A continuous production method for purifying glycolide
Through the series crystallization kettle treatment of alcohol solvent washing and stepwise temperature drop, the problems of high energy consumption and solvent consumption in the glycolide purification process are solved, the continuous production of high-purity glycolide is realized, and the process cost and environmental pollution.
Patent Information
- Application Number
- CN202110467526.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-04-28
AI Technical Summary
The existing glycolide purification process has problems such as high energy consumption, complex equipment, large solvent consumption and low product yield, making it difficult to achieve continuous production of high-purity glycolide.
The continuous crystallization purification process is used to process the crude glycolide through serial crystallization kettles with alcohol solvent washing and stepped temperature drop, to achieve solid-liquid separation of the slurry and recycling of the mother liquor, and gradually improve the purity of glycolide.
It achieves the continuous production of high-purity glycolide, reduces solvent consumption and energy consumption, increases product yield, and has good process stability, making it suitable for industrial expansion of production.
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer preparation, in particular to a method for purifying glycolide by continuous crystallization. Background Art
[0002] Glycolide is a monomer for preparing biodegradable material polyglycolic acid by ring-opening polymerization. The purity of glycolide has a crucial influence on the conversion rate of ring-opening polymerization, the molecular weight of the product polymer, the molecular weight distribution, etc. Therefore, in the production process of polyglycolic acid, it is necessary to strictly control the content of impurities (such as acid, water, glycolic acid dimer or polymer, etc.) of the glycolide monomer used. The crude glycolide obtained by the current synthesis process is usually unable to reach the high purity required for the polymerization reaction. In addition, the impurity content of the high-purity glycolide monomer product, for example, will gradually increase when the storage time is long, and the purity of glycolide will gradually decrease, which is lower than the high purity required for the polymerization reaction. Therefore, purifying the crude glycolide to obtain high-quality refined glycolide plays a crucial role in realizing large-scale and continuous production of high-quality polyglycolic acid.
[0003] At present, the purification processes for crude cyclic lactide mainly include distillation purification process and recrystallization process. For example, in the distillation purification process, US5274073, CN1056689A, etc. use gas-assisted evaporation to separate cyclic lactide from impurities as a vapor component in the gas flow based on the difference in volatility between cyclic lactide and impurities. However, the distillation separation requires a large number of theoretical plates, a high bottom temperature, and a large energy consumption. Excessive temperature will accelerate the polymerization and hydrolysis of cyclic lactide, greatly reducing the product yield. In the recrystallization process, CN110511205A and CN100999516 use organic solvents such as ethyl acetate, acetone, isopropanol, etc. to purify glycolide by recrystallization. However, the purity of glycolide obtained by one recrystallization is not enough, and usually 3-5 recrystallizations are required, the solvent consumption is large, the purification cycle is long, and the product yield is too low. It can be seen that the distillation purification process has defects such as high energy consumption, complex process and equipment, and large investment, while the recrystallization process has problems such as large solvent consumption and low product yield.
[0004] Therefore, there is an urgent need in the art to provide a process for continuously producing purified glycolide, wherein the yield of purified glycolide obtained in each batch is substantially the same, and most of the mother liquor collected after purification can be recycled to save solvent. Summary of the invention
[0005] The present invention aims to provide a process for continuously producing refined glycolide.
[0006] The present invention provides a continuous production method for purifying glycolide, the method comprising the steps of:
[0007] (1) treating a crude glycolide product to obtain a pretreated material;
[0008] (2) mixing and dissolving the pretreated material with a solvent to obtain a liquid material;
[0009] (3) introducing the liquid materials one by one into two or more crystallization kettles connected in series to obtain a slurry; and
[0010] (4) Separating the slurry to obtain refined glycolide and mother liquor, and returning the mother liquor to step (2) for mixing.
[0011] In another embodiment, the treatment in step (1) comprises washing the crude glycolide product with an alcohol solvent, performing solid-liquid separation and retaining the solid.
[0012] In another embodiment, based on the total weight of the pretreated material obtained in step (1), the content of glycolic acid dimer does not exceed 0.25 w / w%.
[0013] In another embodiment, the solvent in step (2) is at least one of acetates, ketones or methane chloride.
[0014] In another embodiment, based on the total weight of the liquid material obtained in step (2), the content of glycolic acid dimer does not exceed 500 ppm.
[0015] In another embodiment, the temperature of the first crystallization kettle introduced in step (3) is 5-30°C lower than the dissolution temperature of step (2), and the temperature of the last crystallization kettle introduced is not higher than 0°C; for example, the temperature settings from the first to the last crystallization kettle decrease one by one, and the temperature difference between each crystallization kettle and the adjacent crystallization kettle in series is between 5-35°C.
[0016] In another embodiment, the residence time of the introduced liquid material in the crystallization kettle is 5-150 minutes.
[0017] In another embodiment, the amount of solvent added when the mother liquor in step (4) is returned to step (2) for mixing is 5-50 w / w% of the returned mother liquor; preferably 5-15 w / w%.
[0018] In another embodiment, after the solid-liquid separation of the slurry, the solid material is dried to obtain refined glycolide.
[0019] Accordingly, the present invention provides a process for continuously producing purified glycolide, and the yield of purified glycolide obtained in each batch is substantially the same, and most of the mother liquor collected after purification can be recycled to save solvent. DETAILED DESCRIPTION
[0020] After extensive and in-depth research, the inventors found that by controlling the content of glycolic acid dimer in the pre-treated material and using a continuous crystallization kettle, the crystallization mother liquor can be recycled to achieve continuous production of refined glycolide. On this basis, the present invention was completed.
