Terbium-doped tin oxide film and preparation method thereof

By combining sol-gel method and rapid heat treatment method, terbium-doped tin oxide film with strong photoluminescence properties was prepared, which solved the problems of complex process, high cost and environmental pollution in the existing technology, and achieved applicable High-efficiency luminescent materials for a variety of light source equipment.

CN115247064BActive Publication Date: 2024-11-05ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110060036.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-18
Publication Date
2024-11-05
Estimated Expiration
2041-01-18

AI Technical Summary

Technical Problem

It is difficult to prepare a terbium-doped tin oxide film with strong photoluminescence properties in the prior art, and it has complex processes, high cost, long reaction cycles, and great environmental pollution.

Method used

The terbium-doped tin oxide film was prepared by combining sol-gel method and rapid heat treatment. A large number of defects were formed by annealing at high temperature for a short time through rapid thermal annealing equipment, resulting in poor crystal field symmetry, increasing the chance of terbium ion transition, thereby improving luminescence strength.

Benefits of technology

The terbium-doped tin oxide film with strong photoluminescence properties has been prepared. The process is simple, the cost is low, and the environment is friendly. It is suitable for silicon-based light sources, LED light sources and display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115247064B_ABST
    Figure CN115247064B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of luminescent materials, and specifically to a terbium-doped tin oxide film and a preparation method thereof, comprising the following steps: step 1, dissolving a tin salt and a terbium salt in a solvent to obtain a solution A; step 2, spin coating the solution A on a substrate to prepare a film, and placing it on a heating table to heat it at a first temperature to obtain a substrate-based film; step 3, annealing the substrate-based film obtained in step 2 at a second temperature using a rapid thermal annealing device to obtain a substrate-based terbium-doped tin oxide film, wherein the terbium-doped tin oxide film is a photoluminescent material, and the second temperature is greater than the first temperature. The method has a simple preparation process, low equipment requirements, and a high degree of controllability. Compared with the traditional tube furnace heat treatment process, the preparation method involves less thermal budget in the preparation process, and the product has excellent photoluminescent properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of luminescent materials, and in particular to a terbium-doped tin oxide film and a preparation method thereof. Background Art

[0002] SnO2 is a wide bandgap semiconductor with a bandgap width of 3.6eV. It has high carrier mobility, low phonon energy, and high transmittance in the visible and near-infrared bands. Currently, high-quality SnO2 thin films can be prepared by vacuum vapor deposition. By doping Sb or F, the electron concentration in SnO2 can be greatly increased, making it an excellent conductive material. Summary of the invention

[0003] The primary technical problem to be solved by the present invention is to provide a terbium-doped tin oxide film and a preparation method thereof. The preparation method has simple process, low cost, short reaction cycle, and can prepare a terbium-doped tin oxide film with strong photoluminescence performance.

[0004] In order to solve the above technical problems, the present invention provides a technical solution: a method for preparing a terbium-doped tin oxide film, comprising the following steps:

[0005] Step 1, dissolving tin salt and terbium salt in a solvent to obtain solution A;

[0006] Step 2, spin coating solution A on a substrate to prepare a film, and placing the solution A on a heating table and heating it at a first temperature to obtain a thin film based on the substrate;

[0007] Step three, annealing the substrate-based film obtained in step two at a second temperature using a rapid thermal annealing device to obtain a terbium-doped tin oxide film based on the substrate, wherein the terbium-doped tin oxide film is a photoluminescent material, and the second temperature is greater than the first temperature.

[0008] The terbium salt includes one or more of terbium chloride hexahydrate, terbium nitrate, terbium sulfate and terbium carbonate; the tin salt includes one or more of stannous chloride dihydrate, stannous sulfate and stannous nitrate.

[0009] The molar ratio of tin salt to terbium salt is 100:(0.06-29).

[0010] Wherein, the molar volume ratio of the tin salt to the solvent is 1mmol:(7.5-113.6)ml.

[0011] Wherein, the solvent includes ethanol.

[0012] The substrate includes a semiconductor substrate, and the semiconductor substrate includes a crystalline silicon substrate, a germanium substrate, a gallium arsenide substrate, and a gallium nitride substrate.

[0013] The first temperature is 10-250° C., the second temperature is 100-1300° C., and the annealing time is 1-100 s.

[0014] The annealing treatment time is 1-40s, and the terbium-doped tin oxide film comprises amorphous terbium-doped tin oxide.

[0015] The number of spin coating layers is 1-10 layers.

[0016] The present application also includes a second technical solution, a terbium-doped tin oxide thin film, which is prepared by the above-mentioned method for preparing the terbium-doped tin oxide thin film, and the terbium-doped tin oxide thin film photoluminescently emits light in the visible band.

[0017] Among them, the terbium-doped tin oxide film photoluminescently emits light in the 500nm, 550nm, 590nm and 630nm bands.

[0018] The terbium-doped tin oxide film comprises amorphous terbium-doped tin oxide.

