Polyester, film and adhesive composition, adhesive sheet, laminate and printed wiring board

By using polycyclic carboxylic acids and polyols with polycyclic structures and long carbon chains to prepare polyester, and combining them with curing agents, the problems of poor dielectric properties of polyester resins and insufficient heat resistance of adhesives in the prior art are solved. Problem, the low dielectric properties and high bonding strength of polyester in the high-frequency region are achieved, and it is suitable for the base film and adhesive of FPC.

CN115298244BActive Publication Date: 2024-10-11TOYOBO MC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180022537.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-30
Filing Date
2021-03-26
Publication Date
2024-10-11
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

The existing polyester resin has poor dielectric properties in the high-frequency region and the adhesive has insufficient heat resistance, making it difficult to meet the high-performance requirements of FPC.

Method used

Using polyester with polycyclic structure of polycarboxylic acid and polyol, combined with long carbon chain polycarboxylic acid and polyol, by controlling the molar ratio and molecular weight, a polyester with low dielectric constant and dielectric loss tangent is prepared. ester and combined with a curing agent to form an adhesive, forming a composition with excellent dielectric properties and heat resistance.

Benefits of technology

A polyester with low dielectric properties and high bonding strength in the high-frequency region has been realized, which is suitable for the base film and adhesive of FPC and improves the performance of printed circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003852679990000211
    Figure BDA0003852679990000211
Patent Text Reader

Abstract

The subject of the present invention is to provide a polyester, film and adhesive composition having excellent solvent solubility, heat resistance, and bonding strength, small relative dielectric constant and dielectric loss tangent, and excellent dielectric properties, as well as adhesive sheets, laminates, and printed circuit boards using the same. As a solution, a polyester contains the following monomers (A) and (B) as constituent components, and when the total amount of all constituent components is set to 100 mol%, it contains more than 25 mol% of monomer (A) and more than 10 mol% of monomer (B), and the total amount of monomer (A) and monomer (B) is more than 60 mol%, monomer (A): a polycarboxylic acid component and / or a polyol component having a polycyclic structure, and monomer (B): a polycarboxylic acid component and / or a polyol component having a continuous carbon chain of more than 10 carbon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to polyester and more particularly to a polyester having excellent dielectric properties, a film and an adhesive composition, and an adhesive sheet, a laminate and a printed wiring board having a layer formed of the polyester and the film. Background Art

[0002] Polyester is widely used as a raw material for resin compositions used in coating agents, inks, adhesives, etc., and is generally composed of polycarboxylic acids and polyols. Since the flexibility and molecular weight can be freely controlled by selecting and combining polycarboxylic acids and polyols, it is widely used in various applications, such as coating applications and adhesive applications.

[0003] Among them, polyester has excellent adhesion to metals including copper, and is mixed with a curing agent such as epoxy resin and used in adhesives for FPCs and the like (for example, Patent Document 1).

[0004] FPC, due to its excellent bending property, can cope with multifunctionalization and miniaturization such as personal computer (PC) or smart phone, and is therefore mostly used to assemble electronic circuit substrate in narrow and complex interior. In recent years, electronic machines are being miniaturized, lightweight, high-densified, and high-output, because these popular requirements for the performance of circuit board (electronic circuit substrate) are getting higher and higher. Especially with the high speed of the transmission signal of FPC, the high frequency of signal is developing. Then the requirement of low dielectric properties (low dielectric constant, low dielectric loss tangent) of FPC in high frequency region becomes higher. In addition, for the substrate used in FPC, not only existing polyimide (PI) or polyethylene terephthalate (PET) are proposed, but also substrate films such as liquid crystal polymer (LCP) or syndiotactic polystyrene (SPS) with low dielectric properties are proposed. As mentioned above, in order to realize low dielectric properties, a strategy for reducing the dielectric loss of the substrate or adhesive of FPC has been made. The development of the combination of polyolefin and epoxy resin as adhesive (patent document 2) etc. is underway.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Publication No. 6-104813

[0008] Patent Document 2: WO2016 / 047289 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] However, the polyester resin described in Patent Document 1 has high relative dielectric constant and dielectric loss tangent, does not have the above-mentioned low dielectric properties and is not suitable for FPC in high-frequency regions. In addition, the adhesive described in Patent Document 2 is difficult to be said to have excellent heat resistance as an adhesive used as a reinforcing plate or between layers.

[0011] The present invention is made with the problems of the related prior art as the background. That is, the purpose of the present invention is to provide polyester, film and adhesive composition having excellent solvent solubility, heat resistance, excellent bonding strength, low relative dielectric constant and dielectric loss tangent, and excellent dielectric properties, and adhesive sheets, laminates and printed wiring boards having layers formed therefrom.

[0012] Means to solve problems

[0013] As a result of intensive studies, the present inventors have found that the above-mentioned problems can be solved by the means described below, thereby completing the present invention.

[0014] That is, the present invention includes the following configurations.

[0015] A polyester comprising the following monomers (A) and (B) as constituent components, wherein when the total amount of all constituent components is taken as 100 mol %, the polyester comprises 25 mol % or more of the monomer (A) and 10 mol % or more of the monomer (B), and the total amount of the monomers (A) and (B) is 60 mol % or more.

[0016] Monomer (A): a polycarboxylic acid component having a polycyclic structure and / or a polyol component having a polycyclic structure

[0017] Monomer (B): a polycarboxylic acid component having a continuous carbon chain of 10 or more carbon atoms and / or a polycarboxylic acid component having a continuous carbon chain of 10 or more carbon atoms; a polyol component

[0018] The glass transition temperature of the polyester is above -30°C.

[0019] The polyester preferably has a relative dielectric constant (εc) of 3.0 or less and a dielectric loss factor (tan δ) of 0.008 or less at 10 GHz.

[0020] A film comprising the polyester.

[0021] An adhesive composition contains the polyester.

[0022] An adhesive sheet having a layer formed of the adhesive composition.

[0023] A laminate having a layer formed from the adhesive composition.

[0024] A printed wiring board includes the laminate as a constituent element.

[0025] Effects of the Invention

[0026] The polyester of the present invention has excellent solvent solubility, heat resistance, adhesive strength, and dielectric properties, and is therefore suitable for base films for FPCs and adhesives for FPCs in high-frequency regions, as well as adhesive sheets, laminates, and printed wiring boards. DETAILED DESCRIPTION

[0027] Hereinafter, one embodiment of the present invention will be described in detail, but the present invention is not limited thereto and can be implemented in various modified embodiments within the scope described above.

[0028] <Polyester>

[0029] The polyester of the present invention is composed of a chemical structure obtainable from a polycondensate of a polycarboxylic acid component and a polyol component, and is composed of one or more components selected from polycarboxylic acid components and polyol components.

