Resin particles, conductive particles, conductive material, and connection structure
By developing resin particles with specific heat resistance and mechanical properties, the problem of insufficient connection reliability of conductive particles under low pressure and heat resistance under high temperature environment is solved, and the hot pressing installation under low pressure is achieved and Stable connection at high temperatures.
Patent Information
- Application Number
- CN202180022047.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-26
- Filing Date
- 2021-03-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-03-26
AI Technical Summary
It is difficult to achieve hot crimping installation of existing conductive particles under low pressure, resulting in reduced connection reliability and insufficient heat resistance to cope with high temperature environments.
Developed a resin particle with a 5% weight reduction temperature of more than 350°C, 10% K and 30% K values are in a specific range, with excellent heat resistance and reliability, suitable for use in thermal pressure at low pressures Connect and install. The material of the resin particles comprises an imidine-based backbone, and its physical and mechanical properties are optimized by adjusting the content of the bismaleimide segment and unsaturated double bonds.
It achieves excellent connection reliability for hot-pressed installation at low pressure and maintains heat resistance in high-temperature environments. It is suitable for high-temperature applications such as automobiles, and the particle size distribution and shape uniformity improve the stability of the conductive layer.
Smart Images

Figure BDA0003850073570000081 
Figure BDA0003850073570000091 
Figure BDA0003850073570000092
Abstract
Description
Technical Field
[0001] The present invention relates to resin particles which are excellent in heat resistance and can be used for substrate particles of conductive particles by thermocompression bonding under low pressure to obtain a connection structure with excellent connection reliability. In addition, the present invention relates to conductive particles, conductive materials and connection structures obtained by using the resin particles. Background Art
[0002] As a method for conducting connection between electrodes of an electronic circuit board, a method using conductive particles having a conductive layer formed on the surface of substrate particles such as resin particles has been proposed (for example, Patent Document 1). Such conductive particles are used, for example, in IC chips, liquid crystal display elements, and the like.
[0003] In the conventional conductive particles, when the electrodes are electrically connected at a relatively low pressure, the connection resistance between the electrodes sometimes becomes high. This is because, under a relatively low pressure, the conductive particles are not fully deformed, and it is difficult for the conductive particles to fully contact the electrodes. Therefore, when using conventional conductive particles, a higher pressure is required in order to fully deform the conductive particles.
[0004] However, when the electrodes are electrically connected with a higher pressure, although the substrate particles or the conductive particles can be deformed, damage is sometimes formed on the electrode, and the connection resistance becomes higher. The compressed substrate particles or the conductive particles return to the original shape to play a role, and sometimes a phenomenon called rebound occurs. If the substrate particles or the conductive particles rebound, the contact area between the conductive particles and the electrode is sometimes reduced, the connection resistance becomes higher, and the conduction reliability is reduced.
[0005] In recent years, various IC chips have also been used in engine peripherals and motor drive parts of automobiles, etc. Unlike the IC chips used in conventional electronic devices, these environments are harsh environments that are repeatedly and long-term subjected to high temperatures. Therefore, each component constituting the IC chip is required to have long-term reliability at high temperatures, and the substrate particles of the conductive particles are required to have excellent heat resistance.
[0006] In addition, in recent years, in liquid crystal display elements, due to the progress of narrow frame and thinning, the situation of using flexible substrates has become more. For example, in the manufacture method of liquid crystal display elements, after the conductive material containing conductive particles is configured on the glass substrate, the flexible substrate is laminated and installed by the FOG process of thermocompression bonding. If thermocompression bonding is performed with high pressure when the flexible substrate is installed using such a FOG process, there is the following problem: sometimes deformation occurs after installation, and the resulting liquid crystal display element produces uneven display. Therefore, for the substrate particles of conductive particles, it is required to have the flexibility of thermocompression bonding installation under low pressure.
[0007] As resin particles with excellent heat resistance, for example, divinylbenzene crosslinked particles are known. However, since these particles are hard, it is difficult to cope with low-pressure thermocompression installation when used as substrate particles of conductive particles in the case of low-pressure installation such as the above-mentioned FOG process.
[0008] In addition, as resin particles with excellent heat resistance, polyimide particles are also known, for example, a method for producing polyimide particles is disclosed in Patent Document 2. However, it is difficult to obtain spherical particles with good reproducibility with the polyimide particles produced by the production method disclosed in Patent Document 2, and there is a problem that the plating process required when used as substrate particles of conductive particles is complicated. In addition, a similar method for producing polyimide particles is also disclosed in Patent Document 3, but its particle diameter is hundreds of nanometers, and the particle diameter is small when used as the above-mentioned conductive particles.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Publication No. 2001-220691
[0012] Patent Document 2: Japanese Patent Application Publication No. 2008-222879
[0013] Patent Document 3: Japanese Patent Application Publication No. 2006-249380
[0014] Non-patent literature
[0015] Non-patent document 1: Katsuya Asao, “Study on the design and application of functional polyimide particles”, 2013, PhD thesis, Osaka Prefecture University, [retrieved on March 22, 2013], available online<URL:http: / / hdl.handle.net / 10466 / 13840> Summary of the invention
[0016] Problems to be solved by the invention
[0017] The object of the present invention is to provide a resin particle having excellent heat resistance and, when used as a substrate particle of a conductive particle, capable of obtaining a connection structure that can cope with thermocompression bonding under low pressure and has excellent connection reliability. In addition, the object of the present invention is to provide a conductive particle, a conductive material and a connection structure formed by using the resin particle.
[0018] Means for solving problems
[0019] The present invention is a resin particle having a 5% weight reduction temperature of 350°C or higher and a 10% K value of 100 N / mm at 25°C. 2Above and 2500N / mm 2 Below, and the 30% K value at 25°C is 100N / mm 2 Above and 1500N / mm 2 the following.
[0020] Hereinafter, the present invention will be described in detail.
[0021] The present inventors have discovered that resin particles having a 5% weight loss temperature above a specific temperature and having a 10% K value and a 30% K value within specific ranges have excellent heat resistance, and in the case of substrate particles used for conductive particles, a connection structure that can cope with thermocompression installation under low pressure and has excellent connection reliability can be obtained, thereby completing the present invention.
[0022] The lower limit of the 5% weight loss temperature of the resin particles of the present invention is 350°C. By setting the 5% weight loss temperature to 350°C or higher, the resin particles of the present invention have excellent heat resistance and are suitable for applications in high temperature environments such as automotive applications. The lower limit of the 5% weight loss temperature is preferably 360°C, more preferably 380°C, and still more preferably 400°C.
[0023] In addition, the preferred upper limit of the 5% weight loss temperature is not particularly limited, but the substantial upper limit is 600°C.
[0024] It should be noted that the 5% weight loss temperature can be obtained as the temperature at which a 5% weight loss occurs when thermogravimetric measurement is performed under a nitrogen atmosphere at a heating rate of 5°C / min under a temperature increase condition of 35°C to 1000°C using a differential thermogravimetric simultaneous measuring apparatus. Examples of the differential thermogravimetric simultaneous measuring apparatus include TG / DTA6300 (manufactured by Hitachi High-Tech Science Co., Ltd.).
