Preparation method of Ga2O3-based heterogeneous integrated pn junction

Through ion beam stripping and transfer technology and homoepitaxial process, a high-quality Ga2O3-based heteropn junction is formed, which solves the p-type doping difficulties and limited electrical performance of Ga2O3 materials, and expands its application in the field of bipolar devices. application.

CN115295404BActive Publication Date: 2024-10-18SHANGHAI INST OF MICROSYSTEM & INFORMATION TECH CHINESE ACAD OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210943233.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-08
Publication Date
2024-10-18
Estimated Expiration
2042-08-08

AI Technical Summary

Technical Problem

The difficulty of p-type doping of Ga2O3 materials and the limited electrical performance after heterogeneous integration of n-type Ga2O3 and p-type semiconductor materials limit the application of Ga2O3 materials in the field of bipolar devices.

Method used

Using ion beam lift-off and transfer technology, the n-type Ga2O3 wafer and the p-type semiconductor wafer are transferred through fracture peeling and bonding after annealing, and a Ga2O3-based heteropn junction is formed through homoepitaxial growth and metal deposition.

Benefits of technology

It achieves a high-quality pn junction, improves the electrical performance, expands the application scope of Ga2O3 materials in the field of bipolar devices, and solves the problems of difficult p-type doping and limited electrical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115295404B_ABST
    Figure CN115295404B_ABST
Patent Text Reader

Abstract

The present invention provides a preparation method of a Ga2O3-based heterogeneous integrated pn junction, which comprises taking at least one of an n-type Ga2O3 wafer and a p-type semiconductor wafer as a material to be stripped, performing ion implantation from the polished surface of the material to be stripped to form a defect layer; bonding the n-type Ga2O3 wafer to the polished surface of the p-type semiconductor wafer; annealing and stripping along the defect layer, removing the surface damage layer, performing homogeneous epitaxy, performing metal deposition and annealing. The preparation method of the present invention transfers the n-type Ga2O3 to the p-type semiconductor wafer through ion beam stripping and transfer and epitaxy processes, solves the problem of difficulty in p-type doping of Ga2O3 materials in the prior art, and the problem of limited electrical performance after heterogeneous integration of n-type Ga2O3 materials and p-type semiconductor materials, which is of great significance to the application of Ga2O3 materials in the field of bipolar devices and greatly expands the application range of Ga2O3 materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of semiconductor materials, and specifically relates to a method for preparing a Ga2O3-based heterogeneous integrated pn junction. Background Art

[0002] Ga2O3 is a very attractive wide bandgap semiconductor material with a bandgap width of 4.6 to 4.9 eV, which is more than 4 times that of Si and much higher than SiC, GaN and other wide bandgap semiconductor materials. This makes it have a breakdown electric field strength of up to 8MV / cm and a Baliga figure of merit of up to 3444. Therefore, devices developed based on Ga2O3 will have smaller conduction losses, higher power conversion efficiency and higher withstand voltage. In addition, the ability to produce large-size, low-cost, high-quality Ga2O3 wafers through the pulling method is also one of its advantages, which makes Ga2O3 have a very broad application prospect in the fields of new energy power generation and high-voltage transmission systems that require high-power and high-voltage devices.

[0003] However, due to the lack of suitable shallow acceptors and the large effective mass of holes and low mobility caused by the flat top of the valence band, p-type doping of Ga2O3 is still a problem. This makes it difficult to realize bipolar devices based on Ga2O3, which greatly limits the application of Ga2O3 materials. The p-type doping of Si, the most widely used semiconductor material, and GaN, SiC, and diamond, which are also wide-bandgap semiconductor materials, is relatively mature. By heterogeneously integrating n-type Ga2O3 with p-type semiconductor materials to form a Ga2O3-based heterogeneous pn junction, the application range of Ga2O3 materials can be greatly expanded.

[0004] At present, the methods to achieve heterogeneous integration of n-type Ga2O3 and p-type semiconductor materials are mainly based on epitaxy and tape stripping. Due to the thermal mismatch and lattice mismatch between the materials, the quality of the n-type Ga2O3 layer grown by the epitaxy method is difficult to control. On the one hand, the mechanical stripping method may have a certain degree of warping because the peeled film may have a certain degree of warping. The mechanical stripping method mainly relies on van der Waals force for bonding. Therefore, the heterogeneous pn junction interface prepared by the mechanical stripping method is not tightly bonded, which affects the electrical performance of the device. At the same time, this method is difficult to achieve the preparation of wafer-level structures and is difficult to apply on a large scale.

[0005] Based on this, it is necessary to provide a method for preparing a Ga2O3-based heterogeneous integrated pn junction. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a Ga2O3-based heterogeneous integrated pn junction to solve the problem in the prior art that p-type doping of Ga2O3 materials is difficult and the electrical performance is limited after heterogeneous integration of n-type Ga2O3 materials and p-type semiconductor materials.

