Preparation of vacancy cerium oxide-loaded bimetallic nanoparticles and their application in electrocatalytic reduction of nitrates
Through the combination of vacant cerium oxide-loaded bimetallic nanoparticles and a dual electrode system, the safety and environmental pollution problems of nitrate treatment in the prior art are solved, and efficient and environmentally friendly nitrate removal effect is achieved, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202210893962.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-07-27
AI Technical Summary
The prior art has safety problems when dealing with nitrate pollution in water. For example, chemical catalysis requires hydrogen reducing agents and environmental pollution, biological denitrification method can produce bacterial pollution and residual sludge, electrochemical catalysis method is in energy shortage and Demand is increasing in the context of environmental pollution, and demand for green technologies is growing.
Using vacancies cerium oxide-supported bimetallic nanoparticles as catalytic reduction of nitrates, cerium hydroxide hydrothermal is generated by cerium salt and sodium hydroxide, and the vacant CeO2 support is prepared by calcining, and bimetals are loaded by chemical impregnation. Vacant cerium oxide supports bimetallic nanoparticles, combined with foam nickel cathode and ruthenium iridium titanium oxide anode to form a dual electrode system to perform electrocatalytic reduction of nitrate.
It has achieved nitrate removal with high catalytic activity, controllability, high product selectivity and good cycle stability. It is suitable for the removal of nitrate in water bodies, and is characterized by safety, environmental protection, low cost and suitable for industrial applications.
Smart Images

Figure CN115287693B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nitrate reduction, and in particular relates to the preparation of vacancy cerium oxide-loaded bimetallic nanoparticles and the application of the same in the electrocatalytic reduction of nitrates. Background Art
[0002] The nitrogen cycle on Earth has been maintaining a dynamic equilibrium state until it was disturbed by human activities. In recent decades, due to the extensive use of fertilizers and pesticides and the continuous discharge of chemical pollutants in industrial wastewater, the nitrate concentration in surface water and groundwater has exceeded the standard, leading to eutrophication of water bodies, reducing the available oxygen content for aquatic organisms, destroying aquatic ecosystems, and significantly reducing the proportion of freshwater suitable for drinking and agricultural use. When the freshwater system is not sufficient to buffer high concentrations of nitrate, nitrite will be generated through nitrate reductase in freshwater, resulting in the mass death of fish and other aquatic organisms. In addition, nitrate can also cause acute and chronic damage to human health. In the human body, nitrate will be reduced to nitrite, oxidizing the ferrous ions of hemoglobin to ferric ions, thereby inactivating the oxygen transport mechanism of red blood cells. At the same time, nitrite is also a precursor of potential carcinogens. The World Health Organization (WHO) recommends that the maximum concentration of nitrate in drinking water is 10 mg / L (in terms of N), while the maximum concentration of nitrite and ammonium ions is 0.03 mg / L and 0.4 mg / L (in terms of N).
[0003] At present, the treatment of nitrate mainly includes ion exchange, reverse osmosis, electrodialysis, chemical catalysis, electrochemical catalysis and biological denitrification. Among them, the chemical catalysis can convert nitrate into harmless nitrogen, but it needs to continuously introduce hydrogen into the system as a reducing agent, and its safety is problematic. The biological denitrification method uses microbial denitrification to remove nitrate, but it will cause bacterial contamination of drinking water and form residual sludge. The electrochemical catalysis method stands out among many methods due to its own advantages. It can not only use the electrode reduction process to treat nitrate, but also safely use the hydrogen generated by the cathode to selectively reduce nitrate to nitrogen, and has good application prospects. However, due to the increasingly prominent global energy shortage problem and the increasingly serious environmental pollution problem, the demand for green technology is increasing, and the use of electrocatalysis can convert nitrogen-containing pollutants into non-toxic and harmless N2, which meets the requirements of green development. Summary of the invention
[0004] In order to overcome the shortcomings of the above-mentioned prior art, the present invention provides a method for preparing vacant cerium oxide-loaded bimetallic nanoparticles. The prepared vacant cerium oxide-loaded bimetallic nanoparticles (also called bimetal-loaded vacant cerium oxide nanoparticles) are used as a catalytic material for the electrocatalytic reduction of nitrates. The particles have the advantages of high catalytic activity, good controllability, high product selectivity, good cycle stability, etc., and are suitable for the removal of nitrates in water bodies.