[0019] Beneficial effects of the present invention:

[0020] (1) The method for preparing the terbium-doped tin oxide thin film of the present invention adopts a sol-gel method and a rapid thermal treatment method to prepare a terbium-doped tin oxide thin film with photoluminescent properties. The present invention adopts a rapid thermal annealing device to prepare the terbium-doped tin oxide thin film, and the substrate-based thin film is further annealed by rapid heating. The short-term heating causes a large number of defects to be formed in the thin film, and the terbium-doped tin oxide thin film is obtained by rapid cooling. During the rapid cooling process, these defects cannot be repaired, resulting in a deterioration of the crystal field symmetry, resulting in an increase in the probability of terbium ion transition, so that the obtained terbium-doped tin oxide thin film has a strong luminous intensity, and can be widely used in silicon-based light sources, LED light sources, display devices and other fields.

[0021] (2) The method for preparing the terbium-doped tin oxide thin film of the present invention has cheap and readily available raw materials, a simple synthesis process with low cost, a short reaction cycle, no pollution to the environment, and a low thermal budget. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a photoluminescence image of the terbium-doped tin oxide film prepared in Examples 1 to 4 of the present application.

[0023] Figure 2 1 is the XRD diagram of the terbium-doped tin oxide thin film prepared in Examples 1 to 4 of the present application. DETAILED DESCRIPTION

[0024] The present invention provides a method for preparing a terbium-doped tin oxide thin film, comprising the following steps:

[0025] Step 1, dissolving tin salt and terbium salt in a solvent to obtain solution A;

[0026] Step 2, spin coating solution A on a substrate to prepare a film, and placing the solution A on a heating table and heating it at a first temperature to obtain a thin film based on the substrate;

[0027] Step three, annealing the substrate-based film obtained in step two at a second temperature using a rapid thermal annealing device to obtain a terbium-doped tin oxide film based on the substrate, wherein the terbium-doped tin oxide film is a photoluminescent material, and the second temperature is greater than the first temperature.

[0028] The embodiment of the present application prepares a terbium-doped tin oxide film with photoluminescence performance by combining a sol-gel method with a rapid thermal treatment method. The raw materials of the present invention are cheap and readily available, the synthesis process is simple and low in cost, the reaction cycle is short, and there is no pollution to the environment, and the thermal budget is low.

[0029] The embodiment of the present application uses a rapid thermal annealing device to prepare a terbium-doped tin oxide film. The film based on the substrate is further annealed by rapid heating. The short-term heating causes a large number of defects to form in the film. The terbium-doped tin oxide film is obtained by rapid cooling. During the rapid cooling process, these defects cannot be repaired, resulting in a deterioration of the crystal field symmetry, which increases the probability of terbium ion transition, so that the terbium-doped tin oxide film has a strong luminescence intensity. Tb 3+ Absorbs visible light, with green emission coming from 5 D4→ 7 F J Transition, higher energy level blue light comes from 5 D3 → 7 F J transition, but this transition is easy to pass through Tb( 5 D3)+Tb( 7 F6)→Tb( 5 D4)+Tb( 7 F6) cross-relaxation process and quenching occurs. The embodiment of the present application can improve Tb 3+ of 5 D4→ 7 F J Transition and 5 D3 → 7 F J The quenching caused by the transition is eliminated to obtain a terbium-doped tin oxide film with a strong luminescence intensity. The terbium-doped tin oxide film prepared in the embodiment of the present application can be widely used in the fields of silicon-based light sources, LED light sources, display devices, etc.

[0030] In the embodiment of the present application, the rapid thermal annealing equipment performs annealing at the second temperature, wherein the rapid thermal annealing temperature rise rate is 200°C / s; the temperature drop rate is 100-200°C / s. In the embodiment of the present application, the annealing atmosphere is air atmosphere.

[0031] In the embodiment of the present application, the terbium salt includes one or more of terbium chloride hexahydrate, terbium nitrate, terbium sulfate, and terbium carbonate; the tin salt includes one or more of stannous chloride dihydrate, stannous sulfate, and stannous nitrate. The embodiment of the present application can prepare a terbium-doped tin oxide film by using the above raw materials.

[0032] In the embodiment of the present application, the molar ratio of tin salt to terbium salt is 100:(0.06-29). By controlling the ratio of tin salt to terbium salt and the doping amount of terbium, the prepared terbium-doped tin oxide film has a strong photoluminescence intensity.

[0033] In the embodiment of the present application, the molar volume ratio of the tin salt to the solvent is 1 mmol: (7.5-113.6) ml. By controlling the amount of the solvent, the concentration of solution A is controlled, so as to control the uniformity and thickness of the film.

[0034] In the embodiment of the present application, the solvent includes ethanol. Tin salt and terbium salt can be dissolved in ethanol, and ethanol is volatile, which can reduce the preparation time of terbium stannate chlorate thin film products.

[0035] In the embodiment of the present application, the substrate includes a semiconductor substrate. Specifically, the semiconductor substrate includes a crystalline silicon substrate, a germanium substrate, a gallium arsenide substrate, and a gallium nitride substrate. The terbium tin chlorate thin film based on the semiconductor substrate can be applied to silicon-based light sources, LED light sources, integrated circuits and other fields.

