Microchannel catalyst and its preparation method and application

By introducing active components of Group VIII metal elements on raspberry-type oxide microsphere carriers and performing re-reduction and passivation treatments, the problems of low catalyst activity and harsh reduction and passivation conditions are solved, and efficient methanol purification and passivation are achieved. Acetaldehyde removal effect.

CN115254122BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110482635.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-30
Publication Date
2024-10-15
Estimated Expiration
2041-04-30

AI Technical Summary

Technical Problem

In the existing technology, the catalytic activity of the methanol purification catalyst is low, and the conditions for reduction and passivation are harsh, making it difficult to effectively process the microchannel small particle catalyst, affecting the methanol purification efficiency.

Method used

Raspberry-type oxide microspheres are used as carriers, and active components of Group VIII metal elements are introduced through the impregnation method, followed by re-reduction and passivation treatments to prepare microchannel catalysts containing multiple active centers to improve the activity and selectivity of the catalyst.

Benefits of technology

It significantly improves the acetaldehyde removal efficiency of the catalyst, shortens the start-up time and reduces the start-up cost, and improves the regeneration performance and reaction activity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115254122B_ABST
    Figure CN115254122B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of catalysts, and in particular to a microchannel catalyst and a preparation method and application thereof, wherein the catalyst comprises a carrier and an active component loaded on the carrier, and the content of the active component is below 40% by weight based on the total amount of the catalyst and the oxide; the carrier is a raspberry-type oxide microsphere, and the raspberry-type oxide microsphere is a hollow microsphere having a large hole on the surface, and the hollow microsphere has a hollow structure inside, and the large hole and the hollow structure are connected to form a cavity with an opening at one end; the number of active centers of the catalyst after the catalyst is reduced is 0.02-0.3 mmol hydrogen / g catalyst, and the reduction treatment conditions include: a temperature of 200 ° C, a time of 2 hours, a reduction atmosphere of a hydrogen concentration of 10% by volume, and an atmosphere containing hydrogen and argon, and a gas-agent volume ratio of 15000. The catalyst provided by the present invention has a high acetaldehyde removal efficiency in the methanol purification process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to a microchannel catalyst and a preparation method and application thereof. Background Art

[0002] The HPPO process uses hydrogen peroxide to epoxidize propylene to produce propylene oxide. The reaction of propylene and hydrogen peroxide is carried out in a methanol solvent. Some by-products generated in the HPPO process and circulating methanol will react with hydrogen peroxide to generate some compounds, such as formaldehyde, acetaldehyde, propylene glycol, hydroxyacetone, formic acid, acetic acid, methyl formate, methyl acetate, acetals, etc. These compounds will accumulate in the circulating methanol and are difficult to separate by distillation, which will directly affect the purity of the PO product. Most of the by-product compounds can be removed by catalytic hydrogenation. The catalyst uses metals such as Pd, Pt, Rh, Ru, Ir, Os, and Ni, and the carrier uses activated carbon or porous metal oxides, such as activated carbon, Al 2 O 3 、SiO 2 , zeolite, aluminosilicate, TiO 2 、ZrO 2 wait.

[0003] The metal components of metal hydrogenation catalysts are usually prepared in the form of oxides. Only by reducing the catalyst can it have methanogenic catalytic activity. The quality of catalyst reduction directly affects the performance of the catalyst. Reasonable selection of catalyst reduction pretreatment conditions can make the catalyst have higher activity in the reaction.

[0004] The catalyst reduction method can adopt ex situ pre-reduction treatment or in situ reduction treatment technology. The ex situ pre-reduction technology can improve the utilization rate of the reducing agent and reduce the amount of reducing agent. The pre-reduced catalyst can be restored to activity through simple reactivation at a lower temperature, thereby reducing the start-up time, reducing the start-up cost, shortening the start-up cycle, and ultimately increasing the economic benefits of the enterprise.

[0005] Microchannel reactors have excellent heat and mass transfer capabilities, and can achieve instantaneous uniform mixing of materials and efficient heat transfer. Therefore, many reactions that cannot be achieved in conventional reactors can be achieved in microreactors.

[0006] For the same catalyst, different reduction and passivation treatment methods have different effects on the activity and selectivity of the reaction. Different catalysts usually use different reduction and passivation treatment methods to achieve better activity and selectivity. The pre-reduction passivation method in the prior art takes a long time and is not suitable for the treatment of microchannel small particle catalysts. It is necessary to develop a pre-reduction method that is simple to operate, safe and reliable for pre-reduction treatment of catalysts. Summary of the invention

[0007] The purpose of the present invention is to overcome the defects of low catalytic activity and harsh reduction passivation conditions of methanol purification catalysts in the prior art, and to provide a microchannel catalyst and a preparation method and application thereof. The catalyst provided by the present invention has a high acetaldehyde removal efficiency in the methanol purification process.

[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides a microchannel catalyst, which includes a carrier and an active component loaded on the carrier, wherein the active component is selected from at least one of the metal elements of Group VIII, and the content of the active component is less than 40% by weight based on the total amount of the catalyst and calculated as oxide; the carrier is a raspberry-shaped oxide microsphere, and the raspberry-shaped oxide microsphere is a hollow microsphere having a large hole on the surface, and the hollow microsphere has a hollow structure inside, and the large hole and the hollow structure are connected to form a cavity with an open end;

[0009] Wherein, the oxide in the raspberry-shaped oxide microspheres is selected from one or more of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, calcium oxide and titanium oxide;

[0010] Among them, the number of active centers of the catalyst after the re-reduction treatment is 0.02-0.3 mmol hydrogen / g catalyst, and the re-reduction treatment conditions include: temperature of 200°C, time of 2 hours, re-reduction atmosphere of an atmosphere containing hydrogen and argon with a hydrogen concentration of 10 volume%, and a gas-to-agent volume ratio of 15000.

[0011] A second aspect of the present invention provides a method for preparing a microchannel catalyst, the method comprising:

[0012] (1) preparing raspberry-shaped oxide microspheres;

[0013] (2) introducing active components into the raspberry-shaped oxide microspheres by an impregnation method to obtain an oxidized catalyst; the active components are selected from at least one of the metal elements of Group VIII;

[0014] (3) reducing the oxidized catalyst under a hydrogen-containing atmosphere;

[0015] (4) after the temperature of the catalyst obtained by reduction in step (3) drops below 60° C., the catalyst obtained by reduction in step (3) is passivated, wherein the passivation comprises: continuously introducing an oxygen-containing gas below 60° C. and controlling the passivation temperature to be no higher than 90° C.; wherein the oxygen concentration of the oxygen-containing gas is continuously increased;

[0016] The amount of the raspberry-shaped oxide microspheres and the active component is such that the content of the active component in the oxidized catalyst is less than 40 wt %, preferably 10-36 wt %, based on the total amount of the oxidized catalyst and calculated as oxide.

[0017] The third aspect of the present invention provides a microchannel catalyst prepared by the preparation method described in the second aspect.

[0018] The fourth aspect of the present invention provides the use of the microchannel catalyst described in the first aspect or the third aspect in a methanol purification reaction.

[0019] Through the above technical scheme, the microchannel catalyst carrier provided by the present invention is a raspberry-shaped oxide microsphere, which has a short diffusion distance and a large macroscopic surface area during application. In addition, the microchannel catalyst provided by the present invention has more active centers and has better acetaldehyde removal performance when applied in the methanol purification process. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a SEM photograph of the raspberry-shaped oxide microspheres prepared in Preparation Example 1 of the present invention. DETAILED DESCRIPTION

[0021] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0022] In the present invention, the gas-to-catalyst ratio refers to the ratio of the volume of gas passing through the catalyst bed per hour to the volume of the catalyst. In the reduction process (or re-reduction process), the gas in the gas-to-catalyst ratio refers to the reducing gas (i.e., hydrogen-containing gas), and in the passivation process, the gas in the gas-to-catalyst ratio refers to the passivating gas (i.e., oxygen-containing passivating gas, also called oxygen-containing gas).

[0023] In the present invention, for the purpose of distinction, the reduction of the catalyst before passivation is referred to as "reduction", and the reduction of the catalyst after passivation is referred to as "re-reduction".

[0024] The first aspect of the present invention provides a microchannel catalyst, which includes a carrier and an active component loaded on the carrier, wherein the active component is selected from at least one of the metal elements of Group VIII, and the content of the active component is less than 40% by weight based on the total amount of the catalyst and calculated as oxide; the carrier is a raspberry-shaped oxide microsphere, and the raspberry-shaped oxide microsphere is a hollow microsphere having a large hole on the surface, and the hollow microsphere has a hollow structure inside, and the large hole and the hollow structure are connected to form a cavity with an open end;

[0025] Wherein, the oxide in the raspberry-shaped oxide microspheres is selected from one or more of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, calcium oxide and titanium oxide;

[0026] Among them, the number of active centers of the catalyst after the re-reduction treatment is 0.02-0.3 mmol hydrogen / g catalyst, and the re-reduction treatment conditions include: temperature of 200°C, time of 2 hours, re-reduction atmosphere of an atmosphere containing hydrogen and argon with a hydrogen concentration of 10 volume%, and a gas-to-agent volume ratio of 15000.

