Adhesive composition

By using a composition of a polyester with a high glass transition temperature and amorphous polyester with a low glass transition temperature, and adding polyisocyanate, the problem of insufficient peel strength of the existing polyester resin at high temperature is solved, and flexibility is achieved The bonding performance of printed circuit boards is improved at high temperatures.

CN115279858BActive Publication Date: 2024-12-03TOYOBO MC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180020026.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-30
Filing Date
2021-03-26
Publication Date
2024-12-03
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

The glass transition temperature of existing polyester resins is lower than 80°C, resulting in insufficient peeling strength at high temperatures and cannot meet the bonding needs of flexible printed circuit boards at high temperatures.

Method used

A composition of polyester (A1) with a glass transition temperature or melting point higher than 80°C and amorphous polyester (A2) with a Tg of 0°C or less, and a polyisocyanate (B) is added thereto to optimize the polyester's Polycarboxylic acid and polyol components improve the heat resistance and peel strength of the adhesive through polycondensation reaction and acid value control.

Benefits of technology

It achieves excellent softness and peel strength at high temperatures, and is suitable for adhesives for flexible printed circuit boards, improving the heat resistance and bonding performance of humidified solder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003838595610000091
    Figure BDA0003838595610000091
  • Figure BDA0003838595610000121
    Figure BDA0003838595610000121
Patent Text Reader

Abstract

The adhesive composition of the present invention provides an adhesive composition having excellent flexibility of an uncured coating film and excellent wet solder heat resistance and high temperature peel strength as an adhesive for a flexible printed wiring board. The adhesive composition of the present invention comprises a polyester having a glass transition temperature or melting point higher than 80°C and a polyisocyanate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive composition and more particularly to an adhesive composition having excellent flexibility of an uncured coating film and excellent wet solder heat resistance and high-temperature peel strength as an adhesive for a flexible printed wiring board. Background Art

[0002] Flexible printed circuit board (FPC) refers to a substrate with a circuit formed on a base material formed by bonding a thin and soft film with insulating properties such as polyimide and a conductive metal such as copper foil with an adhesive. Unlike rigid substrates, since it is very thin and soft, it can be used in small spaces or curved movable parts of electronic devices, and is therefore used in many daily electronic devices such as personal computers and smartphones. In recent years, many FPCs have also been installed in automobiles, so adhesives are required to have high-temperature adhesion.

[0003] Polyester is widely used as a raw material for resin compositions used in coating agents, inks, adhesives, etc., and is generally composed of polycarboxylic acids and polyols. Since the flexibility and molecular weight can be freely controlled by the selection and combination of polycarboxylic acids and polyols, it is widely used in various applications, including coating agents and adhesives.

[0004] Polyester has excellent adhesion (peel strength) to metals including copper, and is used in adhesives for FPCs when mixed with a curing agent.

[0005] (For example, Patent Document 1).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 9-125043 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, the polyester resin described in Patent Document 1 is composed only of a polyester resin having a glass transition temperature (Tg) as low as 80° C. or less, and therefore has insufficient peel strength at high temperatures.

[0011] The present invention was made against the background of the above-mentioned problems of the prior art. That is, the object of the present invention is to provide an adhesive composition having excellent flexibility of an uncured coating film (B stage) and excellent wet solder heat resistance and high temperature peel strength as an adhesive for a flexible printed wiring board.

[0012] Means for solving problems

[0013] As a result of intensive studies, the present inventors have found that the above-mentioned problems can be solved by the means shown below, and have completed the present invention.

[0014] That is, the present invention has the following configurations.

[0015] An adhesive composition comprises a polyester (A1) having a glass transition temperature or a melting point higher than 80° C. and a polyisocyanate (B).

[0016] The adhesive composition preferably further contains a polyester (A2) having a glass transition temperature of 0° C. or lower and a melting point of 80° C. or lower or being amorphous.

[0017] The adhesive composition preferably contains the polyester (A2) in an amount of 10 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the polyester (A1).

[0018] The adhesive composition preferably contains the polyisocyanate (B) in an amount of 0.1 parts by mass or more and 10 parts by mass or less based on 100 parts by mass of the total amount of the polyester (A1) and the polyester (A2).

[0019] The adhesive composition is suitable for use in flexible printed wiring boards.