[0021] The present invention provides a continuous production method for purifying glycolide, the method comprising the steps of:
[0022] The first step is to wash the crude glycolide product with an alcohol solvent to obtain a pretreated material;
[0023] The second step is to mix the pretreated material with an organic solvent to fully dissolve the pretreated material to obtain a liquid material;
[0024] The third step is to sequentially introduce the liquid material into at least two series-connected crystallization kettles with step-wise decreasing temperatures for cooling and crystallization, and obtain slurry from the last crystallization kettle;
[0025] The fourth step is to separate the slurry into solid and liquid to obtain refined glycolide and mother liquor;
[0026] In the fifth step, the mother liquor is returned to the second step to be mixed with the newly obtained pretreated material from the first step, and then the second step to the fourth step are carried out, thereby continuously circulating to continuously obtain refined glycolide.
[0027] In the crude glycolide product in the first step, in addition to glycolide, there are basically heavy impurities and light impurities, the heavy impurities are glycolic acid polymers with poor solubility, such as tetramers, pentamers or hexamers of glycolic acid, etc., and the light impurities are glycolic acid, water, other acids or residual solvents, etc. For example, but not limited to, the crude glycolide product contains about 65-98wt% glycolide, 1-28.5wt% glycolic acid, 0.5-1.5wt% water, and 0.5-5wt% glycolic acid polymers.
[0028] In the first step, the crude glycolide product is washed with an alcohol solvent, mainly to preliminarily clean the light component impurities in the crude glycolide. The alcohol solvent can be selected from one or more of the saturated monohydric alcohols of C1-C4; for example, one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol or tert-butanol, preferably ethanol. In one embodiment of the present invention, anhydrous ethanol is used for washing.
[0029] In one embodiment of the present invention, the crude glycolide product is washed with an alcohol solvent and then solid-liquid separated, and the obtained solid is the pre-treated material. The solid-liquid separation method includes but is not limited to suction filtration, centrifugation, etc.
[0030] In one embodiment of the present invention, the crude glycolide product is washed with an alcohol solvent and then centrifuged to remove the supernatant and retain the solid; this operation can be repeated 1-3 times.
[0031] Based on the total weight of the pretreated material obtained in the first step, the content of glycolic acid dimer is no more than 0.25 wt%, preferably no more than 0.23 wt%.
[0032] In one embodiment of the present invention, based on the total weight of the pretreated material obtained in the first step above, the moisture content (mainly anhydrous ethanol, mixed with glycolic acid, water, etc. in some raw crude glycolide products) does not exceed 5w / w%.
[0033] The organic solvent that can be used in the second step includes at least one of acetates, ketones or methane chlorides; and may also include alcohols.
[0034] The acetates may be selected from at least one of ethyl acetate and methyl acetate; the ketones may be selected from at least one of acetone, butanone, methyl ethyl ketone and methyl isobutyl ketone; the methane chloride may be selected from at least one of dichloromethane, chloroform and carbon tetrachloride; the alcohols may be selected from at least one of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol and tert-butanol.
[0035] The weight of the organic solvent used in the second step is 4-6 times the weight of the crude glycolide product in the first step.
[0036] The second step can be carried out by mixing and dissolving in a container commonly used in the art, such as, but not limited to, a stirred tank.
[0037] In one embodiment of the present invention, the second step is to add the pre-treated material into a stirring tank containing an organic solvent, and raise the temperature while stirring to fully dissolve the pre-treated material.
[0038] The dissolution temperature in the second step depends on the organic solvent used, as long as the pre-treated material can be completely dissolved, but it should be lower than the boiling point of the organic solvent to avoid unnecessary loss of the solvent. Taking ethyl acetate as an example, the dissolution temperature is generally 50-60°C.
[0039] In one embodiment of the present invention, the second step is to filter after the pre-treated material is fully dissolved to remove insoluble matter (such as glycolic acid polymers, etc.) in the crude glycolide product, thereby obtaining a liquid material.
[0040] Based on the total weight of the liquid material obtained in the second step, the content of glycolic acid dimer is no more than 500 ppm.
[0041] The liquid material in the third step is sequentially introduced into two or more series-connected crystallization kettles whose temperatures are gradually reduced. The temperature difference between two adjacent series-connected crystallization kettles needs to be conducive to recrystallization, that is, the degree of temperature reduction is conducive to the reduction of the solubility of glycolide in the liquid material, and the solution is saturated to precipitate refined glycolide. The inventors found that the temperature difference between two adjacent crystallization kettles is too large, which makes the material quench too fast or the degree of quench too strong. In this process, a large amount of glycolide will be rapidly precipitated and accumulated sharply, so that the glycolide precipitated earlier is easily adhered and retained on the inner wall of the crystallization kettle due to the pressure of a large amount of glycolide precipitated relatively later, so that the next batch of materials is difficult to carry out the retained materials of the previous batch when flowing through the crystallization kettle, thereby causing waste of materials and greatly reducing the final glycolide yield.
[0042] By using multiple crystallization kettles, before the material reaches the last crystallization kettle, the appropriate temperature difference between the two adjacent crystallization kettles can be used to appropriately reduce the quenching speed or degree of the material, so that the glycolide in the material can be precipitated more gently, which is beneficial to minimize or eliminate the retention of the precipitated glycolide in the crystallization kettle. Even if a small amount of retention occurs, the retained glycolide can be easily carried out by the next batch of materials.
[0043] The term "crystallization kettle" in the present invention has the common meaning in the art, that is, refers to a container capable of controlling the temperature within a certain range.
[0044] In one embodiment of the present invention, the temperature difference between each crystallization kettle and its adjacent crystallization kettle connected in series is between 5-35°C.
[0045] The temperature of the first crystallization kettle into which the liquid material is introduced in the third step is 5-30°C lower than the dissolution temperature in the second step, and the temperature of the last crystallization kettle into which the liquid material is introduced generally does not exceed 0°C.