[0025] The lower limit of the 10% K value of the resin particles of the present invention at 25°C is 100 N / mm 2 , the upper limit is 2500N / mm 2 By setting the above 10% K value to 100 N / mm 2 When the above-mentioned 10% K value is set to 2500 N / mm, the gap between the conductive particles is uniform and the reliability of the obtained connected structure is excellent. 2 When used as a substrate particle of conductive particles, it can be suitably used for low-pressure thermocompression bonding. The preferred lower limit of the 10% K value is 150 N / mm 2 , the more preferred lower limit is 320N / mm 2, and the further preferred lower limit is 400N / mm 2 The preferred upper limit is 2000N / mm 2 The more preferred upper limit is 1900 N / mm 2 , and the upper limit is preferably 1500N / mm 2 .
[0026] It should be noted that the above 10% K value and the 30% K value described later can be obtained by measuring the compression displacement (μm) when the resin particles are compressed with the smooth indenter end face of a diamond cylinder with a diameter of 50 μm at 25° C., a compression rate of 0.3 mN / sec, and a maximum test load of 10 mN using a compression tester, and the compression displacement (μm) is obtained by the following formula. As the above compression tester, for example, FischerScope H-100 (manufactured by Fischer Co., Ltd.) can be cited.
[0027]
[0028] In the above formula, F is the load value (N) when the particle is compressed and deformed by 10% or 30%, S is the compression displacement (mm) when the particle is compressed and deformed by 10% or 30%, and R is the radius of the short side of the particle (mm).
[0029] The lower limit of the 30% K value of the resin particles of the present invention at 25°C is 100 N / mm 2 , the upper limit is 1500N / mm 2 By setting the above 30% K value to 100 N / mm 2 When the above-mentioned 30% K value is set to 1500 N / mm, the gap between the conductive particles is uniform and the reliability of the obtained connected structure is excellent. 2 When used as a substrate particle of conductive particles, the above-mentioned 30% K value can be appropriately used for low-pressure thermocompression bonding. 2 , the more preferred lower limit is 200N / mm 2 , and the further preferred lower limit is 240N / mm 2 , the preferred upper limit is 900N / mm 2 , the more preferred upper limit is 720N / mm 2 , and the upper limit is preferably 700N / mm 2 .
[0030] The preferred upper limit of the coefficient of variation of the aspect ratio of the resin particles of the present invention is 10%. By making the coefficient of variation of the aspect ratio below 10%, a more uniform gap can be maintained when used as a substrate particle of conductive particles, and a short circuit in the lateral direction between electrodes can be avoided, so that the reliability of the resulting connection structure is more excellent. The more preferred upper limit of the coefficient of variation of the aspect ratio is 3%, the further preferred upper limit is 2%, and the particularly preferred upper limit is 1%.
[0031] The preferred lower limit of the coefficient of variation of the aspect ratio is not particularly limited, but the substantial lower limit is 0.1%.
[0032] It should be noted that the coefficient of variation of the aspect ratio can be obtained by taking a particle image with a scanning electron microscope, measuring the long sides and short sides of 50 particles in the obtained image with a vernier caliper, and then obtaining the aspect ratio by the following formula based on their standard deviation and average value. As the scanning electron microscope, for example, Regulus-8220 (manufactured by Hitachi High-Technologies Co., Ltd.) can be cited.
[0033] Coefficient of variation of aspect ratio (%) = (σa÷∑a) × 100
[0034] In the above formula, σa is the standard deviation of the aspect ratio, and ∑a is the average value of the aspect ratio.
[0035] The preferred lower limit of the average particle size of the resin particles of the present invention is 0.1 μm, and the preferred upper limit is 1000 μm. By making the above average particle size 0.1 μm or more, it is not easy to form agglomerated conductive particles when forming a conductive layer. By making the above average particle size 1000 μm or less, when the electrodes are connected using conductive particles, the contact area between the conductive particles and the electrodes is sufficiently increased. If the average particle size is too large, the conductive particles are difficult to be fully compressed, so sometimes the connection resistance value between the electrodes becomes high. The more preferred lower limit of the above average particle size is 1.0 μm, and the more preferred upper limit is 500 μm.
[0036] The above average particle size is a number average particle size, which can be obtained by taking an image of particles using a scanning electron microscope, measuring the short sides of 50 particles in the image using a vernier caliper, and obtaining the average value thereof.
[0037] The preferred upper limit of the coefficient of variation of the particle size of the resin particles of the present invention based on the particle size distribution measurement is 20%. By making the coefficient of variation of the above particle size 20% or less, when used as a substrate particle of the conductive particles used in the connection structure, a more uniform gap can be maintained, and the reliability of the obtained connection structure is more excellent. The more preferred upper limit of the coefficient of variation of the above particle size is 11%, and the further preferred upper limit is 10%.
[0038] The preferred lower limit of the coefficient of variation of the particle size is not particularly limited, but the substantial lower limit is 0.1%.
[0039] It should be noted that the coefficient of variation of the above-mentioned particle size can be obtained by deriving the standard deviation and mean value of the particle size using a particle size distribution measuring device using a laser diffraction scattering method, and by the following formula. As the above-mentioned particle size distribution measuring device, for example, LS 13 320 (wet system) (Beckman Coulter company system) etc. can be cited.
[0040] Coefficient of variation of particle size (%) = (σs÷∑s) × 100
[0041] In the above formula, σs is the standard deviation of the particle size, and ∑s is the average value of the particle size.
[0042] The preferred upper limit of the change in the 30% K value before and after heating of the resin particles of the present invention at 200°C for 24 hours is 200%. By making the change in the 30% K value before and after heating 200% or less, when used as substrate particles of conductive particles, damage to the conductive layer and the substrate surface due to hardening of the particles can be suppressed when used at high temperatures. The more preferred upper limit of the change in the 30% K value before and after heating is 140%, the further preferred upper limit is 120%, and the particularly preferred upper limit is 90%.
[0043] In addition, the preferred lower limit of the change in the 30% K value before and after the heating is not particularly limited, and the actual lower limit is 0%. When the change in the 30% K value before and after the heating is below the lower limit, the particles are expected to deteriorate, so there is a concern that the electrode portion will become brittle and the conduction reliability of the connection structure will be reduced.
[0044] It should be noted that the change in the 30% K value before and after the heating can be calculated by the following formula.
[0045] Change in 30% K value before and after heating (%) = (BA) ÷ A × 100
[0046] In the above formula, A is the 30% K value at 25°C before heating, and B is the 30% K value at 25°C after heating at 200°C for 24 hours.
[0047] When the resin particles of the present invention are used as substrate particles of conductive particles, the recovery rate is preferably 2.5% or more and 25% or less. By setting the recovery rate to 2.5% or more, the conduction reliability between electrodes can be effectively improved. By setting the recovery rate to 25% or less, the occurrence of springback can be effectively suppressed during installation under low pressure, and the reduction in the conduction reliability of the connection structure can be suppressed. The more preferred lower limit of the recovery rate is 3.5%, and the more preferred upper limit is 21%.