[0030] The polyester of the present invention contains the following monomer (A) and monomer (B) as constituent components.

[0031] Monomer (A): a polycarboxylic acid component and / or a polyol component having a polycyclic structure,

[0032] Monomer (B): a polycarboxylic acid component and / or a polyol component having a continuous carbon chain of 10 or more carbon atoms

[0033] <Single substance (A)>

[0034] Monomer (A) is a polycarboxylic acid component and / or a polyol component having a polycyclic structure. A polycyclic structure refers to a structure formed by combining a plurality of ring structures mainly composed of carbon atoms, for example, structures having aromatic skeletons such as naphthalene, anthracene, indane, tetralin, and structures having alicyclic skeletons such as decalin, norbornane, and tricyclosilane. By having a polycyclic structure, the free volume of the polyester increases, and low dielectric properties are exerted.

[0035] Examples of the monomer (A) of the polyvalent carboxylic acid component or polyol component having a polycyclic structure include 2,6-naphthalene dicarboxylic acid, tricyclodecane dimethanol, pentacyclodecane dimethanol, bisphenol fluorene, bisphenoxyethanol fluorene, bisphenoxymethanol fluorene, biscresol fluorene, spiroglycol, and hydrogenated naphthalene dicarboxylic acid.

[0036] In the polyester of the present invention, when the total amount of all constituent components is set to 100 mol%, the monomer (A) is contained in an amount of 25 mol% or more. Preferably, it is 40 mol% or more, more preferably 50 mol% or more, and further preferably 60 mol% or more. By containing the monomer (A) in an amount above the above value, the low dielectric properties are improved. In particular, the effect on the dielectric loss tangent is large.

[0037] <Single substance (B)>

[0038] Monomer (B) is a polycarboxylic acid component and / or a polyol component with a continuous carbon chain of more than 10 carbon atoms. As a carbochain, it refers to a structure with a continuous carbon-carbon bond. Monomer (B) is a polycarboxylic acid component and / or a polyol component, but by carboxylic acid groups or alcohol groups continuously spaced apart by more than 10 carbon chains, the polar concentration of polyester is reduced, which contributes to low dielectric properties. Ring structure can be provided in the carbochain, but carboxylic acid groups or alcohol groups need to be spaced apart by more than 10 carbon atoms at the shortest. In addition, from the viewpoint of low dielectric properties, it is preferred that the carbochain does not contain heteroatoms such as nitrogen, oxygen, and sulfur except carbolic acid groups or alcohol groups, and it is preferred that the carbochain is hydrocarbon.

[0039] Examples of the monomer (B) of a polycarboxylic acid component or a polyol component having a continuous carbon chain of 10 or more carbon atoms include dimer acid, dimer alcohol, dimer acid ester (polyester polyol derived from dimer acid), hydroxyl-terminated polybutadiene, hydroxyl-terminated hydrogenated polybutadiene, hydroxyl-terminated polyisoprene, and hydroxyl-terminated polyolefin.

[0040] The above-mentioned dimer acid refers to a polymerized fatty acid having 20 to 48 carbon atoms obtained by dimerizing unsaturated fatty acids having C10 to 24. In addition, saturated dimer acids obtained by hydrogenating these unsaturated groups are also included. Dimer alcohols are obtained by reducing the carboxyl groups of dimer acids. Vegetable oils can be used as raw materials for dimer acids and dimer alcohols. In addition, dimer alcohols can also include trimers of trimers of unsaturated fatty acids having 10 to 24 carbon atoms or saturated trimers obtained by hydrogenating trimers.

[0041] The number average molecular weight of the monomer (B) is preferably 300 or more, more preferably 400 or more, and even more preferably 500 or more. As the molecular weight increases, the concentration of polar groups decreases, thereby improving low dielectric properties.

[0042] In the polyester of the present invention, when the total amount of all constituent components is set to 100 mol%, the monomer (B) is contained in an amount of 10 mol% or more. Preferably, it is 15 mol% or more, more preferably 20 mol% or more, and further preferably 25 mol% or more. By containing the monomer (B) in an amount greater than the above value, the low dielectric properties are improved. In addition, the solvent solubility of the polyester is also excellent.

[0043] In the polyester of the present invention, when the total amount of all constituent components is set to 100 mol%, the total amount of monomer (A) and monomer (B) contains 60 mol% or more. More preferably, it is 70 mol% or more, further preferably 80 mol% or more, particularly preferably 85 mol% or more, and most preferably 90 mol% or more. It can be 100 mol%. As described above, by containing 25 mol% or more of monomer (A), 10 mol% or more of monomer (B) and the total amount of monomer (A) and monomer (B) containing more than the value, it is possible to obtain a polyester having excellent low dielectric properties and a good balance of various physical properties such as solvent solubility and glass transition temperature.

[0044] The polyester of the present invention may contain a polycarboxylic acid component and a polyol component other than the monomer (A) and the monomer (B). The polycarboxylic acid component other than the monomer (A) and the monomer (B) is not particularly limited, and the polycarboxylic acid component is preferably an aromatic polycarboxylic acid component or an alicyclic polycarboxylic acid component, and more preferably an aromatic dicarboxylic acid component or an alicyclic dicarboxylic acid component. By using an aromatic polycarboxylic acid component or an alicyclic polycarboxylic acid component as a copolymerization component, excellent dielectric properties can be exhibited.

[0045] The aromatic dicarboxylic acid component is not particularly limited, and terephthalic acid, isophthalic acid, phthalic acid, 4,4′-dicarboxybiphenyl, 5-sodium sulfoisophthalate, and the like can be used.

[0046] The alicyclic dicarboxylic acid is not particularly limited, and 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, tetrahydrophthalic acid, methyltetrahydrophthalic acid, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, and the like can be used.

[0047] The polyol component other than the monomer (A) and the monomer (B) is not particularly limited, and ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 2-methyl-1,3-propanediol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 2-methyl-2-ethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, aliphatic polyols such as 1,4-cyclohexanedimethanol and the like; polyalkylene glycols such as polytetramethylene glycol and polypropylene glycol; and the like. One or more of these may be used.