[0046] In one embodiment of the present invention, the crystallization kettle in the third step is 5 series crystallization kettles with the temperature decreasing in a stepwise manner, wherein the temperature of the first crystallization kettle is set to 42°C, the temperature of the second crystallization kettle is set to 30°C, the temperature of the third crystallization kettle is set to 18°C, the temperature of the fourth crystallization kettle is set to 10°C, and the temperature of the fifth crystallization kettle is set to -5°C.
[0047] In one embodiment of the present invention, the crystallization kettle in the third step is 4 crystallization kettles connected in series with the temperature decreasing in a stepwise manner, wherein the temperature of the first crystallization kettle is set to 35°C, the temperature of the second crystallization kettle is set to 18°C, the temperature of the third crystallization kettle is set to 5°C, and the temperature of the fourth crystallization kettle is set to -5°C.
[0048] In one embodiment of the present invention, the crystallization kettle in the third step is three crystallization kettles connected in series with the temperature decreasing in a stepwise manner, wherein the temperature of the first crystallization kettle is set to 40°C, the temperature of the second crystallization kettle is set to 12°C, and the temperature of the third crystallization kettle is set to -5°C.
[0049] In one embodiment of the present invention, the crystallization kettle in the third step is two crystallization kettles connected in series with the temperature decreasing in a stepwise manner, wherein the temperature of the first crystallization kettle is set to 32°C, and the temperature of the second crystallization kettle is set to -2°C.
[0050] The liquid material introduced into the crystallization kettle in the third step needs to stay in the crystallization kettle for a period of time, such as 5-150 minutes; in one embodiment of the present invention, the higher the temperature of the crystallization kettle, the longer the stay time is generally.
[0051] The solid-liquid separation in the fourth step can be carried out by a method commonly used in the art, such as but not limited to centrifugation.
[0052] In one embodiment of the present invention, the solid material obtained by centrifuging the slurry in the fourth step can be dried to obtain refined glycolide. The drying can be carried out by conventional methods in the art, such as but not limited to vacuum drying at 40-60°C and an absolute pressure of ≤500Pa for 1-2 hours.
[0053] The glycolide purity of the refined glycolide or the refined glycolide product obtained by the present invention can reach more than 99.5%, the residual solvent rate is ≤0.3%, the glycolic acid content is less than 0.03wt%, the glycolic acid dimer content is less than 0.03wt%, and the water content is less than 0.03wt%. The contents of glycolide, residual solvent and glycolic acid dimer in the present invention are all measured by gas chromatography analysis method known in the art, the water content can be measured by Karl Fischer moisture meter, and the glycolic acid content is measured by potentiometric titration method known in the art (for example, automatic potentiometric titrator).
[0054] In one embodiment of the present invention, the solvent lost after drying in the fourth step is collected (for example but not limited to, collected by a heat exchanger) and mixed with the mother liquor. A very small amount of solvent will exist in the dried refined glycolide, which can be ignored if measured in kg.
[0055] In the fifth step, the mother liquor is returned to the container for mixing in the second step, in which the second batch of pre-treated materials from the first step, the mother liquor returned from the fifth step and the supplemented organic solvent are contained, and then the liquid material obtained by full dissolution is subjected to the third step of the second batch and the following steps, thereby carrying out the second batch production of refined glycolide, and so on, the third batch, the fourth batch and other batches of such processes are carried out to achieve continuous circulation / production. Based on the consideration of material balance in industrial production, the next batch circulation will bring out the residual or accumulated materials in the previous batch circulation process, and from the appearance, the amount of refined glycolide obtained in the next batch is basically the same as that in the previous batch.
[0056] The determination of how many batches of such circulation / production are to be carried out generally depends on the accumulated glycolic acid dimer content in the mother liquor to be returned to the second step in the fifth step or the glycolic acid and / or glycolic acid dimer content in the obtained refined glycolide product.
[0057] In one embodiment of the present invention, the supplemented organic solvent is about 5-50 w / w% of the returned mother liquor, for example but not limited to, about 5-15 w / w%, about 8-12 w / w%, about 9-11 w / w%, etc.
[0058] In one embodiment of the present invention, if the accumulated glycolic acid dimer content in the mother liquor to be returned to the second step exceeds 1000 ppm or the content of glycolic acid and / or glycolic acid dimer in the obtained refined glycolide product exceeds 0.03 wt%, the fifth step is stopped.
[0059] Once a round of continuous production process of multiple batches of purified glycolide of the present invention is completed, a new round of such continuous production process can be started, in which all newly added organic solvent is used in the second step (rather than the mother liquor returned and the supplementary organic solvent in the fifth step).
[0060] The various solvents used in the present invention are all of reagent grade and do not require further treatment.
[0061] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0062] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0063] In this article, all features defined in the form of numerical ranges or percentage ranges, such as values, quantities, contents and concentrations, are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0064] The above-mentioned features mentioned in the present invention or the features mentioned in the embodiments can be combined in any way. All the features disclosed in the specification of this case can be used in combination with any combination form. As long as there is no contradiction in the combination of these features, all possible combinations should be considered to be within the scope of this specification. Each feature disclosed in the specification can be replaced by any alternative feature that can provide the same, equal or similar purpose. Therefore, unless otherwise specified, the disclosed features are only general examples of equal or similar features.
[0065] The main advantages of the present invention are:
[0066] 1. The production method provided by the present invention can realize continuous cycle production.
[0067] 2. The production method provided by the present invention obtains high-purity refined glycolide (i.e., the product) in each round of continuous production, and except for the first batch of continuous production (figuratively speaking, the first batch of continuous production is used to pave the way, and once the road is paved, subsequent continuous cycle production can be achieved), the yield of refined glycolide obtained in each subsequent batch of continuous production is basically the same.
