A copper-aluminum composite material for lightweight zipper and preparation method thereof

Through the bimetallic molding process of copper-aluminum composite materials, combined with the advantages of aluminum alloy and copper alloy, the problems of high cost and poor performance of zipper materials are solved, and efficient and low-cost lightweight zipper materials are achieved, suitable for decorations and widely used.

CN115255019BActive Publication Date: 2024-11-01JIANGSU HENGTONG ELECTRICAL SPECIAL WIRE CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202210720049.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-23
Publication Date
2024-11-01
Estimated Expiration
2042-06-23

AI Technical Summary

Technical Problem

Among the existing zipper materials, brass zippers have high cost and high density, resin zippers have low tensile strength and poor wear resistance, which cannot meet the wide application needs, and have low production efficiency and high manufacturing costs.

Method used

Using copper-aluminum composite materials, through the bimetallic molding process of aluminum alloy and copper alloy, the outer layer of copper alloy and the inner layer of aluminum alloy is formed, combining the tensile strength of aluminum alloy and the wear resistance of copper alloy, reducing density and improving production efficiency.

Benefits of technology

It realizes high tensile strength and wear resistance of lightweight zipper materials, reduces density and manufacturing costs, improves production efficiency, and is suitable for decoration and wide application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115255019B_ABST
    Figure CN115255019B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of alloy materials, and specifically relates to a copper-aluminum composite material for a lightweight zipper and a preparation method thereof. The copper-aluminum composite material for a lightweight zipper comprises an aluminum alloy inner layer and a copper alloy outer layer, wherein the aluminum alloy inner layer is composed of the following components in weight percentage: Si: 0.05-0.10%, Fe: 0.08-0.16%, Mn: 0.05-0.09%, Mg: 15-20%, Cr: 0.50-0.70%, V≤0.001%, Ti: 0.01-0.05%, Be: 0.03-0.05%, Er: 0.01-0.02%, and the remainder is Al and other unavoidable impurities. Through this design, it is ensured that the surface material has good wear resistance and good metallic gloss, which is close to the metallic gloss of platinum, and is suitable for decoration. The internal aluminum alloy has sufficient tensile strength and toughness, and can provide sufficient strength and service life during use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of alloy materials, and particularly relates to a copper-aluminum composite material for a lightweight zipper and a preparation method thereof. Background Art

[0002] At present, in the clothing decoration industry, zippers are gradually replacing buttons, and the use of zippers is increasing. There are two main types of zippers. One is a metal zipper mainly made of brass, which has good wear resistance, high tensile strength, long service life, good metallic luster, and is close to the color of gold. It is popular among consumers, but copper is expensive and has a high density, which makes copper alloy zippers expensive to manufacture and has a certain impact on their use. They can only be used in some special industries. The other type of zipper is mainly made of resin material. Resin has low manufacturing cost and light weight, and can be used to manufacture zippers of various colors, but has low tensile strength, poor wear resistance, and is easily deformed by heat, resulting in resin zippers that can only be used in some places and venues with low requirements.

[0003] The brass material used for zippers is produced by the upward drawing method, which has low production efficiency and a production speed of 0.8 tons per hour, making the production cost high. The subsequent drawing from φ12mm copper rod to the conventional specification φ3.6mm has high manufacturing costs, and the price of copper is about 70,000 / ton. The high copper price restricts the development of copper alloys in the zipper industry. Copper has a high density, requiring 8.96 tons of copper per unit volume. The weight of copper required for a zipper of the same size is 3.28 times that of aluminum, and the price of copper of the same weight is 3.5 times that of aluminum. Compared with aluminum, the price of the same volume of copper is 11.5 times. Aluminum alloy has a low price, low density, and a large reserve in nature, which is suitable for vigorous promotion in the zipper industry. However, aluminum alloy has poor wear resistance and a short service life, which cannot meet normal use. Summary of the invention

[0004] In order to solve the above technical problems, the present invention aims to provide a method for preparing a copper-aluminum composite material for a lightweight zipper, comprising the following steps:

[0005] (1) melting the aluminum alloy, adding AlB3 for reaction, and then refining once to obtain aluminum liquid A;