[0048] In the polyester of the present invention, a polycarboxylic acid component of 3 or more and / or a polyol component of 3 or more can be copolymerized. As a polycarboxylic acid component of 3 or more, for example, aliphatic carboxylic acids such as trimellitic acid, pyromellitic acid, benzophenone tetracarboxylic acid, trimellitic acid, trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), 1,2,3,4-butane tetracarboxylic acid, etc. can be listed, and these can use one or more than two kinds. As a polyol component of 3 or more, for example, glycerol, trimethylolpropane, trimethylolethane, pentaerythritol, α-methyl glucose, mannitol, sorbitol can be used, and these can use one or more than two kinds. However, if the copolymerization amount of the polycarboxylic acid component of 3 or more and / or the polyol component of 3 or more is large, the dielectric properties of the polyester are sometimes deteriorated, so it is not preferred. When a trivalent or higher polycarboxylic acid component and / or a trivalent or higher polyol component is copolymerized, the content is preferably 3 mol% or less, more preferably 2 mol% in 100 mol% of the total of all components.

[0049] The dielectric loss tangent of the polyester of the present invention at 10 GHz is preferably 0.008 or less, more preferably 0.005 or less. By using a polyester having a low dielectric loss tangent, an adhesive composition having excellent low dielectric properties can be formed.

[0050] The relative dielectric constant of the polyester of the present invention at 10 GHz is preferably 3.0 or less, more preferably 2.6 or less. By using a polyester having a low relative dielectric constant, an adhesive composition having excellent low dielectric properties can be formed.

[0051] The glass transition temperature of the polyester of the present invention is preferably -30°C or higher, more preferably -20°C or higher. By setting the glass transition temperature to a range of -30°C or higher, good dielectric properties can be exhibited, and further, the stickiness (adhesion) of the resin surface tends to be suppressed, and the handleability of the resin is improved. In addition, the glass transition temperature is preferably 100°C or lower. By setting the glass transition temperature to 100°C or lower, lamination can be performed even at a low temperature of about 80°C. In addition, the lower the glass transition temperature, the better the bonding strength tends to be.

[0052] As methods for the polycondensation reaction of producing the polyester of the present invention, there are, for example, 1) a method of heating a polycarboxylic acid and a polyol in the presence of a known catalyst, and performing a dehydration esterification step to carry out a depolyol removal / polycondensation reaction; 2) a method of heating an alcohol ester of a polycarboxylic acid and a polyol in the presence of a known catalyst, and performing an ester exchange reaction to carry out a depolyol removal / polycondensation reaction; 3) a method of carrying out a depolymerization. In the above methods 1) and 2), part or all of the acid may be replaced by anhydride.

[0053] When producing the polyester of the present invention, a known polymerization catalyst can be used, for example, titanium compounds such as tetra-n-butyl titanate, tetraisopropyl titanate, and titanium acetylacetonate, antimony compounds such as antimony trioxide and antimony butoxide, germanium compounds such as germanium oxide and tetra-n-butoxygermane, and other compounds such as magnesium, iron, zinc, manganese, cobalt, and aluminum. These catalysts can be used alone or in combination of two or more.

[0054] The number average molecular weight of the polyester in the present invention is preferably 5000 or more, more preferably 10000 or more. In addition, it is preferably 100000 or less, more preferably 50000 or less, and further preferably 30000 or less. If it is within the above range, it is easy to dissolve in a solvent, the adhesive strength becomes good, and it is also preferred because of its excellent dielectric properties.

[0055] The acid value of the polyester in the present invention is not particularly limited and can be appropriately designed according to the curing agent used in combination. In the case of isocyanate curing, it is preferably 200 eq / 10 6 g or less, more preferably 100 eq / 10 6 g or less, more preferably 50eq / 10 6 g or less, particularly preferably 40eq / 10 6 g or less, and most preferably 30eq / 10 6 In the case of epoxy curing, it is preferably 20eq / 10 6 g or more, more preferably 50eq / 10 6 g or more, and most preferably 100 eq / 10 6 By setting the acid value of the resin within the above range, it is expected that the pot life, substrate adhesion and crosslinking properties will be improved. From the viewpoint of low dielectric properties, isocyanate curing systems are preferred.

[0056] As methods for increasing the acid value of the polyester in the present invention, there are methods such as (1) adding a trivalent or higher polycarboxylic acid and / or a trivalent or higher polycarboxylic acid anhydride and reacting them after the polycondensation reaction is completed (acid addition); (2) modifying the resin purposefully by the action of heat, oxygen, water, etc. during the polycondensation reaction; and the like, which can be performed arbitrarily. The polycarboxylic acid anhydride used for the acid addition in the acid addition method is not particularly limited, and for example, trimellitic anhydride, pyrophthalic anhydride, hexahydrophthalic anhydride, 3,3,4,4.-benzophenonetetracarboxylic anhydride, 3,3,4,4-biphenyltetracarboxylic anhydride, ethylene glycol ditriphthalic anhydride, etc. can be used, and one or more of these can be used. Triphthalic anhydride is preferred.

[0057] The polyester of the present invention can be used as a film. When the polyester of the present invention is used as a film, the polyester can be directly processed into a film shape, and further, the polyester dispersed with various fillers such as glass fiber and silica can be processed into a film shape. The thickness and shape of the film of the present invention are not particularly limited, and sometimes include a form called a sheet.

[0058] Since the film of the present invention has excellent dielectric properties, it is suitable as a rigid substrate for high-speed transmission or a CCL base film of FPC.

[0059] The polyester of the present invention can be used as an adhesive. In particular, the polyester of the present invention is excellent in dielectric properties and is therefore suitable as an adhesive for FPC in a high-frequency range.

[0060] When the polyester of the present invention is used as an adhesive, it may further contain a curing agent to form an adhesive composition.

[0061] <Curing agent>

[0062] As the curing agent, epoxy resin, polyisocyanate, polycarbodiimide etc. can be used. By using these curing agents to carry out crosslinking, the cohesive force of the resin can be improved and heat resistance can be improved. Among them, polyisocyanate is preferred from the aspect that the influence on heat resistance and dielectric properties is small.

[0063] <Epoxy resin>

[0064] As the epoxy resin used in the present invention, as long as it is an epoxy resin with an epoxy group in the molecule, it is not particularly limited, and preferably an epoxy resin with more than 2 epoxy groups in the molecule. Specifically, it is not particularly limited, but at least one selected from the group consisting of biphenyl type epoxy resin, naphthalene type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, novolac type epoxy resin, alicyclic epoxy resin, dicyclopentadiene type epoxy resin, tetraglycidyl diaminodiphenylmethane, triglycidyl p-aminophenol, tetraglycidyl bisaminomethyl cyclohexanone, N,N,N',N'-tetraglycidyl-m-xylene diamine and epoxy-modified polybutadiene can be cited. Preferred biphenyl type epoxy resin, novolac type epoxy resin, dicyclopentadiene type epoxy resin or epoxy-modified polybutadiene. More preferably dicyclopentadiene type epoxy resin or novolac type epoxy resin.