[0036] In the embodiment of the present application, the first temperature is 10-250°C, the second temperature is 100-1300°C, and the annealing time is 1-100s. As a preferred solution, in the embodiment of the present application, the annealing time is preferably 1-60s, and the photoluminescence intensity of the product is the strongest.

[0037] More preferably, the annealing time is 1-40s, and the terbium-doped tin oxide film contains amorphous terbium-doped tin oxide. By controlling the annealing time to 1-40s, the prepared terbium tin chlorate film can contain an amorphous terbium tin chlorate film, so that the photoluminescence intensity of the product is stronger; and as the annealing time decreases, the content of amorphous terbium tin chlorate film in the terbium tin chlorate film increases, and the photoluminescence intensity of the product is enhanced; in the embodiment of the present application, the second temperature is 1000°C, the annealing time is 1s-9s, and the prepared terbium tin chlorate film is an amorphous terbium tin chlorate film, and the photoluminescence intensity of the terbium tin chlorate film is the strongest, and in the 550nm band, the luminescence intensity is as high as 5.6×104 .

[0038] In the embodiment of the present application, the number of layers of spin coating is 1-10 layers. In the embodiment of the present application, the number of layers of spin coating is 1 layer, 2 layers, 3 layers, 5 layers, 6 layers, 8 layers, 10 layers, etc. By spin coating different layers of solution A, the thickness of the prepared film can be set as needed, and at this thickness, the photoluminescence performance is optimal. In the embodiment of the present application, the thickness of the terbium tin chlorate film is 1-100nm.

[0039] The present application also includes a second technical solution, a terbium-doped tin oxide thin film, prepared by the above-mentioned method for preparing the terbium-doped tin oxide thin film, and the terbium-doped tin oxide thin film photoluminescence in the visible band. The terbium tin chlorate thin film of the embodiment of the present application can be applied to silicon-based light sources, LED light sources, display devices, integrated circuits and other fields. The embodiment of the present application prepares the terbium-doped tin oxide thin film by combining the sol-gel method and the rapid thermal treatment method, and the film is evenly distributed and has a strong photoluminescence intensity in the visible band.

[0040] In the embodiment of the present application, terbium-doped tin oxide photoluminescently emits light in the wavelength bands of 500nm, 550nm, 590nm and 630nm. In the embodiment of the present application, blue-indigo light is emitted at a wavelength of 500nm, green light is emitted at a wavelength of 550nm, yellow light is emitted at a wavelength of 590nm, and red light is emitted at a wavelength of 630nm. The intensity of green light is the strongest.

[0041] The following specific examples are used to further illustrate the method described in the present invention, but it is not intended that the present invention is limited to these examples.

[0042] Embodiment 1:

[0043] A method for preparing a terbium-doped tin oxide thin film, the steps comprising:

[0044] Step 1, dissolving 0.4516 g (2 mmol) of stannous chloride dihydrate and 0.0216 g (0.058 mmol) of terbium chloride hexahydrate in 15 ml of anhydrous ethanol, stirring at room temperature until completely dissolved to form a solution A, wherein the molar ratio of stannous chloride dihydrate to terbium chloride hexahydrate is 100:29; the molar volume ratio of stannous chloride dihydrate to ethanol is 1 mmol:7.5 mL.

[0045] Step 2: Take 40 μl of solution A and prepare a film on a silicon substrate by spin coating. Spin coating 3 layers and heat it on a heating table at 150° C. to obtain a thin film based on a silicon substrate.

[0046] Step 3: anneal the thin film based on silicon substrate obtained in step 2 at 1000°C for 1s using a rapid thermal annealing device (RTP) to obtain a terbium-doped tin oxide thin film based on substrate; wherein the terbium-doped tin oxide thin film is a photoluminescent material that emits photoluminescence in the visible band. The terbium-doped tin oxide thin film is an amorphous terbium-doped tin oxide thin film.

[0047] like Figure 2 As shown, Figure 2 The RTP 1000℃-1s spectrum in the figure is the XRD pattern of the terbium-doped tin oxide film prepared in the embodiment of the present application. Figure 2 It can be seen from the figure that the terbium-doped tin oxide film prepared in the embodiment of the present application is an amorphous film. Figure 1 As shown, Figure 1 The spectrum of RTP 1000℃-1s in the photoluminescence graph of the terbium-doped tin oxide film prepared in the embodiment of the present application shows that the terbium-doped tin oxide film emits photoluminescence at 500nm, 550nm, 590nm and 630nm. Among them, it emits blue-indigo light at 500nm, green light at 550nm, yellow light at 590nm, and red light at 630nm. The green light has the strongest light intensity, and the photoluminescence intensity at 550nm is as high as 5.6×10 4 , the photoluminescence intensity is 1.6×10 4 , the photoluminescence intensity is 1.42×10 4 , the photoluminescence intensity is 1.2×10 4 .