[0007] In order to achieve the above object, the present invention provides a method for preparing a Ga2O3-based heterogeneous integrated pn junction, comprising:

[0008] S1: providing an n-type Ga2O3 wafer, wherein one surface of the n-type Ga2O3 wafer is a polished surface;

[0009] S2: providing a p-type semiconductor wafer, wherein one surface of the p-type semiconductor wafer is a polished surface;

[0010] S3: using at least one of the n-type Ga2O3 wafer and the p-type semiconductor wafer as a material to be stripped, and performing ion implantation from a polished surface of the material to be stripped to form a defect layer in the material to be stripped;

[0011] S4: bonding the polished surface of the n-type Ga2O3 wafer to the polished surface of the p-type semiconductor wafer to prepare a first composite structure;

[0012] S5: performing annealing treatment on the first composite structure, and stripping the material to be stripped along the defective layer to form a second composite structure with a surface damage layer;

[0013] S6: performing surface treatment on the second composite structure with the surface damage layer to remove the surface damage layer to form a third composite structure;

[0014] S7: performing homoepitaxial growth on the third composite structure to grow an epitaxial layer of the peeled material to form a fourth composite structure;

[0015] S8: performing metal deposition and annealing on both side surfaces of the fourth composite structure to prepare ohmic electrodes and form a Ga2O3-based heterogeneous pn junction.

[0016] The n-type gallium oxide wafer includes one of an α-Ga2O3 wafer, a β-Ga2O3 wafer, a γ-Ga2O3 wafer, a δ-Ga2O3 wafer and an ε-Ga2O3 wafer.

[0017] The p-type semiconductor wafer includes one of a silicon wafer, a silicon carbide wafer, a diamond wafer and a gallium nitride wafer.

[0018] In step S3, the ion implantation includes one or more of H ion implantation and He ion implantation; the energy of the ion implantation is 10 keV to 200 keV, and the dose is 1×10 16 ions / cm 2 ~1×10 18 ions / cm 2 , the temperature is 20℃~200℃.

[0019] In step S4, the bonding method includes one of surface activated bonding, metal bonding, hydrophilic bonding and anodic bonding; the bonding vacuum degree is 1×10 -7 Pa~5×10 -5 Pa, pressure is 10MPa~500MPa, and temperature is room temperature.

[0020] In the step S5, the first composite structure is annealed in an atmosphere of at least one of vacuum, nitrogen, oxygen, and inert gas, with an annealing temperature of 200° C. to 1000° C. and an annealing time of 1 min to 72 h.

[0021] In the step S8, annealing is performed in an atmosphere formed by at least one of vacuum, nitrogen, oxygen, and inert gas, the annealing temperature is 200° C. to 1000° C., and the annealing time is 30 seconds to 1 hour.

[0022] In step S6, the surface treatment method includes one or more combinations of mechanical grinding, chemical mechanical polishing, dry etching, and wet etching.

[0023] In step S7, the homoepitaxial growth method includes one or more combinations of vapor phase epitaxy, chemical vapor deposition, molecular beam epitaxy, and pulsed laser deposition.

[0024] In step S7, when the epitaxy method is vapor phase epitaxy, the growth temperature is 800-1000° C., the Ga source used is GaCl with a partial pressure of 20-200 Pa, the O source includes one or more combinations of O2, ozone, oxygen plasma and air, and the carrier gas is one or more combinations of N2 or Ar;

[0025] When the epitaxial method is chemical vapor deposition, the growth temperature is 500-1100°C, the Ga source is high-purity Ga, triethylgallium or gallium acetylacetonate, the O source is O2 or a mixture of O2 and water vapor, the carrier gas is a combination of one or more of Ar, He, and N2, and the growth chamber pressure is 1-100 Torr;

[0026] When the epitaxy method is molecular beam epitaxy, the growth temperature is 600-900°C, the Ga source is high-purity Ga, the O source includes one or more combinations of O2, ozone, and oxygen plasma, the doping source includes one or more combinations of Sn, Si, Mg, Fe, Ge, Al, and In, and the Ga beam equivalent pressure is 5×10 -9 Torr~2×10 -6 Torr;

[0027] When the epitaxial growth method is pulsed laser deposition, the substrate temperature is 400-600°C, the deposition atmosphere is a combination of O2 and Ar, where O2 accounts for 1-20%, and the growth pressure is 1×10 -3 Pa~2Pa, laser power density is 1~10J / cm 2 .

[0028] In step S8, the ohmic electrode is a metal stack formed by a combination of one or more of Ti, Al, Ni, Pt, and Au; the metal deposition method includes a combination of one or more of evaporation, sputtering, and stripping.