[0027] Preferably, the number of active centers of the catalyst after the re-reduction treatment is 0.05-0.25 mmol hydrogen / g catalyst, more preferably 0.15-0.25 mmol hydrogen / g catalyst.

[0028] In the present invention, the number of active centers of the catalyst is determined by H 2 Programmed temperature desorption (TPD) 2 -TPD) test, the test method includes: weighing 0.2000g of 40-60 mesh sample, first performing re-reduction activation, and the re-reduction conditions are: hydrogen content 10 volume % H 2 -Ar mixed gas, the mixed gas flow rate was 50mL / min, and the temperature was raised to 200℃ at a heating rate of 10℃ / min for 2h. The reduced catalyst was heated to 10% by volume H 2 -Ar mixed gas, and when the temperature dropped to 55°C, switch to Ar gas for purging at an Ar flow rate of 20 mL / min until the baseline was stable, and then perform H 2 -TPD experiment. 2 -TPD experimental conditions and procedures are as follows: carrier gas is Ar, carrier gas flow rate is 20 mL / min, heating rate is 10 °C / min, final temperature is 400 °C, thermal conductivity detector (TCD) detects the signal, and obtains the TPD curve.

[0029] According to a preferred embodiment of the present invention, through TPR characterization, in the TPR curve of the catalyst, the temperature corresponding to the peak value of the low-temperature reduction peak with the largest area is 120-240°C, preferably 130-220°C, and more preferably 130-200°C.

[0030] In the present invention, the temperature corresponding to the peak value of the low-temperature reduction peak with the largest area in the TPR spectrum curve can be used as an indicator for evaluating the regeneration performance of the passivated catalyst. The lower the temperature corresponding to the peak value of the low-temperature reduction peak with the largest area, the easier the catalyst is to regenerate. The microchannel catalyst provided by the present invention has good regeneration performance. The TPR (i.e., programmed temperature reduction) characterization is carried out on an Autochem2950 fully automatic high-pressure chemical adsorption instrument produced by Micromeritics, USA. The specific test conditions include: taking 0.20g of sample, first under 50mL / min Ar gas flow, at a heating rate of 10℃ / min, the sample is heated to 120℃ for dehydration treatment for 1 hour, and after the temperature drops to 50℃, a TPR experiment is carried out. The experimental conditions and procedures of TPR are: the reducing gas is 10 volume% H 2 -Ar mixed gas, the reducing gas flow rate is 50mL / min, and the temperature is increased to 900°C at a heating rate of 10°C / min; during the above heating process, the signal is detected by a thermal conductivity detector (TCD) to obtain a TPR spectrum curve.

[0031] According to the present invention, preferably, the content of the active component is 10-36% by weight, calculated as oxide, based on the total amount of the catalyst.

[0032] The present invention has a wide range of selection for the active component. Preferably, the active component is selected from one or more of Co, Ni, Ru, Pd and Pt, and more preferably includes Ni. In the preferred case of the present invention, as long as Ni is included, other components may be optionally included.

[0033] In addition to the above-mentioned active components, the microchannel catalyst provided by the present invention may optionally include an auxiliary agent. There is no particular limitation on the type and content of the auxiliary agent, and those skilled in the art may make appropriate selections according to different fields.

[0034] According to the present invention, specifically, in the catalyst, based on the total amount of the catalyst, the content of the carrier is above 60 wt%, preferably 64-90 wt%.

[0035] According to the microchannel catalyst provided by the present invention, the oxide in the raspberry-shaped oxide microspheres is an inorganic oxide, which can be selected from one or more of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, calcium oxide and titanium oxide, preferably aluminum oxide and / or silicon oxide.

[0036] According to the microchannel catalyst provided by the present invention, the particle size of the raspberry-shaped oxide microspheres is preferably 3 - 2500 μm, more preferably 10 - 500 μm.

[0037] According to the microchannel catalyst provided by the present invention, in the raspberry-shaped oxide microspheres, the diameter of the hollow structure is 1 - 2000 μm, preferably 1 - 400 μm.

[0038] According to the present invention, in the raspberry-shaped oxide microspheres, the pore diameter of the macropores is 0.2 - 1000 μm, preferably 0.5 - 200 μm.

[0039] According to the present invention, in the raspberry-shaped oxide microspheres, the shell thickness of the hollow microspheres is 0.2 - 1000 μm, preferably 0.5 - 200 μm.

[0040] According to the present invention, the appearance of the raspberry-shaped oxide microspheres is close to spherical. Preferably, the sphericity of the raspberry-shaped oxide microspheres is 0.5 - 0.99.

[0041] The sphericity of the microsphere blank is calculated by the formula

[0042] σ = 4πA / L 2 where: σ is the sphericity; A is the projected area of the microsphere, in m 2 ²; L is the projected perimeter of the microsphere, in m; A and L are obtained by processing the SEM photos of the microspheres through the image processing software Image-Pro Plus.

[0043] After the raspberry-shaped oxide microspheres of the present invention are calcined at 400 - 1300 °C, preferably 450 - 1100 °C, and more preferably 500 - 700 °C, an oxide is obtained, and its specific surface area is about 0.1 - 900 m 2 / g, preferably 10 - 300 m 2 / g, and the pore volume is about 0.01 - 3.6 ml / g, preferably 0.1 - 0.9 ml / g.

[0044] The crushing rate of the raspberry-shaped oxide microspheres of the present invention is preferably 0 - 1%, and this crushing rate is measured according to the method provided by the similar strength standard No. Q / SH3360 226 - 2010. The specific method is as follows:

[0045] First, select sieves S1 and S2 with mesh numbers M1 and M2 respectively, where M1 < M2. Pass the microspheres to be measured through the sieve S1 with mesh number M1 first, and then pass the sieved microsphere powder through the sieve S2 with mesh number M2. Finally, use the microsphere powder intercepted by the sieve S2 as the sample to be measured.

[0046] A certain mass of the sample to be tested is added to a cylindrical steel container with a cross-sectional diameter of 10 mm, and then a certain pressure is applied to the microspheres through a cylinder for a certain period of time. The pressed microsphere powder is then sieved with a sieve S2 with a mesh size of M2, and the mass of the microsphere powder under the sieve is recorded. The mass of the microsphere powder under the sieve is then divided by the total mass of the added microspheres to obtain the crushing rate of the microspheres.

[0047] In the present invention, M1 can be 100 mesh, M2 can be 150 mesh, the pressure can be 100N, and the time can be 10s.

[0048] The breakage rate can be used to evaluate the strength of the microspheres; the smaller the breakage rate, the higher the strength of the microspheres.

[0049] The raspberry-shaped oxide microspheres of the present invention have a low breakage rate under pressure and a significantly higher strength than the existing known oxide microspheres, such as the apple-shaped hollow molecular sieve microspheres disclosed in CN108404970A, which is determined by the difference in raw materials and preparation methods. The higher strength makes the raspberry-shaped oxide microspheres have a larger porosity and a significantly reduced pressure drop, while having excellent processing performance and wear resistance.

[0050] The microchannel catalyst provided by the invention has the advantages of multiple active centers, high catalytic activity and good regeneration performance.

[0051] A second aspect of the present invention provides a method for preparing a microchannel catalyst, the method comprising:

[0052] (1) preparing raspberry-shaped oxide microspheres;

[0053] (2) introducing active components into the raspberry-shaped oxide microspheres by an impregnation method to obtain an oxidized catalyst; the active components are selected from at least one of the metal elements of Group VIII;

[0054] (3) reducing the oxidized catalyst under a hydrogen-containing atmosphere;

[0055] (4) after the temperature of the catalyst obtained by reduction in step (3) drops below 60° C., the catalyst obtained by reduction in step (3) is passivated, wherein the passivation comprises: continuously introducing an oxygen-containing gas below 60° C. and controlling the passivation temperature to be no higher than 90° C.; wherein the oxygen concentration of the oxygen-containing gas is continuously increased;

[0056] The amount of the raspberry-shaped oxide microspheres and the active component is such that the content of the active component in the oxidized catalyst is less than 40 wt %, preferably 10-36 wt %, based on the total amount of the oxidized catalyst and calculated as oxide.

[0057] The specific selection and content of the active components are as described above and will not be repeated here.

[0058] The composition and structure of the raspberry-shaped oxide microspheres are as described above and will not be repeated here.