[0068] 3. Most of the crystallization mother liquor collected after the last cooling crystallization can be recycled, that is to say, only a small amount of solvent needs to be added in the next cycle to continue the cycle production, which can effectively save the use of solvent.
[0069] 4. The production method provided by the present invention adopts multiple series-connected crystallization kettles with stepped temperature reduction to continuously cool and crystallize the pretreated crude glycolide. Compared with the existing conventional recrystallization method, it can significantly save the amount of solvent used, there is no need to carry out the residual solvent removal process, there is no waste liquid treatment problem, and there is no pollution to the environment. The entire process flow has good continuity and stability, which can effectively avoid unnecessary material loss, reduce process costs, have low energy consumption, realize low-carbon continuous production, and facilitate industrial expansion of production.
[0070] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods for which specific conditions are not specified in the following examples are usually performed under normal conditions or according to the conditions recommended by the manufacturer. Unless otherwise specified, all percentages, ratios, proportions, or parts are by weight. The units in the weight volume percentages in the present invention are well known to those skilled in the art, for example, refer to the weight (grams) of the solute in 100 ml of solution. Unless otherwise defined, all professional and scientific terms used in the text have the same meaning as those familiar to those skilled in the art. In addition, any method and material similar or equivalent to the recorded content can be applied to the method of the present invention. The preferred implementation methods and materials described in the text are for demonstration purposes only.
[0071] In the following embodiments, the contents of glycolide, residual solvent and glycolic acid dimer in the obtained refined glycolide product are measured by gas chromatography analysis method known in the art, the water content is measured by Karl Fischer moisture meter, and the glycolic acid content is measured by potentiometric titration method known in the art (for example, using automatic potentiometric titrator).
[0072] Example 1 (5 crystallization kettles)
[0073] In the crude glycolide product to be purified in this example, the content of glycolide is about 92.3 wt %, the content of glycolic acid is about 3.6 wt %, the content of water is about 0.8 wt %, and the content of glycolic acid polymer is about 3.3 wt %.
[0074] 10 kg of crude glycolide product to be purified was taken, washed with anhydrous ethanol, and then centrifuged to remove the supernatant and retain the solid. The above operation was repeated twice (about 13.5 kg of anhydrous ethanol was used for each washing), and about 9.57 kg of pretreated material with a moisture content (mainly anhydrous ethanol, mixed with some impurities such as glycolic acid and water in the original crude glycolide) ≤ 5% and a glycolic acid dimer content of less than 0.22 wt% was obtained. The pretreated material was then added to a stirring kettle containing 40 kg of ethyl acetate solvent, and the temperature was raised to about 60° C. while stirring to fully dissolve the pretreated material. After filtering, solid impurities (very few, basically negligible) were removed, and about 49.57 kg of liquid material was retained, of which glycolic acid dimer in the liquid material was 1.34 wt%. The content is ≤500ppm, and then the liquid material is introduced into a first crystallization kettle at a temperature of about 42°C, with a residence time of about 120min, then introduced into a second crystallization kettle at a temperature of about 30°C, with a residence time of about 90min, then introduced into a third crystallization kettle at a temperature of about 18°C, with a residence time of about 50min, then introduced into a fourth crystallization kettle at a temperature of about 10°C, with a residence time of about 35min, and then introduced into a fifth crystallization kettle at a temperature of about -5°C, with a residence time of about 15min, and then about 49.57kg of the slurry of the fifth crystallization kettle is centrifuged, and the obtained solid is dried at 40°C and an absolute pressure of ≤500Pa for 2 hours to obtain about 7.09kg of refined glycolide, with a yield of 70.9%. , and about 89.2% (i.e., about 37.89 kg) of the obtained mother liquor of about 42.48 kg (the solvent lost after drying will be collected (for example, by using a heat exchanger) and mixed with the mother liquor. There will be a very small amount of solvent in the refined glycolide after drying, which can be ignored if measured in kg) is returned to the stirring tank, and then about 4 kg of ethyl acetate solvent is added to the stirring tank. After stirring and dissolving with the next batch of pretreated materials entering the stirring tank (Note: starting from the second batch, the amount of crude glycolide product to be purified in each batch is about 8.02 kg. After washing with anhydrous ethanol and centrifugal separation twice, about 7.68 kg of pretreated materials are obtained, in which the content of glycolic acid dimer is less than 0.22 wt%), the solid is removed by filtration. impurities, retaining about 49.57 kg of liquid material, wherein the content of glycolic acid dimer in the liquid material is ≤500 ppm, then introducing the liquid material into the first crystallization kettle for subsequent continuous cooling and crystallization, finally centrifuging about 49.57 kg of slurry obtained from the fifth crystallization kettle, retaining solids, and drying at 40° C. and absolute pressure ≤500 Pa for 2 hours to obtain about 7.09 kg of refined glycolide (to achieve continuous circulation, the second batch circulation will bring out the residual or accumulated materials in the first batch circulation process, and the amount of refined glycolide obtained in the first batch and the second batch is the same), with a yield of 88.4%, and about 89.2% (that is, about 37.89kg) is then returned to the stirring tank, and so on, to carry out the continuous production of refined glycolide.
[0075] Based on the above steps, in the first batch of refined glycolide products produced by the method of this embodiment, the content of glycolide is about 99.91wt%, the content of residual solvent is about 0.04wt%, the content of glycolic acid is about 0.0107wt%, the content of glycolic acid dimer is about 0.0102wt%, and the water content is less than 0.03wt%;
[0076] In the second batch of refined glycolide products, the content of glycolide was about 99.91wt%, the content of residual solvent was about 0.04wt%, the content of glycolic acid was about 0.0112wt%, the content of glycolic acid dimer was about 0.0105wt%, and the water content was less than 0.03wt%;
[0077] In the third batch of refined glycolide products, the glycolide content was about 99.91wt%, the residual solvent content was about 0.04wt%, the glycolic acid content was about 0.0116wt%, the glycolic acid dimer content was about 0.011wt%, and the water content was <0.03wt%.