[0029] The preparation method of the Ga2O3-based heterogeneous integrated pn junction of the present invention uses ion beam stripping and transfer and epitaxial processes to strip n-type Ga2O3 wafers and / or p-type semiconductor wafers by fracture after annealing and transfer them by bonding, and deposit metal electrodes to obtain a pn junction with good electrical properties. This solves the problem of difficulty in p-type doping of Ga2O3 materials in the prior art and limited electrical properties after heterogeneous integration of n-type Ga2O3 materials and p-type semiconductor materials. This is of great significance to the application of Ga2O3 materials in the field of bipolar devices and greatly expands the application range of Ga2O3 materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Shown is a process flow chart for preparing a Ga2O3-based heterogeneous pn junction according to the present invention.

[0031] Figure 2 Shown is a schematic diagram of the structure of the n-type Ga2O3 wafer provided in Example 1 of the present invention.

[0032] Figure 3 Shown is a schematic structural diagram of a p-type semiconductor wafer provided in Embodiment 1 of the present invention.

[0033] Figure 4 It is a schematic diagram of the structure of forming a defect layer by ion implantation into an n-type Ga2O3 wafer in the first embodiment of the present invention.

[0034] Figure 5 It is a schematic diagram of the structure after preparing the first composite structure in Example 1 of the present invention.

[0035] Figure 6 It is a schematic diagram of the structure of the second composite structure formed after annealing treatment in the first embodiment of the present invention.

[0036] Figure 7 It is a schematic structural diagram of a third composite structure formed after surface treatment in the first embodiment of the present invention.

[0037] Figure 8It is a schematic structural diagram of a fourth composite structure formed after epitaxy in the first embodiment of the present invention.

[0038] Fig. 9 It shows a schematic structural diagram of a Ga2O3-based heterogeneous pn junction formed in the first embodiment of the present invention.

[0039] Fig.10 It is a schematic structural diagram of forming a defect layer by ion implantation into a p-type semiconductor wafer in the second embodiment of the present invention.

[0040] Fig.11 It is a schematic diagram of the structure after preparing the first composite structure in Example 2 of the present invention.

[0041] Fig.12 It is a schematic diagram of the structure of the second composite structure formed after annealing in the second embodiment of the present invention.

[0042] Fig.13 It is a schematic structural diagram of a third composite structure formed after surface treatment in the second embodiment of the present invention.

[0043] Fig.14 It is a schematic structural diagram of a fourth composite structure formed after epitaxy in the second embodiment of the present invention.

[0044] Fig.15 It shows a schematic structural diagram of a Ga2O3-based heterogeneous pn junction formed in the second embodiment of the present invention.

[0045] Reference numerals

[0046] 100, 110: n-type Ga2O3 wafer;

[0047] 100a, 110a: polished surfaces of n-type Ga2O3 wafers;

[0048] 200, 210: p-type semiconductor wafer;

[0049] 200a, 210a: polished surface of a p-type semiconductor wafer;

[0050] 300, 310: defective layer;

[0051] 400, 410: surface damage layer;

[0052] 500: n-type Ga2O3 epitaxial layer;

[0053] 510: p-type semiconductor epitaxial layer;

[0054] 600, 610: Ohmic electrodes. DETAILED DESCRIPTION

[0055] The present invention is further described below in conjunction with specific examples. It should be understood that the following examples are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0056] Example 1 A method for preparing a Ga2O3-based heterogeneous integrated pn junction

[0057] like Figure 1 The method for preparing a Ga2O3-based heterogeneous integrated pn junction according to the first embodiment of the present invention comprises the following steps:

[0058] Step S1: See Figure 2 , providing an n-type Ga2O3 wafer 100, wherein one surface of the n-type Ga2O3 wafer is a polished surface 100a;

[0059] As an example, the n-type Ga2O3 wafer 100 may include one of an α-Ga2O3 wafer, a β-Ga2O3 wafer, a γ-Ga2O3 wafer, a δ-Ga2O3 wafer, and an ε-Ga2O3 wafer.

[0060] Specifically, the size of the n-type Ga2O3 wafer 100 can be selected as needed, such as the wafer diameter of the n-type Ga2O3 wafer 100 can include 2 inches to 12 inches. The surface orientation of the n-type Ga2O3 wafer 100 can include one of (001), (010) and (-201). The surface roughness of the polished surface 100a of the n-type Ga2O3 wafer 100 should be less than 1nm, such as 0.5nm, 0.3nm, etc. The impurity types of the n-type Ga2O3 wafer 100 include Si, Sn, Ge, etc., and the doping concentration is 1×10 10 cm -3 ~1×10 21 cm -3 , you can choose according to your needs.