[0020] Effects of the Invention

[0021] The uncured coating film of the adhesive composition of the present invention is excellent in flexibility, and is excellent in wet solder heat resistance and high-temperature peel strength as an adhesive for FPC. DETAILED DESCRIPTION

[0022] Hereinafter, one embodiment of the present invention will be described in detail below. However, the present invention is not limited thereto, and can be implemented in various modified forms within the scope of the description.

[0023] <Polyester (A1)>

[0024] The adhesive composition of the present invention contains a polyester (A1) having a glass transition temperature or melting point higher than 80° C. By using a polyester (A1) having a glass transition temperature (Tg) or melting point (Tm) higher than 80° C., wet solder heat resistance and high temperature peel strength can be improved.

[0025] The polyester (A1) is composed of a chemical structure obtainable by a polycondensate of a polycarboxylic acid component or a polycarboxylic acid ester component and a polyol component, wherein the polycarboxylic acid component or a polycarboxylic acid ester component and the polyol component are each composed of one or more selected components.

[0026] As the polycarboxylic acid component constituting the above-mentioned polyester (A1), it is not limited, and the polycarboxylic acids or their esters and polycarboxylic anhydrides shown below can be used. Specifically, as the polycarboxylic acid, terephthalic acid, isophthalic acid, phthalic acid, naphthalene dicarboxylic acid, tetrahydrophthalic acid, methyltetrahydrophthalic acid, adipic acid, sebacic acid, dimer acid, 1,3-cyclohexane dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, fumaric acid, maleic acid, dimethyl isophthalate-5-sodium sulfonate, trimellitic acid or pyromellitic acid and their esters can be mentioned. As the polycarboxylic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, succinic anhydride, trimellitic anhydride, pyromellitic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hydrogenated naphthalene dicarboxylic acid, etc. can be mentioned. In particular, aromatic polycarboxylic acid components such as naphthalene dicarboxylic acid and terephthalic acid are preferred. By using an aromatic polycarboxylic acid, Tg becomes higher and the peel strength at high temperature can be improved.

[0027] The polyol constituting the polyester (A1) is not particularly limited, and ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 2-methyl-1,3-propylene glycol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1-methyl-1,8-octanediol, 2-methyl-2-ethyl-1,3-propylene glycol, 2,2-diethyl-1,3-propylene glycol, 2-ethyl-2-n-propyl-1,3-propylene glycol, 2 , 2-di-n-propyl-1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, 2,4-diethyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, polytetramethylene glycol, polypropylene glycol and other polyalkylene ether glycols, glycerol, trimethylolpropane, trimethylolethane, pentaerythritol, α-methyl glucose, mannitol, sorbitol, dimer glycol and other diol components, among which one or more kinds can be used. In particular, polyols without long-chain alkyl groups such as ethylene glycol, 1,2-propylene glycol and 1,3-propylene glycol, or alicyclic polyols such as 1,4-cyclohexanedimethanol and tricyclodecane dimethanol are preferred. By using these polyols, Tg becomes higher, and the peel strength at high temperature can be improved.

[0028] In the above polyester (A1), a trivalent or higher polycarboxylic acid component and / or a trivalent or higher polyol component may also be copolymerized. As the trivalent or higher polycarboxylic acid component, for example, aromatic carboxylic acids such as trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid, trimesic acid, trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and aliphatic carboxylic acids such as 1,2,3,4-butanetetracarboxylic acid may be cited, and one or more of these may be used. As the trivalent or higher polyol component, for example, glycerol, trimethylolpropane, trimethylolethane, pentaerythritol, α-methyl glucose, mannitol, sorbitol may be cited, and one or more of these may be used.

[0029] The polyester (A1) may be copolymerized with lactone or lactam. For example, ε-caprolactone or ε-caprolactam may be used.

[0030] As methods for the polycondensation reaction of producing the polyester (A1), there are, for example: 1) a method of heating a polycarboxylic acid and a polyol in the presence of a known catalyst, and performing a polyol removal and polycondensation reaction via a dehydration esterification step; 2) a method of heating an alcohol ester of a polycarboxylic acid and a polyol in the presence of a known catalyst, and performing a polyol removal and polycondensation reaction via an ester exchange reaction; 3) a method of performing depolymerization; etc. In the above methods 1) and 2), a part or all of the acid components may be replaced by anhydrides.

[0031] When producing the polyester (A1), a conventionally known polymerization catalyst can be used, for example, titanium compounds such as tetra-n-butyl titanate, tetraisopropyl titanate, and titanium acetylacetonate, antimony compounds such as antimony trioxide and antimony tributoxy, germanium compounds such as germanium oxide and tetra-n-butoxygermanium, and other catalysts such as acetates of magnesium, iron, zinc, manganese, cobalt, and aluminum. These catalysts can be used alone or in combination of two or more.