[0078] Only three batches of refined glycolide products are listed here, but it should be noted that the liquid material formed in the stirring tank can be continuously introduced into the first crystallization tank for continuous cooling and crystallization, so the fourth batch, fifth batch, sixth batch... and even Nth batch of output can be achieved, until the accumulated glycolic acid dimer content in the mother liquor to be returned to the stirring tank exceeds 1000ppm or the content of glycolic acid and / or glycolic acid dimer in the obtained refined glycolide product exceeds 0.03wt%, the continuous production is stopped, new ethyl acetate solvent is replaced, and then new continuous production is restarted.
[0079] Comparative Example
[0080] In the crude glycolide product to be purified in this comparative example, the content of glycolide was about 92.3 wt %, the content of glycolic acid was about 3.6 wt %, the content of water was about 0.8 wt %, and the content of glycolic acid polymer was about 3.3 wt %.
[0081] 10 kg of the crude glycolide product to be purified was taken, washed with anhydrous ethanol, and then centrifuged to remove the supernatant and retain the solid. The above operation was repeated once (about 7.5 kg of anhydrous ethanol was used for each washing) to obtain about 9.64 kg of pretreated material with a moisture content (mainly anhydrous ethanol, mixed with some impurities such as glycolic acid and water in the original crude glycolide) ≤ 5%, and a glycolic acid dimer content of about 0.3 wt%). The pretreated material was then added to a stirred tank containing 40 kg of ethyl acetate solvent, and the temperature was raised to about 60° C. while stirring to fully dissolve the pretreated material. After filtering, solid impurities (very few, basically negligible) were removed, and about 49.64 kg of liquid material was retained, of which the liquid The content of glycolic acid dimer in the material is about 630ppm, and then the liquid material is introduced into a first crystallization kettle at a temperature of about 42°C, with a residence time of about 120min, then introduced into a second crystallization kettle at a temperature of about 30°C, with a residence time of about 90min, then introduced into a third crystallization kettle at a temperature of about 18°C, with a residence time of about 50min, then introduced into a fourth crystallization kettle at a temperature of about 10°C, with a residence time of about 35min, then introduced into a fifth crystallization kettle at a temperature of about -5°C, with a residence time of about 15min, and then about 49.64kg of the slurry of the fifth crystallization kettle is centrifuged, and the obtained solid is dried at 40°C and an absolute pressure of ≤500Pa for 2 hours to obtain About 7.1 kg of refined glycolide was obtained, with a yield of 71.0%, and about 89.1% (i.e., about 37.89 kg) of the obtained mother liquor of about 42.54 kg (the solvent lost after drying will be collected (for example, by using a heat exchanger) and mixed with the mother liquor. A very small amount of solvent will exist in the refined glycolide after drying, which can be ignored if measured in kg) was returned to the stirring tank, and about 4 kg of ethyl acetate solvent was added to the stirring tank to mix with the next batch of pretreated materials entering the stirring tank (Note: starting from the second time, the amount of crude glycolide product to be purified each time is about 8.02 kg. After washing with anhydrous ethanol and centrifugal separation twice, about 7.75 kg of pretreated materials were obtained, of which glycolic acid dimer The solid content is about 0.3wt%), and then filtered to remove solid impurities, and about 49.64kg of liquid material is retained, wherein the content of glycolic acid dimer in the liquid material is about 960ppm. The liquid material is then introduced into the first crystallization kettle for subsequent continuous cooling and crystallization. Finally, about 49.64kg of the slurry obtained from the fifth crystallization kettle is centrifuged, and the solid is retained. It is dried at 40°C and an absolute pressure of ≤500Pa for 2 hours to obtain about 7.1kg of refined glycolide with a yield of 88.5%, and about 89.1% (i.e., about 37.89kg) of the separated mother liquor of about 42.54kg is returned to the stirring kettle, and so on, for continuous production of refined glycolide.
[0082] Based on the above steps, in the first batch of refined glycolide products produced by the comparative method, the content of glycolide is about 99.50wt%, the content of residual solvent is about 0.4wt%, the content of glycolic acid is about 0.0242wt%, the content of glycolic acid dimer is about 0.0226wt%, and the water content is less than 0.03wt%;
[0083] In the second batch of refined glycolide products, the content of glycolide was about 99.50wt%, the content of residual solvent was about 0.4wt%, the content of glycolic acid was about 0.0298wt%, the content of glycolic acid dimer was about 0.0285wt%, and the water content was less than 0.03wt%;
[0084] In the third batch of refined glycolide products, the glycolide content was about 99.50wt%, the residual solvent content was about 0.4wt%, the glycolic acid content was about 0.0386wt%, the glycolic acid dimer content was about 0.0362wt%, and the water content was <0.03wt%.
[0085] It can be seen that the comparative method did not strictly control the content of glycolic acid dimer in the pretreated material and the liquid material, resulting in a sharp increase in the content of glycolic acid and glycolic acid dimer in the next batch of refined glycolide products (compared with the refined glycolide products produced in the previous batch). Only by the third batch, the contents of glycolic acid and glycolic acid dimer in the obtained refined glycolide products exceeded 0.03wt%, which did not meet the product standards and needed to be stopped. It was impossible to achieve stable and continuous production of refined glycolide.
[0086] Example 2 (4 crystallization kettles)
[0087] In the crude glycolide product to be purified in this example, the content of glycolide is about 84.9 wt %, the content of glycolic acid is about 12.6 wt %, the content of water is about 0.9 wt %, and the content of glycolic acid polymer is about 1.6 wt %.