[0006] (2) adding a master alloy to the aluminum liquid A and performing secondary refining to remove impurities to obtain aluminum liquid B;

[0007] (3) casting the aluminum liquid B into a copper alloy strip to obtain a copper-aluminum composite material to be treated;

[0008] (4) rolling and quenching the copper-aluminum composite material to be processed to obtain the copper-aluminum composite material to be formed;

[0009] (5) drawing the copper-aluminum composite material to be formed, and performing bimetallic bright annealing, so that the copper alloy strip forms a copper alloy outer layer, and the aluminum liquid B forms an aluminum alloy inner layer, thereby obtaining the copper-aluminum composite material for the lightweight zipper;

[0010] The aluminum alloy inner layer is composed of the following components in weight percentage:

[0011] Si: 0.05-0.10%, Fe: 0.08-0.16%, Mn: 0.05-0.09%, Mg: 15-20%, Cr: 0.50-0.70%, V≤0.001%, Ti: 0.01-0.05%, Be: 0.03-0.05%, Er: 0.01-0.02%, the balance is Al and other unavoidable impurities;

[0012] The copper alloy outer layer is composed of the following components in weight percentage:

[0013] Si: 0.8-1.6%, Ni: 15-20%, Al: 8-12.0%, Mn: 5.2-6.0%, Ti: 0.05-0.1%, B: 0.02-0.06%, Fe: 0.2-0.06%, and the balance is Cu and other unavoidable impurities.

[0014] The intermediate alloy is aluminum-manganese alloy, aluminum-chromium alloy, aluminum-titanium alloy, aluminum-beryllium alloy, aluminum-erbium alloy and magnesium ingot; the intermediate alloy is added to the aluminum liquid A after calculation according to the weight percentage of each element in the aluminum alloy inner layer.

[0015] Preferably, in step (1), the purity of the aluminum alloy is not less than 99.75%.

[0016] Preferably, in step (1), the refining gas in the primary refining is chlorine, the temperature is 720-740° C., and the time is 20-30 min.

[0017] Furthermore, in the primary refining, the powder blowing time is required to be 15-20 minutes to ensure the refining effect; after the primary refining is completed, it is allowed to stand for 2 hours to ensure that the impurity elements in the aluminum liquid A are fully separated by floating and sinking.

[0018] Preferably, in step (2), the refining gas in the secondary refining is chlorine, the temperature is 720-740° C., and the time is 40-45 min.

[0019] Preferably, in step (2), the impurity removal method is as follows: after the secondary refining, the aluminum liquid A is allowed to stand for 30-35 minutes, then the slag is removed and then allowed to stand for 1-3 hours.

[0020] Preferably, in step (3), the casting temperature is 700-720°C.

[0021] Furthermore, in the step (3), the degassing vertical bimetallic casting machine includes a round billet support wheel and a round billet approach bridge, and the bimetallic round billet is driven by the round billet support wheel to be sent into the round billet approach bridge, and then enters the two-roll rolling mill from the round billet approach bridge.

[0022] Specifically, in step (3), the casting method is as follows: the aluminum alloy melt after refining and standing is released by tilting, and continuously cast after filtering, degassing and refining treatment, and the casting is carried out by degassing vertical bimetallic casting. The aluminum liquid is poured into a φ40mm straight cylinder made of a copper alloy strip (width 125.6mm, thickness 2mm) curled by a pressure wheel, and then the interface is welded by laser, and then the aluminum alloy liquid is poured from the ladle into the copper alloy cylinder, and the degassing vertical bimetallic casting machine is used to directly spray cooling water on the copper alloy to cool and solidify the aluminum liquid in the middle, and then the bimetallic round billet is sent to the round billet approach bridge under the drive of the round billet support wheel, and then enters the two-roll rolling mill from the round billet approach bridge. The speed of the round billet support wheel and the cooling water pressure are controlled so that the temperature of the round billet from the transmission support wheel to the approach bridge is 360-420℃.

[0023] Preferably, in step (4), the rolling temperature is 360-420°C.

