100 can be peeled off from the front panel 1, and the second protective film 200 can be peeled off from the first protective film 100.

[0142] [Second protective film]

[0143] The second protective film is equivalent to a so-called surface protective film, and one surface of the second resin film has a second adhesive layer. The second protective film is laminated on the first protective film via the second adhesive layer. After the cutting process of obtaining the laminated sheet from the laminate is completed, the second protective film is peeled off together with the second adhesive layer it has. Therefore, the second protective film can be peeled off from the first protective film, and the second adhesive layer adjusts its adhesive force in a manner that it can be peeled off from the first protective film.

[0144] The adhesion between the second protective film and the first protective film is preferably smaller than the adhesion between the first protective film and the front panel. In another embodiment, the adhesion between the second protective film and the first protective film is preferably smaller than the adhesion between the first protective film and the polarizing layer. When peeling off the second protective film, it is not easy to accidentally peel off the first protective film.

[0145] The thickness of the second protective film may be, for example, 30 μm to 200 μm, or 40 μm to 150 μm.

[0146] [Second resin film]

[0147] As the resin constituting the second resin film, the same resin as the resin constituting the first resin film can be cited. The resin constituting the second resin film is preferably a polyester resin such as polyethylene terephthalate. The second resin film may be a single-layer structure or a multi-layer structure, and is preferably a single-layer structure from the viewpoints of ease of manufacture and manufacturing cost. The thickness of the second resin film may be, for example, 20 μm to 100 μm, 30 μm to 80 μm, or 40 μm or more.

[0148] [Second adhesive layer]

[0149] The second adhesive layer may be composed of the same adhesive composition as the first adhesive layer. The thickness of the second adhesive layer is preferably 3 μm or more, more preferably 5 μm or more. The upper limit of the thickness of the first adhesive layer is not particularly limited, and may be 50 μm or less, or 40 μm or less.

[0150] The laminate is produced by laminating the layers mutually, and the order of laminating the layers is not particularly limited. The laminate is obtained, for example, by a manufacturing method including a step of laminating the front panel and the polarizing layer, a step of laminating the first protective film on the front panel, and a step of laminating the second protective film on the first protective film. In another embodiment, the laminate is obtained, for example, by a manufacturing method including a step of laminating the first protective film on the polarizing layer, and a step of laminating the second protective film on the first protective film.

[0151] The cutting process of obtaining the laminated sheet from the laminate is carried out by irradiating the laminate with laser from the polarizing layer side (from the side opposite to the visual side) to cut the laminate into a specified shape. That is, the surface of the laser emission side is composed of the second protective film. By providing the laminate with the second protective film, the first protective film is not the outermost layer constituting the laminate, but becomes a layer existing inside the laminate. The outer peripheral edge of the laser emission side surface is more likely to form relatively large burrs than the outer peripheral edge of the layer existing inside the laminate. Therefore, by providing the laminate with the second protective film, it is easy to make the height of the burrs on the outer peripheral edge of the first protective film less than 6.0 μm.

[0152] The laser used is, for example, a laser that radiates light having a wavelength in the range of 200 nm to 11 μm. The laser may be a continuous wave (CW) laser or a pulsed laser. Examples of the types of lasers include CO 2 Gas lasers such as lasers, solid lasers such as YAG lasers, and semiconductor lasers. CO is preferred because it is easily suitable for the absorption region of the laminate. 2 laser.

[0153] The height of the burrs on the outer peripheral edge of the first protective film tends to decrease when the laser output is high. 2 In the case of laser, the output of the laser is preferably 50 W or more, more preferably 60 W or more, and further preferably 100 W or more. The upper limit of the output of the laser is not particularly limited, and may be, for example, 200 W or less.

[0154] From the same point of view, the energy of the laser irradiated by scanning with a unit step length (hereinafter, sometimes referred to as irradiation energy) is preferably 100 mJ / mm or more, more preferably 200 mJ / mm or more, and further preferably 250 mJ / mm or more. The upper limit of the irradiation energy is not particularly limited, for example, it can be 1000 mJ / mm or less, 500 mJ / mm or less.

[0155] The speed at which the laser moves on the surface of the laminate (hereinafter sometimes referred to as the moving speed) is preferably 50 mm / sec to 2000 mm / sec, more preferably 100 mm / sec to 1000 mm / sec, further preferably 150 mm / sec to 700 mm / sec, and may be 300 mm / sec or more.