[0048] It should be noted that the above recovery rate refers to the value of L2 / L1 expressed as a percentage when the compression displacement from the origin load value to the specified reversal load value when the load is applied is set to L1 and the unloading displacement (Japanese: deload displacement) from the reversal load value to the origin load value when the load is released is set to L2. Specifically, it can be derived by using a compression tester, applying a load to the resin particles with a smooth end face of a diamond cylinder with a diameter of 50 μm at 25°C, a compression speed of 0.3 mN / second, an origin load value of 1.0 mN, and a reversal load value of 10 mN, and analyzing the recovery behavior after the load is removed.
[0049] Recovery rate (%) = [L2 / L1] × 100
[0050] The 5% weight loss temperature, the 10% K value at 25°C, and the 30% K value at 25°C in the resin particles of the present invention can be easily adjusted to the above ranges by selecting the material constituting the resin particles.
[0051] The resin particles of the present invention preferably have a main chain skeleton containing an imide group, and specific examples thereof include resin particles composed of polybismaleimide, a copolymer of bismaleimide and a compound having an unsaturated double bond, and polyimide.
[0052] The resin particles of the present invention preferably have a segment derived from bismaleimide. By preparing a polymer having the segment derived from bismaleimide, i.e., using bismaleimide as a polymerizable monomer, it is easier to make the 5% weight loss temperature, the 10% K value at 25°C, and the 30% K value at 25°C within the above ranges.
[0053] Specific examples of the bismaleimide include compounds represented by the following formula (1), compounds represented by the following formula (2), compounds represented by the following formula (3), BMI-1700 (manufactured by DESIGNER MOLECULES), BMI-2500 (manufactured by DESIGNER MOLECULES), BMI-3000 (manufactured by DESIGNER MOLECULES), BMI-5000 (manufactured by DESIGNER MOLECULES), BMI-6000 (manufactured by DESIGNER MOLECULES), MOLECULES Co., Ltd.), 1,2-bis(maleimide)ethane, 1,4-bis(maleimide)butane, 4,4'-bismaleimide diphenylmethane, 4,4'-diphenylmethane bismaleimide, bis-(3-ethyl-4-maleimide phenyl)methane, 2,2'-bis-[4-(4-maleimide phenoxy)phenyl]propane, 4,4'-diphenylmethane bismaleimide, 1,4-phenylene bismaleimide, 1,3-phenylene bismaleimide, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1,6'-bismaleimide-(2,2,4-trimethyl)- )hexane, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenyl sulfone bismaleimide, 1,3-bis(3-maleimide phenoxy)benzene, 1,3-bis(4-maleimide phenoxy)benzene, 1-maleimide-3-maleimidemethyl-3,5,5-trimethylcyclohexane, 1,1'-(cyclohexane-1,3-diylbis(methylene))bis(1 H-pyrrole-2,5-dione), 1,1'-(4,4'-methylenebis(cyclohexane-4,1-diyl))bis(1H-pyrrole-2,5-dione), 1,1'-(3,3'-(piperazine-1,4-diyl)bis(propane-3,1-diyl))bis(1H-pyrrole-2,5-dione), 2,2'-(ethylenedioxy)bis(ethylmaleimide), etc. Among them, the compound represented by the following formula (1), the compound represented by the following formula (2), and the compound represented by the following formula (3) are preferred.
[0054] Examples of commercially available products of the compound represented by the following formula (1) include BMI-689 (manufactured by DESIGNER MOLECULES).
[0055] Examples of commercially available products of the compound represented by the following formula (2) include BMI-1400 (manufactured by DESIGNER MOLECULES CO., LTD.).
[0056] Examples of commercially available products of the compound represented by the following formula (3) include BMI-1500 (manufactured by DESIGNER MOLECULES).
[0057]
Chemical formula 1
[0058]
[0059]
Chemical formula 2
[0060]
[0061] In formula (2), n is 1 or more and 10 or less.
[0062]
Chemical formula 3
[0063]
[0064] In formula (3), m is 1 or more and 2 or less.
[0065] The compound having an unsaturated double bond may be a non-crosslinking monomer or a crosslinking monomer.
[0066] Examples of the non-crosslinking monomer include styrene monomers, N-alkyl-substituted maleimide monomers, N-aryl-substituted maleimide monomers, N-acyl-substituted maleimide monomers, other non-crosslinking maleimide monomers, carboxyl-containing monomers, (meth)acrylate alkyl esters, oxygen-containing (meth)acrylate esters, nitrile-containing monomers, vinyl ester compounds, unsaturated hydrocarbons, and halogen-containing monomers.
[0067] Examples of the styrene-based monomer include styrene and α-methylstyrene.
[0068] Examples of the N-alkyl-substituted maleimide monomer include N-methylmaleimide, N-ethylmaleimide, and N-benzylmaleimide.
[0069] Examples of the N-aryl-substituted maleimide monomer include N-ethylmaleimide, N-(4-aminophenyl)maleimide, and N-(9-acridyl)maleimide.
[0070] Examples of the N-acyl-substituted maleimide monomer include N-methoxycarbonylmaleimide and the like.
[0071] Examples of the other non-crosslinkable maleimide monomers include succinimidyl-4-(N-maleimidomethyl)cyclohexane-1-carboxylate and N-succinimidyl-3-maleimidopropionate.
[0072] As said carboxyl group-containing monomer, (meth)acrylic acid, maleic acid, maleic anhydride etc. are mentioned, for example.
[0073] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate.
[0074] Examples of the oxygen atom-containing (meth)acrylate include 2-hydroxyethyl (meth)acrylate, glyceryl (meth)acrylate, polyoxyethylene (meth)acrylate, and glycidyl (meth)acrylate.
[0075] Examples of the nitrile-containing monomer include (meth)acrylonitrile and the like.
[0076] Examples of the acid vinyl ester compound include vinyl acetate, vinyl butyrate, vinyl laurate, and vinyl stearate.
[0077] Examples of the unsaturated hydrocarbons include ethylene, propylene, isoprene, and butadiene.
[0078] Examples of the halogen-containing monomer include trifluoromethyl (meth)acrylate, pentafluoroethyl (meth)acrylate, vinyl chloride, vinyl fluoride, and chlorostyrene.
[0079] As said crosslinking monomer, a polyfunctional (meth)acrylate, a silane-containing monomer, etc. are mentioned, for example.
[0080] Examples of the polyfunctional (meth)acrylate include tetramethylolmethane tetra(meth)acrylate, tetramethylolmethane tri(meth)acrylate, tetramethylolmethane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, glycerol tri(meth)acrylate, glycerol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, (poly)tetramethylene glycol di(meth)acrylate, and 1,4-butanediol di(meth)acrylate.
[0081] Examples of the silane-containing monomer include triallyl (iso)cyanurate, triallyl trimellitate, divinylbenzene, diallyl phthalate, diallyl acrylamide, diallyl ether, γ-(meth)acryloxypropyltrimethoxysilane, trimethoxysilylstyrene, and vinyltrimethoxysilane.