[0032] As methods for increasing the acid value of the polyester (A1), there are, for example: (1) a method of adding a trivalent or higher polycarboxylic acid and / or a trivalent or higher polycarboxylic acid anhydride to react after the polycondensation reaction (acid addition); (2) intentionally modifying the resin by the action of heat, oxygen, water, etc. during the polycondensation reaction; and the like. These methods may be carried out arbitrarily. The polycarboxylic anhydride used in the acid addition in the acid addition method is not particularly limited, and examples thereof include phthalic anhydride, tetrahydrophthalic anhydride, succinic anhydride, maleic anhydride, trimellitic anhydride, pyromellitic anhydride, hexahydrophthalic anhydride, 3,3′,4,4′-benzophenonetetracarboxylic dianhydride, 3,3′,4,4′-biphenyltetracarboxylic dianhydride, ethylene glycol dianhydrotrimellitic acid ester, and the like. One or more of these may be used.

[0033] The acid value of the polyester (A1) is preferably 200 eq / 10 6g or less, more preferably 100 eq / 10 6 g or less, more preferably 50eq / 10 6 g or less, particularly preferably 30 eq / 10 6 g or less, and most preferably 20eq / 10 6 By making the resin acid value within the above range, it is expected that a good pot life, substrate adhesion, and crosslinking properties will be improved. In addition, the lower the acid value, the more hygroscopicity can be suppressed, and the heat resistance of humidified solder can be improved.

[0034] The number average molecular weight of the polyester (A1) is preferably 5000 to 100000. More preferably, it is 10000 or more. In addition, it is more preferably 50000 or less. By making the number average molecular weight within the above range, the operation when dissolved in a solvent is easy, and after curing, it has high cohesion, so that excellent peel strength can be exerted.

[0035] In order to make the Tg or Tm of the polyester higher than 80° C., this can be achieved by, for example, introducing a rigid structure such as an aromatic compound or an alicyclic compound, or increasing the ester bond concentration.

[0036] <Polyester (A2)>

[0037] The adhesive composition of the present invention preferably further contains a polyester (A2) having a Tg of 0°C or less and a melting point of 80°C or less or being amorphous. By containing a polyester (A2) having a Tg of 0°C or less and a melting point of 80°C or less or being amorphous, flexibility can be imparted to the uncured coating film and wet solder heat resistance can be imparted. The Tg of the polyester (A2) is preferably -10°C or less.

[0038] In addition, the amorphous property means that a material does not show a melting peak in the melting point measurement described later.

[0039] The content of the polyester (A2) is preferably 10 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the polyester (A1) having a Tg or Tm exceeding 80°C. It is more preferably 25 parts by mass or more. Furthermore, it is more preferably 70 parts by mass or less. By making the content of the polyester (A2) within the above range, the uncured coating film has excellent flexibility, peel strength at high temperature, and wet solder heat resistance.

[0040] The acid value of the polyester (A2) is preferably 200 eq / 10 6 g or less, more preferably 100 eq / 10 6 g or less, more preferably 50eq / 10 6 g or less, particularly preferably 30 eq / 10 6 g or less, and most preferably 20eq / 10 6By making the resin acid value within the above range, it is expected that a good pot life, substrate adhesion, and crosslinking properties will be improved. In addition, the lower the acid value, the more hygroscopicity can be suppressed, and the heat resistance of humidified solder can be improved.

[0041] The number average molecular weight of the polyester (A2) is preferably 5000 to 100000. More preferably 10000 or more, further preferably 20000 or more, particularly preferably 25000 or more. When the number average molecular weight is above the above value, the concentration of the polar group decreases relatively, thereby suppressing hygroscopicity and improving the heat resistance of humidified solder. In addition, the number average molecular weight is more preferably 50000 or less. By making the number average molecular weight below the above value, the operation when dissolved in the solvent is easy, and the cohesion can be maintained even before curing, and the softness of the uncured coating film can be exerted.

[0042] The polyester can be made to have a glass transition temperature of 0°C or lower and a melting point of 80°C or lower or to be amorphous by, for example, copolymerizing a monomer component having a long-chain alkyl group or copolymerizing a monomer component having an asymmetric structure to destroy crystallinity.