[0059] Any method that can obtain the above-mentioned raspberry-shaped oxide microspheres of composition and structure can be used to prepare raspberry-shaped oxide microspheres in step (1) of the present invention. Preferably, step (1) of preparing raspberry-shaped oxide microspheres comprises:

[0060] (1-1) adding nitrate, peptizing agent, pore former, the oxide and / or its precursor into a dispersant and stirring to obtain a dispersed slurry;

[0061] (1-2) subjecting the dispersed slurry to an aging treatment;

[0062] (1-3) The aged dispersed slurry is sent to a drying device, and dried and molded under the conditions of an inlet air temperature of 400-1200° C., preferably 450-700° C., and an outlet air temperature of 50-300° C., preferably 120-200° C., to obtain the raspberry-shaped oxide microspheres.

[0063] According to the present invention, preferably, the nitrate is selected from one or more of aluminum nitrate, zirconium nitrate, lanthanum nitrate and yttrium nitrate. Nitrate ions in the nitrate can promote the oxidant that can be used as a pore-forming agent under high temperature conditions. They undergo a self-propagating combustion reaction at high temperatures to generate gas and steam, so that the oxide material forms a cavity.

[0064] According to the present invention, preferably, the peptizing agent is selected from one or more of acids, bases and salts. The acids can be selected from: inorganic acids (such as hydrochloric acid, sulfuric acid, nitric acid, etc.), organic acids (formic acid, acetic acid, oxalic acid, etc.) and combinations of one or more of inorganic acids or organic acids; the bases can be selected from: inorganic bases (sodium hydroxide, potassium hydroxide, barium hydroxide, calcium hydroxide, aluminum hydroxide, lithium hydroxide, magnesium hydroxide, zinc hydroxide, copper hydroxide, iron hydroxide, lead hydroxide, cobalt hydroxide, chromium hydroxide, zirconium hydroxide, nickel hydroxide, ammonium hydroxide, soda ash (anhydrous sodium carbonate), sodium carbonate (monohydrate, heptahydrate, decahydrate), sodium bicarbonate (baking soda), potassium carbonate, potassium bicarbonate, etc.), organic bases (such as amine compounds, alkali metal salts of alcohols, alkaloids, alkyl metal lithium compounds, etc.) and combinations of one or more of inorganic bases or organic bases; the salts can be selected from: inorganic acid salts (such as hydrochloric acid, sulfates, nitrates, etc.), organic acid salts (formates, acetates, oxalates, etc.) and combinations of one or more of inorganic acid salts or organic acid salts.

[0065] According to the preparation method of the present invention, preferably, the pore-forming agent is selected from one or more of starch, synthetic cellulose, polymeric alcohol and surfactant. The synthetic cellulose is preferably one or more of carboxymethyl cellulose, methyl cellulose, ethyl cellulose, hydroxycellulose fatty alcohol polyvinyl ether; the polymeric alcohol is preferably one or more of polyethylene glycol, polypropylene glycol, polyvinyl alcohol, polypropylene glycol PPG; the surfactant is preferably one or more of fatty alcohol polyvinyl ether, fatty alcohol amide and its derivatives, acrylic acid copolymer with a molecular weight of 200-2000000 and maleic acid copolymer.

[0066] In the present invention, specifically, the oxide and / or its precursor can directly use aluminum oxide, silicon oxide, zirconium oxide and titanium oxide, or can use precursors to form these oxides, which can be specifically selected from one or more of aluminum sources, silicon sources, zirconium sources and titanium sources, wherein the aluminum source is preferably selected from one or more of pseudo-boehmite, aluminum alcohol, aluminum nitrate, aluminum sulfate, aluminum chloride and sodium aluminate, the silicon source is preferably selected from one or more of silicates, sodium silicate, water glass and silica sol, the zirconium source is preferably selected from one or more of zirconium dioxide, zirconium tetrachloride, zirconium oxychloride, zirconium hydroxide, zirconium sulfate, zirconium phosphate, zirconium oxynitrate, zirconium nitrate, basic zirconium carbonate and tetrabutoxy zirconium, and the titanium source is preferably selected from one or more of titanium dioxide, metatitanic acid, titanium nitrate, titanyl sulfate, titanium dichloride, titanium trichloride, titanium tetrachloride, titanium aluminum chloride, tetraethyl titanate, tetrabutyl titanate, tetra-n-propyl titanate and tetraisopropyl titanate.

[0067] When using the above-mentioned aluminum source, silicon source, zirconium source and titanium source, chemical reagents for precipitating or gelling them are also included, such as acids (such as inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid or organic acids such as acetic acid), and / or alkalis (such as sodium carbonate, sodium hydroxide, etc.).

[0068] When it is necessary to prepare an oxide composition containing other components, oxides such as vanadium oxide, chromium oxide, manganese oxide, molybdenum oxide, tungsten oxide, iron oxide, cobalt oxide, nickel oxide, copper oxide, etc. may also be added, and precursors that can form these oxides may also be added.

[0069] According to the present invention, preferably, the dispersant is selected from one or more of water, alcohols, ketones and acids, wherein the alcohols are preferably methanol, ethanol, propanol, etc., the ketones are preferably acetone, butanone, etc., and the acids are preferably formic acid, acetic acid, propionic acid, etc. The dispersant is preferably a mixture of water and a small amount of ethanol. A small amount of ethanol in water can have a better dispersing effect and can be used as a boiling point regulator. By adjusting the dispersant, the water evaporation effect and the droplet shrinkage effect are more matched and matched, and the appearance of the microspheres is more regular and smooth.

[0070] According to the present invention, preferably, the mass ratio of the nitrate, the peptizing agent, the pore former and the oxide and / or its precursor is (10-500):(1-10):(10-500):(10-1000).

[0071] According to the present invention, nitrate, peptizing agent, pore former and oxide and / or its precursor can be added to the dispersant in sequence or simultaneously. The order of addition can also be adjusted according to the dissolution conditions of each raw material. It is preferred to stir while adding to ensure uniform mixing.

[0072] According to the present invention, preferably, step (1-1) further comprises adding a blasting agent to the dispersant. The blasting agent may be added before or after the oxide. Preferably, the blasting agent is selected from one or more of picric acid, trinitrotoluene, digested glycerol, nitrocellulose, dynamite, hexogen and C4 plastic explosive. Preferably, before drying and forming, the blasting agent is mixed evenly with other materials. Preferably, the amount of the blasting agent added is 0-1% of the total dry weight of the nitrate, peptizing agent, pore-forming agent and oxide and / or its precursor.

[0073] According to a specific embodiment of the present invention, nitrate, peptizing agent, pore-forming agent and oxide precursor are sequentially added to a dispersant for slurrying, and the slurry is stirred evenly and then pumped into a sand mill or a colloid mill for grinding to obtain a dispersed slurry. The solid content of the slurry during slurrying is preferably 5-60% by weight, and the grinding time is preferably 1-30 minutes. After mixing and grinding, the average particle size of the aluminum source, silicon source, zirconium source and titanium source particles in the slurry can be ground to 0.01-10 μm.

[0074] After the raw material mixing and grinding process, it is fully dissolved and dispersed to make the dispersed slurry uniform. The grinding equipment used can be a colloid mill, a sand mill or other equipment. The selection standard is that the catalyst fine powder reaches the required average particle size after grinding, preferably less than 10 μm.

[0075] The present invention has a wide range of conditions for the aging treatment. Preferably, in step (1-2), the temperature of the aging treatment is 0-90° C., preferably 20-60° C. Preferably, the treatment time of the aging treatment is 0.1-24 hours, preferably 0.5-2 hours.

[0076] The drying device used in the present invention can be a flash drying device and a spray drying device, preferably a spray drying device. Flash drying and spray drying are commonly used methods for drying materials. After the wet material is dispersed in a drying tower, the water vaporizes rapidly in contact with hot air to obtain a dry product. The spray drying method can directly dry a solution or emulsion into a powder or granular product, eliminating the processes of evaporation and crushing.

[0077] According to the present invention, preferably, the aged dispersed slurry is sent to a spray drying device for drying and molding at an inlet air temperature of 400-1200° C., preferably 450-700° C., and an outlet air temperature of 50-300° C., preferably 120-200° C. The pressure in the spray tower can be equivalent to that of conventional spraying, and raspberry-shaped oxide microspheres can be obtained.

[0078] The working principle of spray drying is to disperse the material to be dried into very fine mist-like particles through mechanical action (such as pressure, centrifugal, and airflow spray), increase the water evaporation area, accelerate the drying process, contact with hot air, remove most of the water in a shorter time, and dry the solid matter in the material into powder.