[0082] When the resin particles of the present invention have the above-mentioned segments derived from bismaleimide, the preferred lower limit of the content of the above-mentioned segments derived from bismaleimide is 0.1 mol%. By setting the content of the above-mentioned segments derived from bismaleimide to 0.1 mol% or more, it is easier to set the 5% weight reduction temperature, the 10% K value at 25°C, and the 30% K value at 25°C to the above-mentioned ranges. The more preferred lower limit of the content of the above-mentioned segments derived from bismaleimide is 3.0 mol%, the further preferred lower limit is 9.0 mol%, and the particularly preferred lower limit is 20 mol%.
[0083] In particular, the 5% weight loss temperature can be easily adjusted by the content ratio of the above-mentioned segments derived from bismaleimide contained in the resin particles, can be increased by increasing the content ratio of the above-mentioned segments derived from bismaleimide, and can be decreased by decreasing the content ratio of the above-mentioned segments derived from bismaleimide. In addition, the 10% K value at 25°C and the 30% K value at 25°C can be decreased by increasing the content ratio of the above-mentioned segments derived from bismaleimide, and can be increased by decreasing the content ratio of the above-mentioned segments derived from bismaleimide.
[0084] When the resin particles of the present invention have an imide group, the preferred lower limit of the imide group content is 0.01%, and the preferred upper limit is 80%. By making the imide group content 0.01% or more, polymer particles having a main chain skeleton with better heat resistance are obtained. By making the imide group content 80% or less, it is easier to make the 10% K value at 25°C and the 30% K value at 25°C within the above range. The more preferred lower limit of the imide group content is 5%, the further preferred lower limit is 7.5%, and the more preferred upper limit is 50%.
[0085] In particular, the 5% weight loss temperature can be easily adjusted according to the content of the imide groups contained in the resin particles, and can be increased by increasing the content of the imide groups, or can be decreased by decreasing the content of the imide groups.
[0086] In addition, the content rate of the said imide group can be calculated|required by the following formula.
[0087] Imide group content (%) = C ÷ D × 100
[0088] In the above formula, C is the total molecular weight of the imide group part contained in the repeating unit, and D is the total molecular weight of the repeating structural unit of the resin constituting the resin particles.
[0089] It should be noted that, when the resin particles of the present invention are copolymer particles, the molar fraction of each repeating structural unit is calculated, and the calculated total molecular weight is set as D. For example, in the case of Example 2 described later, the molar fraction of the structural unit of the compound represented by formula (1) is 0.5, and the molar fraction of the structural unit of styrene is 0.5, so it is calculated as:
[0090] D = molecular weight of the compound represented by formula (1) × molar fraction + molecular weight of styrene × molar fraction
[0091] =689×0.5+104.15×0.5
[0092] =396.575.
[0093] As the polymerization method for producing the resin particles of the present invention, specifically, for example, conventionally known polymerization methods such as suspension polymerization, emulsion polymerization, seed polymerization, and dispersion polymerization can be cited. Among them, since polymer particles having a wide particle size distribution and polydispersity can be obtained, the above-mentioned suspension polymerization method and the above-mentioned emulsion polymerization method are suitable for the purpose of producing microparticles of various particle sizes. When using the above-mentioned suspension polymerization method and the above-mentioned emulsion polymerization method, it is preferred to classify the polymer particles obtained by polymerization and select polymer particles having a desired particle size or particle size distribution.
[0094] Conductive particles including the resin particles of the present invention and a conductive layer formed on the surface of the resin particles are also one of the present invention.
[0095] As materials constituting the above-mentioned conductive layer, for example, gold, silver, palladium, copper, platinum, zinc, iron, tin, lead, aluminum, cobalt, indium, nickel, chromium, titanium, antimony, bismuth, thallium, germanium, cadmium, silicon, tungsten, molybdenum and alloys thereof, tin-doped indium oxide (ITO), etc. Among them, alloys containing tin, nickel, palladium, gold, copper or silver are preferred, alloys containing tin, nickel, palladium, gold or copper are more preferred, and nickel or palladium is further preferred because the connection resistance between electrodes can be further reduced.
[0096] As a method for forming the conductive layer on the surface of the resin particles, for example, a method using chemical plating, a method using electroplating, a method using physical vapor deposition, a method of applying a metal powder or a paste containing a metal powder and a binder on the surface of the resin particles, etc. From the aspect of the simplicity of forming the conductive layer, the method for forming the conductive layer is preferably a method using chemical plating. As the method of the physical vapor deposition, for example, vacuum evaporation, ion plating, ion sputtering and the like can be cited.
[0097] The conductive particles of the present invention preferably have an insulating material on the outer surface of the conductive layer. By having an insulating material on the outer surface of the conductive layer, when the obtained conductive particles are used for connection between electrodes, short circuits between adjacent electrodes can be further prevented. Specifically, when a plurality of conductive particles are in contact, since there is an insulating material between the plurality of electrodes, short circuits between electrodes adjacent to each other in the transverse direction can be prevented, rather than short circuits between upper and lower electrodes. It should be noted that when connecting between electrodes, by pressurizing the conductive particles with two electrodes, the insulating substance between the conductive layer of the conductive particles and the electrodes can be easily removed. In addition, when the conductive particles have a plurality of protrusions on the outer surface of the conductive layer, the insulating substance between the conductive layer of the conductive particles and the electrodes can be further easily removed.
[0098] The insulating material is preferably insulating particles because the insulating material can be more easily removed during pressure bonding between electrodes.
[0099] Examples of the insulating material include polyolefin compounds, (meth)acrylate polymers, (meth)acrylate copolymers, block polymers, thermoplastic resins, crosslinked products of thermoplastic resins, thermosetting resins, water-soluble resins, etc. The insulating material may be used alone or in combination of two or more.
[0100] Examples of the polyolefin compound include polyethylene, ethylene-vinyl acetate copolymer, and ethylene-acrylate copolymer.
[0101] Examples of the (meth)acrylate polymer include polymethyl (meth)acrylate, polydodecyl (meth)acrylate, and polystearyl (meth)acrylate.
[0102] Examples of the block polymer include polystyrene, styrene-acrylate copolymers, SB-type styrene-butadiene block copolymers, SBS-type styrene-butadiene block copolymers, and hydrogenated products thereof.
[0103] Examples of the thermoplastic resin include vinyl polymers and vinyl copolymers.
[0104] Examples of the thermosetting resin include epoxy resins, phenol resins, and melamine resins.
[0105] Examples of the cross-linked product of the thermoplastic resin include introduction of polyethylene glycol methacrylate, alkoxylated trimethylolpropane methacrylate, alkoxylated pentaerythritol methacrylate, and the like.
[0106] Examples of the water-soluble resin include polyvinyl alcohol, polyacrylic acid, polyacrylamide, polyvinyl pyrrolidone, polyethylene oxide, and methyl cellulose.
[0107] When producing the above insulating material, a chain transfer agent may be used to adjust the degree of polymerization.
[0108] Examples of the chain transfer agent include mercaptan and carbon tetrachloride.
[0109] Examples of a method for disposing the insulating material on the outer surface of the conductive layer include a chemical method, a physical method, a mechanical method, and the like.
[0110] Examples of the chemical method include interfacial polymerization, suspension polymerization in the presence of particles, and emulsion polymerization.