[0065] In the adhesive composition of the present invention, relative to 100 mass parts of polyester, the content of epoxy resin is preferably more than 0.1 mass parts, more preferably more than 0.5 mass parts, further preferably more than 1 mass parts, particularly preferably more than 2 mass parts. By being set to more than the above-mentioned lower limit, sufficient curing effect can be obtained, and excellent adhesion and solder heat resistance can be exerted. In addition, preferably less than 60 mass parts, more preferably less than 50 mass parts, further preferably less than 40 mass parts, particularly preferably less than 35 mass parts. By being set to less than the above-mentioned upper limit, the service life and low dielectric properties become good. That is, by being set within the above-mentioned range, it is possible to obtain an adhesive composition having excellent low dielectric properties in addition to adhesion, solder heat resistance and service life.

[0066] <Polycarbodiimide>

[0067] The polycarbodiimide used in the present invention is not particularly limited as long as it has a carbodiimide group in the molecule. Preferably, it is a polycarbodiimide having two or more carbodiimide groups in the molecule. By using the polycarbodiimide, the carboxyl group of the polyester reacts with the carbodiimide group, which can enhance the interaction between the adhesive composition and the substrate and improve the adhesion.

[0068] In the adhesive composition of the present invention, the content of polycarbodiimide is preferably more than 0.1 mass parts relative to 100 mass parts of polyester, more preferably more than 0.5 mass parts, further preferably more than 1 mass parts, particularly preferably more than 2 mass parts. When being set to above the lower limit, the interaction with the substrate is shown and the adhesion becomes good. In addition, preferably less than 30 mass parts, more preferably less than 25 mass parts, further preferably less than 20 mass parts, further preferably less than 15 mass parts, particularly preferably less than 10 mass parts. By being set to below the upper limit, excellent applicability and low dielectric properties can be brought into play. That is, by within the above range, it is possible to obtain an adhesive composition having excellent low dielectric properties in addition to adhesion, solder heat resistance and applicability.

[0069] <Polyisocyanate>

[0070] The polyisocyanate used in the present invention is not particularly limited as long as it is an isocyanate compound that reacts with a polyester to be cured.

[0071] As polyisocyanates, aromatic or aliphatic diisocyanate compounds, trivalent or higher polyisocyanate compounds can be cited. These isocyanate compounds can be low molecular weight compounds or high molecular weight compounds. For example, aliphatic diisocyanates such as tetramethylene diisocyanate and hexamethylene diisocyanate, aromatic diisocyanates such as toluene diisocyanate, diphenylmethane diisocyanate, and xylene diisocyanate, alicyclic diisocyanates such as hydrogenated diphenylmethane diisocyanate, hydrogenated xylene diisocyanate, dimer acid diisocyanate, and isophorone diisocyanate, or trimers of their isocyanate compounds can be cited. In addition, compounds containing terminal isocyanate groups obtained by reacting excessive amounts of the above-mentioned isocyanate compounds with low molecular weight active hydrogen compounds such as ethylene glycol, propylene glycol, trimethylolpropane, glycerol, sorbitol, ethylenediamine, monoethanolamine, diethanolamine, and triethanolamine can be cited. In addition, compounds containing terminal isocyanate groups obtained by reacting excessive amounts of the above-mentioned isocyanate compounds with various polyester polyols, polyether polyols, and high molecular active hydrogen compounds of polyamides can be cited. These isocyanate compounds can be used alone or in combination of two or more. Among them, trimers of hexamethylene diisocyanate compounds are particularly preferred.

[0072] In the adhesive composition of the present invention, the content of polyisocyanate is preferably 0.1 mass parts or more relative to 100 mass parts of polyester, more preferably 0.5 mass parts or more, further preferably 1 mass parts or more, particularly preferably 2 mass parts or more. By being set to more than the above-mentioned lower limit, the interaction with the substrate is shown and the adhesion becomes good. In addition, preferably less than 30 mass parts, more preferably less than 25 mass parts, further preferably less than 20 mass parts, further preferably less than 15 mass parts, particularly preferably less than 10 mass parts. By being set to less than the above-mentioned upper limit, excellent workability and low dielectric properties can be exerted. That is, by being set within the above-mentioned range, an adhesive composition having particularly excellent low dielectric properties in addition to adhesion, solder heat resistance and workability can be obtained.

[0073] <Organic solvents>

[0074] The adhesive composition of the present invention may also contain an organic solvent. The organic solvent used in the present invention is not particularly limited as long as it can dissolve the polyester and the curing agent. Specifically, for example, aromatic hydrocarbons such as benzene, toluene, and xylene, aliphatic hydrocarbons such as hexane, heptane, octane, and decane, alicyclic hydrocarbons such as cyclohexane, cyclohexene, methylcyclohexane, and ethylcyclohexane, halogenated hydrocarbons such as trichloroethylene, dichloroethylene, chlorobenzene, and chloroform, alcohol solvents such as methanol, ethanol, isopropanol, butanol, pentanol, hexanol, propylene glycol, and phenol, acetone, methyl isobutyl ketone, methyl ethyl ketone, pentanone, hexanone, cyclopentane, and the like can be used. Ketone solvents such as hexanone, isophorone, and acetophenone, cellosolves such as methyl cellosolve and ethyl cellosolve, ester solvents such as methyl acetate, ethyl acetate, butyl acetate, methyl propionate, and butyl formate, and glycol ether solvents such as ethylene glycol mono-n-butyl ether, ethylene glycol mono-isobutyl ether, ethylene glycol mono-tert-butyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol mono-isobutyl ether, triethylene glycol mono-n-butyl ether, and tetraethylene glycol mono-n-butyl ether may be used in combination of one or more thereof. In particular, methylcyclohexane and toluene are preferred from the viewpoint of working environment and drying properties.

[0075] The organic solvent is preferably in the range of 100 to 1000 parts by mass relative to 100 parts by mass of the polyester. By setting it to be above the lower limit, the liquid state and shelf life become good. In addition, by setting it to be below the upper limit, it is advantageous in terms of manufacturing cost and transportation cost.

[0076] The adhesive composition of the present invention may further contain other components as necessary. Specific examples of the above-mentioned components include flame retardants, tackifiers, fillers, and silane coupling agents.

[0077] <Flame retardant>

[0078] The adhesive composition of the present invention can be mixed with a flame retardant as needed. Examples of flame retardants include bromine, phosphorus, nitrogen or metal hydroxide compounds. Among them, phosphorus flame retardants are preferred, and known phosphorus flame retardants such as phosphates (such as trimethyl phosphate, triphenyl phosphate, tricresyl phosphate, etc.), phosphates (such as aluminum phosphite), and phosphazenes can be used. They can be used alone or in any combination of two or more. When containing a flame retardant, it is preferably 1 to 200 parts by mass, more preferably 5 to 150 parts by mass, and most preferably 10 to 100 parts by mass relative to 100 parts by mass of the total amount of polyester and curing agent components. Within the above range, flame retardancy can be exhibited while maintaining adhesion, solder heat resistance and electrical properties.