[0079] The spray drying device used in the present invention is a conventional device in the existing process, and the present invention has no special restrictions on it. The spray drying device usually includes: a feeding system, a hot air system, a drying tower system, a collecting system and a sealing system. The feeding system is connected to the drying tower system in the middle of the top, the hot air system is connected to the top side of the drying tower system, the collecting system is connected to the bottom of the drying tower system, and the sealing system is connected to the hot air system. In the spray drying process, it is basically necessary to have three functions: spraying of the stock solution; drying of tiny droplets in the spray; separation and recovery of fine powder products. The spray drying device is usually equipped with an atomizer, a drying chamber and a fine powder recoverer corresponding to the above functions.

[0080] Due to the large number of control parameters and complex factors in the spray drying process, the particle size and shape after spray drying are very complex. The general product particle size range is micron-level, and is generally a mixture of spheres, discs, apples, grapes, cavities, meniscuses, etc. How to selectively shape them into an ideal single shape, such as a cavity, is one of the difficulties.

[0081] One method in the prior art is to form a spherical emulsion under the action of the surface tension of a surfactant, and then at a relatively low temperature, the pore-forming agent is vaporized or pyrolyzed inside the spherical emulsion. The gases generated by these vaporizations and pyrolysis will cause the internal cavities of the microsphere emulsion; the slow release of the gas leads to the formation of large pores on the surface that are connected to the internal hollow structure, and the molecular sieve particles form secondary stacking pores during the spray molding process to become mesopores on the surface of the molecular sieve microspheres. Combined with the subsequent calcination process, large-particle hollow molecular sieve microspheres are obtained.

[0082] In the present invention, under the high temperature of 400-1200℃ inlet air temperature, the oxide and the reducing agent in the slurry undergo a strong redox self-propagating combustion reaction, instantly generating a large amount of gas; at the same time, the droplet spray enters the high temperature zone and evaporates strongly, and the surface tension formed by the concentrated slurry causes the droplets to shrink sharply. The strong explosion inside and the strong contraction outside form a raspberry-shaped hollow material with good strength. The obtained raspberry-shaped oxide microspheres have high strength, high sphericity and high yield rate.

[0083] According to the present invention, the raspberry-shaped oxide microspheres can be calcined before step (2) and then used as a carrier. Preferably, the calcination temperature can be 400°C-1300°C, preferably 450-1100°C, and more preferably 500-700°C; the calcination time can be 1-12h, preferably 2-8h, and more preferably 3-4h.

[0084] The present invention does not particularly limit the specific implementation of step (2), as long as the active component is introduced into the raspberry-type oxide microspheres by an impregnation method. Preferably, it includes preparing an impregnation solution of a compound containing an active metal component, and then impregnating the raspberry-type oxide microspheres with the solution. The impregnation method is a conventional method, for example, it can be an excess liquid impregnation or a pore saturation impregnation. Among them, by adjusting and controlling the concentration, dosage of the impregnation solution of the compound containing the active component or the dosage of the raspberry-type oxide microspheres, a catalyst of a specified content can be prepared, which is easily understood and implemented by those skilled in the art.

[0085] When there are more than two types of active components, the active components can be co-impregnated into the raspberry-shaped oxide microspheres, or can be impregnated into the raspberry-shaped oxide microspheres in steps, preferably co-impregnated. The specific operation is well known to those skilled in the art, and the present invention will not be repeated here.

[0086] According to a specific embodiment of the present invention, the raspberry-shaped oxide microspheres are impregnated with an impregnation solution containing an active component precursor, and then dried and calcined. Preferably, the drying temperature can be 80°C-200°C, and more preferably 100-150°C. Preferably, the calcination temperature is 200°C-800°C, and preferably 300-600°C. The present invention does not impose any restrictions on the drying and calcination time, and those skilled in the art can freely choose according to actual needs. The calcination device used and its operating conditions are conventional equipment and operating parameters in existing calcination technology, and the present invention has no special restrictions on them.

[0087] The present invention has no particular limitation on the type of the active component precursor, which can be selected from water-soluble compounds corresponding to the active component, such as nitrates, acetates, chlorides, etc. For example, the nickel precursor can be at least one of nickel nitrate, nickel chloride and nickel acetate.

[0088] The present invention adopts raspberry-shaped oxide microspheres, which can reduce the waste of carriers and catalysts and save materials; at the same time, due to the improvement of the shape efficiency factor, it can also promote diffusion, improve reaction efficiency and target product selectivity. In reactions with relatively large thermal effects, the hollow carrier can also reduce the generation of hot spots and has good intrinsic safety.

[0089] According to the present invention, the hydrogen-containing atmosphere contains hydrogen and may optionally contain a protective gas.

[0090] Preferably, the concentration of hydrogen in the hydrogen-containing atmosphere is not less than 5% by volume, more preferably 5-90% by volume, and further preferably 40-90% by volume.

[0091] The protective gas is a gas that does not participate in the reaction. The protective gas is preferably selected from at least one of nitrogen, helium, argon and neon, and more preferably nitrogen.

[0092] In the present invention, specifically, before the reduction, the method further comprises introducing a protective gas into the reduction device for displacement, then introducing hydrogen to obtain the hydrogen-containing atmosphere, and then performing the reduction. According to the present invention, specifically, the oxidized catalyst is loaded into the pre-reduction reactor, and a protective gas (e.g., N 2 ) replacement system, preferably ensuring that the system has O 2 The volume percentage is ≤0.5%, start the compressor, maintain the system pressure at 0.0-2MPa (gauge pressure), and carry out reduction according to the temperature increase and hydrogen preparation procedure.

[0093] Further preferably, the preparation method further comprises a heat exchange step: the introduced hydrogen and optionally the protective gas are first heat exchanged with the reduced gas, then optionally heated, and then introduced into the reduction system. The reduced tail gas is cooled by heat exchange and preferentially separated by gas-liquid separation, and the tail gas after water removal can be recycled for the reduction process.

[0094] According to the present invention, there is no particular limitation on the equipment for carrying out the reduction. It is preferably a rotary kiln reactor, a fluidized bed reactor or a drum reactor, more preferably a fluidized bed reactor, and most preferably a fluidized reactor with a riser, in which the catalyst is in a fluidized state.

[0095] The present invention has no particular limitation on the amount of reducing gas, and it is preferably selected based on the principle of keeping the powder in a fluidized state.

[0096] Preferably, the reduction conditions in step (3) include: a temperature of 200-600°C, more preferably 250-550°C.

[0097] Preferably, the reduction conditions in step (3) include: a time of no more than 2 hours, more preferably no more than 1 hour. The time refers to the residence time of the oxidized catalyst at the highest reduction temperature in the equipment for performing the reduction.

[0098] Preferably, the reduction conditions in step (3) include: the oxidized catalyst is in a fluidized state and in contact with the reducing gas; the gas-to-agent ratio is 500-5000 and the gas-to-agent ratio is 600-4500. It is understood that the catalyst is in a moving state, enabling it to fully contact with the reducing gas.

[0099] The present invention has a wide range of pressure selection for the reduction, preferably 0-2 MPa. The pressure is a gauge pressure.

[0100] The oxidized catalyst using raspberry-shaped oxide microspheres as carriers can be quickly reduced, and the obtained microchannel catalyst has good regeneration performance and a large number of active centers.

[0101] According to the present invention, in step (4), preferably, after the temperature of the catalyst obtained by reduction in step (3) drops to below 55° C., oxygen-containing gas below 55° C. is continuously introduced to passivate the catalyst obtained by reduction in step (3).

[0102] In the present invention, there is no limitation on the method of cooling the catalyst obtained by reduction in step (3), as long as the catalyst can be cooled to the desired temperature, for example, by heat exchange, cold exchange, water cooling, ammonia cooling, purging, etc.

[0103] According to a preferred embodiment of the present invention, the method provided by the present invention further comprises a process of replacing the hydrogen in the system before the passivation. According to a specific embodiment of the present invention, carbon dioxide or carbon dioxide and nitrogen are used to replace the H in the system. 2 The purge process can not only achieve rapid cooling but also achieve the replacement of hydrogen in the system.

[0104] Preferably, when the temperature of the catalyst obtained by reduction in step (3) drops to below 50° C. (more preferably below 40° C.) and the hydrogen content in the system is ≤ 1% by volume, the catalyst obtained by reduction in step (3) is passivated.

[0105] In the preparation method of the present invention, it can be understood that the passivation temperature is not higher than 90° C. means that the passivation temperature of the catalyst bed is not higher than 90° C. Preferably, the passivation temperature is controlled to be not higher than 85° C., and more preferably not higher than 80° C.

[0106] According to the method provided by the present invention, as long as the concentration of the oxygen-containing gas introduced during the passivation process shows an increasing trend, it is within the scope of "the oxygen concentration of the oxygen-containing gas continues to increase" described in the present invention. The oxygen concentration of the oxygen-containing gas continues to increase may be a uniform increase or an irregular increase, and the present invention has no particular limitation on this.