[0111] Examples of the physical or mechanical method include spray drying, hybridization, an electrostatic adhesion method, a spray method, immersion, and a method based on vacuum deposition.
[0112] Among them, from the viewpoint that the insulating material is not easily detached, a method of arranging the insulating material on the outer surface of the conductive layer via a chemical bond is preferred.
[0113] The outer surface of the conductive layer and the surface of the insulating material may be coated with a compound having a reactive functional group, respectively. The outer surface of the conductive layer and the surface of the insulating material may not be directly chemically bonded, but may be indirectly chemically bonded through a compound having a reactive functional group. For example, after a carboxyl group is introduced into the outer surface of the conductive layer, the carboxyl group may be chemically bonded to a functional group on the surface of the insulating material via a polymer electrolyte such as polyethyleneimine.
[0114] The conductive particles of the present invention preferably have protrusions on the outer surface of the conductive layer. By having protrusions on the outer surface of the conductive layer, the conductive particles obtained can further improve the conduction reliability between electrodes. On the surface of the electrode connected by the conductive particles, an oxide film is mostly formed. In addition, an oxide film is mostly formed on the surface of the conductive layer of the conductive particles. By using the conductive particles with protrusions, the conductive particles are arranged between the electrodes and then crimped, thereby effectively eliminating the oxide film by using the protrusions. Therefore, the electrode and the conductive particles can be further reliably contacted, and the connection resistance between the electrodes can be further effectively reduced. In addition, in the case where the conductive particles have the insulating material on the surface, or the conductive particles are dispersed in a binder resin and used as a conductive material, the insulating material and the binder resin between the conductive particles and the electrode are effectively eliminated by the protrusions of the conductive particles. Therefore, the conduction reliability between the electrodes can be further effectively improved.
[0115] As a method for forming protrusions on the outer surface of the conductive layer, for example, a method of embedding a core material in the conductive layer can be cited. By embedding the core material in the conductive layer, a plurality of protrusions can be easily formed on the outer surface of the conductive layer. However, in order to form protrusions on the outer surface of the conductive layer of the conductive particles, it is not necessary to use a core material.
[0116] As a method for forming the above-mentioned protrusions, specifically, for example, there can be mentioned a method of attaching a core material to the surface of a resin particle and then forming a conductive layer by chemical plating, a method of attaching a core material after forming a conductive layer by chemical plating on the surface of a resin particle and further forming a conductive layer by chemical plating, etc. As other methods for forming the above-mentioned protrusions, for example, there can be mentioned a method of forming a first conductive layer on the surface of a resin particle, arranging a core material on the first conductive layer, and then forming a second conductive layer, a method of adding a core material in the middle of forming a conductive layer (first conductive layer or second conductive layer, etc.) on the surface of a resin particle, etc. In addition, in order to form the above-mentioned protrusions, the following method can be used: without using the above-mentioned core material, after forming a conductive layer on a resin particle by chemical plating, a plating layer is precipitated in the form of a protrusion on the surface of the conductive layer, and a conductive layer is further formed by chemical plating.
[0117] As a method for attaching the core material to the surface of the resin particles, for example, there can be mentioned a method of adding the core material to a dispersion of the resin particles and aggregating the core material to attach to the surface of the resin particles by utilizing van der Waals force, a method of adding the core material to a container containing the resin particles and attaching the core material to the surface of the resin particles by utilizing a mechanical action based on the rotation of the container, etc. Among them, in order to easily control the amount of the attached core material, a method of aggregating the core material to attach to the surface of the resin particles in the dispersion is preferred.
[0118] The material of the core material may be a conductive material or a non-conductive material.
[0119] Examples of the conductive substance include metals, metal oxides, conductive nonmetals such as graphite, and conductive polymers.
[0120] Examples of the conductive polymer include polyacetylene and the like.
[0121] Examples of the non-conductive substance include silicon dioxide, aluminum oxide, titanium oxide, barium titanate, and zirconium oxide.
[0122] Among them, as the material of the core substance, metal is preferred because it can improve conductivity and thus effectively reduce connection resistance, and the core substance is preferably metal particles. As the metal of the material of the core substance, the metals listed as the materials constituting the conductive layer can be appropriately used.
[0123] A conductive material including the conductive particles of the present invention and a binder resin is also one of the present invention.
[0124] As the binder resin, an insulating resin is used, and examples thereof include vinyl resins, thermoplastic resins, curable resins, thermoplastic block copolymers, elastomers, etc. The binder resins may be used alone or in combination of two or more.
[0125] Examples of the vinyl resin include vinyl acetate resin, acrylic resin, and styrene resin.
[0126] Examples of the thermoplastic resin include polyolefin resins, ethylene-vinyl acetate copolymers, and polyamide resins.
[0127] Examples of the curable resin include epoxy resins, urethane resins, polyimide resins, unsaturated polyester resins, etc. It should be noted that the curable resin may be any one of a room temperature curable resin, a thermosetting resin, a light curable resin, and a moisture curable resin. In addition, the curable resin may be used in combination with a curing agent.
[0128] Examples of the thermoplastic block copolymer include styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene block copolymers, hydrogenated products of styrene-butadiene-styrene block copolymers, and hydrogenated products of styrene-isoprene-styrene block copolymers.
[0129] Examples of the elastomer include styrene-butadiene copolymer rubber and acrylonitrile-styrene block copolymer rubber.
[0130] The conductive material of the present invention may contain various additives such as fillers, extenders, softeners, plasticizers, polymerization catalysts, curing catalysts, colorants, antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, lubricants, antistatic agents, flame retardants, etc. in addition to the conductive particles and the binder resin.
[0131] In the conductive material of the present invention, the conductive particles of the present invention are preferably dispersed in the above-mentioned binder resin.
[0132] The method for dispersing the conductive particles in the above-mentioned binder resin can use a conventionally known dispersion method. Specifically, for example, there can be cited a method in which the conductive particles are added to the binder resin and then dispersed by kneading using a planetary mixer or the like, a method in which the conductive particles are uniformly dispersed in water or an organic solvent using a homogenizer or the like and then added to the binder resin and then dispersed by kneading using a planetary mixer or the like, a method in which the conductive particles are diluted with water or an organic solvent or the like and then added to the binder resin and then dispersed by kneading using a planetary mixer or the like, and the like.
[0133] The conductive material of the present invention can be used as, for example, anisotropic conductive paste, anisotropic conductive ink, anisotropic conductive adhesive, anisotropic conductive film, anisotropic conductive sheet, etc. When the conductive material of the present invention is used as a film-like adhesive such as anisotropic conductive film or anisotropic conductive sheet, a film-like adhesive not containing conductive particles may be laminated on the film-like adhesive containing the conductive particles.
[0134] The preferred lower limit of the content of the above-mentioned binder resin in 100 parts by weight of the conductive material of the present invention is 10 parts by weight, and the preferred upper limit is 99.99 parts by weight. By making the content of the above-mentioned binder resin within this range, the conductive particles are effectively arranged between the electrodes, and the connection reliability of the connection object member connected by the conductive material of the present invention is further improved. The more preferred lower limit of the content of the above-mentioned binder resin is 30 parts by weight, the further preferred lower limit is 50 parts by weight, the particularly preferred lower limit is 70 parts by weight, and the more preferred upper limit is 99.9 parts by weight.