[0048] The embodiment of the present application prepares an amorphous terbium-doped tin oxide film by combining a sol-gel method with a rapid thermal treatment method, and the prepared amorphous terbium-doped tin oxide film has good photoluminescence performance. The implementation of the present application adopts a rapid thermal annealing device to prepare a terbium-doped tin oxide film, and the film based on the substrate is further annealed by rapid heating. The short-term heating causes a large number of defects to be formed in the film, and the terbium-doped tin oxide film is obtained by rapid cooling. During the rapid cooling process, these defects cannot be repaired, resulting in a deterioration of the crystal field symmetry, resulting in an increase in the probability of terbium ion transition, so that the obtained terbium-doped tin oxide film has a strong luminescence intensity.

[0049] Embodiment 2:

[0050] A method for preparing a terbium-doped tin oxide thin film, the steps comprising:

[0051] Step 1: dissolve 0.4516 g of stannous chloride dihydrate and 0.0216 g of terbium chloride hexahydrate in 15 ml of anhydrous ethanol, and stir at room temperature until completely dissolved to form solution A.

[0052] Step 2: Take 40 μl of solution A and prepare a film on a silicon substrate by spin coating. Spin coating 3 layers and heat it on a heating table at 150° C. to obtain a thin film based on a silicon substrate.

[0053] Step 3: anneal the thin film based on silicon substrate obtained in step 2 at 1000°C for 10s using a rapid thermal annealing device (RTP) to obtain a terbium-doped tin oxide thin film based on substrate; wherein the terbium-doped tin oxide thin film is a photoluminescent material that emits photoluminescence in the visible band. The terbium-doped tin oxide thin film is a terbium-doped tin oxide thin film that is a mixture of amorphous and crystalline states.

[0054] like Figure 2 As shown, Figure 2 The spectrum of RTP 1000℃-10s in the figure is the XRD pattern of the terbium-doped tin oxide film prepared in the embodiment of the present application. Figure 2 It can be seen that the diffraction peaks at (110), (101) and (211) crystal planes correspond to the characteristic peaks of the tin oxide phase. The terbium content in the embodiment of the present application is relatively low and is not shown in the XRD spectrum, indicating that a terbium-doped tin oxide film containing a crystalline state is formed. In the embodiment of the present application, the peak intensity of the diffraction peaks at (110), (101) and (211) crystal planes is relatively weak, indicating that the terbium-doped tin oxide film in the embodiment of the present application is a terbium-doped tin oxide film mixed with amorphous and crystalline states. Figure 1 As shown, Figure 1 The X-ray photoluminescence graph of the terbium-doped tin oxide film prepared in the embodiment of the present application shows that the film emits light at 500nm, 550nm, 590nm and 630nm, among which it emits blue-indigo light at 500nm, green light at 550nm, yellow light at 590nm and red light at 630nm. The green light has the strongest light intensity, and the photoluminescence intensity at 550nm is as high as 3.95×10 4 , the photoluminescence intensity is 0.8×10 4 , the photoluminescence intensity is 0.75×10 4 , the photoluminescence intensity is 0.6×10 4 .

[0055] Embodiment 3:

[0056] A method for preparing a terbium-doped tin oxide thin film, the steps comprising:

[0057] Step 1: dissolve 0.4516 g of stannous chloride dihydrate and 0.0216 g of terbium chloride hexahydrate in 15 ml of anhydrous ethanol, and stir at room temperature until completely dissolved to form solution A.

[0058] Step 2: Take 40 μl of solution A and prepare a film on a silicon substrate by spin coating. Spin coating 3 layers and heat it on a heating table at 150° C. to obtain a thin film based on a silicon substrate.

[0059] Step 3: anneal the thin film based on silicon substrate obtained in step 2 at 1000°C for 20s using a rapid thermal annealing device (RTP) to obtain a terbium-doped tin oxide thin film based on substrate; wherein the terbium-doped tin oxide thin film is a photoluminescent material that emits photoluminescence in the visible band. The terbium-doped tin oxide thin film is a terbium-doped tin oxide thin film that is a mixture of amorphous and crystalline states.

[0060] like Figure 2 As shown, Figure 2 The spectrum of RTP 1000℃-20s in the figure is the XRD pattern of the terbium-doped tin oxide film prepared in the embodiment of the present application. Figure 2 It can be seen that the diffraction peaks at (110), (101) and (211) crystal planes correspond to the characteristic peaks of the tin oxide phase. The terbium content in the embodiment of the present application is relatively low and is not shown in the XRD spectrum, indicating that a terbium-doped tin oxide film containing a crystalline state is formed. In the embodiment of the present application, the peak intensity of the diffraction peaks at (110), (101) and (211) crystal planes is relatively weak, indicating that the terbium-doped tin oxide film in the embodiment of the present application is a terbium-doped tin oxide film mixed with amorphous and crystalline states. Figure 1 As shown, Figure 1 The spectrum of RTP 1000℃-20s in the photoluminescence graph of the terbium-doped tin oxide film prepared in the embodiment of the present application shows that the terbium-doped tin oxide film emits photoluminescence at 500nm, 550nm, 590nm and 630nm. Among them, it emits blue indigo light at 500nm, green light at 550nm, yellow light at 590nm, and red light at 630nm. The green light has the strongest light intensity, and the photoluminescence intensity at 550nm is as high as 2.5×10 4 , the photoluminescence intensity is 0.72×10 4 , the photoluminescence intensity is 0.70×10 4 , the photoluminescence intensity is 0.48×10 4 .