[0061] Step S2: See Figure 3 , providing a p-type semiconductor wafer 200, wherein one surface of the p-type semiconductor wafer is a polished surface 200a;

[0062] As an example, the p-type semiconductor wafer 200 may include one of a silicon wafer, a silicon carbide wafer, a diamond wafer, and a gallium nitride wafer.

[0063] Specifically, the size of the p-type semiconductor wafer 200 can be selected as needed. For example, the wafer diameter of the p-type semiconductor wafer 200 may include 2 inches to 12 inches. The surface roughness of the polished surface 200a of the p-type semiconductor wafer 200 should be less than 1 nm, such as 0.5 nm, 0.3 nm, etc. The doping concentration of the p-type semiconductor wafer 200 is 1×10 10 cm-3 ~1×10 21 cm -3 , which can be selected according to needs. The type of the p-type semiconductor wafer 200 is not limited to the silicon wafer, silicon carbide wafer, diamond wafer, gallium nitride wafer, and can also be other semiconductor materials that can achieve p-type doping. Depending on the material of the p-type semiconductor wafer 200, the impurities doped therein are also different. For example, the more common doping impurities in Si, SiC, and diamond are Al, B, Ga, etc., and the doping impurities in GaN are Mg, etc.

[0064] Step S3: See Figure 4 , using an n-type Ga2O3 wafer 100 as a material to be stripped, and performing ion implantation from a polished surface of the material to be stripped (i.e., a polished surface 100a of the n-type Ga2O3 wafer 100), thereby forming a defect layer 300 in the material to be stripped;

[0065] There is no particular requirement for the thickness of the p-type semiconductor wafer 200. The thickness of the currently used thickness is generally 10-1000 μm. The thickness of the defect layer 300 is 20-100 nm.

[0066] As an example, the ion implantation includes a combination of one or more of H ion implantation and He ion implantation.

[0067] As an example, the energy of the ion implantation is 10 keV to 200 keV, and the dose is 1×10 16 ions / cm 2 ~1×10 18 ions / cm 2 , the temperature is 20℃~200℃.

[0068] Specifically, Figure 4 The arrow in indicates the direction of ion implantation. In the example, a single type of ion implantation may be performed from the polished surface 100a of the n-type Ga2O3 wafer 100, which may include H ion implantation or He ion implantation. When the implanted ions are H ions, the H ions may damage the lattice at a preset depth of the n-type Ga2O3 wafer 100, forming the defect layer 300, and realizing peeling in the subsequent annealing process, wherein the depth of the defect layer 300 is determined by the energy of the ion implantation, and whether the defect density required for separation can be formed is determined by the dose of the ion implantation. After the ion implantation, the defect layer 300, on the one hand, causes lattice distortion due to the addition of the implanted ions, and on the other hand, the ions collide with the original lattice during the implantation process, causing a certain amount of atomic displacement, wherein the former is the main formation factor of the defect layer 300.

[0069] The calculation formula of the depth of the defect layer and the energy of ion implantation is:

[0070]

[0071] Where E0 is the implantation energy, N is the ion concentration, Sn(E) is the nuclear energy loss, Se(E) is the electronic energy loss, and R p is the depth where the ion concentration is maximum.

[0072] When the implanted ions are He ions, the He ions will form the defect layer 300 at a preset depth of the n-type Ga2O3 wafer. The He ions are captured by the defect layer 300 to form defect clusters. In the subsequent annealing process, part of the n-type Ga2O3 wafer 100 can be peeled off from the location with the maximum defect concentration.

[0073] In another example, two types of ions may be co-implanted from the polished surface 100a of the gallium oxide single crystal wafer, that is, the implanted ions are a combination of H ions and He ions, wherein the H ions may be used to form defects as described above, and the He ions may be captured by the defects formed by the H ions, generating additional pressure, so that the defect clusters continue to expand and combine with each other to form cracks that can be used for the stripping of the n-type Ga2O3 wafer 100, which can effectively promote the stripping of part of the n-type Ga2O3 wafer 100 under the condition of low ion implantation dose, and can effectively reduce the total ion implantation dose (when H ions are used, the dose is 1×10 16 -1×10 18 ions / cm 2 , He ion, the dose is 1×10 15 -1×10 17 ions / cm 2 When H and He are co-injected, the H dose is 5×10 15 -5×10 17 ions / cm 2 , He dose is 5×10 14 -5×10 16 ions / cm 2 ), shortening the total process time and improving efficiency. The energy of the ion implantation can be 10keV, 50keV, 100keV, 150keV, 200keV, etc., and the dose can be 1×10 16 ions / cm 2 , 5×10 16 ions / cm 2 , 1×10 17 ions / cm 2 , 5×10 17 ions / cm 2 , 1×10 18 ions / cm 2The temperature may be 20° C., 50° C., 100° C., 150° C., 200° C., etc. The type, energy, dosage, and temperature of the implanted ions may be selected as required and are not excessively limited herein.