[0088] 5 kg of crude glycolide product to be purified was taken, washed with anhydrous ethanol, and then centrifuged to remove the supernatant and retain the solid. The above operation was repeated twice (about 6.75 kg of anhydrous ethanol was used for each washing), and about 4.40 kg of pretreated material with a moisture content of ≤5% and a glycolic acid dimer content of less than 0.22 wt% was obtained. The pretreated material was then added to a stirring kettle containing 25 kg of ethyl acetate solvent, and the temperature was raised to about 60° C. while stirring to fully dissolve the pretreated material. The solid impurities (very few, basically negligible) were removed by filtration, and about 29.40 kg of liquid material was retained. The content of glycolic acid dimer in the liquid material is ≤500ppm, and then the liquid material is introduced into a first crystallization kettle at a temperature of about 35°C, with a residence time of about 100min, then introduced into a second crystallization kettle at a temperature of about 18°C, with a residence time of about 60min, then introduced into a third crystallization kettle at a temperature of about 5°C, with a residence time of about 30min, and then introduced into a fourth crystallization kettle at a temperature of about -5°C, with a residence time of about 8min, and then about 29.40kg of the slurry in the fourth crystallization kettle is centrifuged, and the obtained solid is dried at 40°C and an absolute pressure of ≤500Pa for 2 hours , that is, about 2.93 kg of refined glycolide was obtained, with a yield of 58.6%, and about 89% (about 23.56 kg) of the obtained mother liquor of about 26.47 kg was returned to the stirring tank, and about 2.5 kg of ethyl acetate solvent was added to the stirring tank, and the mixture was stirred and dissolved with the next batch of pre-treated materials entering the stirring tank (Note: starting from the second batch, the amount of crude glycolide product to be purified in each batch is about 3.8 kg. After washing with anhydrous ethanol and centrifugal separation twice, about 3.34 kg of pre-treated materials were obtained, in which the content of glycolic acid dimer was less than 0.22 wt%), and then filtered to remove solid impurities. Retain about 29.4 kg of liquid material, wherein the content of glycolic acid dimer in the liquid material is ≤500 ppm, and then introduce the liquid material into the first crystallization kettle for subsequent continuous cooling and crystallization. Finally, about 29.4 kg of slurry obtained from the fourth crystallization kettle is centrifuged and the solid is retained. It is dried at 40°C and absolute pressure ≤500 Pa for 2 hours to obtain about 2.93 kg of refined glycolide with a yield of 77.1%. About 89% (i.e., about 23.56 kg) of the separated mother liquor of about 26.47 kg is returned to the stirring kettle, and so on, for continuous production of refined glycolide.
[0089] Based on the above steps, in the first batch of refined glycolide products produced by the method of this embodiment, the content of glycolide is about 99.86wt%, the content of residual solvent is about 0.06wt%, the content of glycolic acid is about 0.011wt%, the content of glycolic acid dimer is about 0.0104wt%, and the water content is less than 0.03wt%;
[0090] In the second batch of refined glycolide products, the content of glycolide was about 99.86wt%, the content of residual solvent was about 0.06wt%, the content of glycolic acid was about 0.0114wt%, the content of glycolic acid dimer was about 0.0107wt%, and the water content was less than 0.03wt%;
[0091] In the refined glycolide product produced in the third batch, the glycolide content was about 99.86wt%, the residual solvent content was about 0.06wt%, the glycolic acid content was about 0.012wt%, the glycolic acid dimer content was about 0.0112wt%, and the water content was <0.03wt%.
[0092] Only three batches of refined glycolide products are listed here, but it should be noted that the liquid material formed in the stirring tank can be continuously introduced into the first crystallization tank for continuous cooling and crystallization, so the fourth batch, fifth batch, sixth batch... and even Nth batch of output can be achieved, until the accumulated glycolic acid dimer content in the mother liquor to be returned to the stirring tank exceeds 1000ppm or the content of glycolic acid and / or glycolic acid dimer in the obtained refined glycolide product exceeds 0.03wt%, the continuous production is stopped, new ethyl acetate solvent is replaced, and then new continuous production is restarted.
[0093] Example 3 (3 crystallization kettles)
[0094] In the crude glycolide product to be purified in this example, the content of glycolide was about 81.6 wt %, the content of glycolic acid was about 14.8 wt %, the content of water was about 1.2 wt %, and the content of glycolic acid polymer was about 2.4 wt %.
[0095] 5 kg of crude glycolide product to be purified was taken, washed with anhydrous ethanol, centrifuged, the supernatant was removed, and the solid was retained. The above operation was repeated twice (about 6.75 kg of anhydrous ethanol was used for each washing), and about 4.22 kg of pretreated material with a moisture content of ≤5% and a glycolic acid dimer content of less than 0.22 wt% was obtained. The pretreated material was then added to a stirring kettle containing 28 kg of ethyl acetate solvent, and the temperature was raised to about 60° C. while stirring to fully dissolve the pretreated material. The solid impurities (very few, basically negligible) were removed by filtration, and about 32. 22kg, wherein the content of glycolic acid dimer in the liquid material is ≤500ppm, and then the liquid material is introduced into a first crystallization kettle at a temperature of about 40°C, with a residence time of about 95min, then introduced into a second crystallization kettle at a temperature of about 12°C, with a residence time of about 30min, and then introduced into a third crystallization kettle at a temperature of about -5°C, with a residence time of about 10min, and then about 32.22kg of the slurry in the third crystallization kettle is centrifuged, and the obtained solid is dried at 52°C and an absolute pressure of ≤500Pa for 2 hours to obtain about 2.89kg of refined glycolide, with a yield of 5 7.85%, and about 89.2% (i.e., about 26.15kg) of the obtained mother liquor of about 29.33kg was returned to the stirring tank, and about 2.8kg of ethyl acetate solvent was added to the stirring tank, and the mixture was stirred and dissolved with the next batch of pre-treated materials (Note: starting from the second batch, the amount of crude glycolide product to be purified in each batch is about 3.88kg, and after washing with anhydrous ethanol and centrifugal separation twice, about 3.27kg of pre-treated materials were obtained, in which the content of glycolic acid dimer was less than 0.22wt%), and then filtered to remove solid impurities, retaining about 32. 22kg, wherein the content of glycolic acid dimer in the liquid material is ≤500ppm, and then the liquid material is introduced into the first crystallization kettle for subsequent continuous cooling and crystallization. Finally, about 32.22kg of the slurry obtained from the third crystallization kettle is centrifuged to retain the solid and dried at 52°C and absolute pressure ≤500Pa for 2 hours to obtain about 2.89kg of refined glycolide with a yield of 74.48%. About 89.2% (i.e., about 26.15kg) of the separated mother liquor of about 29.33kg is returned to the stirring kettle, and so on, for continuous production of refined glycolide.