[0079] <Thickener>

[0080] In the adhesive composition of the present invention, a tackifier can be mixed as needed. As a tackifier, polyterpene resin, rosin resin, aliphatic petroleum resin, alicyclic petroleum resin, copolymerized petroleum resin, styrene resin and hydrogenated petroleum resin etc. can be listed, which are used for the purpose of improving bonding strength. These can be used alone or in any combination of two or more. When containing a tackifier, relative to the total amount of 100 parts by mass of polyester and curing agent components, it is preferably contained 1 to 200 parts by mass, more preferably contains 5 to 150 parts by mass, and most preferably contains 10 to 100 parts by mass. By setting it within the above range, the effect of the tackifier can be shown while maintaining adhesion, solder heat resistance and electrical properties.

[0081] <Packing>

[0082] In the adhesive composition of the present invention, fillers can be mixed as needed. In addition, as an organic filler, powders of polyimide, polyamide-imide, etc. as heat-resistant resins can be cited. In addition, as an inorganic filler, for example, silicon dioxide (SiO2), aluminum oxide (Al2O3), titanium dioxide (TiO2), tantalum oxide (Ta2O5), zirconium oxide (ZrO2), silicon nitride (Si3N4), boron nitride (BN), calcium carbonate (CaCO3), calcium sulfate (CaSO4), zinc oxide (ZnO), magnesium titanate (MgO / TiO2), barium sulfate (BaSO4), organic bentonite, clay, mica, aluminum hydroxide, magnesium hydroxide, etc., wherein silicon dioxide is preferred from the effect of improving the heat resistance of the dispersant. As silicon dioxide, it is known that there are common hydrophobic silicon dioxide and hydrophilic silicon dioxide, here based on imparting hygroscopicity resistance, preferably hydrophobic silicon dioxide after treatment with dimethyldichlorosilane or hexamethyldisilazane, octylsilane, etc. When silica is mixed, its proportion is preferably 0.05 to 30 parts by mass relative to 100 parts by mass of the total amount of the polyester and the curing agent component. By being above the above lower limit, further heat resistance can be exhibited. In addition, by being below the above upper limit, poor dispersion of silica and excessively high solution viscosity can be suppressed, and operability is good.

[0083] <Silane coupling agent>

[0084] In the adhesive composition of the present invention, a silane coupling agent may be mixed as needed. By mixing the silane coupling agent, it is very preferred because it can improve the adhesion and heat resistance to metal. As the silane coupling agent, there is no particular limitation, and examples thereof include silane coupling agents with unsaturated groups, silane coupling agents with glycidyl groups, silane coupling agents with amino groups, etc. Among these, from the viewpoint of heat resistance, silane coupling agents with epoxy groups such as γ-glycidyloxypropyltrimethoxysilane or β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane or β-(3,4-epoxycyclohexyl)ethyltriethoxysilane are further preferred. When the silane coupling agent is mixed, the mixing amount is preferably 0.5 to 20 parts by mass relative to 100 parts by mass of the total amount of the polyester and the curing agent component. By being within the above range, the heat resistance and adhesion of solder can be improved.

[0085] <Laminated body>

[0086] The laminate of the present invention is a laminate obtained by laminating the adhesive composition on a substrate (a two-layer laminate of substrate / adhesive layer), or a laminate obtained by further laminating a substrate (a three-layer laminate of substrate / adhesive layer / substrate). Here, the adhesive layer refers to a layer of the adhesive composition after the adhesive composition of the present invention is applied to a substrate and dried. The laminate of the present invention can be obtained by applying the adhesive composition of the present invention to various substrates according to conventional methods, drying and further laminating other substrates.

[0087] <Base material>

[0088] The substrate in the present invention is not particularly limited as long as it can be coated with the adhesive composition of the present invention and dried to form an adhesive layer, and examples thereof include resin substrates such as film-like resins, metal substrates such as metal plates and metal foils, and paper.

[0089] Examples of the resin substrate include polyester resins, polyamide resins, polyimide resins, polyamideimide resins, liquid crystal polymers, polyphenylene sulfide, syndiotactic polystyrene, polyolefin resins, and fluorine resins, etc. Film-like resins (hereinafter also referred to as substrate film layers) are preferred.

[0090] As a metal substrate, any known conductive material that can be used for a circuit board can be used. As a material, various metals such as SUS, copper, aluminum, iron, steel, zinc, nickel, and their respective alloys, plated products, metals treated with other metals such as zinc or chromium compounds, etc. can be exemplified. It is preferably a metal foil, and more preferably a copper foil. There is no particular limitation on the thickness of the metal foil, but it is preferably 1 μm or more, more preferably 3 μm or more, and more preferably 10 μm or more. In addition, it is preferably 50 μm or less, more preferably 30 μm or less, and more preferably 20 μm or less. When the thickness is too thin, the circuit sometimes cannot obtain sufficient electrical performance. On the other hand, when the thickness is too thick, there will be a decrease in processing efficiency when making the circuit. The metal foil is usually provided in a roll form. There is no particular limitation on the form of the metal foil used when manufacturing the printed wiring board of the present invention. When a strip-shaped metal foil is used, there is no particular limitation on its length. In addition, there is no particular limitation on its width, but it is preferably about 250 to 500 cm. The surface roughness of the substrate is not particularly limited, but is preferably 3 μm or less, more preferably 2 μm or less, and further preferably 1.5 μm or less. In practical terms, it is preferably 0.3 μm or more, more preferably 0.5 μm or more, and further preferably 0.7 μm or more.

[0091] Examples of paper include woodfree paper, kraft paper, toilet paper, glassine, etc. Examples of composite materials include glass epoxy resin, etc.

[0092] Based on the adhesion and durability with the adhesive composition, the substrate is preferably a polyester resin, a polyamide resin, a polyimide resin, a polyamideimide resin, a liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene, a polyolefin resin, a fluorine resin, a SUS steel plate, a copper foil, an aluminum foil or a glass epoxy resin.

[0093] <Adhesive Sheet>

[0094] In the present invention, the adhesive sheet refers to the adhesive sheet obtained by laminating the above-mentioned laminate and the release substrate via the adhesive composition. As a specific configuration mode, it can be exemplified that the laminate / adhesive layer / release substrate, or release substrate / adhesive layer / laminated body / adhesive layer / release substrate. By laminating the release substrate, it can function as a protective layer of the substrate. In addition, by using the release substrate, the release substrate can be demoulded from the adhesive sheet, and the adhesive layer can be further transferred to other substrates.