[0107] According to a specific embodiment of the present invention, for ease of operation, a certain concentration of oxygen-containing gas may be introduced for a certain period of time, and then a higher concentration of oxygen-containing gas may be introduced for a certain period of time, and so on. In this case, that is, the oxygen concentration increases in stages, for example, in multiple stages, in one specific embodiment, the oxygen concentration in the latter stage is higher than the oxygen concentration in the previous stage, and in another specific embodiment, the oxygen concentrations in the first few stages are the same and lower than the oxygen concentration in the subsequent stages, thereby showing an overall upward trend.

[0108] In the present invention, preferably, the oxygen concentration of the oxygen-containing gas is continuously increased in stages. In this case, the present invention has a wide range of optional durations for the various stages, as long as it is beneficial to improving the performance of the obtained catalyst. More preferably, during the passivation process, when the oxygen-containing gas introduced in the previous stage makes the oxygen concentration in the passivation outlet gas equal to the oxygen concentration of the introduced oxygen-containing gas, the operation of introducing the oxygen-containing gas in the next stage is entered.

[0109] According to the present invention, preferably, during the passivation process, the oxygen concentration of the oxygen-containing gas is continuously increased in at least 2 stages, more preferably in 3-10 stages, and more preferably in 4-8 stages, for example, the number of stages may be 4, 5, 6, 7, 8. By adopting this preferred solution, the catalyst can be passivated more uniformly, so that the catalyst has more active centers after re-reduction activation.

[0110] It is understood that, under the preferred embodiment, the oxygen concentration of the oxygen-containing gas in the first stage is lower than the oxygen concentration of the oxygen-containing gas in the second stage, and the oxygen concentration of the oxygen-containing gas in the second stage is lower than the oxygen concentration of the oxygen-containing gas in the third stage, and so on. Further, it is understood that the relative multiples of the oxygen concentration of the oxygen-containing gas in each adjacent two stages can be independently the same or different, for example, the relative multiple of the oxygen concentration of the oxygen-containing gas in the first stage and the second stage is 1.5, and the relative multiple of the oxygen concentration of the oxygen-containing gas in the second stage and the third stage can be 1.5 or 2.

[0111] Preferably, during the passivation process, the catalyst is in a fluidized state, and the gas-to-agent ratio of the passivation is 200-4500, more preferably 200-4000.

[0112] According to a preferred embodiment of the present invention, during the passivation process, the gas-to-agent ratio in the first stage is not lower than that in the second stage. There is no particular limitation on the specific multiple relationship between the gas-to-agent ratio in the first stage and the gas-to-agent ratio in the second stage. As long as the gas-to-agent ratio in the first stage is not lower than that in the second stage, it is more conducive to promoting the uniform passivation process of the catalyst and improving the passivation efficiency.

[0113] According to a preferred embodiment of the present invention, the passivation time is no more than 5 hours, preferably no more than 2 hours. The passivation method provided by the present invention can be completed in a short time, has a good passivation effect, and reduces catalyst wear.

[0114] In the present invention, the oxygen-containing gas is preferably a mixture of a protective gas and oxygen, and the protective gas is selected from one or more of helium, argon, carbon dioxide and nitrogen.

[0115] Preferably, the concentration of the oxygen-containing gas is 0.05-21% by volume, preferably 0.1-21% by volume.

[0116] According to a preferred embodiment of the present invention, during the passivation process, the initial oxygen concentration of the oxygen-containing gas introduced is 0.1-1% by volume, preferably 0.1-0.5% by volume. The use of oxygen-containing gas with a lower initial oxygen concentration can make the passivation uniform and controllable, and is more conducive to obtaining a catalyst with good reproducibility.

[0117] According to a preferred embodiment of the present invention, during the passivation process, the oxygen concentration of the oxygen-containing gas introduced in the latter stage is 1.5-6 times the oxygen concentration of the oxygen-containing gas introduced in the previous stage. Under this preferred embodiment, the catalyst can be passivated more uniformly and controllably, so that the obtained catalyst has more active centers after the re-reduction treatment, and the passivation efficiency is high.

[0118] In the present invention, the method further comprises: before the passivation, a protective gas (preferably a mixture of carbon dioxide and N in a volume ratio of 10-20) is introduced. 2 ), and then oxygen is introduced to make the oxygen content in the passivation atmosphere meet the required oxygen concentration, and then the passivation is carried out. The passivated gas is recycled or directly discharged.

[0119] According to the present invention, when the reduction and passivation are carried out using the same equipment, it is preferred that a protective gas is introduced after the reduction to replace the hydrogen in the system before the passivation is carried out.

[0120] Preferably, the passivation temperature is ensured to be no higher than 90° C. by adjusting the amount of protective gas (preferably carbon dioxide) pumped in.

[0121] In the present invention, the reducing gas (i.e. the hydrogen-containing atmosphere) and the passivating gas (i.e. the oxygen-containing gas) can be used once or recycled; preferably, the hydrogen-containing gas is recycled and the passivating gas is not recycled.

[0122] The present invention has no particular limitation on the device for passivation, which can share the same set of devices with the reduction or can be set separately. Its type can refer to the device used in the reduction process, such as a fluidized bed reactor, in which the catalyst is in a fluidized state.

[0123] The third aspect of the present invention provides a microchannel catalyst prepared by the preparation method described in the second aspect. The microchannel catalyst has the composition and structure of the microchannel catalyst described in the first aspect, which will not be described in detail here.

[0124] The fourth aspect of the present invention provides the use of the microchannel catalyst described in the first aspect or the third aspect in a methanol purification reaction.

[0125] The present invention reduces smaller particles quickly, which, on the one hand, fully reduces the oxides in the catalyst, improves the reduction degree of the catalyst, and can keep the crystals smaller. Thus, the oxidized catalyst is efficiently reduced to a catalyst with high activity. On the other hand, the method of the present invention has the advantages of high efficiency, and can obtain a very uniform and easily regenerated catalyst with many active centers. Thus, the overall reaction activity of the catalyst is improved. It has a good industrial application prospect.

[0126] The present invention will be described in detail below by way of examples. In the following examples, the test method is as follows:

[0127] The temperature corresponding to the peak of the low-temperature reduction peak with the largest area in the TPR spectrum curve is used as a measure to evaluate the regeneration of the passivated catalyst: the lower the temperature corresponding to the peak of the low-temperature reduction peak with the largest area, the easier the catalyst is to regenerate. The programmed temperature reduction (TPR) was carried out on an Autochem2950 fully automatic high-pressure chemical adsorption instrument produced by Micromeritics, USA. The test conditions were: 0.20g of the sample was first heated to 120℃ for dehydration treatment for 1 hour at a heating rate of 10℃ / min under a 50mL / min Ar gas flow, and after the temperature dropped to 50℃, a TPR experiment was carried out. The experimental conditions and procedures of TPR were: the reducing gas was H with a hydrogen content of 10 volume % 2 -Ar mixed gas, the reducing gas flow rate is 50mL / min, and the temperature is increased to 900°C at a heating rate of 10°C / min; during the above heating process, the signal is detected by a thermal conductivity detector (TCD) to obtain a TPR spectrum curve.

[0128] The number of active centers was measured on an Autochem 2950 fully automatic high-pressure chemical adsorption instrument produced by Micromeritics, USA. 2 Programmed temperature desorption (TPD) 2 -TPD) test, the test method is: weigh 0.2000g of 40-60 mesh sample, first perform re-reduction activation, the re-reduction conditions are: hydrogen content of 10 volume % H 2 -Ar mixed gas, the mixed gas flow rate was 50mL / min, and the temperature was raised to 200℃ at a heating rate of 10℃ / min for 2h. The reduced catalyst was heated to 10% by volume in H 2 -Ar mixed gas, and when the temperature dropped to 55°C, switch to Ar gas for purging at an Ar flow rate of 20 mL / min until the baseline was stable, and then perform H 2 -TPD experiment. 2 -TPD experimental conditions and procedures are as follows: carrier gas is Ar, carrier gas flow rate is 20 mL / min, heating rate is 10 °C / min, final temperature is 400 °C, thermal conductivity detector (TCD) detects the signal, and obtains the TPD curve.