[0156] When the laser is focused by the lens, the focus of the laser can be directed to the surface of the polarizing layer side of the laminate, the surface of the second protective film side, or the inside of the laminate. The spot size of the laser can be 5 μm to 100 μm, or 10 μm to 70 μm. The depth of focus (DOF) of the lens can be 10 μm to 500 μm, or 100 μm to 300 μm.

[0157] The cutting process can be performed in a full cutting manner, or it can be temporarily cut in a half cutting manner to a depth that does not cut the laminate, and the laminate is completely cut by irradiating the laser once or multiple times. Full cutting means cutting all layers throughout the stacking direction with one laser irradiation. From the viewpoint of reducing the height of the burrs on the outer peripheral portion of the first protective film, it is preferred to perform the cutting process in a full cutting manner.

[0158] The method for manufacturing the laminated sheet may include a peeling step of peeling off the second protective film. By peeling off the second protective film, a laminated sheet having the first protective film, the front panel, and the polarizing layer stacked in sequence may be obtained. In another embodiment, by peeling off the second protective film, a laminated sheet having the first protective film and the polarizing layer stacked in sequence may be obtained.

[0159] <Display device>

[0160] The display device holds the laminate by adsorbing the first protective film, peels off the third resin film to expose the adhesive layer, and adheres the laminate to the panel via the adhesive layer. The laminate is particularly preferably used for the display surface of a flexible display panel. The display panel can be constructed in a manner that can be folded with the visual side surface as the inner side, or in a manner that can be wound. As specific examples of display panels, liquid crystal display elements, organic EL display elements, inorganic EL display elements, plasma display elements, and field emission display elements can be cited.

[0161] Display devices can be used as portable devices such as smartphones and tablets, televisions, digital photo frames, electronic signage, detectors, instruments, office equipment, medical equipment, computer equipment, etc.

[0162] Example

[0163] The present invention will be described in more detail below based on Examples, but the present invention is not limited thereto. In the present Examples, the unit "part" of the ratio of the compounding substances is based on weight unless otherwise specified.

[0164] [Measurement of burr height]

[0165] The measurement was performed using a stylus film thickness meter (DEKTAK32, manufactured by VEECO). The height of the burrs was measured at 11 locations within a range of 60 mm along the edge of the laminated sheet, and the average value was obtained. The same operation was repeated 5 times, and the average value was taken as the height of the burrs.

[0166] [1st protective film]

[0167] A surface protective film was prepared in which an acrylic pressure-sensitive adhesive layer (10 μm thick) was formed on one surface of a polyethylene terephthalate film (125 μm thick).

[0168] [Second protective film]

[0169] A surface protective film was prepared in which an acrylic pressure-sensitive adhesive layer (6 μm thick) was formed on one surface of a polyethylene terephthalate film (50 μm thick).

[0170] [Third resin film]

[0171] A polyethylene terephthalate film subjected to mold release treatment, namely, a separator, is prepared.

[0172] [Front panel]

[0173] As the front panel, a laminated body in which a hard coating layer was formed on one surface of a polyimide (PI) film was used. The thickness of the polyimide film was 50 μm, and the thickness of the hard coating layer was 10 μm.

[0174] [Circular polarizing plate]

[0175] An orientation film is formed on one surface of a triacetyl cellulose (TAC) film. A composition having a polymerizable liquid crystal compound and a dichroic pigment is coated on the orientation film. The coating film is oriented and cured to obtain a polarizer. An ultraviolet curable resin is coated on the polarizer. The coating film is cured to form a cover layer. Thus, a linear polarizer is obtained. The thickness of the TAC film is 25 μm, the thickness of the polarizer is 2.5 μm, and the thickness of the cover layer is 1.0 μm. The polarizer is obtained by dispersing and oriented the dichroic pigment in the layer obtained by curing the polymerizable liquid crystal compound.

[0176] As the retardation layer, a λ / 4 layer having a layer obtained by curing a polymerizable liquid crystal compound and a positive C layer having a layer obtained by curing a polymerizable liquid crystal compound were prepared, and the two layers were bonded together with an ultraviolet curable adhesive to produce a retardation film.

[0177] The linear polarizing plate and the phase difference film were bonded together via an acrylic adhesive layer to obtain a circular polarizing plate. The phase difference film was laminated on the cover layer side of the linear polarizing plate. The angle between the absorption axis of the polarizer and the slow axis of the λ / 4 layer was 45°.

[0178] [Examples 1 to 4, Comparative Example 2]

[0179] The front plate and the circular polarizer were laminated to each other via an acrylic adhesive layer. The thickness of the acrylic adhesive layer was 25 μm. The front plate was laminated on the TAC film side of the circular polarizer. The acrylic adhesive layer was laminated on the retardation film of the circular polarizer, and further laminated on the third resin film.