[0061] Embodiment 4:

[0062] A method for preparing a terbium-doped tin oxide thin film, the steps comprising:

[0063] Step 1: dissolve 0.4516 g of stannous chloride dihydrate and 0.0216 g of terbium chloride hexahydrate in 15 ml of anhydrous ethanol, and stir at room temperature until completely dissolved to form solution A.

[0064] Step 2: Take 40 μl of solution A and prepare a film on a silicon substrate by spin coating. Spin coating 3 layers and heat it on a heating table at 150° C. to obtain a thin film based on a silicon substrate.

[0065] Step 3: anneal the thin film based on silicon substrate obtained in step 2 at 1000°C for 40s using a rapid thermal annealing device (RTP) to obtain a terbium-doped tin oxide thin film based on substrate; wherein the terbium-doped tin oxide thin film is a photoluminescent material that emits photoluminescence in the visible band. The terbium-doped tin oxide thin film is a terbium-doped tin oxide thin film that is a mixture of amorphous and crystalline states.

[0066] like Figure 2 As shown, Figure 2 The spectrum of RTP 1000℃-40s in the figure is the XRD pattern of the terbium-doped tin oxide film prepared in the embodiment of the present application. Figure 2 It can be seen that the diffraction peaks at (110), (101) and (211) crystal planes correspond to the characteristic peaks of the tin oxide phase. The terbium content in the embodiment of the present application is relatively low and is not shown in the XRD spectrum, indicating that a crystalline terbium-doped tin oxide film is formed. In the embodiment of the present application, the peak intensity of the diffraction peaks at (110), (101) and (211) crystal planes is relatively weak, indicating that the terbium-doped tin oxide film in the embodiment of the present application has a relatively high content of crystalline terbium-doped tin oxide. The terbium-doped tin oxide film in the embodiment of the present application is a terbium-doped tin oxide film containing a mixture of amorphous and crystalline states. Figure 1 As shown, Figure 1 The spectrum of RTP 1000℃-40s in the photoluminescence graph of the terbium-doped tin oxide film prepared in the embodiment of the present application shows that the terbium-doped tin oxide film emits photoluminescence at 500nm, 550nm, 590nm and 630nm. Among them, it emits blue-indigo light at 500nm, green light at 550nm, yellow light at 590nm, and red light at 630nm. The green light has the strongest light intensity, and the photoluminescence intensity at 550nm is as high as 1.3×10 4 , the photoluminescence intensity is 0.4×10 4 , the photoluminescence intensity is 0.39×10 4 , the photoluminescence intensity is 0.28×10 4 .

[0067] Embodiment 4:

[0068] A method for preparing a terbium-doped tin oxide thin film, the steps comprising:

[0069] Step 1: dissolve 0.4516 g of stannous chloride dihydrate and 0.0216 g of terbium chloride hexahydrate in 15 ml of anhydrous ethanol, and stir at room temperature until completely dissolved to form solution A.

[0070] Step 2: Take 40 μl of solution A and prepare a film on a silicon substrate by spin coating. Spin coating 3 layers and heat it on a heating table at 150° C. to obtain a thin film based on a silicon substrate.

[0071] Step 3: anneal the thin film based on silicon substrate obtained in step 2 at 1000°C for 40s using a rapid thermal annealing device (RTP) to obtain a terbium-doped tin oxide thin film based on substrate; wherein the terbium-doped tin oxide thin film is a photoluminescent material, which emits photoluminescence in the visible band. The terbium-doped tin oxide thin film is a crystalline terbium-doped tin oxide thin film.

[0072] like Figure 2 As shown, Figure 2 The spectrum of RTP 1000℃-60s in the figure is the XRD pattern of the terbium-doped tin oxide film prepared in the embodiment of the present application. Figure 2 It can be seen that the diffraction peaks at (110), (101) and (211) crystal planes correspond to the characteristic peaks of the tin oxide phase. The terbium content in the embodiment of the present application is relatively small and is not shown in the XRD spectrum, indicating that a crystalline terbium-doped tin oxide film is formed. The terbium-doped tin oxide film in the embodiment of the present application is a crystalline terbium-doped tin oxide film. Figure 1 As shown, Figure 1 The spectrum of RTP1000℃-60s in the photoluminescence graph of the terbium-doped tin oxide film prepared in the embodiment of the present application shows that the terbium-doped tin oxide film emits photoluminescence at 500nm, 550nm, 590nm and 630nm. Among them, it emits blue indigo light at 500nm, green light at 550nm, yellow light at 590nm, and red light at 630nm. The green light has the strongest light intensity, and the photoluminescence intensity at 550nm is 0.8×10 4 , the photoluminescence intensity is 0.25×10 4 , the photoluminescence intensity is 0.25×10 4 , the photoluminescence intensity is 0.2×10 4 .