[0129] In the following examples, preparation examples and comparative examples, the specifications of some raw materials used are as follows:

[0130] Pseudo-boehmite powder (produced by Changling Catalyst Factory, solid content 69.5% by weight, γ-Al 2 O 3 Content is not less than 98% by weight);

[0131] Alumina sol (produced by Zhoucun Catalyst Factory, containing 22 wt% Al 2 O 3 );

[0132] Sodium silicate (Jinan Huifengda Chemical Co., Ltd., modulus 3.1-3.4, insoluble matter less than 0.4%);

[0133] Ammonia water, hydrochloric acid, nitric acid, sulfuric acid, aluminum sulfate, aluminum chloride, zirconium hydroxide, zirconium oxychloride, titanium tetrachloride, titanium dioxide (Sinopharm Chemical Reagent Co., Ltd., industrial grade);

[0134] Polyethylene glycol PEG4000 powder (Wenzhou Shuangxiao Rubber and Plastic Material Co., Ltd.);

[0135] Methyl cellulose (Hubei Jiangmin Taihua Chemical Co., Ltd.);

[0136] Tetraethyl orthosilicate (TEOS, Jinan Huate Chemical Co., Ltd., content about 99%);

[0137] Aluminum nitrate, titanium nitrate, zirconium nitrate, yttrium nitrate, magnesium nitrate (Yutai Qixin Chemical Co., Ltd., industrial grade)

[0138] The breakage rate of the carrier and catalyst can be measured as follows:

[0139] The microspheres to be tested are first passed through a 100-mesh sieve, and then the sieved microsphere powder is passed through a 150-mesh sieve, and finally the microsphere powder intercepted by the 150-mesh sieve is used as the sample to be tested. A certain mass of microspheres (particle size of 100-150 mesh) is added to a cylindrical steel container with a cross-sectional diameter of 10mm, and then a certain pressure (100N) is applied to the microspheres through a cylinder for a certain period of time (10 seconds), and then the pressed microsphere powder is sieved with a 150-mesh sieve, and the mass of the microsphere powder under the sieve is recorded, and then the mass of the microsphere powder under the sieve is divided by the total mass of the added microspheres to obtain the crushing rate of the microspheres.

[0140] The following preparation example is used to illustrate the preparation of raspberry-shaped oxide microspheres.

[0141] Preparation Example 1

[0142] Add 20 kg of water to the reactor, add 0.5 kg of zirconium nitrate, then add 175 g of concentrated nitric acid, add 2 kg of PEG4000 and 5 g of digested glycerol, and finally add 4.6 kg of pseudo-boehmite powder, stir evenly and grind to obtain a dispersed slurry.

[0143] The dispersion slurry was aged at 25°C with stirring for 0.5 hours.

[0144] The aged dispersed slurry is sent to a spray drying device for drying and forming to obtain raspberry-shaped oxide microspheres, wherein the atomization pressure of the spray drying is 0.3 to 3.0 MPa, the pressure in the tower is -0.0010 to -0.0090 MPa; the initial air inlet temperature of the drying is 560°C, and the air outlet temperature at the end of the drying is 140°C.

[0145] SEM images of raspberry-shaped oxide microspheres are shown in Figure 1 shown.

[0146] Preparation Example 2

[0147] Add 40 kg of water into the reactor, add 0.5 kg of cerium nitrate, then add 200 g of concentrated sulfuric acid, then add 1 kg of PEG4000 and 5 g of picric acid, and finally add 3 kg of sodium silicate, stir evenly and grind to obtain a dispersed slurry.

[0148] The dispersion slurry was aged at 25°C with stirring for 1 hour.

[0149] The aged dispersed slurry is sent to a spray drying device for drying and forming to obtain raspberry-shaped oxide microspheres, wherein the atomization pressure of the spray drying is 0.3 to 3.0 MPa, the pressure in the tower is -0.0010 to -0.0090 MPa; the initial air inlet temperature of the drying is 600°C, and the air outlet temperature at the end of the drying is 180°C.

[0150] The SEM images of the obtained raspberry-shaped oxide microspheres are Figure 1 resemblance.

[0151] Preparation Example 3

[0152] Add 30 kg of water to the reactor, add 0.7 kg of zirconium nitrate, then add 2 L of concentrated ammonia water, add 1.5 kg of PEG4000 and 8 g of picric acid, and finally add 7 kg of zirconium hydroxide, stir evenly and grind to obtain a dispersed slurry.

[0153] The dispersion slurry was aged at 25°C with stirring for 2 hours.

[0154] The aged dispersed slurry is sent to a spray drying device for drying and forming to obtain raspberry-shaped oxide microspheres, wherein the atomization pressure of the spray drying is 0.3 to 3.0 MPa, the pressure in the tower is -0.0010 to -0.0090 MPa; the initial air inlet temperature of the drying is 560°C, and the air outlet temperature at the end of the drying is 140°C.

[0155] SEM and Figure 1 resemblance.

[0156] Preparation Example 4

[0157] Add 30 kg of water to the reactor, add 0.7 kg of titanium nitrate, then add 2.6 L of concentrated ammonia water, add 1.5 kg of PEG4000 and 6 g of picric acid, and finally add 500 g of concentrated nitric acid and 7 kg of titanium nitrate, stir evenly and grind to obtain a dispersed slurry.

[0158] The dispersion slurry was aged at 25°C with stirring for 2 hours.

[0159] The aged dispersed slurry is sent to a spray drying device for drying and forming to obtain raspberry-shaped oxide microspheres, wherein the atomization pressure of the spray drying is 0.3 to 3.0 MPa, the pressure in the tower is -0.0010 to -0.0090 MPa; the initial air inlet temperature of the drying is 560°C, and the air outlet temperature at the end of the drying is 141°C.

[0160] SEM and Figure 1 resemblance.

[0161] The following examples are used to illustrate the microchannel catalyst provided by the present invention.

[0162] Example 1

[0163] The raspberry-shaped oxide microspheres obtained in Preparation Example 1 were calcined at 600° C. for 3 hours to obtain carrier ZT1, whose physical properties are shown in Table 1.

[0164] The carrier ZT1 is impregnated with nickel nitrate solution for many times to prepare a catalyst with a Ni content of 35% by weight, dried at 120°C for 2 hours, and calcined at 420°C for 2 hours to obtain the catalyst CAT1, and the calcined powder is transported to a fluidized bed reduction system. First, a nitrogen replacement system is introduced into the reactor until the oxygen content is qualified (oxygen content ≤ 0.5 volume %), and then the hydrogen content in the hydrogen-nitrogen mixed gas is 40 volume % by hydrogen supplementation, and then a one-step reduction process is started: the above-mentioned mixed gas with a gas-agent ratio of 1500 is introduced to make the catalyst in a fluidized state, and the temperature of the catalyst is raised to 420°C at a heating rate of 80°C / hour, and the temperature is kept constant for 1 hour; the reduction step is ended.

[0165] Then, the hydrogen in the nitrogen replacement system is introduced, and the catalyst after the reduction is cooled to below 55°C, and an oxygen-containing gas with an oxygen concentration of 0.2-21% by volume composed of air and nitrogen is introduced at normal pressure below 55°C. The oxygen-containing gas with oxygen concentrations of 0.2%, 0.6%, 1.0%, 3.0%, 8.0% and 21% by volume is introduced in 6 sections, wherein after the oxygen-containing gas of the previous stage is introduced, when the oxygen concentration at the gas outlet is equal to the oxygen concentration at the gas inlet, the oxygen-containing gas of the next stage is introduced, and the oxygen concentration is gradually increased for passivation until the passivation is completed. The passivation gas-agent ratio is 2000. During this period, the passivation temperature of the catalyst bed is controlled to be less than 70°C, and the total passivation time is 1 hour. A passivated hydrogenation catalyst (i.e., a pre-reduction type hydrogenation catalyst) is obtained.

[0166] Comparative Example 1

[0167] The method of Example 1 is different in that the passivation is not segmented, specifically including: the oxygen concentration of the oxygen-containing gas used is 21% by volume, the gas-to-agent ratio is 500, the passivation time is 0.5 hours, and the passivation temperature of the catalyst bed is controlled to be less than 150°C.

[0168] Comparative Example 2

[0169] The method of Example 1 is different in that the passivation process is different. Specifically, the passivation is divided into two stages, the gas-to-agent ratio is 500, the oxygen concentration of the oxygen-containing gas used in the first stage passivation is 1.5 volume %; the oxygen concentration of the oxygen-containing gas used in the second stage passivation is 21 volume %, wherein after the oxygen-containing gas of the first stage is introduced, when the oxygen concentration at the gas outlet is equal to the oxygen concentration at the gas inlet, the oxygen-containing gas of the second stage is introduced, and the total passivation time is 1 hour. During this period, the passivation temperature of the catalyst bed is controlled to be less than 150°C.

[0170] Example 2

[0171] The raspberry-shaped oxide microspheres obtained in Preparation Example 2 were calcined at 500° C. for 3 hours to obtain carrier ZT2, whose physical properties are shown in Table 1.

[0172] The carrier ZT2 was impregnated with solutions containing nickel nitrate and copper nitrate multiple times to prepare a catalyst with a Ni content of 35 wt% and a Cu content of 2 wt%. The catalyst was dried at 110°C for 4 hours and calcined at 350°C for 2 hours to obtain the catalyst CAT2.

[0173] The catalyst CAT2 was reduced and passivated according to the method of Example 1 to obtain a microchannel catalyst.