[0005] To achieve the above object, the present invention is implemented by the following technical solutions:
[0006] The present invention provides a method for preparing vacancy cerium oxide loaded bimetallic nanoparticles, firstly, cerium salt and sodium hydroxide are hydrothermally generated into cerium hydroxide, and then calcined in air to obtain CeO with different vacancies. 2 The carrier is then loaded with bimetallic materials by chemical impregnation to prepare vacancy cerium oxide loaded bimetallic nanoparticles.
[0007] As a preferred embodiment of the present invention, the method for preparing the above-mentioned vacancy cerium oxide-loaded bimetallic nanoparticles comprises the following steps:
[0008] S1, CeCl 3 7H 2 O and citric acid are dissolved in water to form a clear solution, and NaOH is added at room temperature for hydrothermal treatment, and the precipitate is collected, washed and dried to obtain a precursor powder;
[0009] S2. The precursor powder is calcined at 300-600°C for 3-5h to obtain CeO with different vacancies. 2 Carrier;
[0010] S3, CeO 2 The carrier is placed in a metal mixed solution of palladium salt and copper salt, the molar ratio of palladium in the palladium salt to copper in the copper salt is 1 to 4:1, stirred until a dry solid is obtained, and then calcined in air to obtain CeO loaded with metal oxide. 2 Carrier;
[0011] S4. Using excess NaBH 4 CeO loaded with metal oxides 2 After the support is completely reduced, vacancy cerium oxide-loaded bimetallic nanoparticles are obtained.
[0012] Preferably, in step S1, CeCl 3 7H 2 The molar ratio of O, citric acid and NaOH is 1:0.34:1.
[0013] Preferably, in step S1, the temperature of the hydrothermal treatment is 100-300°C and the time is 12-36h.
[0014] Preferably, in step S2, the palladium salt is selected from palladium chloride, the copper salt is selected from copper chloride, and the molar ratio of palladium in the palladium salt to copper in the copper salt is 3: 1. Of course, the palladium salt can also be selected from salts other than palladium chloride, and the copper salt can also be selected from salts other than copper chloride.
[0015] The vacancy cerium oxide has different vacancy contents according to different calcination temperatures. Preferably, in step S2, the calcination temperature is 450°C and the calcination time is 4 hours.
[0016] Preferably, in step S3, the calcination temperature is 300-500°C and the calcination time is 1-3h.
[0017] Preferably, step S4 is specifically: at room temperature, excess NaBH 4 The solution was slowly added dropwise to the CeO containing metal oxide under stirring. 2 The carrier solution was reacted for no less than 4 hours to make CeO 2 The vector was completely reduced.
[0018] The present invention also provides vacancy cerium oxide loaded bimetallic nanoparticles prepared by the above-mentioned preparation method.
[0019] The present invention also provides the use of the above-mentioned vacancy cerium oxide-loaded bimetallic nanoparticles in the electrocatalytic reduction of nitrates.
[0020] The present invention also provides a method for electrocatalytic reduction of nitrates, which uses nickel foam as a cathode and a ruthenium-iridium-titanium oxide electrode as an anode to form a double electrode system, and then places the double electrode system and the above-mentioned vacancy cerium oxide-loaded bimetallic nanoparticles together in a reaction solution containing nitrates, sodium sulfate and sodium chloride to electrocatalytically reduce the nitrates.
[0021] Preferably, the effective area of the nickel foam and ruthenium iridium titanium oxide electrode is 4 cm 2 .