[0096] Based on the above steps, in the first batch of refined glycolide products produced by the method of this embodiment, the content of glycolide is about 99.82wt%, the content of residual solvent is about 0.09wt%, the content of glycolic acid is about 0.0136wt%, the content of glycolic acid dimer is about 0.0128wt%, and the water content is less than 0.03wt%;
[0097] In the second batch of refined glycolide products, the content of glycolide was about 99.82wt%, the content of residual solvent was about 0.09wt%, the content of glycolic acid was about 0.0145wt%, the content of glycolic acid dimer was about 0.0134wt%, and the water content was less than 0.03wt%;
[0098] In the third batch of refined glycolide products, the glycolide content was about 99.82wt%, the residual solvent content was about 0.09wt%, the glycolic acid content was about 0.0152wt%, the glycolic acid dimer content was about 0.0139wt%, and the water content was <0.03wt%.
[0099] Only three batches of refined glycolide products are listed here, but it should be noted that the liquid material formed in the stirring tank can be continuously introduced into the first crystallization tank for continuous cooling and crystallization, so the fourth batch, fifth batch, sixth batch... and even Nth batch of output can be achieved, until the accumulated glycolic acid dimer content in the mother liquor to be returned to the stirring tank exceeds 1000ppm or the content of glycolic acid and / or glycolic acid dimer in the obtained refined glycolide product exceeds 0.03wt%, the continuous production is stopped, new ethyl acetate solvent is replaced, and then new continuous production is restarted.
[0100] Example 4 (2 crystallization kettles)
[0101] In the crude glycolide product to be purified in this example, the content of glycolide is about 92.2 wt %, the content of glycolic acid is about 5.7 wt %, the content of water is about 0.7 wt %, and the content of glycolic acid polymer is about 1.4 wt %.
[0102] 5 kg of crude glycolide product to be purified was taken, washed with anhydrous ethanol, and then centrifuged to remove the supernatant and retain the solid. The above operation was repeated twice (about 6.75 kg of anhydrous ethanol was used for each washing), and about 4.78 kg of pretreated material with a moisture content of ≤5% and a glycolic acid dimer content of less than 0.22 wt% was obtained. The pretreated material was then added to a stirring tank containing 30 kg of ethyl acetate solvent, and the temperature was raised to about 60° C. while stirring to fully dissolve the pretreated material. The solid impurities (very few, basically negligible) were removed by filtration. Retain about 34.78 kg of liquid material, wherein the content of glycolic acid dimer in the liquid material is ≤500 ppm, then introduce the liquid material into a first crystallization kettle at a temperature of about 32° C., with a residence time of about 60 min, then introduce it into a second crystallization kettle at a temperature of about -2° C., with a residence time of about 15 min, then centrifuge about 34.78 kg of slurry in the second crystallization kettle, and dry the obtained solid at 60° C. and absolute pressure ≤500 Pa for 2 hours to obtain about 3.34 kg of refined glycolide, with a yield of 66.8%, and the obtained mother liquor About 66.8% (i.e., about 21 kg) of about 31.44 kg was returned to the stirring tank, and about 10.5 kg of ethyl acetate solvent was added to the stirring tank. After stirring and dissolving with the next batch of pretreated materials (Note: starting from the second batch, the amount of crude glycolide product to be purified in each batch is about 3.94 kg. After washing with anhydrous ethanol and centrifugal separation twice, about 3.76 kg of pretreated materials were obtained, in which the content of glycolic acid dimer was less than 0.22 wt%), the solid impurities were removed by filtration, and about 35.44 kg of liquid materials were retained. The content of glycolic acid dimer in the liquid material is ≤500ppm, and the liquid material is then introduced into the first crystallization kettle for subsequent continuous cooling and crystallization. Finally, about 35.44kg of the slurry obtained from the second crystallization kettle is centrifuged, and the solid is retained and dried at 60°C and absolute pressure ≤500Pa for 2 hours to obtain about 3.12kg of refined glycolide with a yield of 79.19%. About 65% (i.e., about 21kg) of the separated mother liquor of about 32.32kg is returned to the stirring kettle, and so on, for continuous production of refined glycolide.
[0103] Based on the above steps, in the first batch of refined glycolide products produced by the method of this embodiment, the content of glycolide is about 99.80wt%, the content of residual solvent is about 0.1wt%, the content of glycolic acid is about 0.0142wt%, the content of glycolic acid dimer is about 0.013wt%, and the water content is less than 0.03wt%;
[0104] In the second batch of refined glycolide products, the content of glycolide was about 99.80wt%, the content of residual solvent was about 0.1wt%, the content of glycolic acid was about 0.0156wt%, the content of glycolic acid dimer was about 0.0148wt%, and the water content was less than 0.03wt%;
[0105] In the refined glycolide product produced in the third batch, the glycolide content was about 99.80wt%, the residual solvent content was about 0.1wt%, the glycolic acid content was about 0.0172wt%, the glycolic acid dimer content was about 0.0159wt%, and the water content was less than 0.03wt%.