[0024] Specifically, the rolling mill adopts a full two-roll rolling mill, and the round billet is hot-deformed to φ9.5 mm by circular + elliptical mutual deformation.

[0025] Preferably, in step (4), the quenching method is: reducing the temperature to 110-130° C. within 4-6 seconds.

[0026] Preferably, in step (5), the number of drawing is 6-8 times, and the deformation amount each time is 25-30%.

[0027] Specifically, the deformation process of drawing is: -Bright annealing - Bright annealing.

[0028] Preferably, in step (5), the bimetallic bright annealing comprises the following steps: heating the copper-aluminum composite material to be formed to 520-560°C at 4-6°C / min after drawing, keeping the temperature for 44-52h and then cooling to room temperature (25±5°C).

[0029] The present invention also provides a copper-aluminum composite material for a lightweight zipper prepared by the above preparation method.

[0030] The technical solution of the present invention has the following advantages over the prior art:

[0031] 1. The bimetallic one-piece molding method can make the two metals tightly combined and will not fall off during subsequent processing;

[0032] 2. Continuous casting and rolling of bimetallic alloy materials, high efficiency, high production efficiency, 375% faster than brass production speed, low manufacturing cost;

[0033] 3. Through the design of copper alloy and aluminum alloy components, the surface material has good wear resistance and good metallic gloss, close to the metallic gloss of platinum, which is suitable for decoration. The internal aluminum alloy has sufficient tensile strength and toughness to ensure easy molding in subsequent processing projects, and can provide sufficient strength and service life during use;

[0034] 4. The finished product of the copper-aluminum composite material for the lightweight zipper has a low density, which can be reduced by 57% compared with copper alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of copper-aluminum composite material for lightweight zippers.

[0036] Figure 2 This is the front view of the degassing vertical bimetallic casting machine.

[0037] Figure 3 This is the left view of the degassing vertical bimetallic casting machine.

[0038] Figure 4 A top view of a degassing vertical bimetallic casting machine.

[0039] Figure 5 This is a three-dimensional structural diagram of a degassing vertical bimetallic casting machine.

[0040] Explanation of the reference numerals: 1-copper alloy outer layer, 2-aluminum alloy inner layer, 3-round billet support wheel, 4-bimetallic round billet, 5-round billet approach bridge. DETAILED DESCRIPTION

[0041] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0042] The copper-aluminum composite material for a lightweight zipper in Examples 1-3 comprises an aluminum alloy inner layer 2 and a copper alloy outer layer 1.

[0043] The aluminum alloy inner layer 2 is composed of the following components in weight percentage:

[0044] Si: 0.05-0.10%, Fe: 0.08-0.16%, Mn: 0.05-0.09%, Mg: 15-20%, Cr: 0.50-0.70%, V≤0.001%, Ti: 0.01-0.05%, Be: 0.03-0.05%, Er: 0.01-0.02%, the balance is Al and other unavoidable impurities;

[0045] The copper alloy outer layer 1 is composed of the following components in weight percentage:

[0046] Si: 0.8-1.6%, Ni: 15-20%, Al: 8-12.0%, Mn: 5.2-6.0%, Ti: 0.05-0.1%, B: 0.02-0.06%, Fe: 0.2-0.06%, and the balance is Cu and other unavoidable impurities.

[0047] Example 1

[0048] (1) Melting: 99.75% aluminum ingots are put into a melting furnace for melting. After melting, aluminum-boron alloy gold is added according to the vanadium content of the aluminum liquid to carry out the first step of reducing impurity elements. The molten alloy is heated to 730°C, and a refining agent is added at a ratio of 0.1%. 99.999% chlorine is used for refining. The refining time is 20 minutes, and the powder blowing time is required to be 15 minutes to ensure the refining effect. After the aluminum liquid is refined, it is allowed to stand for 2 hours to ensure that the impurity elements in the aluminum liquid are fully separated by floating and sinking.