[0073] Combined with the experimental results of Example 1 to Example 4, it can be known that as the rapid annealing time of the rapid thermal annealing equipment (RTP) increases, the amorphous terbium-doped tin oxide film gradually turns into a crystalline terbium-doped tin oxide film, until the annealing time reaches 60s, and a completely crystalline terbium-doped tin oxide film is formed. And from Example 1 to Example 4, as the annealing time increases, the content of crystalline terbium-doped tin oxide increases; as the crystalline content increases, the photoluminescence intensity of the terbium-doped tin oxide film gradually weakens, and when the terbium-doped tin oxide film is completely amorphous terbium-doped tin oxide, the photoluminescence intensity of the terbium-doped tin oxide film product is the strongest.

[0074] Combining Examples 1-4 of the present application with Comparative Example 1, it can be seen that the terbium-doped tin oxide film prepared by a tube furnace under the same conditions has a slow heating speed, a large thermal budget, and the prepared terbium-doped tin oxide film has no photoluminescence properties. However, the terbium-doped tin oxide film prepared by the preparation method of the embodiment of the present application has a strong photoluminescence property, wherein when the terbium-doped tin oxide film contains an amorphous terbium-doped tin oxide film, the luminescence intensity is the strongest.

[0075] Embodiment 5:

[0076] The difference between this embodiment and embodiment 1 is that the amount of terbium chloride hexahydrate in step 1 is changed to 0.0036 g, and the rest is the same as embodiment 1. Specifically, a method for preparing a terbium-doped tin oxide thin film comprises the following steps:

[0077] Step 1, dissolving 0.4516g (2mmol) of stannous chloride dihydrate and 0.0036g (0.001mmol) of terbium chloride hexahydrate in 15ml of anhydrous ethanol in sequence, stirring at room temperature until completely dissolved to form a mixed solution A, wherein the molar ratio of stannous chloride dihydrate to terbium chloride hexahydrate is 100:0.5; the molar volume ratio of stannous chloride dihydrate to ethanol is 1mmol:7.5mL.

[0078] Step 2: Take 40 μl of solution A and prepare a film on a silicon substrate by spin coating. Spin coat 3 layers and heat it on a heating table at 150°C.

[0079] Step three, annealing the prepared film at 1000° C. for 1 second using a rapid thermal annealing device (RTP) to obtain an amorphous terbium-doped tin oxide film.

[0080] Embodiment 6:

[0081] The difference between this embodiment and embodiment 1 is that the amount of ethanol in step 1 is changed to 20 ml, and the rest is the same as embodiment 1. Specifically, a method for preparing a terbium-doped tin oxide thin film comprises the following steps:

[0082] Step 1, dissolving 0.4516g of stannous chloride dihydrate and 0.0216g of terbium chloride hexahydrate in 20ml of anhydrous ethanol in sequence, stirring at room temperature until completely dissolved, to form a mixed solution A, wherein the molar ratio of stannous chloride dihydrate to terbium chloride hexahydrate is 100:29; and the molar volume ratio of stannous chloride dihydrate to ethanol is 1mmol:10mL.

[0083] Step 2: Take 40 μl of solution A and prepare a film on a silicon substrate by spin coating. Spin coating 3 layers and heat it on a heating table at 150° C. to obtain a thin film based on a silicon substrate.

[0084] Step three, annealing the silicon substrate-based film prepared in step two at 1000° C. for 1 second using a rapid thermal annealing device (RTP) to obtain an amorphous terbium-doped tin oxide film, which is a photoluminescent material.

[0085] Embodiment 7:

[0086] The difference between this embodiment and embodiment 1 is that the temperature of the RTP treatment in step 3 is changed to 900° C., and the rest is the same as embodiment 1. Specifically, a method for preparing a terbium-doped tin oxide thin film comprises the following steps:

[0087] Step 1: dissolve 0.4516 g of stannous chloride dihydrate and 0.0216 g of terbium chloride hexahydrate in 15 ml of anhydrous ethanol, and stir at room temperature until they are completely dissolved to form a mixed solution A.

[0088] Step 2: Take 40 μl of solution A and prepare a film on a silicon substrate by spin coating. Spin coating 3 layers and heat it on a heating table at 150° C. to obtain a thin film based on a silicon substrate.

[0089] Step three, annealing the thin film on the silicon substrate prepared in step two at 900° C. for 1 second using a rapid thermal annealing device (RTP) to obtain an amorphous terbium-doped tin oxide thin film, which is a photoluminescent material.