[0095] The adhesive composition of the present invention can be applied to various laminates and dried according to a conventional method to obtain the adhesive sheet of the present invention. In addition, after drying, if a release substrate is pasted on the adhesive layer, it can be rolled up without being sticky with the substrate, and the workability is excellent. At the same time, since the adhesive layer is protected, the preservation is excellent and easy to use. In addition, after being applied to a release substrate and dried, other release substrates are pasted as needed, and the adhesive layer itself can be transferred to other substrates.

[0096] <Mold release substrate>

[0097] There is no particular limitation on the release substrate, but for example, a release substrate obtained by providing a coating of a filler such as clay, polyethylene, or polypropylene on both sides of paper such as woodfree paper, kraft paper, toilet paper, or glassine paper, and further applying a silicone, fluorine, or alkyd release agent on each coating. In addition, a release substrate obtained by applying the above release agent on a single olefin film such as polyethylene, polypropylene, ethylene-α-olefin copolymer, propylene-α-olefin copolymer, or a film such as polyethylene terephthalate can also be cited. Based on the reasons of the release force between the release substrate and the adhesive layer, and the negative impact of silicone on electrical properties, a release substrate obtained by using an alkyd release agent after filling the holes on both sides of woodfree paper with polypropylene, or a release substrate obtained by using an alkyd release agent on polyethylene terephthalate is preferred.

[0098] In addition, as the method of applying the adhesive composition to the substrate in the present invention, there is no particular limitation, and examples thereof include a comma coater, a reverse roll coater, and the like. Alternatively, as required, an adhesive layer may be provided directly or by a transfer method on a rolled copper foil or a polyimide film as a constituent material of a printed wiring board. The thickness of the adhesive layer after drying may be appropriately changed as required, but is preferably in the range of 5 to 200 μm. By making the thickness of the adhesive film 5 μm or more, sufficient bonding strength can be obtained. In addition, by setting it to less than 200 μm, it is easy to control the amount of residual solvent in the drying process, and it is not easy to produce blistering during the manufacturing and pressing of the printed wiring board. There is no particular limitation on the drying conditions, and the residual solvent rate after drying is preferably less than 1% by mass. By being less than 1% by mass, the blistering of the residual solvent during the pressing of the printed wiring board can be suppressed, and it is not easy to produce blistering.

[0099] <Printed circuit board>

[0100] The "printed wiring board" in the present invention refers to a printed wiring board containing a laminate formed by a metal foil and a resin substrate forming a conductor circuit as a constituent element. The printed wiring board is manufactured, for example, by using a metal-clad laminate by a subtractive method or other existing known methods. As required, so-called flexible printed circuits (FPCs), flat cables, and circuit boards for tape automated bonding (TAB) that partially or fully cover a conductor circuit formed by a metal foil using a covering film or screen printing ink are collectively referred to as printed wiring boards.

[0101] The printed wiring board of the present invention can be composed of any laminate that can be used as a printed wiring board. For example, it can be a printed wiring board composed of four layers of a base film layer, a metal foil layer, an adhesive layer, and a cover film layer. Another example is that it can be a printed wiring board composed of five layers of a base film layer, an adhesive layer, a metal foil layer, an adhesive layer, and a cover film layer.

[0102] Furthermore, the printed wiring board may be formed by laminating two or three or more layers as required.

[0103] The adhesive composition of the present invention can be applied to each adhesive layer of a printed wiring board. In particular, when the adhesive composition of the present invention is used as an adhesive, it has high adhesion to existing polyimide, polyester film, copper foil constituting a printed wiring board, and low-polarity resin substrates such as LCP, and can obtain reflow resistance, and the adhesive layer itself has excellent low dielectric properties. Therefore, it is suitable for use as an adhesive composition used in a coverlay film, a laminate, an incidental resin copper foil, and an adhesive sheet.

[0104] In the printed wiring board of the present invention, as the substrate film, any resin film used as the substrate of the existing printed wiring board can be used. As the resin of the substrate film, polyester resin, polyamide resin, polyimide resin, polyamide-imide resin, liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene, polyolefin resin and fluorine resin can be exemplified. In particular, it has excellent adhesion to low-polarity substrates such as liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene and polyolefin resin.

[0105] <Cover film>

[0106] As the cover film, as the insulating film for the printed circuit board, any known insulating film can be used. For example, films made of various polymers such as polyimide, polyester, polyphenylene sulfide, polyether sulfone, polyether ether ketone, aramid, polycarbonate, polyarylate, polyamide-imide, liquid crystal polymer, syndiotactic polystyrene, polyolefin resin, etc. can be used. More preferably, it is a polyimide film or a liquid crystal polymer film.

[0107] The printed wiring board of the present invention can be produced by any conventionally known process except for using the materials of each layer described above.

[0108] A preferred embodiment is to manufacture a semi-finished product having an adhesive layer laminated on a covering film layer (hereinafter, also referred to as a "covering film side semi-finished product"). On the other hand, a semi-finished product having a metal foil layer laminated on a substrate film layer to form a desired circuit pattern (hereinafter, also referred to as a "substrate film side 2-layer semi-finished product") or a semi-finished product having an adhesive layer laminated on a substrate film layer and a metal foil layer laminated thereon to form a desired circuit pattern (hereinafter, also referred to as a "substrate film side 3-layer semi-finished product") (hereinafter, the substrate film side 2-layer semi-finished product and the substrate film side 3-layer semi-finished product are collectively referred to as the "substrate film side semi-finished product"). By laminating the obtained covering film side semi-finished product with the substrate film side semi-finished product, a 4-layer or 5-layer printed wiring board can be obtained.

[0109] The semi-finished product on the substrate film side can be obtained, for example, by a manufacturing method comprising the steps of (A) coating a resin solution as a substrate film on the above-mentioned metal foil and subjecting the coating film to initial drying; and (B) subjecting the laminate of the metal foil obtained in (A) and the initial dried coating film to a heat treatment and / or drying step (hereinafter referred to as the "heat treatment·desolventization step").

[0110] The circuit in the metal foil layer can be formed by a conventionally known method, either an additive method or a subtractive method, preferably a subtractive method.

[0111] The obtained substrate film side semi-finished product may be used directly for laminating with the cover film side semi-finished product, or may be laminated with a release film and then stored for laminating with the cover film side semi-finished product.

[0112] The semi-finished product on the cover film side can be produced, for example, by applying an adhesive on the cover film. If necessary, a crosslinking reaction can be carried out in the applied adhesive. In a preferred embodiment, the adhesive layer is semi-cured.