[0074] The injected ions are mainly concentrated in the defect layer 300 and are Gaussian distributed. The injected ions retained in the area between the defect layer 300 and the polished surface 100a are basically negligible. The area between the defect layer 300 and the polished surface 100a, i.e. the thin film subsequently peeled off, can still maintain its lattice intact.

[0075] In addition, in other embodiments, the p-type semiconductor wafer 200 may be used as the material to be stripped and ion implanted into its polished surface, or both the n-type Ga2O3 wafer 100 and the p-type semiconductor wafer 200 may be ion implanted into their polished surfaces. However, when both the n-type Ga2O3 wafer 100 and the p-type semiconductor wafer 200 are ion implanted, the overall thickness is small during subsequent stripping, and the manufacturing difficulty is high.

[0076] Step S4: See Figure 5 , bonding the polished surface of the n-type Ga2O3 wafer 100 (which has been ion-implanted in this embodiment) to the polished surface of the p-type semiconductor wafer 200 (which has not been ion-implanted in this embodiment) to prepare a first composite structure;

[0077] As an example, the bonding method includes one of surface activated bonding, metal bonding, hydrophilic bonding and anodic bonding.

[0078] As an example, the bonding vacuum is 1×10 -7 Pa~5×10 -5 Pa, pressure is 10MPa~500MPa, and temperature is room temperature.

[0079] Specifically, the bonding vacuum degree may be 1×10 -7 Pa, 2×10 -6 Pa, 5×10 -5 Pa, etc., the pressure can be 10MPa, 100MPa, 500MPa, etc., and can be selected according to needs. Through the bonding, the n-type Ga2O3 wafer 100 and the p-type semiconductor wafer 200 can be bonded relatively well to achieve heterogeneous integration.

[0080] Step S5: See Figure 6 , performing annealing treatment on the first composite structure, stripping the material to be stripped along the defective layer 300, and forming a second composite structure with a surface damage layer 400;

[0081] The surface damaged layer 400 is the defective layer left after peeling. In this embodiment, the second composite structure includes the p-type semiconductor wafer 200, the n-type Ga2O3 wafer 100 and the surface damaged layer 400 stacked in sequence.

[0082] As an example, the first composite structure is annealed in an atmosphere formed by at least one of vacuum, nitrogen, oxygen, and inert gas, with an annealing temperature of 200°C to 1000°C and an annealing time of 1 min to 72 h. The annealing temperature may be 200°C, 400°C, 600°C, 800°C, 1000°C, etc., and the annealing time may be 1 min, 30 min, 1 h, 24 h, 48 h, 72 h, etc., which may be selected according to needs.

[0083] Compared with the existing mechanical stripping method, the ion stripping transfer method of the present invention is different from the conventional mechanical stripping method in that, on the one hand, the mechanical stripping method has a limited bonding area due to the fact that the stripped film may have a certain warping, and it is more difficult to control the surface flatness and warping than bonding the entire wafer in the ion stripping transfer. On the other hand, the mechanical stripping method mainly relies on van der Waals forces for bonding, while the bonding methods used in the ion stripping transfer method, such as surface activated bonding, hydrophilic bonding, etc., form chemical bonds, which are more tightly bonded.

[0084] Currently, the mechanical stripping process uses van der Waals forces for direct bonding without using a specific bonding method. Adding bonding may strengthen the bonding to a certain extent, but it still does not change the problem that it cannot prepare wafer-level structures. In addition, the mechanical stripping process is more difficult to control than the ion stripping transfer parameters, which is also a reason why it is difficult to achieve large-scale application.

[0085] Step S6: See Figure 7 , performing surface treatment on the second composite structure with the surface damaged layer 400 to remove the surface damaged layer 400 to form a third composite structure;

[0086] The third composite structure includes a p-type semiconductor wafer 200 and the material to be stripped (ie, the stripped n-type Ga2O3 wafer 100) stripped in step S5, and the thickness of the stripped n-type Ga2O3 wafer 100 is 20nm-10μm.

[0087] As an example, the surface treatment method includes one or more combinations of mechanical grinding, chemical mechanical polishing, dry etching, and wet etching. The removal thickness can be determined by specific removal rate and removal time to ensure that the surface damage layer 400 is completely removed.

[0088] Step S7: See Figure 8, epitaxially growing the third composite structure, growing an epitaxial layer of the peeled material (i.e., the n-type Ga2O3 epitaxial layer 500), and forming a fourth composite structure;

[0089] The thickness of the grown n-type Ga2O3 epitaxial layer 500 is 20nm-1mm.