[0049] (2) Alloying: After refining and standing in the melting furnace, pour the molten aluminum from the middle part of the liquid surface into the holding furnace. The temperature of the molten aluminum is 730°C. According to the alloy composition and the weight of the molten aluminum, add the intermediate alloy by calculation, turn on the electromagnetic stirring, stir for 30 minutes, stand for 30 minutes, and then take samples to test the composition. After the composition is qualified, add molten sodium removal particle refining agent to the refining tank according to 0.1% by weight, use 99.999% chlorine for refining, and the refining time is 42 minutes. After the refining is completed, stand for 30 minutes, remove the slag on the liquid surface, and stand for 2 hours.

[0050] (3) Bimetallic one-piece molding: The aluminum alloy melt after refining and standing is released by tilting, and then continuously cast after filtering, degassing and refining. The casting temperature is controlled at 710℃, and the degassing vertical bimetallic casting method is used for casting. The aluminum liquid is poured into a φ40mm straight cylinder made of a copper alloy strip (width 125.6mm, thickness 2mm) rolled by a pressure wheel, and then the interface is welded by laser. Then the aluminum alloy liquid is poured from the ladle into the copper alloy cylinder, and the degassing vertical bimetallic casting machine is used to directly spray cooling water on the copper alloy to cool and solidify the aluminum liquid in the middle. Then, the bimetallic round billet 4 is sent to the round billet approach bridge 5 under the drive of the round billet support wheel 3, and then enters the two-roll rolling mill from the round billet approach bridge 5. The speed of the round billet support wheel 3 and the cooling water pressure are controlled so that the temperature of the round billet from the transmission support wheel to the approach bridge is 400℃.

[0051] (4) Rolling: Rolling and casting are carried out continuously. The rolling mill adopts a full two-roll rolling mill. The round billet is thermally deformed to φ9.5mm by circular + elliptical mutual deformation. The heat of the aluminum liquid is fully utilized during the rolling process. Then, a heater is used for secondary online temperature increase to ensure the temperature of the round billet before rolling and to ensure that the round billet has sufficient plasticity, which greatly reduces the manufacturing cost and improves the production efficiency. After rolling, quenching treatment is carried out. The rolled and deformed rod is put into cold water for rapid cooling, and the temperature is reduced from 400℃ to 120℃ within 5s.

[0052] (5) Drawing: The rolled material obtained above is cold drawn. The deformation amount is 27.5% each time, and the finished product is φ3.60mm after 8 drawing passes. It is annealed twice in the middle, all of which are bimetallic bright annealing. (φ9.5mm-φ8.41mm-φ7.45mm-φ6.60mm-φ5.84mm-bright annealing-φ5.18mm-φ4.58mm-φ4.06mm-φ3.60mm-bright annealing)

[0053] (6) Bimetallic bright annealing: The cold-drawn monofilament is subjected to bimetallic bright annealing. In order to ensure the surface brightness after annealing, a low-pressure nitrogen-filled normal pressure annealing + rapid heating and extended heat preservation + nitrogen-filled cooling annealing process is adopted. The temperature is rapidly increased during the heating stage, and after reaching the heat preservation stage, it is kept warm for 48 hours, and then quickly cooled to room temperature to obtain the finished product. (After the composite metal monofilament is wound into a roll, it is placed in a vacuum annealing furnace and sealed, and then evacuated to -0.1MPa, and then filled with 99.999% nitrogen. After filling to normal pressure, stop, turn on the power for heating, and heat to 540°C at a heating rate of 5°C / min, keep warm for 48 hours, and then fill with nitrogen to cool down and ensure surface brightness)

[0054] Example 2

[0055] (1) Melting: 99.75% aluminum ingots are put into a melting furnace for melting. After melting, aluminum-boron alloy gold is added according to the vanadium content of the aluminum liquid to carry out the first step of reducing impurity elements. The molten alloy is heated to 720°C, and a refining agent is added at a ratio of 0.1%. 99.999% chlorine is used for refining. The refining time is 20 minutes, and the powder blowing time is required to be 15 minutes to ensure the refining effect. After the aluminum liquid is refined, it is allowed to stand for 2 hours to ensure that the impurity elements in the aluminum liquid are fully separated by floating and sinking.