[0174] Example 3

[0175] The raspberry-shaped oxide microspheres obtained in Preparation Example 3 were calcined at 550° C. for 3 hours to obtain carrier ZT3, whose physical properties are shown in Table 1.

[0176] The carrier ZT3 was immersed in nickel nitrate solution for many times to prepare a catalyst with a Ni content of 35 wt%. The catalyst was dried at 120°C for 2 hours and calcined at 420°C for 2 hours to obtain the catalyst CAT3.

[0177] The catalyst CAT3 was reduced and passivated according to the method of Example 1 to obtain a microchannel catalyst.

[0178] Example 4

[0179] The raspberry-shaped oxide microspheres obtained in Preparation Example 4 were calcined at 700° C. for 3 hours to obtain carrier ZT4, whose physical properties are shown in Table 1.

[0180] The carrier ZT4 was impregnated with nickel nitrate and copper nitrate solutions multiple times to prepare a catalyst with a Ni content of 35.0 wt% and a Cu content of 1.0 wt%. The catalyst was dried at 130°C for 2 hours and calcined at 370°C for 3 hours to obtain catalyst CAT4.

[0181] The catalyst CAT4 was reduced and passivated according to the method of Example 1 to obtain a microchannel catalyst.

[0182] Table 1 Physical properties of carriers

[0183]

[0184]

[0185] As can be seen from Table 1, when the raspberry-shaped oxide microspheres prepared in the present invention are used as carriers, they are similar in specific surface area, pore volume, and average pore diameter, but have greatly improved sphericity and strength, and are significantly better than existing solid oxide microspheres, providing the possibility of using these carriers.

[0186] Example 5

[0187] The method of Example 1 is different in that the reduction process specifically includes: first, a nitrogen replacement system is introduced into the reactor until the oxygen content is qualified (oxygen content ≤ 0.5 volume %), and a hydrogen-containing gas (a mixture of 70 volume % hydrogen and argon) is kept at a constant temperature of 440°C for 1 hour, and the gas-to-agent ratio is 2000.

[0188] Example 6

[0189] According to the method of Example 1, the difference is that the passivation process specifically includes: cooling the above-mentioned reduced catalyst to below 45°C, and introducing an oxygen-containing gas with an oxygen concentration of 0.1-21% by volume composed of air and nitrogen at below 45°C under normal pressure. Introduce oxygen-containing gases with oxygen concentrations of 0.1% by volume, 0.2% by volume, 0.4% by volume, 0.8% by volume, 1.2% by volume, 3.0% by volume, 8.0% by volume, and 21% by volume in 8 stages, wherein after the oxygen-containing gas of the previous stage is introduced, when the oxygen concentration at the gas outlet is equal to the oxygen concentration at the gas inlet, the oxygen-containing gas of the next stage is introduced, and the oxygen concentration is gradually increased for passivation until the passivation is completed. The gas-agent ratio of the first two stages of passivation is 2200, and the gas-agent ratio of the last six stages of passivation is 2000. During this period, the passivation temperature of the catalyst bed is controlled to be less than 65°C, and the total passivation time is 1 hour. Obtain a microchannel catalyst.

[0190] Example 7

[0191] According to the method of Example 1, the difference is that the passivation process specifically includes: cooling the reduced catalyst to below 40°C, introducing an oxygen-containing gas composed of air and nitrogen at below 40°C with an oxygen concentration of 0.15-21% by volume under normal pressure, and sequentially introducing oxygen-containing gases with oxygen concentrations of 0.15%, 0.3%, 1.0%, 6%, 12% and 21.0% by volume in 6 stages; the gas-to-agent ratio in the first 2 stages of passivation is 2000, and the gas-to-agent ratio in the last 4 stages of passivation is 1000, and the total passivation time is 2 hours. During this period, the passivation temperature of the catalyst bed is controlled to be less than 60°C. A microchannel catalyst is obtained.

[0192] Example 8

[0193] The method of Example 1 is different, except that the passivation process is different. Specifically, during the passivation process, oxygen-containing gas composed of air and nitrogen with oxygen concentrations of 0.5 volume %, 2 volume %, and 21 volume % is introduced in three stages, and the passivation gas-agent ratio is 1000. After the oxygen-containing gas of the previous stage is introduced, when the oxygen concentration at the gas outlet is equal to the oxygen concentration at the gas inlet, the oxygen-containing gas of the next stage is introduced, and the oxygen concentration is gradually increased for passivation until the passivation is completed. The total passivation time is 2 hours, during which the passivation temperature of the catalyst bed is controlled to be less than 90° C. A microchannel catalyst is obtained.

[0194] The catalysts prepared in the above examples and comparative examples were characterized and analyzed, and the number of active centers of the catalysts after re-reduction treatment and the temperature corresponding to the peak value of the low-temperature reduction peak with the largest area in the TPR spectrum curve are listed in Table 2.

[0195] Table 2

[0196]

[0197]

[0198] It can be seen from Table 2 that the microchannel catalyst obtained by the method of the present invention has a higher number of active centers, and the temperature corresponding to the peak value of the low-temperature reduction peak with the largest area is lower, and the catalyst is easier to regenerate.

[0199] Test Example 1

[0200] The reaction performance of the catalyst prepared above was tested in a small microchannel reactor (the minimum dimension of the channel cross section is 1000 μm). The small microchannel reactor module has 16 reaction channels and 36 cooling channels. The reaction channel is 200 mm long and the maximum catalyst loading is 6 mL.

[0201] 4.0 ml of the above catalyst was loaded into the constant temperature zone of a small microchannel reactor, and the pre-reduced catalysts obtained in the above examples and comparative examples were tested respectively. Acetaldehyde was added to a methanol aqueous solution having a methanol content of 85 wt %, and the acetaldehyde concentration was 1400 ppm to obtain a mixture as a raw material.

[0202] The test method is:

[0203] First, the pre-reduced catalyst is re-reduced in a re-reduction atmosphere of 70% by volume of hydrogen and nitrogen; the re-reduction reaction conditions are: normal pressure, gas-to-agent ratio of 1500, heating rate of 5°C / min, re-reduction temperature of 200°C, and re-reduction time of 2 hours.

[0204] Then the temperature is 80℃, the pressure is 2.0MPa, and the volume space velocity of the raw material liquid is 8h-1 、V(H 2 The catalyst performance was evaluated under the condition that V(V) / V(raw material) was 500. The product sample was taken after 24 hours of reaction for analysis. The catalyst was compared with the catalyst reduced in the reactor under the same reduction conditions as in Example 2.

[0205] The reaction performance test results are shown in Table 3.

[0206] Table 3 Catalyst reaction performance test results

[0207] Example No. Acetaldehyde conversion rate, % Example 1 90 Comparative Example 1 0 Comparative Example 2 10 Example 2 90 In-device restoration 90 Example 3 85 Example 4 86 Example 5 93 Example 6 91 Example 7 90 Example 8 60

[0208] The test results in Table 3 show that the acetaldehyde conversion rate of the catalyst provided by the present invention is significantly higher than that of the catalyst of the comparative example when other conditions are the same when the catalyst provided by the present invention is used for methanol purification, indicating that the catalyst has better acetaldehyde removal performance and is equivalent to the in-vessel reduction effect. Among them, by comparing Example 1 with Example 8, it can be seen that the catalyst prepared by the preferred reduction passivation of the present invention has better acetaldehyde removal performance.

[0209] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A microchannel catalyst, comprising a carrier and an active component supported on the carrier, wherein the active component is selected from at least one of the metal elements of Group VIII, and the content of the active component is less than 40 wt % based on the total amount of the catalyst and calculated as oxide; the carrier is a raspberry-shaped oxide microsphere, which is a hollow microsphere having a large hole on the surface, and the hollow microsphere has a hollow structure inside, wherein the large hole and the hollow structure are connected to form a cavity with an open end; in, The oxide in the raspberry-shaped oxide microspheres is selected from one or more of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, calcium oxide and titanium oxide; The number of active centers of the catalyst after the reduction treatment is 0.02-0.3 mmol hydrogen / g catalyst, and the reduction treatment conditions include: temperature of 200° C., time of 2 hours, reduction atmosphere of 10% by volume hydrogen-containing and argon-containing atmosphere, and gas-to-agent volume ratio of 15000; Wherein, the preparation method of the raspberry-shaped oxide microspheres comprises: (1-1) adding nitrate, peptizing agent, pore former, the oxide and / or its precursor into a dispersant and stirring to obtain a dispersed slurry; (1-2) subjecting the dispersed slurry to an aging treatment; (1-3) The aged dispersed slurry is sent to a drying device, and dried and molded under the conditions of an inlet air temperature of 400-1200° C. and an outlet air temperature of 50-300° C. to obtain the raspberry-shaped oxide microspheres.