[0135] The preferred lower limit of the content of the conductive particles in 100 parts by weight of the conductive material of the present invention is 0.01 parts by weight, and the preferred upper limit is 80 parts by weight. By making the content of the conductive particles within this range, it is possible to suppress the deterioration of coating properties, etc., and further exert the effect of improving conductivity, etc. The more preferred lower limit of the content of the conductive particles is 0.1 parts by weight, and the more preferred upper limit is 10 parts by weight.
[0136] The conductive material of the present invention may contain various additives such as fillers, extenders, softeners, plasticizers, polymerization catalysts, curing catalysts, colorants, antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, lubricants, antistatic agents, flame retardants, etc. within the range that does not hinder the purpose of the present invention.
[0137] By using the conductive particles of the present invention, a connection structure having excellent connection reliability can be obtained.
[0138] The present invention also provides a connection structure comprising a first connection object member having a first electrode on its surface, a second connection object member having a second electrode on its surface, and a connection portion connecting the first connection object member and the second connection object member, wherein the connecting portion is made of the conductive particles of the present invention or the conductive material of the present invention.
[0139] The resin particles of the present invention have high compression modification during initial compression, can maintain a certain gap, and can suppress damage to the substrate. Therefore, they are also suitable for use as spacers for liquid crystal display elements and the like.
[0140] Effects of the Invention
[0141] According to the present invention, a resin particle having excellent heat resistance can be provided, and when used as a substrate particle of conductive particles, a connection structure that can cope with thermocompression mounting under low pressure and has excellent connection reliability can be obtained. In addition, according to the present invention, conductive particles, conductive materials, and connection structures formed by using the resin particles can be provided. DETAILED DESCRIPTION
[0142] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.
[0143] (Example 1)
[0144] In a reaction vessel equipped with a thermometer and a condenser, 4.6 parts by weight of the compound represented by the above formula (1) (manufactured by DESIGNER MOLECULES, "BMI-689") and 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") as a dispersion stabilizer, 0.4 parts by weight of sodium dodecylbenzene sulfate, and 180 parts by weight of ultrapure water were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Chuo Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 1.
[0145] (Example 2)
[0146] In a reaction container equipped with a thermometer and a condenser, 4.0 parts by weight of the compound represented by the above formula (1) (manufactured by DESIGNER MOLECULES, "BMI-689"), 0.6 parts by weight of styrene, and 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20"), 0.4 parts by weight of sodium dodecylbenzene sulfate, and 180 parts by weight of ultrapure water were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Chuo Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 2.
[0147] (Example 3)
[0148] In a reaction container equipped with a thermometer and a condenser, 3.5 parts by weight of the compound represented by the above formula (1) (manufactured by DESIGNER MOLECULES, "BMI-689"), 1.1 parts by weight of styrene, and 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Central Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 3.
[0149] (Example 4)
[0150] In a reaction container equipped with a thermometer and a condenser, 2.8 parts by weight of the compound represented by the above formula (1) (manufactured by DESIGNER MOLECULES, "BMI-689"), 0.5 parts by weight of ethylmaleimide, 1.3 parts by weight of styrene, and 0.2 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Central Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 4.
[0151] (Example 5)
[0152] In a reaction vessel equipped with a thermometer and a condenser, 1.8 parts by weight of the compound represented by the above formula (1) (manufactured by DESIGNER MOLECULES, "BMI-689"), 1.3 parts by weight of ethylmaleimide, 1.6 parts by weight of styrene, and 0.2 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Chuo Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 5.
[0153] (Example 6)
[0154] In a reaction container equipped with a thermometer and a condenser, 0.7 parts by weight of the compound represented by the above formula (1) (manufactured by DESIGNER MOLECULES, "BMI-689"), 2.0 parts by weight of ethylmaleimide, 1.9 parts by weight of styrene, and 0.2 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Chuo Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 6.
[0155] (Example 7)
[0156] In a reaction container equipped with a thermometer and a condenser, 0.3 parts by weight of the compound represented by the above formula (1) (manufactured by DESIGNER MOLECULES, "BMI-689"), 2.4 parts by weight of ethylmaleimide, 2.0 parts by weight of styrene, and 0.2 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Chuo Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 7.
[0157] (Example 8)
[0158] In a reaction container equipped with a thermometer and a condenser, 4.6 parts by weight of the compound represented by the above formula (2) (manufactured by DESIGNER MOLECULES, "BMI-1400") and 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") as a dispersion stabilizer, 0.4 parts by weight of sodium dodecylbenzene sulfate, and 180 parts by weight of ultrapure water were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Central Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 8.
[0159] (Example 9)
[0160] In a reaction container equipped with a thermometer and a condenser, 4.1 parts by weight of the compound represented by the above formula (2) (manufactured by DESIGNER MOLECULES, "BMI-1400"), 0.5 parts by weight of styrene, and 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and stirred using a high-speed homogenizer (manufactured by Central Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 9.
[0161] (Example 10)
[0162] In a reaction container equipped with a thermometer and a condenser, 4.6 parts by weight of the compound represented by the above formula (3) (manufactured by DESIGNER MOLECULES, "BMI-1500") and 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and stirred using a high-speed homogenizer (manufactured by Central Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 10.
[0163] (Example 11)
[0164] In a reaction container equipped with a thermometer and a condenser, 4.0 parts by weight of the compound represented by the above formula (3) (manufactured by DESIGNER MOLECULES, "BMI-1500"), 0.6 parts by weight of styrene, and 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and stirred using a high-speed homogenizer (manufactured by Central Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 11.
[0165] (Example 12)
[0166] In a reaction container equipped with a thermometer and a condenser, 3.9 parts by weight of the compound represented by the above formula (1) (manufactured by DESIGNER MOLECULES, "BMI-689"), 0.5 parts by weight of divinylbenzene, 0.2 parts by weight of styrene, and 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOLGH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Central Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 12.
[0167] (Example 13)
[0168] In a reaction container equipped with a thermometer and a condenser, 3.9 parts by weight of the compound represented by the above formula (1) (manufactured by DESIGNER MOLECULES, "BMI-689"), 0.7 parts by weight of divinylbenzene, and 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 4.6 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Central Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 13.
[0169] (Example 14)
[0170] In a reaction container equipped with a thermometer and a condenser, 2.4 parts by weight of ethylmaleimide, 2.0 parts by weight of styrene, 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator, and 4.4 parts by weight of toluene were mixed. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and stirred using a high-speed homogenizer (manufactured by Central Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 14.
[0171] (Example 15)
[0172] In a reaction container equipped with a thermometer and a condenser, 4.6 parts by weight of the compound represented by the above formula (1) (manufactured by DESIGNER MOLECULES, "BMI-689"), 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator, and 3.0 parts by weight of toluene were mixed. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20"), 0.4 parts by weight of sodium dodecylbenzene sulfate, and 180 parts by weight of ultrapure water were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Central Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 15.