[0056] (2) Alloying: After refining and standing in the melting furnace, pour the molten aluminum from the middle of the liquid surface into the holding furnace. The temperature of the molten aluminum is 720°C. According to the alloy composition and the weight of the molten aluminum, add the intermediate alloy by calculation, turn on the electromagnetic stirring, stir for 30 minutes, stand for 30 minutes, and then take samples to test the composition. After the composition is qualified, add molten sodium removal particle refining agent to the refining tank according to 0.1% by weight, use 99.999% chlorine for refining, and the refining time is 40 minutes. After refining, let it stand for 30 minutes, remove the slag on the liquid surface, and let it stand for 2 hours.

[0057] (3) Bimetallic one-piece forming: The aluminum alloy melt after refining and standing is released by tilting, and then continuously cast after filtering, degassing and refining. The casting temperature is controlled at 700℃, and the degassing vertical bimetallic casting method is used for casting. The aluminum liquid is poured into a φ40mm straight cylinder made of a copper alloy strip (width 125.6mm, thickness 2mm) rolled by a pressure wheel, and then the interface is welded by laser. Then, the aluminum alloy liquid is poured from the ladle into the copper alloy cylinder, and the degassing vertical bimetallic casting machine is used to directly spray cooling water on the copper alloy to cool and solidify the aluminum liquid in the middle. Then, the bimetallic round billet 4 is sent to the round billet approach bridge 5 under the drive of the round billet support wheel 3, and then enters the two-roll rolling mill from the round billet approach bridge 5. The speed of the round billet support wheel 3 and the cooling water pressure are controlled so that the temperature of the round billet from the transmission support wheel to the approach bridge is 360-420℃.

[0058] (4) Rolling: Rolling and casting are carried out continuously. The rolling mill adopts a full two-roll rolling mill. The round billet is thermally deformed to φ9.5mm by circular + elliptical mutual deformation. The heat of the aluminum liquid is fully utilized during the rolling process. Then, a heater is used for secondary online temperature increase to ensure the temperature of the round billet before rolling and to ensure that the round billet has sufficient plasticity, which greatly reduces the manufacturing cost and improves the production efficiency. After rolling, quenching treatment is carried out. The rolled and deformed rod is quickly cooled in cold water, and the temperature is reduced from 360℃ to 120℃ within 5s.

[0059] (5) Drawing: The rolled material obtained above is cold drawn. The deformation amount is 27.5% each time, and the finished product is φ3.60mm after 8 drawing passes. It is annealed twice in the middle, all of which are bimetallic bright annealing. (φ9.5mm-φ8.41mm-φ7.45mm-φ6.60mm-φ5.84mm-bright annealing-φ5.18mm-φ4.58mm-φ4.06mm-φ3.60mm-bright annealing)

[0060] (6) Bimetallic bright annealing: The cold-drawn monofilament is subjected to bimetallic bright annealing. In order to ensure the surface brightness after annealing, a low-pressure nitrogen-filled normal pressure annealing + rapid heating and extended heat preservation + nitrogen-filled cooling annealing process is adopted. The temperature is rapidly increased during the heating stage, and after reaching the heat preservation stage, it is kept warm for 48 hours, and then quickly cooled to room temperature to obtain the finished product. (After the composite metal monofilament is wound into a roll, it is placed in a vacuum annealing furnace and sealed, and then evacuated to -0.1MPa, and then filled with 99.999% nitrogen. After filling to normal pressure, stop, turn on the power for heating, and heat to 540°C at a heating rate of 5°C / min, keep warm for 48 hours, and then fill with nitrogen to cool down and ensure surface brightness)

[0061] Example 3

[0062] (1) Melting: 99.75% aluminum ingots are put into a melting furnace for melting. After melting, aluminum-boron alloy gold is added according to the vanadium content of the aluminum liquid to carry out the first step of reducing impurity elements. The molten alloy is heated to 740°C, and a refining agent is added at a ratio of 0.1%. 99.999% chlorine is used for refining. The refining time is 30 minutes, and the powder blowing time is required to be 15-20 minutes to ensure the refining effect. After the aluminum liquid is refined, it is allowed to stand for 2 hours to ensure that the impurity elements in the aluminum liquid are fully separated by floating and sinking.