[0090] Embodiment 8:

[0091] The difference between this embodiment and embodiment 1 is that the temperature of the RTP treatment in step 3 is changed to 800° C., and the rest is the same as embodiment 1. Specifically, a method for preparing a terbium-doped tin oxide thin film comprises the following steps:

[0092] Step 1: dissolve 0.4516 g of stannous chloride dihydrate and 0.0216 g of terbium chloride hexahydrate in 15 ml of anhydrous ethanol, and stir at room temperature until they are completely dissolved to form a mixed solution A.

[0093] Step 2: Take 40 μl of solution A and prepare a film on a silicon substrate by spin coating. Spin coating 3 layers and heat it on a heating table at 150° C. to obtain a thin film based on a silicon substrate.

[0094] Step three, annealing the thin film on the silicon substrate prepared in step two at 800° C. for 1 second using a rapid thermal annealing device (RTP) to obtain an amorphous terbium-doped tin oxide thin film, which is a photoluminescent material.

[0095] Embodiment 9:

[0096] The difference between this embodiment and embodiment 1 is that the temperature of the RTP treatment in step 3 is changed to 700° C., and the rest is the same as embodiment 1. Specifically, a method for preparing a terbium-doped tin oxide thin film comprises the following steps:

[0097] Step 1: dissolve 0.4516 g of stannous chloride dihydrate and 0.0216 g of terbium chloride hexahydrate in 15 ml of anhydrous ethanol, and stir at room temperature until they are completely dissolved to form a mixed solution A.

[0098] Step 2: Take 40 μl of solution A and prepare a film on a silicon substrate by spin coating. Spin coating 3 layers and heat it on a heating table at 150° C. to obtain a thin film based on a silicon substrate.

[0099] Step three, annealing the thin film on the silicon substrate prepared in step two at 1000° C. for 1 second using a rapid thermal annealing device (RTP) to obtain an amorphous terbium-doped tin oxide thin film, which is a photoluminescent material.

[0100] Embodiment 10:

[0101] A method for preparing a terbium-doped tin oxide thin film comprises the following steps:

[0102] Step 1, dissolving 0.1g of stannous chloride dihydrate and 0.0001g of terbium chloride hexahydrate in 0.5ml of anhydrous ethanol in sequence, stirring at room temperature until completely dissolved, to form a mixed solution A, wherein the molar ratio of stannous chloride dihydrate to terbium chloride hexahydrate is 100:0.6; the molar volume ratio of stannous chloride dihydrate to ethanol is 1mmol:11.36mL.

[0103] Step 2: Take solution A and prepare a film on a germanium substrate by spin coating. Spin coating 3 layers and heat it on a heating table at 150° C. for 10 minutes to obtain a thin film based on a germanium substrate.

[0104] Step three, annealing the germanium substrate-based film prepared in step two at 200° C. for 1 second using a rapid thermal annealing device (RTP) to obtain an amorphous terbium-doped tin oxide film, which is a photoluminescent material.

[0105] Embodiment 11:

[0106] A method for preparing a terbium-doped tin oxide thin film comprises the following steps:

[0107] Step 1: dissolve 0.1 g of stannous chloride dihydrate and 0.0001 g of terbium chloride hexahydrate in 0.5 ml of anhydrous ethanol, and stir at room temperature until completely dissolved to form a mixed solution A.

[0108] Step 2: Take solution A and prepare a film on a gallium arsenide substrate by spin coating. Spin coat one layer and heat it on a heating table at 10° C. for 10 minutes to obtain a thin film based on a gallium arsenide substrate.

[0109] Step three, annealing the GaAs substrate-based film prepared in step two at 100° C. for 10 seconds using a rapid thermal annealing device (RTP) to obtain a terbium-doped tin oxide film, which is a photoluminescent material.

[0110] Embodiment 12:

[0111] A method for preparing a terbium-doped tin oxide thin film comprises the following steps:

[0112] Step 1, dissolving 1g of stannous chloride dihydrate and 0.1g of terbium chloride hexahydrate in 50ml of anhydrous ethanol in turn, stirring at room temperature until completely dissolved, to form a mixed solution A, wherein the molar ratio of stannous chloride dihydrate to terbium chloride hexahydrate is 100:6; and the molar volume ratio of stannous chloride dihydrate to ethanol is 1mmol:113.6mL.

[0113] Step 2: Take solution A and prepare a film on a gallium nitride substrate by spin coating. Spin coating 10 layers and heat it on a heating table at 250° C. for 10 minutes to obtain a thin film based on a gallium nitride substrate.

[0114] Step three, annealing the film based on the gallium nitride substrate prepared in step two at 1300° C. for 1 second using a rapid thermal annealing device (RTP) to obtain a terbium-doped tin oxide film, which is a photoluminescent material.

[0115] Embodiment 13:

[0116] A method for preparing a terbium-doped tin oxide thin film comprises the following steps:

[0117] Step 1: dissolve 0.5 g of stannous chloride dihydrate and 0.1 g of terbium chloride hexahydrate in 20 ml of anhydrous ethanol, and stir at room temperature until they are completely dissolved to form a mixed solution A.