[0022] Preferably, the working conditions of the dual electrode system are: the initial nitrate concentration is 20-50 mg / L (in terms of nitrogen), the initial pH is 3-11, the working current is 25-100 mA, the chloride ion concentration is 0-1000 mg / L, and the sodium sulfate concentration is not less than 0.02 mol / L.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The invention discloses a method for preparing vacant cerium oxide loaded bimetallic nanoparticles, wherein cerium hydroxide is firstly generated by hydrothermal reaction of cerium salt and sodium hydroxide, and then calcined in air to obtain a vacant cerium oxide carrier, and then a simple chemical impregnation method is used to load bimetallic to prepare vacant cerium oxide loaded bimetallic nanoparticles, which are denoted as M. 1 -M 2 / CeO 2 At the same time, a double electrode system is formed by using nickel foam as a cathode and a ruthenium iridium titanium oxide electrode as an anode. The double electrode system and the prepared vacancy cerium oxide-loaded bimetallic nanoparticles are directly added to a reaction solution (such as sewage) containing nitrate and sodium sulfate, and nitrate can be reduced by electrocatalysis. 1 -M 2 / CeO 2 The invention has the advantages of simple preparation, multiple adsorption active sites, high stability, high yield, etc.; the constructed dual-electrode system is easy to use, flexible in operation, and has low electrode cost, and is suitable for large-scale industrial applications; the vacant cerium oxide carrier-loaded bimetallic nanoparticles of the invention can utilize cathode hydrogen evolution to reduce nitrate, has high reduction activity for nitrate, high product selectivity, few reaction by-products, simple preparation process, low requirements for preparation conditions, and can be reused many times without the need for a complicated regeneration process. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 CeO 2 -450 and Pd–Cu / CeO 2 -450 XRD spectrum;
[0026] Figure 2 (a) CeO 2 -450 and Pd–Cu / CeO 2 -450 SEM image; Figure 2 (b) is the ESR test results of cerium oxide calcined at different temperatures;
[0027] Figure 3 is the removal rate of nitrate and total nitrogen by cerium oxide support at different calcination temperatures;
[0028] Figure 4 Pd–Cu / CeO with different bimetallic ratios 2 -450 for nitrate and total nitrogen removal;
[0029] Figure 5 Pd–Cu / CeO 2 -450 Product selection diagram and rate constant diagram for nitrate reduction under different chloride ion concentration conditions;
[0030] Figure 6 Pd–Cu / CeO2 -450 Product selection diagram for nitrate reduction under different current conditions;
[0031] Figure 7 Pd–Cu / CeO 2 -450 product selection diagram for reducing nitrates with different initial concentrations and the amount of nitrogen removed per unit mass of catalyst;
[0032] Figure 8 Pd–Cu / CeO 2 -450Product selection diagram for nitrate reduction under different initial reaction pH conditions;
[0033] Fig. 9 Pd–Cu / CeO 2 Cyclic stability of the -450 catalyst for nitrate reduction. DETAILED DESCRIPTION
[0034] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0035] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0036] Example 1 Preparation of vacant cerium oxide-loaded bimetallic nanoparticles at different calcination temperatures
[0037] The specific preparation method comprises the following steps:
[0038] (1) CeCl 3 7H 2 O and citric acid were dissolved in deionized water, CeCl 3 7H 2 O: water in a molar ratio of 1:25 to form a clear solution, then NaOH was added at room temperature and magnetic stirring was performed for 30 min. 3 7H 2 O: The molar ratio of citric acid: NaOH is 1:0.34:1. Subsequently, the mixture is transferred to an autoclave and hydrothermally treated at 200°C for 24 hours. After cooling to room temperature, the precipitate is collected by filtration and washed three times with anhydrous ethanol and deionized water respectively. The product is placed in an oven and stored at 80°C for 12 hours until dry to obtain a precursor powder.
[0039] (2) The precursor powder was calcined in a muffle furnace for 4 hours. CeO with different vacancies was obtained at different calcination temperatures (350, 450, 550, 650 °C). 2 The carrier is denoted as CeO 2 -350, CeO 2 -450, CeO 2 -550, CeO 2 -650;
[0040] (3) A catalyst with a molar ratio of Pd:Cu of 3:1 was prepared by impregnation. 2 The carrier was poured into a metal mixed solution of palladium chloride and copper chloride (solvent was water) and vigorously stirred with a magnetic stirrer at 80°C until a dry solid was obtained. Subsequently, the obtained solid powder was calcined in air at 400°C for 2 hours to load the metal oxide on CeO 2 On the support, CeO loaded with metal oxides was obtained. 2 carrier.
[0041] (4) At room temperature, 0.5 mol / L NaBH 4 The solution (solvent is water) is slowly added dropwise to the CeO containing metal oxide under a magnetic stirrer. 2 The carrier was reacted in a small amount of aqueous solution (no more than 2 ml) for 4 h, wherein NaBH 4 :CeO 2 The molar ratio of the carrier was 10:1, so that the catalyst was completely reduced. The reduced powder was then filtered and rinsed three times with deionized water to remove the residual chemicals, and the 350-650°C calcined vacancy cerium oxide-supported bimetallic nanoparticles were prepared, which were denoted as Pd-Cu / CeO 2 -350, Pd-Cu / CeO 2 -450, Pd-Cu / CeO 2 -550, Pd-Cu / CeO 2 -650, and finally dried in a vacuum oven at 60 °C for 24 h and stored in a nitrogen desiccator at room temperature.
[0042] The prepared CeO 2 -450 and Pd–Cu / CeO 2 -450 for X-ray powder diffraction (XRD) test, the test instrument is: Bruker D8. The test conditions are: scanning range between 20 and 80 degrees, scanning speed is 10 degrees / min. The test results are as follows Figure 1 shown.