[0173] (Example 16)
[0174] In a reaction container equipped with a thermometer and a condenser, 4.0 parts by weight of the compound represented by the above formula (1) (manufactured by DESIGNER MOLECULES, "BMI-689"), 0.6 parts by weight of styrene, and 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 2.0 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and the mixture was stirred using a high-speed homogenizer (manufactured by Central Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 16.
[0175] (Comparative Example 1)
[0176] Polyimide P84 NT (manufactured by Daicel Evonik) was used as the resin particles 17 .
[0177] (Comparative Example 2)
[0178] Divinylbenzene copolymer resin particles (manufactured by Sekisui Chemical Co., Ltd., “Micropearl”) were used as resin particles 18 .
[0179] (Comparative Example 3)
[0180] In a reaction vessel equipped with a thermometer and a condenser, LIGHT ACRYLATE 4.4 parts by weight of MPD-A (manufactured by Kyoeisha Chemical Co., Ltd.), 0.2 parts by weight of A-TMMT (manufactured by Shin-Nakamura Chemical Co., Ltd.), and 0.3 parts by weight of 2,2'-azobis(isobutyronitrile) as a polymerization initiator were dissolved in 2.0 parts by weight of toluene. 13.1 parts by weight of a 5.5% by weight aqueous solution of polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Co., Ltd., "GOHSENOL GH-20") and 0.4 parts by weight of sodium dodecylbenzene sulfate as a dispersion stabilizer were added to the obtained solution, and stirred using a high-speed homogenizer (manufactured by Chuo Science Trading Co., Ltd., "POLYTRON PT-3100") to obtain a suspension. The obtained suspension was heated to 65°C and heated and stirred for 24 hours to obtain resin particles 19.
[0181] (Comparative Example 4)
[0182] According to Non-Patent Document 1, resin particles were prepared as follows.
[0183] In a reaction vessel equipped with a thermometer, a stirrer and a condenser, 0.1 mol of 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 0.05 mol of 1,4-bis(4-aminophenoxy)benzene and 0.05 mol of bis[4-(3-aminophenoxy)phenyl]sulfone were dissolved in 500 mL of N,N-dimethylformamide. The obtained solution was stirred at 25° C. for 24 hours to obtain a solution of polyamic acid as a prepolymer of polyimide. 100 mL of toluene was added to the obtained solution, and heated under reflux for 4 hours under a nitrogen atmosphere to obtain resin particles 20.
[0184] (5% thermal weight reduction temperature)
[0185] 10 mg of each resin particle obtained in the examples and comparative examples was weighed in an aluminum pan, and thermogravimetric measurement was performed using a differential thermogravimetric simultaneous measuring apparatus under a nitrogen atmosphere at a heating rate of 5°C / min under the temperature rising condition of 35°C to 1000°C, and the temperature at which a 5% weight loss occurred was determined. The results are shown in Tables 1 and 2.
[0186] As a differential thermogravimetric simultaneous measurement apparatus, TG / DTA6300 (manufactured by Hitachi High-Tech Science Co., Ltd.) was used.
[0187] (10% K value and 30% K value)
[0188] For each resin particle obtained in Examples 1 to 16 and Comparative Examples 2 and 3, a compression tester was used to measure the compression displacement (μm) when the compression was performed under the conditions of 25°C, a compression rate of 0.3 mN / sec, and a maximum test load of 10 mN using a smooth diamond cylindrical indenter end face with a diameter of 50 μm, and the 10% K value and 30% K value were obtained by the above formula. The results are shown in Tables 1 and 2.
[0189] As a compression tester, FischerScope H-100 (manufactured by Fischer) was used.
[0190] (Coefficient of variation of aspect ratio and average particle size)
[0191] For each resin particle obtained in the embodiment and the comparative example, a particle image was taken with a scanning electron microscope, and the long sides and short sides of 50 particles in the obtained image were measured with a vernier caliper, respectively, and the aspect ratio was obtained. Then, the coefficient of variation of the aspect ratio was obtained by the above formula from their standard deviation and average value. In addition, the average value of the short sides of 50 particles in the obtained image was obtained as the average particle size. The results are shown in Tables 1 and 2.
[0192] As a scanning electron microscope, Regulus-8220 (manufactured by Hitachi High-Technologies Corporation) was used.
[0193] (Coefficient of variation of particle size)
[0194] For each of the resin particles obtained in Examples and Comparative Examples, a standard deviation and an average value of the particle size were derived using a laser diffraction scattering particle size distribution measuring apparatus, and the coefficient of variation of the particle size was determined using the above formula.
[0195] As a particle size distribution measuring apparatus, LS 13 320 (wet system) (manufactured by Beckman Coulter) was used.
[0196] (30% K value change before and after heating)
[0197] The resin particles obtained in Examples 1 to 16 and Comparative Examples 2 to 4 were heated at 200°C for 24 hours. The change in 30% K value before and after heating was determined by the above formula from the measurement results of 30% K value at 25°C before and after heating. The results are shown in Tables 1 and 2.
[0198] (Recovery rate)
[0199] For each resin particle obtained in Examples 1 to 16 and Comparative Examples 2 to 4, a compression tester was used to apply a load to the resin particle using the smooth end surface of a diamond cylinder with a diameter of 50 μm at 25°C, a compression rate of 0.3 mN / sec, an origin load value of 1.0 mN, and a reversal load value of 10 mN, and the recovery behavior after the load was removed was analyzed, thereby deriving the recovery rate using the above method. The results are shown in Tables 1 and 2.
[0200] As a compression tester, FischerScope H-100 (manufactured by Fischer) was used.
[0201] (Content ratio of imide group)
[0202] The imide group content was determined by the above formula for each of the resin particles obtained in Examples 1 to 16 and Comparative Examples 2 to 4. The results are shown in Tables 1 and 2.
[0203] <Evaluation>
[0204] The following evaluations were performed on each of the resin particles obtained in Examples and Comparative Examples.
[0205] (1) Long-term connection reliability under high temperature conditions
[0206] (1-1) Preparation of Conductive Particles
[0207] After using an ultrasonic disperser to disperse 10 parts by weight of each resin particle obtained in the embodiment and the comparative example in 100 parts by weight of an alkaline solution containing 5% by weight of a palladium catalyst solution, the solution was filtered to remove the resin particles. Next, the resin particles were added to 100 parts by weight of a 1% by weight solution of dimethylamine borane to activate the surface of the resin particles. After the surface-activated resin particles were thoroughly washed with water, they were added to 500 parts by weight of distilled water to disperse them, thereby obtaining a dispersion. Next, 1 g of nickel particle slurry (average particle size 100 nm) was added to the above dispersion for 3 minutes to obtain a suspension containing resin particles with a core material attached. In addition, a nickel plating solution (pH 8.5) containing 0.35 mol / L of nickel sulfate, 1.38 mol / L of dimethylamine borane and 0.5 mol / L of sodium citrate was prepared. While stirring the obtained suspension at 60°C, the above nickel plating solution was slowly added dropwise to the suspension to perform electroless nickel plating. Then, the suspension was filtered to take out particles, which were then washed with water and dried to obtain conductive particles having a nickel-boron conductive layer (thickness 0.15 μm) on the surface of the resin particles.