[0043] <Polyisocyanate (B)>

[0044] The adhesive composition of the present invention contains a polyisocyanate (B). The polyisocyanate (B) used in the present invention is not particularly limited as long as it is an isocyanate compound that reacts with a polyester resin to be cured.

[0045] As polyisocyanate (B), aromatic or aliphatic diisocyanate compounds, trivalent or higher polyisocyanate compounds, etc. can be cited. These isocyanate compounds can be any of low molecular weight compounds and high molecular weight compounds. For example, aliphatic diisocyanates such as tetramethylene diisocyanate and hexamethylene diisocyanate, aromatic diisocyanates such as toluene diisocyanate, diphenylmethane diisocyanate, and benzyl diisocyanate, alicyclic diisocyanates such as hydrogenated diphenylmethane diisocyanate, hydrogenated benzyl diisocyanate, dimer acid diisocyanate, and isophorone diisocyanate, or trimers of these isocyanate compounds can be cited. In addition, compounds containing terminal isocyanate groups obtained by reacting excessive amounts of the above-mentioned isocyanate compounds with low molecular weight active hydrogen compounds such as ethylene glycol, propylene glycol, trimethylolpropane, glycerol, sorbitol, ethylenediamine, monoethanolamine, diethanolamine, and triethanolamine can be cited. Further, compounds containing terminal isocyanate groups obtained by reacting an excess of the above-mentioned isocyanate compounds with various polyester polyols, polyether polyols, and high molecular active hydrogen compounds of polyamides can be cited. These isocyanate compounds can be used alone or in combination of two or more. Among them, trimers of hexamethylene diisocyanate compounds are particularly preferred.

[0046] For the adhesive composition of the present invention, the content of the polyisocyanate (B) is preferably 0.1 to 10 parts by mass relative to a total of 100 parts by mass of the polyester (A1) and the polyester (A2). It is more preferably 5 parts by mass or less. In addition, it is more preferably 1 part by mass or more. By making the content of the polyisocyanate (B) within the above range, excellent peel strength at high temperature can be exerted.

[0047] Furthermore, in the present invention, inorganic flame retardants such as organic phosphorus compounds, zinc oxide, zinc sulfate, aluminum hydroxide, and barium hydroxide, leveling agents, and colorants such as dyes and pigments may be appropriately blended within a range that does not impair the properties of the adhesive composition of the present invention.

[0048] Example

[0049] Hereinafter, the present invention will be specifically described with reference to Examples. In the Examples and Comparative Examples, the abbreviation "part" means part by mass.

[0050] (1) Determination of polyester composition

[0051] Using 400MHz 1 The molar ratio of the polycarboxylic acid component and the polyol component constituting the polyester was quantitatively determined by H-nuclear magnetic resonance spectrometry (hereinafter sometimes referred to as NMR). Deuterated chloroform was used as a solvent. In addition, when the acid value of the polyester was increased by acid post-addition, the total amount of the acid components other than the acid components used for acid post-addition was set to 100 mol % to calculate the molar ratio of each component.

[0052] (2) Determination of glass transition temperature and melting point

[0053] The measurement was performed using a differential scanning calorimeter (DSC-200, SII Company). 5 mg of polyester was placed in an aluminum lid-type container and sealed, and cooled to -50°C using liquid nitrogen. Then, the temperature was raised to 150°C at a rate of 20°C / min. In the endothermic curve obtained during the heating process, the temperature of the intersection of the extension line of the baseline before the endothermic peak appeared (below the glass transition temperature) and the tangent line of the endothermic peak (the tangent line with the largest slope from the rising section of the peak to the peak apex) was taken as the glass transition temperature (Tg, unit: °C).

[0054] In the same endothermic curve, the temperature at the top of the crystal melting peak was taken as the melting point (Tm, unit: °C).

[0055] (3) Determination of number average molecular weight

[0056] The polyester sample was dissolved and / or diluted in tetrahydrofuran in such a way that the resin concentration was about 0.5% by weight, and filtered through a polytetrafluoroethylene membrane filter with a pore size of 0.5 μm as a sample for measurement. The molecular weight was determined by gel permeation chromatography (GPC) using tetrahydrofuran as the mobile phase and a differential refractometer as the detector. The flow rate was 1 mL / min and the column temperature was 30°C. The chromatographic columns used were KF-802, 804L, and 806L manufactured by Showa Denko. Monodisperse polystyrene was used as the molecular weight standard.