[0043] from Figure 1 It can be seen that the measured XRD results are consistent with the standard card (CeO 2: JCPDS 43-1002), no new characteristic peaks appeared after Pd and Cu loading, probably because the particles were too small. However, the appearance of the characteristic peaks of cerium oxide proved the successful synthesis of cerium oxide.
[0044] The vacant cerium oxide loaded bimetallic nanoparticles (Pd-Cu / CeO 2 -350, Pd-Cu / CeO 2 -450, Pd-Cu / CeO 2 -550, Pd-Cu / CeO 2 -650) as an example to conduct scanning electron microscope test and EPR test. Among them, the instrument used for scanning electron microscope test is: Quanta FEG 450. The test conditions are: the material is evenly loaded on the conductive glue, and the test is carried out at room temperature after gold spraying. The instrument used for EPR test is: Bruker A300. The test conditions are: use 1.0g standard modulation amplitude for testing. The results of scanning electron microscope test and ESR test are shown as follows: Figure 2 (a) and Figure 2 (b) as shown.
[0045] from Figure 2 As can be seen from (a), the particle size of the obtained cerium oxide particles is about 10 to 20 nm; Figure 2 (b) It can be seen that the CeO obtained in Example 1 2 The vacancies of the catalyst vary with the temperature, among which CeO 2 -450 The vacancy signal is stronger.
[0046] At the same time, nickel foam was used as the cathode, and the ruthenium iridium titanium oxide electrode (effective area of 4 cm 2 ) as the anode to form a double electrode system, and then the double electrode system and vacancy cerium oxide loaded bimetallic nanoparticles (added in an amount of 50 mg / L) are placed together in an aqueous solution containing nitrate, sodium sulfate and sodium chloride, the initial nitrate concentration is 40 mg / L (in terms of nitrogen), the initial pH is 7, the working current is 50 mA, the chloride ion concentration is 500 mg / L, the sodium sulfate concentration is 0.02 mol / L, after the electrocatalytic reduction of nitrate, the nitrogen-containing anions are tested by ion chromatography, the model is ICS-600, and the analytical column is AS23 4×250 mm; and the ammonia nitrogen is tested by ultraviolet-visible spectrophotometer, and the test method is standard colorimetry.
[0047] Figure 3 The vacant cerium oxide-loaded bimetallic nanoparticles (Pd-Cu / CeO 2 -350, Pd-Cu / CeO 2 -450, Pd-Cu / CeO2 -550, Pd-Cu / CeO 2 -650) for nitrate and total nitrogen removal. It can be seen that with the increase of calcination temperature, the nitrate reduction ability decreases and reaches the maximum value at 450℃. 2 -450 has the highest nitrate reduction performance and total nitrogen removal rate.
[0048] Example 2 Preparation of vacant cerium oxide loaded bimetallic nanoparticles at different bimetallic ratios
[0049] Steps (1) and (4) are the same as those in Example 1, except that step (2) is to calcine the precursor powder in a muffle furnace for 4 hours at 450°C to obtain CeO 2 Carrier; Step (3) is different in that: samples with different bimetallic ratios (molar ratios of Pd:Cu are 1:1, 2:1, 3:1, 4:1, 0:1, 1:0) are loaded by impregnation method, and are denoted as Pd 1 -Cu 1 / CeO 2 , Pd 2 -Cu 1 / CeO 2 , Pd 3 -Cu 1 / CeO 2 , Pd 4 -Cu 1 / CeO 2 ,Pd / CeO 2 ,Cu / CeO 2 The vacancy cerium oxide-loaded bimetallic nanoparticles prepared were named Pd 1 -Cu 1 / CeO 2 , Pd 2 -Cu 1 / CeO 2 , Pd 3 -Cu 1 / CeO 2 , Pd 4 -Cu 1 / CeO 2 ,Pd / CeO 2 ,Cu / CeO 2 .
[0050] Figure 4 The vacant cerium oxide-loaded bimetallic nanoparticles (Pd 1 -Cu 1 / CeO 2 , Pd 2 -Cu1 / CeO 2 , Pd 3 -Cu 1 / CeO 2 , Pd 4 -Cu 1 / CeO 2 ,Pd / CeO 2 ,Cu / CeO 2 ) for nitrate and total nitrogen removal rates. It can be seen that when only a single metal exists, the removal rate is not ideal. When the two metals work together, the nitrate removal rate is improved. Combined with the total nitrogen removal rate, it can be seen that when Pd:Cu=3:1, the sample has the best total nitrogen removal rate, that is, nitrogen selectivity. Therefore, Pd 3 -Cu 1 / CeO 2 Has the best nitrate and total nitrogen removal performance.