[0063] (2) Alloying: Pour the molten aluminum from the middle of the liquid surface after refining and standing in the melting furnace into the holding furnace. The temperature of the molten aluminum is 740°C. According to the alloy composition and the weight of the molten aluminum, add the intermediate alloy by calculation, turn on the electromagnetic stirring, stir for 35 minutes, and then stand for 35 minutes to take samples for composition testing. After the composition is qualified, add molten sodium removal particle refining agent to the refining tank according to 0.2% by weight, use 99.999% chlorine for refining, and the refining time is 45 minutes. After refining, let it stand for 35 minutes, remove the slag on the liquid surface, and let it stand for 2 hours.

[0064] (3) Bimetallic one-piece forming: The aluminum alloy melt after refining and standing is released by tilting, and then continuously cast after filtering, degassing and refining. The casting temperature is controlled at 720℃, and the degassing vertical bimetallic casting method is used for casting. The aluminum liquid is poured into a φ40mm straight cylinder made of a copper alloy strip (width 125.6mm, thickness 2mm) rolled by a pressure wheel, and then the interface is welded by laser. Then, the aluminum alloy liquid is poured from the ladle into the copper alloy cylinder, and the degassing vertical bimetallic casting machine is used to directly spray cooling water on the copper alloy to cool and solidify the aluminum liquid in the middle. Then, the bimetallic round billet 4 is sent to the round billet approach bridge 5 under the drive of the round billet support wheel 3, and then enters the two-roll rolling mill from the round billet approach bridge 5. The speed of the round billet support wheel 3 and the cooling water pressure are controlled so that the temperature of the round billet from the transmission support wheel to the approach bridge is 360-420℃.

[0065] (4) Rolling: Rolling and casting are carried out continuously. The rolling mill adopts a full two-roll rolling mill. The round billet is thermally deformed to φ9.5mm by circular + elliptical mutual deformation. The heat of the aluminum liquid is fully utilized during the rolling process. Then, a heater is used for secondary online temperature increase to ensure the temperature of the round billet before rolling and to ensure that the round billet has sufficient plasticity, which greatly reduces the manufacturing cost and improves the production efficiency. After rolling, quenching treatment is carried out. The rolled and deformed rod is put into cold water for rapid cooling, and the temperature is reduced from 440℃ to 120℃ within 5s.

[0066] (5) Drawing: The rolled material obtained above is cold drawn. The deformation amount is 27.5% each time, and the finished product is φ3.60mm after 8 drawing passes. It is annealed twice in the middle, all of which are bimetallic bright annealing. (φ9.5mm-φ8.41mm-φ7.45mm-φ6.60mm-φ5.84mm-bright annealing-φ5.18mm-φ4.58mm-φ4.06mm-φ3.60mm-bright annealing)

[0067] (6) Bimetallic bright annealing: The cold-drawn monofilament is subjected to bimetallic bright annealing. In order to ensure the surface brightness after annealing, a low-pressure nitrogen-filled normal pressure annealing + rapid heating and extended heat preservation + nitrogen-filled cooling annealing process is adopted. The temperature is rapidly increased during the heating stage, and after reaching the heat preservation stage, it is kept warm for 48 hours, and then quickly cooled to room temperature to obtain the finished product. (After the composite metal monofilament is wound into a roll, it is placed in a vacuum annealing furnace and sealed, and then evacuated to -0.1MPa, and then filled with 99.999% nitrogen. After filling to normal pressure, stop, turn on the power for heating, and heat to 540°C at a heating rate of 5°C / min, keep warm for 48 hours, and then fill with nitrogen to cool down and ensure surface brightness)

[0068] Effect evaluation

[0069] The chemical compositions of Examples 1-3 are shown in Table 1 and Table 2:

[0070] Table 1 Chemical composition of aluminum alloy in Examples 1-3

[0071]

[0072] Table 2 Chemical composition of copper alloy in Examples 1-3

[0073]

[0074] Table 3 Performance analysis data in Examples 1-3

[0075]

[0076] Table 4 Performance analysis data of prior art annealed copper

[0077]

[0078] The performance analysis comparison of Examples 1-3 and prior art annealed copper (copper alloy) is shown in Table 3 and Table 4. The conventional product currently used in the industry is annealed copper, which has a tensile strength of about 320-350 MPa and an average density of 8.9 kg / cm 3 Comparing the product performance in Examples 1-3 of the present invention, the specifications are (±0.01mm), actual specifications The elongation is 15-30%, and the tensile strength is 400-470MPa, which is much greater than the tensile strength of annealed copper; at the same time, the composite material obtained by the present invention has a density of 3.90-3.95kg / cm 3 The mass wear amount is 0.008-0.009g, which is much smaller than the annealed copper in the prior art.