[0106] Only three batches of refined glycolide products are listed here, but it should be noted that the liquid material formed in the stirring tank can be continuously introduced into the first crystallization tank for continuous cooling and crystallization, so the fourth batch, fifth batch, sixth batch... and even Nth batch of output can be achieved, until the accumulated glycolic acid dimer content in the mother liquor to be returned to the stirring tank exceeds 1000ppm or the content of glycolic acid and / or glycolic acid dimer in the obtained refined glycolide product exceeds 0.03wt%, the continuous production is stopped, new ethyl acetate solvent is replaced, and then new continuous production is restarted.
[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of the substantial technical content of the present invention. The substantial technical content of the present invention is broadly defined in the scope of the claims of the application. Any technical entity or method completed by others, if it is exactly the same as that defined in the scope of the claims of the application or an equivalent variation, will be deemed to be included in the scope of the claims.
Claims
1. A continuous production method for purifying glycolide, characterized in that: The method comprises the steps of: (1) washing the crude glycolide product with an alcohol solvent, performing solid-liquid separation and retaining the solid to obtain a pretreated material, wherein the content of glycolic acid dimer is no more than 0.25 w / w % based on the total weight of the pretreated material; (2) mixing and dissolving the pretreated material with a solvent to obtain a liquid material, wherein the content of glycolic acid dimer in the liquid material is less than 500 ppm based on the total weight of the liquid material; (3) introducing the liquid materials one by one into two or more crystallization kettles connected in series to obtain a slurry; (4) Separating the slurry to obtain refined glycolide and mother liquor, returning the mother liquor to step (2) for mixing, and stopping continuous production when the accumulated glycolic acid dimer content in the mother liquor exceeds 1000 ppm or the glycolic acid and / or glycolic acid dimer content in the obtained refined glycolide exceeds 0.03 wt%.
2. The production method according to claim 1, characterized in that In step (1), based on the total weight of the pretreated material, the content of glycolic acid dimer does not exceed 0.23 w / w%.
3. The production method according to claim 1, characterized in that In step (1), based on the total weight of the pretreated material, the moisture content does not exceed 5 w / w%, and the moisture content includes anhydrous ethanol, glycolic acid and water.
4. The production method according to claim 1, characterized in that The crude glycolide product in step (1) contains heavy component impurities and light component impurities, wherein the heavy component impurities are glycolic acid polymers, and the light component impurities are glycolic acid, water, other acids or residual solvents.
5. The production method according to claim 4, characterized in that The heavy component impurities are tetramers, pentamers or hexamers of glycolic acid.
6. The production method according to claim 1, characterized in that The crude glycolide product contains 65-98 wt % of glycolide, 1-28.5 wt % of glycolic acid, 0.5-1.5 wt % of water, and 0.5-5 wt % of glycolic acid polymer.
7. The production method according to claim 1, characterized in that The alcohol solvent is selected from one or more of C1-C4 saturated monohydric alcohols.
8. The production method according to claim 1, characterized in that The alcohol solvent is selected from one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol and tert-butanol.
9. The production method according to claim 1, characterized in that The alcohol solvent is ethanol.
10. The production method according to claim 1, characterized in that In step (1), anhydrous ethanol is used for washing.
11. The production method according to claim 1, characterized in that The solvent in step (2) is at least one of acetates, ketones or methane chloride.
12. The production method according to claim 11, characterized in that The solvent in step (2) also includes alcohols.
13. The production method according to claim 12, characterized in that In step (2), the acetate is selected from at least one of ethyl acetate and methyl acetate; the ketone is selected from at least one of acetone, butanone, methyl ethyl ketone and methyl isobutyl ketone; the methane chloride is selected from at least one of dichloromethane, chloroform and carbon tetrachloride; the alcohol is selected from at least one of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol and tert-butanol.
14. The production method according to claim 1, characterized in that The weight of the solvent used in step (2) is 4-6 times the weight of the crude glycolide product in step (1).
15. The production method according to claim 1, characterized in that The temperature of the first crystallization kettle introduced in step (3) is 5-30°C lower than the dissolution temperature of step (2), and the temperature of the last crystallization kettle introduced is not higher than 0°C.
16. The production method according to claim 15, characterized in that The temperature settings of the first to the last crystallization kettles are gradually decreased, and the temperature difference between each crystallization kettle and the adjacent crystallization kettles in series is between 5-35°C.
17. The production method according to claim 1, characterized in that The residence time of the introduced liquid material in the crystallization kettle is 5-150 minutes.
18. The production method according to claim 1, characterized in that When the mother liquor of step (4) is returned to step (2) for mixing, the amount of solvent added is 5-50w / w% of the returned mother liquor.
19. The production method according to claim 18, characterized in that When the mother liquor of step (4) is returned to step (2) for mixing, the amount of solvent added is 5-15w / w% of the returned mother liquor.
20. The production method according to any one of claims 1 to 19, characterized in that: After the slurry is separated from the solid and the liquid, the solid material is dried to obtain refined glycolide.
21. The production method according to claim 20, characterized in that The solvent lost after drying is collected and mixed with the mother liquor.
22. The production method according to claim 1, characterized in that In the refined glycolide, the glycolide purity is above 99.5%, the solvent residual rate is ≤0.3%, the glycolic acid content is less than 0.03wt%, the glycolic acid dimer content is less than 0.03wt%, and the water content is less than 0.03wt%.
Citation Information
Patent Citations
Process for purification of cyclic esters
CN1056689A
High-purity glycolide preparation method
CN110511205A
Continuous process for manufacture of a purified lactide
US5274073A
Purifying process of glycolide
CN100999516A
Preparation method for glycolide
CN101054371A