[0051] Figure 5 Pd 3 -Cu 1 / CeO 2 -450 product selection diagram and rate constant diagram for nitrate reduction under different chloride ion concentration conditions. It can be seen that as Cl - As the concentration increases, the nitrogen content in the final product increases, that is, the nitrogen selectivity increases, and excessive Cl - The dosage will lead to an increase in reaction by-products, which is not conducive to the impact on the environment. Therefore, 500 mg / L Cl - The dosage is more appropriate.
[0052] Figure 6 Pd 3 -Cu 1 / CeO 2 -450 Product selection diagram of nitrate reduction under different current conditions. It can be seen that as the current increases, the amount of hydrogen released at the cathode increases, the amount of adsorbed hydrogen that can be used also increases, and the reduction performance increases, but it is accompanied by an increase in energy consumption. Therefore, a higher nitrate reduction activity and total nitrogen removal rate can be achieved under a current of 50mA.
[0053] Figure 7 Pd 3 -Cu 1 / CeO 2 The product selection diagram of the reduction of nitrate with different initial concentrations at -450 and the denitrification amount of catalyst per unit mass. It can be seen that when the nitrate concentration increases, nitrite appears in the final product, while higher concentrations of nitrate remain in the solution, which also shows that nitrite, as an intermediate product of the reaction, can be converted into the next reaction product as the reaction time increases. However, the catalytic sample has a low reaction rate for 50 mg / L NO3 The removal rate of —N still reaches 80%, and the denitrification amount per unit mass of catalyst increases with the increase of concentration, indicating that the sample has a strong denitrification ability.
[0054] Figure 8 Pd 3 -Cu 1 / CeO 2 -450 product selection diagram of nitrate reduction under different initial reaction pH conditions. It can be seen that when pH = 3, some ammonia nitrogen accumulates, but when it is in alkaline conditions, the performance of the sample can still be maintained.
[0055] Fig. 9 Pd 3 -Cu 1 / CeO 2 -450 Cyclic stability of nitrate reduction. It can be seen that after 4 cycles, the catalyst still maintains excellent nitrate reduction ability and high selectivity for nitrogen.
[0056] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. An application of vacancy cerium oxide-loaded bimetallic nanoparticles in electrocatalytic reduction of nitrates, characterized in that: The vacancy cerium oxide loaded bimetallic nanoparticles are prepared by firstly using cerium salt and sodium hydroxide to generate cerium hydroxide by hydrothermal method, then calcining in air to obtain CeO2 carriers with different vacancies, and finally loading bimetallic by chemical impregnation method. The method for preparing vacancy cerium oxide-loaded bimetallic nanoparticles specifically comprises the following steps: S1. CeCl3·7H2O and citric acid are dissolved in water to form a clear solution, and NaOH is added at room temperature for hydrothermal treatment. The precipitate is collected, washed and dried to obtain a precursor powder; S2, calcining the precursor powder at 300-600°C for 3-5h to obtain CeO2 carriers with different vacancies; S3, placing the CeO2 carrier in a metal mixed solution of palladium salt and copper salt, wherein the molar ratio of palladium in the palladium salt to copper in the copper salt is 1 to 4:1, stirring until a dry solid is obtained, and then calcining in air to obtain a CeO2 carrier loaded with metal oxide; S4, using excess NaBH4 to completely reduce the CeO2 carrier loaded with metal oxides to obtain vacant cerium oxide-loaded bimetallic nanoparticles; The method for electrocatalytic reduction of nitrate is: using nickel foam as a cathode and a ruthenium-iridium-titanium oxide electrode as an anode to form a double electrode system, and then placing the double electrode system and the vacancy cerium oxide-loaded bimetallic nanoparticles in a reaction solution containing nitrate, sodium sulfate and sodium chloride to electrocatalytically reduce the nitrate.
2. The use according to claim 1, characterized in that: In step S1, the molar ratio of CeCl3·7H2O, citric acid and NaOH is 1:0.34:
1.
3. The use according to claim 1, characterized in that: In step S1, the temperature of the hydrothermal treatment is 100-300°C and the time is 12-36 hours.
4. The use according to claim 1, characterized in that: In step S2, the palladium salt is selected from palladium chloride, the copper salt is selected from copper chloride, and the molar ratio of palladium in the palladium salt to copper in the copper salt is 3:
1.
5. The use according to claim 1, characterized in that: In step S2, the calcination temperature is 450°C and the calcination time is 4 hours.
6. The use according to claim 1, characterized in that: In step S3, the calcination temperature is 300-500°C and the calcination time is 1-3h.