[0057] (4) Determination of acid value

[0058] 0.2 g of polyester sample was dissolved in 40 ml of chloroform and titrated with 0.01 N potassium hydroxide ethanol solution. 6 g polyester equivalent (eq / 10 6 g). Use phenolphthalein as an indicator.

[0059] Hereinafter, production examples of adhesive compositions containing the polyester of the present invention, polyester as a comparative example, and polyisocyanate are shown.

[0060] Production Example of Polyester (a1)

[0061] In a reaction vessel equipped with a stirrer, a condenser, and a thermometer, 359 parts of terephthalic acid, 58 parts of dimethyl 2,6-naphthalene dicarboxylate, 67 parts of ethylene glycol, 189 parts of propylene glycol, 5 parts of trimethylolpropane, and tetrabutyl orthotitanate as a catalyst in an amount of 0.03 mol% relative to the total acid components were added, and the temperature was raised from 160°C to 220°C over 4 hours, and an esterification reaction was carried out while passing through a dehydration process. Then, the system was depressurized to 5 mmHg over 20 minutes, and the temperature was further raised to 250°C to carry out a polycondensation reaction process. Then, the pressure was reduced to less than 0.3 mmHg, and after a polycondensation reaction for 60 minutes, it was taken out. As for the result of the composition analysis of the obtained polyester (a1) using NMR, the molar ratio was terephthalic acid / 2,6-naphthalene dicarboxylic acid / ethylene glycol / propylene glycol / trimethylolpropane=90 / 10 / 27 / 72 / 1 [molar ratio]. In addition, the glass transition temperature was 89°C. The results are recorded in Table 1.

[0062] Production Examples of Polyesters (a2) to (a11)

[0063] According to the manufacturing example of polyester (a1), the types and mixing ratios of raw materials were changed to synthesize polyesters (a2) to (a11). In addition, in polyester (a2), after the polymerization reaction was completed, ε-caprolactone was further added, reacted at 200°C for 30 minutes, and post-addition was carried out. In addition, in polyester (a3), after the polymerization reaction was completed, trimellitic anhydride was further added, reacted at 230°C for 30 minutes, and acid post-addition was carried out. The composition analysis values, melting points (Tm) and glass transition temperatures (Tg) of each polyester are recorded in Table 1. In addition, PTMG 1000 is polytetramethylene ether glycol (average molecular weight 1000). In addition, in Table 1, the situation where the melting point (Tm) cannot be observed is indicated as "-".

[0064]

[0065] Example 1

[0066] An adhesive composition was prepared by mixing 80 parts (solid content) of a polyester (a1) having a solid content concentration of 50% dissolved in toluene, 20 parts (solid content) of a polyester (a2) having a solid content concentration of 50% dissolved in toluene, and 2 parts of SUMIDUR N3300 (Sumidur N3300, manufactured by Sumika Covestro Urethane Co., Ltd.) as a polyisocyanate. The obtained adhesive composition was subjected to various evaluations of peel strength, wet solder heat resistance, and flexibility of an uncured coating film. The results are shown in Table 2.

[0067] Examples 2 to 14, Comparative Examples 1 to 4

[0068] According to Example 1, the types and mixing ratios of the raw materials were changed as shown in Table 2 to prepare adhesive compositions, and various evaluations were performed. The results are shown in Table 2.

[0069] Peel strength (adhesion)

[0070] The adhesive composition prepared in each of the above embodiments is applied to a polyimide film with a thickness of 12.5 μm (Apical (registered trademark) manufactured by Kaneka Co., Ltd.) in such a manner that the thickness after drying becomes 25 μm, and is dried at 140°C for 3 minutes. The adhesive film (B-stage product) thus obtained is bonded to a rolled copper foil with a thickness of 18 μm (BHY series manufactured by JX Metal Co., Ltd.). The bonding is performed by pressing at 160°C and a pressure of 2 MPa for 30 seconds in such a manner that the glossy surface of the rolled copper foil contacts the adhesive layer. Subsequently, it is cured by heat treatment at 170°C for 3 hours to obtain a sample for peel strength evaluation. For the peel strength, the film is pulled at 125°C, and a 180° peel test is performed at a tensile speed of 50 mm / min to measure the peel strength. This test indicates the bonding strength at 125°C.