2. The catalyst according to claim 1, in, The content of the active component is 10-36% by weight, calculated as oxide, based on the total amount of the catalyst; And / or, the active component is selected from one or more of Co, Ni, Ru, Pd and Pt; And / or, the oxide in the raspberry-shaped oxide microspheres is aluminum oxide and / or silicon oxide; And / or, in step (1-3), the inlet air temperature is 450-700°C, and the outlet air temperature is 120-200°C. The catalyst according to claim 1 or 2, wherein the active component is Ni.

4. The catalyst according to claim 1 or 2, in, After the catalyst is subjected to re-reduction treatment, the number of active centers of the catalyst is 0.05-0.25 mmol hydrogen / g catalyst; And / or, the catalyst is characterized by TPR, and in its TPR curve, the temperature corresponding to the peak value of the low-temperature reduction peak with the largest area is 120-240°C.

5. The catalyst according to claim 4, in, In its TPR curve, the temperature corresponding to the peak of the low-temperature reduction peak with the largest area is 130-220°C.

6. The catalyst according to any one of claims 1 to 2 and 5, in, The particle size of the raspberry-shaped oxide microspheres is 3-2500 μm; And / or, the diameter of the hollow structure is 1-2000 μm; And / or, the pore size of the macropore is 0.2-1000 μm; And / or, the shell thickness of the hollow microsphere is 0.2-1000 μm.

7. The catalyst according to claim 6, in, The particle size of the raspberry-shaped oxide microspheres is 10-500 μm; And / or, the diameter of the hollow structure is 1-400 μm; And / or, the pore size of the macropore is 0.5-200 μm; And / or, the shell thickness of the hollow microsphere is 0.5-200 μm.

8. The catalyst according to any one of claims 1 to 2, 5 and 7, in, The sphericity of the raspberry-shaped oxide microspheres is 0.5-0.99; And / or, the breakage rate of the raspberry-shaped oxide microspheres is 0-1%.

9. A method for preparing a microchannel catalyst, the method include: (1) preparing raspberry-shaped oxide microspheres; (2) introducing active components into the raspberry-shaped oxide microspheres by an impregnation method to obtain an oxidized catalyst; The active component is selected from at least one of the metal elements of Group VIII; (3) reducing the oxidized catalyst under a hydrogen-containing atmosphere; (4) after the temperature of the catalyst obtained by reduction in step (3) drops below 60° C., the catalyst obtained by reduction in step (3) is passivated, wherein the passivation comprises: continuously introducing an oxygen-containing gas below 60° C. and controlling the passivation temperature to be no higher than 90° C.; wherein the oxygen concentration of the oxygen-containing gas is continuously increased; The amount of the raspberry-shaped oxide microspheres and the active component is such that the content of the active component in the oxidized catalyst is less than 40% by weight, calculated as oxide, based on the total amount of the oxidized catalyst; Step (1) The preparation of raspberry-shaped oxide microspheres comprises: (1-1) adding nitrate, peptizing agent, pore former, the oxide and / or its precursor into a dispersant and stirring to obtain a dispersed slurry; (1-2) subjecting the dispersed slurry to an aging treatment; (1-3) The aged dispersed slurry is sent to a drying device, and dried and molded under the conditions of an inlet air temperature of 400-1200° C. and an outlet air temperature of 50-300° C. to obtain the raspberry-shaped oxide microspheres.

10. The preparation method according to claim 9, in, The amount of the raspberry-shaped oxide microspheres and the active component is such that the content of the active component in the oxidized catalyst is 10-36% by weight, calculated as oxide, based on the total amount of the oxidized catalyst.

11. The preparation method according to claim 10, in, In step (1-3), the inlet air temperature is 450-700°C, and the outlet air temperature is 120-200°C.

12. The preparation method according to any one of claims 9 to 11, in, The active component is selected from one or more of Co, Ni, Ru, Pd and Pt; And / or, the oxide in the raspberry-shaped oxide microspheres is selected from one or more of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, calcium oxide and titanium oxide; And / or, the particle size of the raspberry-shaped oxide microspheres is 3-2500 μm.

13. The preparation method according to claim 12, in, The active component is Ni; And / or, the oxide in the raspberry-shaped oxide microspheres is aluminum oxide and / or silicon oxide; And / or, the particle size of the raspberry-shaped oxide microspheres is 10-500 μm.

14. The preparation method according to claim 9, in, The nitrate is selected from one or more of aluminum nitrate, zirconium nitrate, lanthanum nitrate and yttrium nitrate; and / or, The peptizing agent is selected from one or more of acids, bases and salts; and / or, The pore-forming agent is selected from one or more of starch, synthetic cellulose, polymer alcohol and surfactant; and / or, The oxide and / or its precursor is selected from one or more of an aluminum source, a silicon source, a zirconium source and a titanium source, wherein the aluminum source is selected from one or more of pseudo-boehmite, aluminum alcohol, aluminum nitrate, aluminum sulfate, aluminum chloride and sodium aluminate, the silicon source is selected from one or more of silicates, sodium silicate, water glass and silica sol, the zirconium source is selected from one or more of zirconium dioxide, zirconium tetrachloride, zirconium oxychloride, zirconium hydroxide, zirconium sulfate, zirconium phosphate, zirconium oxynitrate, zirconium nitrate, basic zirconium carbonate and tetrabutoxy zirconium, the titanium source is selected from one or more of titanium dioxide, metatitanic acid, titanium nitrate, titanium oxysulfate, titanium dichloride, titanium trichloride, titanium tetrachloride, titanium aluminum chloride, tetraethyl titanate, tetrabutyl titanate, tetra-n-propyl titanate and tetraisopropyl titanate; and / or, The dispersant is selected from one or more of water, alcohols, ketones and acids; And / or, the mass ratio of the nitrate, the peptizing agent, the pore former and the oxide and / or its precursor is (10-500):(1-10):(10-500):(10-1000).

15. The preparation method according to claim 9, in, Step (1-1) further comprises adding a blasting agent to the dispersant, wherein the blasting agent is selected from one or more of picric acid, trinitrotoluene, digested glycerol, nitrocellulose, dynamite, hexogen and C4 plastic explosive.

16. The preparation method according to claim 15, in, The added amount of the blasting agent is 0-1% of the total dry weight of the nitrate, the peptizing agent, the pore-forming agent and the oxide and / or its precursor.

17. The preparation method according to claim 9, in, In step (1-2), the aging treatment temperature is 0-90°C; and / or, In step (1-3), the drying device is a flash drying device or a spray drying device.

18. The preparation method according to claim 17, in, In step (1-2), the temperature of the aging treatment is 20-60°C.

19. The preparation method according to claim 9, in, The reduction conditions in step (3) include: the oxidized catalyst is in a fluidized state and in contact with the reducing gas; the gas-to-agent ratio is 500-5000; the temperature is 200-600° C., and the time is not more than 2 hours; and / or, the hydrogen-containing atmosphere contains hydrogen and optionally a protective gas, and the hydrogen concentration in the hydrogen-containing atmosphere is not less than 5 volume %; And / or, the reduction is carried out in a fluidized bed reactor.

20. The preparation method according to claim 19, in, The reduction conditions in step (3) include: a gas-agent ratio of 600-4500; a temperature of 250-550° C., and a time of no more than 1 hour; And / or, the hydrogen-containing atmosphere contains hydrogen and optionally a protective gas, and the concentration of hydrogen in the hydrogen-containing atmosphere is 5-90 volume %.

21. The preparation method according to claim 9, in, The passivation time is not more than 5h; and / or, during the passivation process, the oxygen concentration of the oxygen-containing gas is continuously increased in at least two stages; And / or, during the passivation process, the catalyst is in a fluidized state, and the gas-to-agent ratio of the passivation is 200-4500; And / or, the reduction is carried out in a fluidized bed reactor.

22. The preparation method according to claim 21, in, The passivation time is not more than 2h; and / or, during the passivation process, the oxygen concentration of the oxygen-containing gas is continuously increased in 3-10 stages; And / or, during the passivation process, the catalyst is in a fluidized state, and the gas-to-agent ratio of the passivation is 200-4000.

23. The preparation method according to claim 9, in, The concentration of the oxygen-containing gas is 0.05-21% by volume; And / or, during the passivation process, the initial oxygen concentration of the oxygen-containing gas introduced is 0.1-1% by volume; And / or, during the passivation process, the oxygen concentration of the oxygen-containing gas introduced in the latter stage is 1.5-6 times the oxygen concentration of the oxygen-containing gas introduced in the former stage.

24. The preparation method according to claim 23, in, The concentration of the oxygen-containing gas is 0.1-21 volume %; And / or, during the passivation process, the initial oxygen concentration of the oxygen-containing gas introduced is 0.1-0.5 volume %.

25. A microchannel catalyst obtained by the preparation method according to any one of claims 9 to 24.

26. Use of the microchannel catalyst according to any one of claims 1 to 8 and 25 in methanol purification reaction.