[0090] The grown n-type Ga2O3 epitaxial layer 500 and the peeled n-type Ga2O3 wafer 100 are both made of gallium oxide and have complete lattice structures. The difference is that their doping concentrations may be different.

[0091] It should be noted that although the lattice of the peeled material to be peeled off is complete, there will be some electron traps, which will affect the concentration of activated carriers in the film. The present invention uses a method of homoepitaxial growth after peeling off the transferred material to be peeled off. On the one hand, a gallium oxide epitaxial layer with a complete lattice structure and few electron traps can be grown to enhance the electrical performance of the device. On the other hand, since the carrier concentration of the epitaxial layer can be freely changed as needed, the flexibility of the overall device preparation can be improved.

[0092] As an example, in step S7, the epitaxy is homoepitaxial, and the method used for homoepitaxiality includes one or more combinations of vapor phase epitaxy, chemical vapor deposition, molecular beam epitaxy, and pulsed laser deposition, and the impurity type and doping concentration can be controlled as needed.

[0093] Specifically, in step S7, when the epitaxial method is vapor phase epitaxy, the Ga source is GaCl, the partial pressure of which is 20-200 Pa, the growth temperature is 800-1000°C, the O source includes one or more combinations of O2, ozone, oxygen plasma, and air, and the carrier gas is one or more combinations of N2 or Ar.

[0094] Specifically, when the epitaxial method is chemical vapor deposition, the Ga source is high-purity Ga, triethylgallium or gallium acetylacetonate, the O source is O2 or a mixture of O2 and water vapor, the carrier gas is a combination of one or more of Ar, He, and N2, the growth temperature is 500-1100°C, and the growth chamber pressure is 1-100Torr.

[0095] Specifically, when the epitaxy method is molecular beam epitaxy, the growth temperature is 600-900°C, the Ga source is high-purity Ga, the O source includes one or more combinations of O2, ozone, and oxygen plasma, the doping source includes one or more combinations of Sn, Si, Mg, Fe, Ge, Al, and In, and the Ga beam equivalent pressure is 5×10 -9 Torr~2×10 -6 Torr.

[0096] Specifically, when the epitaxial method is pulsed laser deposition, the substrate temperature is 400-600°C, the deposition atmosphere is a combination of O2 and Ar, wherein O2 accounts for 1-20%, and the growth pressure is 1×10 -3 Pa~2Pa, laser power density is 1~10J / cm 2 .

[0097] Step S8: See Fig. 9 , metal deposition and annealing are performed on both side surfaces of the third composite structure to prepare an ohmic electrode 600 and form a Ga2O3-based heterogeneous integrated pn junction.

[0098] The surface of the third composite structure on which metal deposition is performed includes the surfaces of the n-type Ga2O3 wafer and the p-type semiconductor wafer.

[0099] As an example, in the step S8, the ohmic electrode 600 is a metal stack formed by a combination of one or more of Ti, Al, Ni, Pt, and Au.

[0100] Specifically, the ohmic electrode 600 may be a Ti / Al / Pt / Au metal stack, a Ti / Al / Ni / Au metal stack, a Ti / Au metal stack, etc., which may be selected according to needs.

[0101] As an example, the metal deposition method includes one or more combinations of evaporation, sputtering, and stripping.

[0102] As an example, the annealing treatment of the third composite structure is carried out in an atmosphere formed by at least one of vacuum, nitrogen, oxygen, and inert gas, the annealing temperature is 200°C to 1000°C, and the annealing time is 30s to 1h. Among them, the annealing temperature can be 200°C, 400°C, 600°C, 800°C, 1000°C, etc., and the annealing time can be 30s, 1min, 5min, 10min, 30min, 1h, etc., which can be selected according to needs. In the example, the annealing treatment can improve the interface characteristics between the ohmic electrode and the semiconductor, make the interface contact good, reduce the contact resistance, and ensure the formation of ohmic contact.

[0103] Example 2 A method for preparing a Ga2O3-based heterogeneous integrated pn junction

[0104] Figure 10 to Figure 15 This is a method for preparing a Ga2O3-based heterogeneous integrated pn junction according to Example 2 of the present invention. The difference between Example 2 and Example 1 is that: a p-type semiconductor wafer is used as a material to be stripped for ion implantation to form a defect layer, and then stripping is performed at the defect layer during the annealing process.

[0105] The preparation method of the Ga2O3-based heterogeneous integrated pn junction comprises the following steps:

[0106] Step S1: Referring to the first embodiment, an n-type Ga2O3 wafer 110 is provided, wherein one surface of the n-type Ga2O3 wafer 110 is a polished surface 110a;

[0107] Among them, the types of the n-type Ga2O3 wafers are not described here in detail.