[0071] <Evaluation Criteria>

[0072] ○: 0.3N / mm or more

[0073] △: 0.1N / mm or more and less than 0.3N / mm

[0074] ×: 0.1N / mm or less

[0075] Wet solder heat resistance

[0076] The sample was prepared in the same manner as for the peel strength evaluation, cut into 2.0 cm x 2.0 cm pieces, allowed to absorb moisture for 2 days at 40°C and 80% humidity, floated in a molten solder bath at 260°C, and the time until swelling occurred was measured.

[0077] <Evaluation Criteria>

[0078] ○: No swelling for more than 60 seconds

[0079] △: Swelling occurs within 30 seconds or more and less than 60 seconds

[0080] ×: Swelling occurs within 30 seconds

[0081] Softness of uncured coating film

[0082] The adhesive composition prepared in each of the above examples was applied to a polyimide film having a thickness of 12.5 μm (Apical (registered trademark) manufactured by Kaneka Corporation) so that the thickness after drying was 25 μm, and dried at 140° C. for 3 minutes. The adhesive film (B-stage product) thus obtained was bent at 90° to confirm whether cracks occurred in the coating film and evaluated.

[0083] <Evaluation Criteria>

[0084] ○: No cracks

[0085] △: There are creases

[0086] ×: Cracked

[0087] [Table 2]

[0088]

[0089] Industrial Applicability

[0090] The uncured coating film of the adhesive composition of the present invention is excellent in flexibility, wet solder heat resistance, and peel strength at high temperatures. Therefore, the adhesive composition is suitable for FPCs such as automotive FPCs that are exposed to high temperatures.

Claims

1. An adhesive composition comprising a polyester (A1) having a glass transition temperature or melting point higher than 80° C. and a polyisocyanate (B); wherein: When the adhesive composition does not contain the polyester (A2), the adhesive composition contains 0.1 to 10 parts by mass of the polyisocyanate (B) based on 100 parts by mass of the polyester (A1); when the adhesive composition contains the polyester (A2), the adhesive composition contains 0.1 to 10 parts by mass of the polyisocyanate (B) based on 100 parts by mass of the total amount of the polyester (A1) and the polyester (A2); The polyester (A2) has a glass transition temperature of 0°C or less and a melting point of 80°C or less or is amorphous; The polycarboxylic acid constituting the polyester (A1) is at least one selected from terephthalic acid, isophthalic acid, phthalic acid, naphthalene dicarboxylic acid, tetrahydrophthalic acid, methyltetrahydrophthalic acid, adipic acid, sebacic acid, dimer acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, fumaric acid, maleic acid, sodium dimethyl isophthalate-5-sulfonate, trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid, trimesic acid, 1,2,3,4-butanetetracarboxylic acid, and esters and anhydrides thereof; The polyol constituting the polyester (A1) is selected from ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 2-methyl-1,3-propylene glycol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1-methyl-1,8-octanediol, 2-methyl-2-ethyl-1,3-propylene glycol, 2,2-diethyl-1,3-propylene glycol, 2-ethyl-2-n-propyl ...,8-octanediol, 2-methyl-2-ethyl-1,3-propylene glycol, 2,2-diethyl-1,3-propylene glycol, 2-ethyl-2-n-propyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 2-methyl-2-ethyl-1,3-propylene glycol, 2,2-diethyl-1,3-propylene glycol, 2-ethyl-2-n-propyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 2-methyl-2-ethyl-1,3-propylene glycol, 2-methyl-2-ethyl-1,3-propylene glycol, 2-ethyl-2-n-propyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 2-methyl-2-ethyl-1,3 One or more of 1,3-propanediol, 2,2-di-n-propyl-1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, 2,4-diethyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 1,4-cyclohexanedimethanol, tricyclodecanedimethanol, polyalkylene ether glycol, glycerol, trimethylolpropane, trimethylolethane, pentaerythritol, α-methylglucose, mannitol, sorbitol, and dimer glycol. 2 . The adhesive composition according to claim 1 , wherein the polyol is at least one selected from the group consisting of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-cyclohexanedimethanol, and tricyclodecanedimethanol. 3 . The adhesive composition according to claim 1 , wherein the polycarboxylic acid is at least one selected from terephthalic acid and naphthalene dicarboxylic acid.

4. The adhesive composition according to claim 1, wherein The present invention contains a polyester (A2) having a glass transition temperature of -10°C or lower and a melting point of 80°C or lower or being amorphous.

5. The adhesive composition according to claim 4, wherein The content of the polyester (A2) is 10 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the polyester (A1). 6 . The adhesive composition according to claim 1 , which is used for a flexible printed wiring board.