[0180] The first protective film is laminated on the front panel via the adhesive layer possessed by the first protective film. The second protective film is laminated on the first protective film via the adhesive layer possessed by the second protective film. Thus, a laminated body in which the second protective film, the first protective film, the front panel, the circular polarizer, the third adhesive layer and the third resin film are sequentially laminated is prepared. The first protective film can be peeled off from the front panel, and the second protective film can be peeled off from the first protective film.

[0181] The laminate was irradiated with laser light under the conditions shown in Table 1 and cut into a predetermined shape (20 mm long x 100 mm wide) to obtain a laminate sheet. The second protective film was peeled off and the height of the burrs on the outer peripheral edge of the first protective film was measured. The results are shown in Table 1.

[0182] [Examples 5-6]

[0183] An acrylic adhesive layer is stacked on the phase difference film possessed by the circular polarizer, and then a third resin film is stacked. The first protective film is stacked on the circular polarizer via the adhesive layer possessed by the first protective film. It should be noted that the adhesive layer possessed by the first protective film is stacked on the TAC film side of the circular polarizer. The second protective film is stacked on the first protective film via the adhesive layer possessed by the second protective film. Thus, a laminated body in which the second protective film, the first protective film, the circular polarizer, the third adhesive layer and the third resin film are stacked in sequence is prepared. The first protective film can be peeled off from the circular polarizer, and the second protective film can be peeled off from the above-mentioned first protective film.

[0184] The laminate was irradiated with laser light under the conditions shown in Table 2 and cut into a predetermined shape (20 mm in length x 100 mm in width) to obtain a laminate sheet. The second protective film was peeled off and the height of the burrs on the outer peripheral edge of the first protective film was measured. The results are shown in Table 2.

[0185] [Comparative Examples 1, 3 and 4]

[0186] The front panel and the circular polarizer are stacked with each other via an acrylic adhesive layer. The thickness of the acrylic adhesive layer is 25 μm. The front panel is stacked on the TAC film side of the circular polarizer. An acrylic adhesive layer is stacked on the phase difference film possessed by the circular polarizer, and then a third resin film is stacked. The first protective film is stacked on the front panel via the adhesive layer possessed by the first protective film. Thus, a laminated body in which the first protective film, the front panel, the circular polarizer, the third adhesive layer and the third resin film are stacked in sequence is prepared. The first protective film can be peeled off from the front panel.

[0187] The laminate was irradiated with laser light under the conditions shown in Table 1 and cut into a predetermined shape (20 mm in length×100 mm in width) to obtain a laminate sheet. The height of the burrs was measured at the outer peripheral edge of the first protective film. The results are shown in Table 1.

[0188] [Comparative Examples 5-6]

[0189] An acrylic adhesive layer is stacked on the phase difference film possessed by the circular polarizer, and then a third resin film is stacked. The first protective film is stacked on the circular polarizer via the adhesive layer possessed by the first protective film. It should be noted that the adhesive layer possessed by the first protective film is stacked on the TAC film side of the circular polarizer. Thus, a laminated body in which the first protective film, the circular polarizer, the third adhesive layer and the third resin film are stacked in sequence is prepared. The first protective film can be peeled off from the circular polarizer.

[0190] The laminate was irradiated with laser light under the conditions shown in Table 2, and the laminate was cut into a predetermined shape (20 mm in length×100 mm in width) to obtain a laminate sheet. The height of the burrs was measured at the outer peripheral edge of the first protective film. The results are shown in Table 2.

[0191] [Table 1]

[0192]

[0193] [Table 2]

[0194]

[0195] In the table, 1 laser irradiation means that the laminate is cut completely, and 10 laser irradiations means that all layers in the lamination direction are completely cut at the 10th irradiation. Figure 3 In the case where the laser is irradiated from the second protective film 200 toward the polarizing layer 2, "from the side opposite to the viewing side" means, for example, Figure 3 The laser beam is irradiated in the direction from the polarizing layer 2 toward the second protective film 200 .

[0196] The height of the burrs on the outer peripheral portion of the first protective film of the laminated sheet of the present invention is 6.0 μm or less, and the adsorption force is unlikely to decrease when the laminated sheet is bonded to a display panel.