[0108] Step S2: Referring to the first embodiment, a p-type semiconductor wafer 210 is provided, wherein one surface of the heterogeneous semiconductor wafer 210 is a polished surface 210a;

[0109] The type of the p-type semiconductor wafer 210 is not described in detail herein.

[0110] Step S3: See Fig.10 , using a p-type semiconductor wafer 210 as a material to be stripped, ion implantation is performed from the polished surface 210a of the material to be stripped (i.e., the p-type semiconductor wafer 210) to form a defect layer 310 in the material to be stripped;

[0111] The specific preparation can be found in Example 1 and will not be described in detail here.

[0112] Step S4: See Fig.11 , bonding the polished surface 110a of the n-type Ga2O3 wafer 110 (which has not been ion-implanted in this embodiment) to the polished surface 210a of the p-type semiconductor wafer 210 (which has been ion-implanted in this embodiment) to prepare a first composite structure;

[0113] The specific preparation can be found in Example 1 and will not be described in detail here.

[0114] Step S5: See Fig.12 , performing annealing treatment on the composite structure, and stripping the material to be stripped along the defective layer 310 to obtain a second composite structure with a surface damage layer 410;

[0115] The specific preparation can be found in Example 1 and will not be described in detail here.

[0116] Step S6: See Fig.13 , performing surface treatment on the second composite structure with the surface damaged layer 410 to remove the surface damaged layer 410 to form a third composite structure;

[0117] The specific preparation can be found in Example 1 and will not be described in detail here.

[0118] Step S7: See Fig.14, performing epitaxy on the third composite structure to grow an epitaxial layer of the peeled material (ie, the p-type semiconductor epitaxial layer 510 ) to form a fourth composite structure;

[0119] The specific preparation can be found in Example 1 and will not be described in detail here.

[0120] Step S8: See Fig.15 , metal deposition and annealing are performed on both side surfaces of the fourth composite structure to prepare an ohmic electrode 610 and form a Ga2O3-based heterogeneous pn junction.

[0121] The specific preparation can be found in Example 1 and will not be described in detail here.

[0122] In summary, the preparation method of Ga2O3-based heterogeneous integrated pn junction provided by the present invention, through ion beam stripping and transfer and epitaxial process, n-type Ga2O3 wafer and / or p-type semiconductor wafer are stripped by fracture after annealing and transferred by bonding, and metal electrodes are deposited to obtain a pn junction with good electrical properties, which solves the problem of difficulty in p-type doping of Ga2O3 materials in the prior art and limited electrical performance after heterogeneous integration of n-type Ga2O3 materials and p-type semiconductor materials. It is of great significance to the application of Ga2O3 materials in the field of bipolar devices and greatly expands the application scope of Ga2O3 materials.

[0123] Specifically, the present invention adopts a heterostructure bonded at the interface and further epitaxially grows on the bonded structure, which has higher bonding quality and single crystal quality.

[0124] The existing mechanical stripping method may have a certain degree of warping in the stripped film, which is more difficult to control the surface flatness and warping than the heterogeneous bonding of the whole wafer in the ion stripping transfer of the present invention. Therefore, the obtained bonding area is limited, resulting in limited overall bonding strength; on the other hand, the existing mechanical stripping method mainly relies on van der Waals force for bonding, while the heterogeneous bonding methods used in the ion stripping transfer method, such as surface activated bonding, hydrophilic bonding, etc., form chemical bonds, which are more tightly bonded. Therefore, the heterostructure bonded at the interface has a higher bonding area quality. At the same time, it avoids the problem that the quality of n-type Ga2O3 wafers and / or p-type semiconductor wafers grown directly epitaxially without heterogeneous bonding is difficult to control. The heterostructure bonded at the interface can maintain intact single crystal quality, while the existing ones grown directly epitaxially without heterogeneous bonding are basically amorphous or polycrystalline.

[0125] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing a Ga2O3-based heterogeneous integrated pn junction, characterized in that: include: Step S1: providing an n-type Ga2O3 wafer, wherein one surface of the n-type Ga2O3 wafer is a polished surface; Step S2: providing a p-type semiconductor wafer, wherein one surface of the p-type semiconductor wafer is a polished surface; Step S3: using at least one of the n-type Ga2O3 wafer and the p-type semiconductor wafer as a material to be stripped, and performing ion implantation from a polished surface of the material to be stripped to form a defect layer in the material to be stripped; Step S4: bonding the polished surface of the n-type Ga2O3 wafer to the polished surface of the p-type semiconductor wafer to prepare a first composite structure; Step S5: performing annealing treatment on the first composite structure, and stripping the material to be stripped along the defective layer to form a second composite structure with a surface damage layer; Step S6: performing surface treatment on the second composite structure with the surface damage layer to remove the surface damage layer to form a third composite structure; Step S7: performing homoepitaxial growth on the third composite structure to grow an epitaxial layer of the peeled material to form a fourth composite structure; Step S8: performing metal deposition and annealing on both side surfaces of the fourth composite structure to prepare ohmic electrodes and form a Ga2O3-based heterogeneous pn junction.