[0113] The obtained semi-finished product on the cover film side can be directly used for laminating with the semi-finished product on the base film side, or can be laminated with a release film and then stored for laminating with the semi-finished product on the base film side.

[0114] The semi-finished product on the substrate film side and the semi-finished product on the cover film side can be stored in the form of, for example, rolls, and then laminated to produce a printed circuit board. As a laminating method, any method can be used, for example, laminating can be performed by pressing or using a roll. In addition, the two can be laminated while heating by a method such as heating pressing or using a heating roller device.

[0115] The semi-finished product on the reinforcing material side is preferably manufactured by coating an adhesive on the reinforcing material when it is a soft and reelable reinforcing material such as a polyimide film. In addition, when it is a hard and non-reelable reinforcing plate such as a metal plate such as SUS, aluminum, or a plate after epoxy resin-cured glass fiber, it is preferably manufactured by transfer coating an adhesive pre-coated on a demoulding substrate. In addition, as needed, a cross-linking reaction can be carried out in the coated adhesive. In a preferred embodiment, the adhesive layer is semi-cured.

[0116] The obtained reinforcing material side semi-finished product can be directly used for lamination to the back surface of the printed wiring board, or can be laminated with a release film and then stored for lamination to the substrate film side semi-finished product.

[0117] The semi-finished product on the substrate film side, the semi-finished product on the cover film side, and the semi-finished product on the reinforcing material side are all the laminated bodies for printed wiring boards in the present invention.

[0118] Example

[0119] The present invention is described in more detail below with reference to Examples. However, the present invention is not limited to the Examples. Parts in the Examples and Comparative Examples are expressed as parts by mass.

[0120] (Physical property evaluation method)

[0121] Determination of the composition of polyester

[0122] Using 400MHz 1 H-nuclear magnetic resonance spectrometer (hereinafter referred to as NMR) was used to quantify the molar ratio of the polycarboxylic acid component and the polyol component constituting the polyester. Deuterated chloroform was used as the solvent. In addition, when the acid value of the polyester was increased by post-addition of an acid, the total amount of the acid component other than the acid component used for the post-addition of the acid was set to 100 mol % to calculate the molar ratio of each component.

[0123] Determination of glass transition temperature

[0124] The measurement was performed using a differential scanning calorimeter (DSC-200, manufactured by SII). 5 mg of the sample (polyester) was placed in an aluminum pressure-capped container and sealed, cooled to -50°C with liquid nitrogen, and then heated to 150°C at a rate of 20°C / min. For the endothermic curve obtained in this process, the temperature of the intersection of the baseline before the endothermic peak appears (below the glass transition temperature) and the tangent of the endothermic peak (indicating the tangent with the largest slope from the peak portion to the peak apex) was defined as the glass transition temperature (Tg, unit: °C).

[0125] Determination of number average molecular weight

[0126] The polyester sample was dissolved in tetrahydrofuran to a resin concentration of about 0.5 mass %, and filtered using a polytetrafluoroethylene membrane filter with a pore size of 0.5 μm. The sample was used as a measurement sample, and the number average molecular weight was measured by a gel permeation chromatograph (GPC) using tetrahydrofuran as a mobile phase and a differential refractometer as a detector. The flow rate was 1 mL / min, and the column temperature was 30°C. The chromatographic columns used were KF-802, 804L, and 806L manufactured by Showa Denko K.K. Monodisperse polystyrene was used as a molecular weight standard.

[0127] Determination of acid value

[0128] 0.2 g of polyester sample was dissolved in 40 ml of chloroform and titrated with 0.01 N potassium hydroxide ethanol solution. 6 g polyester equivalent (eq / 10 6 g). Use phenolphthalein as an indicator.

[0129] Relative dielectric constant (ε c ) and dielectric loss tangent (tanδ)

[0130] A polyester dissolved in toluene with a solid content concentration of 30% by mass was coated on a Teflon (registered trademark) sheet with a thickness of 100 μm, and dried at 130°C for 3 minutes to a thickness of 25 μm after drying and curing. The Teflon (registered trademark) sheet was then peeled off to obtain a test resin sheet. The obtained test resin sheet was then cut into 8 cm × 3 mm strips to obtain a test sample. Relative dielectric constant (ε c ) and dielectric loss tangent (tanδ) were measured using a network analyzer (manufactured by Anritsu Co., Ltd.) by the cavity perturbation method at a temperature of 23°C and a frequency of 10 GHz.

[0131] <Evaluation criteria for relative dielectric constant>

[0132] ◎: 2.3 or less

[0133] ○: greater than 2.3 and less than 3.0

[0134] ×: greater than 3.0

[0135] <Evaluation criteria for dielectric loss tangent>

[0136] ◎: 0.005 or less

[0137] ○: greater than 0.005 and less than 0.008

[0138] ×: greater than 0.008

[0139] viscosity

[0140] A polyester varnish dissolved in toluene and having a solid content concentration of 30% by mass was applied to a polyester film (E5101 manufactured by Toyobo Co., Ltd., thickness 50 μm, corona treated surface), and dried at 130°C for 3 minutes to a thickness of 25 μm after drying and curing. At room temperature (23°C), the dried adhesive sheet was cut into 25 mm wide and 200 mm long, and the adhesive layer was attached to a rolled copper foil substrate (BHY series manufactured by JX Metal Co., Ltd.), and a 2 kg rubber roller was used to reciprocate 2 times at a speed of 20 mm / second from the top to press the adhesive sheet. Then, a 180° peeling was performed at a peeling speed of 300 mm / minute to confirm the state of the peeled substrate. The case where there is no residual adhesive on the substrate and the interface is peeled off is set as ○, and the case where the adhesive layer is transferred to the substrate side is set as ×.

[0141] <Evaluation criteria for viscosity>

[0142] ○: No residual adhesive and peeling at the interface

[0143] ×: There is residual adhesive, or the adhesive layer is transferred to the substrate side

[0144] Solvent solubility

[0145] The solubility of the polyester when dissolved in toluene at 80° C. for 6 hours while stirring so as to have a solid content concentration of 60% by mass or 50% by mass was evaluated according to the following criteria.

[0146] <Evaluation criteria for solvent solubility>

[0147] ◎: Completely dissolved without residue at a solid content concentration of 60% by mass

[0148] ○: Completely dissolved without residue at a solid content concentration of 50% by mass

[0149] ×: There is a dissolved residue of resin at a solid content concentration of 50% by mass

[0150] Peel strength (adhesion)

[0151] The polyester of the present invention was mixed with a curing agent to prepare an adhesive composition, and the adhesiveness was evaluated. The following curing agents were used.