[0079] In summary, the copper-aluminum composite material for a lightweight zipper obtained by the present invention has high strength, light material, and excellent application effect.

[0080] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from them are still within the protection scope of the invention.

Claims

1. A method for preparing a copper-aluminum composite material for a lightweight zipper, characterized in that: The steps include: (1) Melting the aluminum alloy, adding AlB3 for reaction and then refining once to obtain aluminum liquid A; (2) adding a master alloy to the aluminum liquid A, performing secondary refining to remove impurities, and obtaining aluminum liquid B; (3) casting the aluminum liquid B into a copper alloy strip to obtain a copper-aluminum composite material to be treated; (4) rolling and quenching the copper-aluminum composite material to be processed to obtain the copper-aluminum composite material to be formed; (5) Drawing the copper-aluminum composite material to be formed, and performing bimetallic bright annealing, so that the copper alloy strip forms a copper alloy outer layer, and the aluminum liquid B forms an aluminum alloy inner layer, thereby obtaining the copper-aluminum composite material for the lightweight zipper; The aluminum alloy inner layer is composed of the following components in weight percentage: composition: Si: 0.05-0.10%, Fe: 0.08-0.16%, Mn: 0.05-0.09%, Mg: 15-20%, Cr: 0.50-0.70%, V≤0.001%, Ti: 0.01-0.05%, Be: 0.03-0.05%, Er: 0.01-0.02%, the balance is Al and other unavoidable impurities; The copper alloy outer layer is composed of the following components in weight percentage: composition: Si: 0.8-1.6%, Ni: 15-20%, Al: 8-12.0%, Mn: 5.2-6.0%, Ti: 0.05-0.1%, B: 0.02-0.06%, Fe: 0.2-0.06%, the balance is Cu and other unavoidable impurities; In the step (3), the casting temperature is 700-720°C; in the step (4), the rolling temperature is 360-420°C, and the quenching method is: reducing the temperature to 110-130°C within 4-6 seconds; in the step (5), the number of drawing is 6-8 times, and the deformation amount of each time is 25-30%; in the step (5), the bimetallic bright annealing adopts low-pressure nitrogen filling and normal pressure annealing, rapid heating and long-term insulation, and nitrogen filling and cooling annealing processes, including the following steps: after drawing the copper-aluminum composite material to be formed, heating it to 520-560°C at 4-6°C / min, insulation for 44-52 hours, and then cooling it to room temperature.

2. The preparation method according to claim 1, characterized in that In the step (1), the refining gas in the primary refining is chlorine, the temperature is 720-740° C., and the time is 20-30 min.

3. The preparation method according to claim 1, characterized in that: In the step (2), the refining gas in the secondary refining is chlorine, the temperature is 720-740°C, and the time is 40-45 minutes.

4. The preparation method according to claim 1, characterized in that: In the step (2), the impurity removal method is as follows: after the secondary refining, the aluminum liquid A is allowed to stand for 30-35 minutes, then the slag is removed and then allowed to stand for another 1-3 hours.

5. A copper-aluminum composite material for a lightweight zipper prepared by the preparation method according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Manufacturing method of copper-clad aluminum busbar

    CN101060025A

  • Ingot casting and stretch forming process and equipment of copper and aluminium composite bus-bar wire

    CN101433947A

  • Method for manufacturing copper-clad aluminum composite panel belt

    CN101447258A

  • Preparation technology of copper and aluminum combined flat wire

    CN105206351A

  • Isothermal processed copper cladded aluminum composite and method and system for manufacturing the same

    CN105792955A