[0118] Step 2: Take solution A and prepare a film on a gallium nitride substrate by spin coating. Spin coating 8 layers and heat it on a heating table at 200° C. for 5 minutes to obtain a thin film based on a gallium nitride substrate.

[0119] Step three, annealing the film based on the gallium nitride substrate prepared in step two at 1200° C. for 1 second using a rapid thermal annealing device (RTP) to obtain a terbium-doped tin oxide film, which is a photoluminescent material.

[0120] Embodiment 14:

[0121] A method for preparing a terbium-doped tin oxide thin film comprises the following steps:

[0122] Step 1: dissolve 0.5 g of stannous nitrate 20 hydrate and 0.00572 g of terbium nitrate in 20 ml of anhydrous ethanol, and stir at room temperature until completely dissolved to form a mixed solution A.

[0123] Step 2: Take solution A and prepare a film on a germanium substrate by spin coating. Spin coating 6 layers and heat it on a heating table at 200° C. for 20 minutes to obtain a thin film based on a germanium substrate.

[0124] Step three, annealing the germanium substrate-based film prepared in step two at 1100° C. for 1 second using a rapid thermal annealing device (RTP) to obtain a terbium-doped tin oxide film, which is a photoluminescent material.

[0125] Comparative Example 1:

[0126] A method for preparing a terbium-doped tin oxide thin film, the steps comprising:

[0127] Step 1: dissolve 0.4516 g of stannous chloride dihydrate and 0.0216 g of terbium chloride hexahydrate in 15 ml of anhydrous ethanol, and stir at room temperature until completely dissolved to form solution A.

[0128] Step 2: Take 40 μl of solution A and prepare a film on a silicon substrate by spin coating. Spin coating 3 layers and heat it on a heating table at 150° C. to obtain a thin film based on a silicon substrate.

[0129] Step 3: Place the thin film based on silicon substrate obtained in step 2 in a tube furnace, heat up at a rate of 10°C / s, anneal at 1000°C for 1s, cool at a rate of 10°C / s, and obtain a terbium-doped tin oxide thin film based on substrate; obtain a terbium-doped tin oxide thin film without photoluminescence performance. The terbium-doped tin oxide thin film is a crystalline terbium-doped tin oxide thin film.

[0130] Obviously, the above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, any modification, substitution, or improvement made on the basis of the above description and within the method and principle of the present invention should be included in the protection scope of the present invention. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the protection scope of the present invention.

Claims

1. A method for preparing a terbium-doped tin oxide thin film, characterized in that: The following steps are involved: Step 1, dissolving tin salt and terbium salt in a solvent to obtain solution A; Step 2, spin coating solution A on a substrate to prepare a film, and placing the solution A on a heating table and heating it at a first temperature to obtain a thin film based on the substrate; Step three, annealing the substrate-based film obtained in step two at a second temperature using a rapid thermal annealing device, the rapid thermal annealing heating rate is 200°C / s; the cooling rate is 100-200°C / s, to obtain a terbium-doped tin oxide film based on the substrate, wherein the terbium-doped tin oxide film is a photoluminescent material, and the second temperature is greater than the first temperature.

2. The method for preparing a terbium-doped tin oxide thin film according to claim 1, characterized in that: The terbium salt includes one or more of terbium chloride hexahydrate, terbium nitrate, terbium sulfate, and terbium carbonate; the tin salt includes one or more of stannous chloride dihydrate, stannous sulfate, and stannous nitrate.

3. The method for preparing the terbium-doped tin oxide thin film according to claim 2, characterized in that: The molar ratio of the tin salt to the terbium salt is 100:(0.06-29).

4. The method for preparing the terbium-doped tin oxide thin film according to claim 3, characterized in that: The molar volume ratio of the tin salt to the solvent is 1 mmol:(7.5-113.6) ml.

5. The method for preparing the terbium-doped tin oxide thin film according to claim 1, characterized in that: The solvent includes ethanol, and the number of layers of the spin coating is 1-10 layers.

6. The method for preparing a terbium-doped tin oxide thin film according to claim 1, characterized in that: The substrate includes a semiconductor substrate, and the semiconductor substrate includes a crystalline silicon substrate, a germanium substrate, a gallium arsenide substrate, or a gallium nitride substrate.

7. The method for preparing a terbium-doped tin oxide thin film according to claim 1, characterized in that: The first temperature is 10-250° C., the second temperature is 100-1300° C., and the annealing treatment time is 1-100 s.

8. The method for preparing a terbium-doped tin oxide thin film according to claim 7, characterized in that: The annealing treatment time is 1-40s, and the terbium-doped tin oxide film comprises amorphous terbium-doped tin oxide.

9. A terbium-doped tin oxide thin film, characterized in that: The terbium-doped tin oxide film is prepared by the method for preparing the terbium-doped tin oxide film according to any one of claims 1 to 8.

10. The terbium-doped tin oxide thin film according to claim 9, characterized in that: The terbium-doped tin oxide film emits photoluminescence in the wavelength bands of 500nm, 550nm, 590nm and 630nm.