[0152] (b1): Polyisocyanate (Desmodur N3300 (manufactured by Sumika Polyurethane Co., Ltd.))

[0153] (b2): Epoxy resin (EPICLON HP-7200H (manufactured by DIC Corporation))

[0154] A curing agent was mixed with a toluene varnish having a solid content concentration of 30% by mass, wherein the polyester was dissolved in toluene, so as to be in the ratio (parts by mass) shown in Table 1 relative to 100 parts of the polyester, thereby preparing an adhesive composition.

[0155] The adhesive composition is applied to a polyimide film having a thickness of 12.5 μm (manufactured by Kaneka Co., Ltd., Apical (registered trademark)) so that the thickness after drying is 25 μm, and dried at 130°C for 3 minutes. The adhesive film (B stage product) obtained as described above is bonded to a rolled copper foil having a thickness of 18 μm (BHY series manufactured by JX Metal Co., Ltd.). The bonding is carried out by contacting the shiny surface of the rolled copper foil with the adhesive layer, and the bonding is carried out by pressing at 160°C under a pressure of 2 MPa for 30 seconds. Then, a heat treatment is carried out at 170°C for 3 hours to cure it, and a sample for peel strength evaluation is obtained. The peel strength is measured by pulling the film at 25°C and performing a 90° peel test at a pulling speed of 50 mm / min. This test is an experiment to show the bonding strength at room temperature.

[0156] <Evaluation Criteria>

[0157] ◎: 1.0N / mm or more

[0158] ○: 0.8N / mm or more but less than 1.0N / mm

[0159] △: 0.5N / mm or more but less than 0.8N / mm

[0160] ×: less than 0.5N / mm

[0161] Heat resistance

[0162] The measurement was performed using a differential thermal / thermogravimetric simultaneous measurement device (Shimadzu Corporation, DTG-60). 50 mg of the polyester was placed in a platinum sample cell, and the temperature was raised to 1000° C. at a flow rate of 20 ml / min and a heating rate of 5° C. / min in a nitrogen atmosphere. The temperature at which decomposition was performed at a high temperature and the weight reached 95% of the initial weight was defined as the 5% weight loss temperature, which was used as an indicator of heat resistance.

[0163] <Evaluation criteria for heat resistance>

[0164] ○: 5% weight loss temperature is above 300°C

[0165] ×: 5% weight loss temperature is less than 300℃

[0166] Hereinafter, production examples of the polyester of the present invention and the polyester of comparative examples are shown.

[0167] (Example 1)

[0168] Production Example of Polyester (a1)

[0169] In a reaction vessel equipped with a stirrer, a condenser and a thermometer, 326 parts of dimethyl 2,6-naphthalene dicarboxylate, 1520 parts of dimer alcohol (Croda, Pripol 2033) and 0.03 mol% of tetrabutyl orthotitanate relative to the total acid component were added as a catalyst, and the temperature was raised from 160°C to 220°C in 4 hours. The esterification reaction was carried out after a dehydration step. Then, in the polycondensation reaction step, the system was depressurized to 5 mmHg in 20 minutes and the temperature was further raised to 250°C. Then, the system was depressurized to less than 0.3 mmHg, and the polycondensation reaction was carried out for 60 minutes, and then it was taken out. The component analysis result of the obtained polyester (a1) by NMR was 2,6-naphthalene dicarboxylic acid / dimer alcohol = 100 / 100 [molar ratio] in terms of molar ratio. In addition, the glass transition temperature was -17°C. The obtained polyester (a1) was evaluated for solvent solubility, viscosity, heat resistance, relative dielectric constant, dielectric loss tangent, and adhesiveness. The evaluation results are shown in Table 1.

[0170] (Examples 2 to 10, Comparative Examples 1 to 6)

[0171] Production Examples of Polyesters (a2) to (a16)

[0172] Based on the manufacturing example of polyester (a1), the types and mixing ratios of raw materials were changed to synthesize polyesters (a2) to (a16). In addition, after the polymerization reaction of polyester (a9) was completed, 8 parts by mass of trimellitic anhydride was further added, reacted at 230°C for 30 minutes, and then acid was added. The physical properties and evaluation results are shown in Table 1. In addition, PTMG1000 is polytetramethylene ether glycol (average molecular weight 1000).

[0173] The monomers (B) used in the examples are shown below.

[0174] Dimer acid: manufactured by Croda, Pripol 1013 (number average molecular weight 565)

[0175] Dimer alcohol: Pripol 2033 manufactured by Croda (number average molecular weight about 560)

[0176] Dimer acid ester: manufactured by Croda, Priplast 3197 (number average molecular weight about 2000, polyester polyol derived from dimer acid)

[0177]

[0178] Industrial Applicability

[0179] The polyester of the present invention is excellent in solvent solubility, heat resistance, adhesive strength, and particularly excellent in low dielectric properties, and can be used for adhesives and base films for FPCs in high-frequency regions.

Claims

1. A polyester, characterized in that The present invention comprises the following monomer (A) and monomer (B) as constituent components, wherein when the total amount of all constituent components is 100 mol %, 30 mol % to 83 mol % of the monomer (A) and 15 mol % to 60 mol % of the monomer (B) are contained, and the total amount of the monomer (A) and the monomer (B) is 75 mol % or more, The polyester has a relative dielectric constant εc of 3.0 or less and a dielectric loss tangent tanδ of 0.008 or less at 10 GHz. Monomer (A): at least one selected from 2,6-naphthalene dicarboxylic acid, tricyclodecane dimethanol, pentacyclodecane dimethanol, bisphenol fluorene, bisphenoxyethanol fluorene, bisphenoxymethanol fluorene, biscresol fluorene, spiroglycol, and hydrogenated naphthalene dicarboxylic acid, Monomer (B): at least one selected from dimer acid, dimer alcohol, dimer acid ester, hydroxyl-terminated polybutadiene, hydroxyl-terminated hydrogenated polybutadiene, hydroxyl-terminated polyisoprene, and hydroxyl-terminated polyolefin, a polycarboxylic acid component having a continuous carbon chain of 10 or more carbon atoms and / or a polyol component having a continuous carbon chain of 10 or more carbon atoms having a number average molecular weight of 300 or more.

2. The polyester according to claim 1, which has a glass transition temperature of -30°C or higher.

3. A film comprising the polyester according to claim 1 or 2. 4 . An adhesive composition comprising the polyester according to claim 1 or 2 . 5 . An adhesive sheet comprising a layer formed from the adhesive composition according to claim 4 . 6 . A laminate comprising a layer formed from the adhesive composition according to claim 4 .

7. A printed wiring board comprising the laminate according to claim 6 as a constituent element.