[0197] Explanation of symbols

[0198] 1…front panel, 2…polarizing layer, 3…bonding layer, 20…linear polarizing plate, 22…phase difference film, 40…burrs, 41…height of burrs, 50…third adhesive layer, 51…third resin film, 100…first protective film, 101…first resin film, 102…first adhesive layer, 200…second protective film, 201…second resin film, 202…second adhesive layer, 300…laminated sheet, 301…laminated sheet, 302…laminated sheet, 303…laminated sheet, 400…laminated body.

Claims

1. A laminated sheet, comprising a second protective film, a first protective film and a polarizing layer laminated in sequence, The first protective film has a first adhesive layer on one surface of the first resin film. The first protective film is laminated on the polarizing layer via the first adhesive layer. The second protective film has a second adhesive layer on one surface of the second resin film. The second protective film is laminated on the first protective film via the second adhesive layer. The first protective film can be peeled off from the polarizing layer, The second protective film can be peeled off from the first protective film, The height of the burrs on the outer peripheral edge of the first protective film is 6.0 μm or less. The burrs are formed by irradiating laser light from the polarizing layer side, wherein: The burrs are melted and solidified materials constituting the laminated sheet that are present on the surface of the first protective film on the side opposite to the first adhesive layer and at the outer peripheral portion thereof.

2. A laminated sheet, comprising a second protective film, a first protective film, a front panel and a polarizing layer laminated in sequence, The first protective film has a first adhesive layer on one surface of the first resin film. The first protective film is laminated on the front panel via the first adhesive layer. The second protective film has a second adhesive layer on one surface of the second resin film. The second protective film is laminated on the first protective film via the second adhesive layer. The first protective film can be peeled off from the front panel, The second protective film can be peeled off from the first protective film, The height of the burrs on the outer peripheral edge of the first protective film is 6.0 μm or less. The burrs are formed by irradiating laser light from the polarizing layer side, wherein: The burrs are melted and solidified materials constituting the laminated sheet that are present on the surface of the first protective film on the side opposite to the first adhesive layer and at the outer peripheral portion thereof.

3. The laminated sheet according to claim 1 or 2, wherein: The height of the burrs is greater than 0.1 μm.

4. The laminated sheet according to claim 1 or 2, wherein: The polarizing layer includes a layer obtained by curing a polymerizable liquid crystal compound.

5. A method for manufacturing a laminate, comprising: Preparation step: preparing the laminated body, The laminated body is sequentially laminated with a second protective film, a first protective film and a polarizing layer, The first protective film has a first adhesive layer on one surface of the first resin film. The first protective film is laminated on the polarizing layer via the first adhesive layer. The second protective film has a second adhesive layer on one surface of the second resin film. The second protective film is laminated on the first protective film via the second adhesive layer. The first protective film can be peeled off from the polarizing layer, The second protective film can be peeled off from the first protective film; and a cutting step of cutting the laminate into a predetermined shape by irradiating the laminate with laser light from the polarizing layer side to obtain a laminate sheet, The height of the burrs on the outer peripheral edge of the first protective film is 6.0 μm or less. The burrs are melted and solidified materials constituting the laminated sheet that are present on the surface of the first protective film on the side opposite to the first adhesive layer and at the outer peripheral portion thereof.

6. A method for manufacturing a laminate, comprising: Preparation step: preparing the laminated body, The laminated body is sequentially laminated with a second protective film, a first protective film, a front panel and a polarizing layer. The first protective film has a first adhesive layer on one surface of the first resin film. The first protective film is laminated on the front panel via the first adhesive layer. The second protective film has a second adhesive layer on one surface of the second resin film. The second protective film is laminated on the first protective film via the second adhesive layer. The first protective film can be peeled off from the front panel, The second protective film can be peeled off from the first protective film; and a cutting step of cutting the laminate into a predetermined shape by irradiating the laminate with laser light from the polarizing layer side to obtain a laminate sheet, The height of the burrs on the outer peripheral edge of the first protective film is 6.0 μm or less. The burrs are melted and solidified materials constituting the laminated sheet that are present on the surface of the first protective film on the side opposite to the first adhesive layer and at the outer peripheral portion thereof.

7. The method for producing a laminated sheet according to claim 5 or 6, wherein: In the cutting process, the output of the laser is 50W to 200W.

8. The method for producing a laminated sheet according to claim 5 or 6, wherein: In the cutting step, the laminate is cut into a predetermined shape by full cutting.

9. The method for producing a laminated sheet according to claim 5 or 6, wherein: The second resin film has a thickness of 40 μm or more.

10. The method for producing a laminated sheet according to claim 5 or 6, wherein: The polarizing layer includes a layer obtained by curing a polymerizable liquid crystal compound.