2. The method for preparing a Ga2O3-based heterogeneous integrated pn junction according to claim 1, characterized in that: The n-type gallium oxide wafer includes one of an α-Ga2O3 wafer, a β-Ga2O3 wafer, a γ-Ga2O3 wafer, a δ-Ga2O3 wafer and an ε-Ga2O3 wafer.

3. The method for preparing a Ga2O3-based heterogeneous integrated pn junction according to claim 1, characterized in that: The p-type semiconductor wafer includes one of a silicon wafer, a silicon carbide wafer, a diamond wafer and a gallium nitride wafer.

4. The method for preparing a Ga2O3-based heterogeneous integrated pn junction according to claim 1, characterized in that: In step S3, the ion implantation includes one or more of H ion implantation and He ion implantation; the energy of the ion implantation is 10 keV to 200 keV, and the dose is 1×10 16 ions / cm 2 ~1×10 18 ions / cm 2 , the temperature is 20℃~200℃.

5. The method for preparing a Ga2O3-based heterogeneous integrated pn junction according to claim 1, characterized in that: In step S4, the bonding method includes one of surface activated bonding, metal bonding, hydrophilic bonding and anodic bonding; the bonding vacuum degree is 1×10 -7 Pa~5×10 -5 Pa, pressure is 10MPa~500MPa, and temperature is room temperature.

6. The method for preparing a Ga2O3-based heterogeneous integrated pn junction according to claim 1, characterized in that: In the step S5, the first composite structure is annealed in an atmosphere of at least one of vacuum, nitrogen, oxygen, and inert gas, with an annealing temperature of 200° C. to 1000° C. and an annealing time of 1 min to 72 h. In the step S8, annealing is performed in an atmosphere formed by at least one of vacuum, nitrogen, oxygen, and inert gas, the annealing temperature is 200° C. to 1000° C., and the annealing time is 30 seconds to 1 hour.

7. The method for preparing a Ga2O3-based heterogeneous integrated pn junction according to claim 1, characterized in that: In step S6, the surface treatment method includes one or more combinations of mechanical grinding, chemical mechanical polishing, dry etching, and wet etching.

8. The method for preparing a Ga2O3-based heterogeneous integrated pn junction according to claim 1, characterized in that: In step S7, the homoepitaxial growth method includes one or more combinations of vapor phase epitaxy, chemical vapor deposition, molecular beam epitaxy, and pulsed laser deposition.

9. The method for preparing a Ga2O3-based heterogeneous integrated pn junction according to claim 8, characterized in that: In step S7, when the epitaxy method is vapor phase epitaxy, the growth temperature is 800-1000° C., the Ga source used is GaCl with a partial pressure of 20-200 Pa, the O source includes one or more combinations of O2, ozone, oxygen plasma and air, and the carrier gas is one or more combinations of N2 or Ar; When the epitaxial method is chemical vapor deposition, the growth temperature is 500-1100°C, the Ga source is high-purity Ga, triethylgallium or gallium acetylacetonate, the O source is O2 or a mixture of O2 and water vapor, the carrier gas is a combination of one or more of Ar, He, and N2, and the growth chamber pressure is 1-100 Torr; When the epitaxy method is molecular beam epitaxy, the growth temperature is 600-900°C, the Ga source is high-purity Ga, the O source includes one or more combinations of O2, ozone, and oxygen plasma, the doping source includes one or more combinations of Sn, Si, Mg, Fe, Ge, Al, and In, and the Ga beam equivalent pressure is 5×10 -9 Torr~2×10 -6 Torr; When the epitaxial growth method is pulsed laser deposition, the substrate temperature is 400-600°C, the deposition atmosphere is a combination of O2 and Ar, where O2 accounts for 1-20%, and the growth pressure is 1×10 -3 Pa~2Pa, laser power density is 1~10J / cm 2 .

10. The method for preparing a Ga2O3-based heterogeneous integrated pn junction according to claim 1, characterized in that: In step S8, the ohmic electrode is a metal stack formed by a combination of one or more of Ti, Al, Ni, Pt, and Au; the metal deposition method includes a combination of one or more of evaporation, sputtering, and stripping.

Citation Information

Patent Citations

  • Method for preparing a gallium oxide semiconductor structure

    CN109671612A

  • Preparation method of heterogeneous integrated monocrystal diamond film

    CN110970363A