[0208] (1-2) Preparation of insulating particles
[0209] In a separable flask, a monomer composition containing 100 mmol of methyl methacrylate, 1 mmol of N, N, N-trimethyl-N-2-methacryloyloxyethylammonium chloride and 1 mmol of 2,2'-azobis(2-amidinopropane) dihydrochloride is weighed into ion exchange water in such a way that the solid content is 5% by weight. As a separable flask, a separable flask of 1000 mL capacity equipped with a 4-mouth separable cover, a stirring blade, a three-way stopcock, a condenser and a temperature probe is used. Then, stirring is carried out at 200 rpm, and polymerization is carried out at 70°C for 24 hours under a nitrogen atmosphere. After the reaction is completed, freeze drying is carried out to obtain insulating particles having ammonium groups on the surface, an average particle size of 220 nm, and a particle size CV value of 10%.
[0210] (1-3) Preparation of Conductive Particles with Insulating Particles
[0211] The insulating particles obtained in the above "(1-2) Preparation of insulating particles" were dispersed in distilled water under ultrasonic irradiation to obtain a 10 wt% aqueous dispersion of insulating particles. Next, 10 g of the conductive particles obtained in the above "(1-1) Preparation of conductive particles" were dispersed in 500 mL of distilled water, 1 g of the 10 wt% aqueous dispersion of insulating particles was added, and stirred at room temperature for 8 hours. After filtering with a 3 μm mesh filter, the mixture was further washed with methanol and dried to obtain conductive particles with insulating particles.
[0212] (1-4) Preparation of conductive material (anisotropic conductive paste)
[0213] 7 parts by weight of the obtained conductive particles with insulating particles, 25 parts by weight of bisphenol A type phenoxy resin, 4 parts by weight of fluorene type epoxy resin, 30 parts by weight of phenol novolac type epoxy resin and SI-60L (manufactured by Sanshin Chemical Industry Co., Ltd.) were mixed and degassed and stirred for 3 minutes to obtain a conductive material (anisotropic conductive paste).
[0214] (1-5) Fabrication of connection structure
[0215] A transparent glass substrate (first connection object component) is prepared on the upper surface of which an aluminum electrode pattern (first electrode) with a height of 0.2 μm and an L / S of 10 μm / 10 μm is formed. In addition, a double-layer flexible substrate (second connection object component) is prepared on the lower surface of which an aluminum electrode pattern (second electrode) with an L / S of 10 μm / 10 μm is formed. On the above-mentioned transparent glass substrate, the obtained anisotropic conductive paste is applied in a manner to a thickness of 15 μm to form an anisotropic conductive paste layer. Next, a double-layer flexible substrate is stacked on the anisotropic conductive paste layer in a manner in which the electrodes are opposite to each other. Then, while adjusting the temperature of the head in a manner in which the temperature of the anisotropic conductive paste layer becomes 180°C, a pressurized heating head is placed on the upper surface of the semiconductor chip, and a pressure of 1 MPa is applied to cure the anisotropic conductive paste layer at 180°C to obtain a connection structure.
[0216] (1-6) Evaluation of long-term connection reliability under high temperature conditions
[0217] 100 of the obtained connection structures were left standing at 200° C. for 24 hours. The 100 connection structures after standing were checked for the occurrence of poor conduction between the upper and lower electrodes.
[0218] The case where the number of connected structures with poor conductivity is less than 1 is recorded as "○○○", the case where the number of connected structures with poor conductivity is more than 2 and less than 5 is recorded as "○○", the case where the number of connected structures with poor conductivity is more than 6 and less than 10 is recorded as "○", and the case where the number of connected structures with poor conductivity is more than 11 is recorded as "×", and the long-term connection reliability under high temperature conditions is evaluated.
[0219] (2) Adhesion between resin particles and conductive parts
[0220] The connection structure obtained in the same manner as in the above "(1) Long-term connection reliability under high temperature conditions" was observed using a scanning electron microscope (manufactured by Hitachi High-Technologies, "Regulus 8220"). For the 100 observed conductive particles, it was confirmed whether the conductive portion (conductive layer) disposed on the surface of the resin particle was peeled off.
[0221] The case where the number of conductive particles peeled off from the conductive part was 0 was marked as "○○○", the case where it was more than 0 and 15 or less was marked as "○○", the case where it was more than 15 and 30 or less was marked as "○", the case where it was more than 30 and 50 or less was marked as "×", and the case where it was more than 50 was marked as "××", and the adhesion between the resin particles and the conductive part was evaluated.
[0222] (3) Insulation reliability (horizontal)
[0223] 100 connection structures obtained in the same manner as in the above "(1) Long-term connection reliability under high temperature conditions" were left at 200°C for 24 hours. The resistance values of the 100 connection structures after leaving were measured with a tester to confirm whether there was leakage between adjacent electrodes.
[0224] Set the resistor value to 10 8 The case where the number of connection structures with Ω or more is 100 is set as "○○○", the case where the number is 90 or more and less than 100 is set as "○○", the case where the number is 80 or more and less than 90 is set as "○", the case where the number is 70 or more and less than 80 is set as "×", and the case where the number is less than 70 is set as "××", and the insulation reliability (horizontal) is evaluated.
[0225]
Table 1
[0226]
[0227]
Table 2
[0228]
[0229] Industrial Applicability
[0230] According to the present invention, a resin particle having excellent heat resistance can be provided, and when used as a substrate particle of conductive particles, a connection structure that can cope with thermocompression mounting under low pressure and has excellent connection reliability can be obtained. In addition, according to the present invention, conductive particles, conductive materials, and connection structures formed by using the resin particles can be provided.
Claims
1. A conductive particle, characterized in that: The invention comprises a resin particle and a conductive layer formed on the surface of the resin particle. The resin particles have a main chain skeleton including an imide group. The resin particles have segments derived from bismaleimide. The content ratio of the segment derived from bismaleimide is 1 mol% or more, The resin particles have a 5% weight loss temperature of 350°C or higher and a 10% K value of 100 N / mm at 25°C. 2 Above and 2500N / mm 2 Below, 30% K value at 25℃ is 100N / mm 2 Above and 1500N / mm 2 The coefficient of variation of the aspect ratio is less than 10%.
2. The conductive particle according to claim 1, wherein The average particle diameter of the resin particles is 0.1 μm or more and 1000 μm or less.
3. The conductive particle according to claim 1 or 2, wherein The coefficient of variation of the particle diameter of the resin particles obtained by particle size distribution measurement is 20% or less.
4. The conductive particle according to claim 1 or 2, wherein When the resin particles are heated at 200° C. for 24 hours, a change in 30% K value before and after heating is 200% or less.
5. The conductive particle according to claim 1, wherein An insulating material is provided on the outer surface of the conductive layer. The conductive particle according to claim 1, wherein The conductive layer has protrusions on its outer surface. 7 . A conductive material comprising the conductive particles according to claim 1 and a binder resin.
8. A connection structure comprising a first connection object member having a first electrode on its surface, a second connection object member having a second electrode on its surface, and a connection portion connecting the first connection object member and the second connection object member, The constituent material of the connecting portion is the conductive particle according to any one of claims 1 to 6 or the conductive material according to claim 7 .