A tetrachlorocobalt composite diquaternary phosphonium salt, a sustained-release film material, and a preparation method and application thereof
Through the combination of tetrachlorocobalt composite biquaternary phosphine salt and polyacrylonitrile, the fiber film is prepared by electrospinning technology, which solves the problems of high cost and short use time of existing quaternary phosphine salts, and effectively inhibits microorganisms and The extension of antibacterial aging is suitable for large-scale promotion.
Patent Information
- Application Number
- CN202210972155.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-08-15
AI Technical Summary
The production cost of existing quaternary salts is high and the use time is short, making it difficult to promote on a large scale, and cannot effectively prevent the spread of microbial pathogens.
Using tetrachlorocobalt composite bisquare phosphonium salt as antibacterial active material, fiber films were prepared by electrospinning technology, combined with polyacrylonitrile (PAN) solvent for spinning to form tetrachlorocobalt composite bisquare phosphonium with good antibacterial activity Salt fiber film material.
Effective inhibition of E. coli and Staphylococcus aureus has been achieved, antibacterial aging is extended, production costs are reduced, preparation process is simplified, and the feasibility of industrial promotion is improved.
Smart Images

Figure CN115304639B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanofiber films, and in particular relates to a tetrachlorocobalt composite diquaternary phosphonium salt, a sustained-release film material, a preparation method thereof and antibacterial application thereof. Background Art
[0002] Microbial pathogens can easily cause diseases in animals, plants and humans, and have long been a threat to human health and social development. Microorganisms are everywhere and can be spread through air, water or food. Quaternary phosphonium salts are a new generation of highly effective, broad-spectrum, low-toxic fungicides. The P element in their compounds has positive charges around them, making it easier to adsorb microorganisms with negative charges on the surface, thus enhancing their ability to adsorb electrons to bacteria. The two attract each other, causing enzyme metabolic dysfunction in bacterial cells and ultimately inactivation.
[0003] However, existing quaternary phosphonium salts have high production costs and short sustainable use time, making them difficult to promote and use on a large scale.
[0004] The combination of organic antibacterial agents and electrospinning technology can expand their application areas, and non-toxic or low-toxic, green and environmentally friendly materials also conform to the trend of the times. Summary of the invention
[0005] The purpose of the present invention is to provide a tetrachlorocobalt composite diquaternary phosphonium salt with antibacterial activity and a fiber film material thereof, and discloses a method for preparing the fiber film material.
[0006] In order to achieve the above object, the present invention is implemented by the following technical solutions:
[0007] Provided is a tetrachlorocobalt complex diquaternary phosphonium salt, with tetrachlorocobalt as anion and diquaternary phosphonium salt as cation, and the specific chemical structure is shown in formula (I):
[0008] (Ι).
[0009] Preferably, the tetrachlorocobalt complex diquaternary phosphonium salt is in single crystal form, triclinic system, P-1 space group, and the specific unit cell parameters are: a is 10.520-10.528Å, b is 11.228-11.236Å, c is 13.978-13.988Å, a is 97.265-97.289°, β is 104.284-104.310°, and g is 104.234-104.258°.
[0010] The present invention also provides a method for preparing the above-mentioned tetrachlorocobalt composite diquaternary phosphonium salt, comprising the following steps:
[0011] (1) placing a certain ratio of 1, 4-dichlorobenzyl and tri(p-methyl)phenylphosphine in a container (the molar ratio is preferably 1:1.5-2), adding an appropriate amount of an organic solvent (preferably acetone) to dissolve, heating to react (stirring and refluxing at 65-70°C for 18-24 hours), separating the solid and the liquid after the reaction is completed, washing the solid phase product (preferably acetone) and drying to obtain a diquaternary phosphonium salt;
[0012] (2) placing a certain amount of diquaternary phosphonium salt and cobalt chloride hexahydrate in a container (the molar ratio is preferably 1:0.8-1.2), using an appropriate amount of methanol as a solvent, and adding an appropriate amount of concentrated hydrochloric acid, and reacting at 65-70° C.; after the reaction is completed, the solid and liquid are separated, and the liquid is naturally volatilized and crystallized to obtain a crystalline material, which is the tetrachlorocobalt composite diquaternary phosphonium salt of the present invention.
[0013] The tetrachlorocobalt composite diquaternary phosphonium salt of the present invention is further used to prepare a fiber film material, comprising the following steps:
[0014] A certain amount of polyacrylonitrile (PAN) is added to a mixed solvent of DMSO and DMF (preferably the volume ratio of DMSO to DMF is 1: 0.8-1.2), and then 15-25% of the mass of PAN is weighed and added to the mixed solvent. The mixture is heated and stirred for 30-100 min, and then allowed to stand for defoaming and then electrospun to obtain a tetrachlorocobalt complex diquaternary phosphonium salt fiber film material.
[0015] Optimization of electrospinning conditions: the voltage of the high-voltage power supply of the instrument was adjusted to 16 kV, the receiving distance was 5 cm, and the liquid supply rate was 0.8 mL·h -1 , the slide speed is 15.0 mm·s -1 , the ambient temperature is 22℃ and the relative humidity is 40%-70%.
[0016] The present invention has the following positive and beneficial effects:
[0017] The tetrachlorocobalt composite diquaternary phosphonium salt material of the present invention exhibits good antibacterial activity against Escherichia coli and Staphylococcus aureus, is an excellent antibacterial material, and has a long sustained release time after being spun into a film, and has a certain antibacterial time effect. The preparation method of the present invention is simple to operate and has a high yield; the required instruments and equipment are simple and easy to operate; the required solvent consumption is small, the cost is saved, the application range is wide, and it is conducive to industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The crystal structure diagram of the tetrachlorocobalt composite diquaternary phosphonium salt of the present invention;
[0019] Figure 2This is a macroscopic photograph of the tetrachlorocobalt composite diquaternary phosphonium salt fiber film material of the present invention (left: blank PAN film; right: tetrachlorocobalt composite diquaternary phosphonium salt fiber film);
[0020] Figure 3 This is a microscopic photograph of the tetrachlorocobalt composite diquaternary phosphonium salt fiber film material of the present invention (left: blank PAN film; right: tetrachlorocobalt composite diquaternary phosphonium salt fiber film);
[0021] Figure 4 The antibacterial circle diagram of the tetrachlorocobalt composite diquaternary phosphonium salt of the present invention on Escherichia coli and Staphylococcus aureus (upper left: Escherichia coli; upper right: Staphylococcus aureus) and the antibacterial circle diagram of the monoquaternary phosphonium salt on Escherichia coli and Staphylococcus aureus (lower left: Escherichia coli; lower right: Staphylococcus aureus);
[0022] Figure 5 The MIC determination diagram of the tetrachlorocobalt composite diquaternary phosphonium salt of the present invention on Escherichia coli and Staphylococcus aureus (top: Escherichia coli; middle: Staphylococcus aureus) and the MIC determination diagram of the monoquaternary phosphonium salt on Escherichia coli and Staphylococcus aureus (bottom: Escherichia coli and Staphylococcus aureus);
[0023] Figure 6 The figure is the ultraviolet absorption spectrum of the tetrachlorocobalt composite diquaternary phosphonium salt of the present invention;
[0024] Figure 7 The infrared spectrum of the tetrachlorocobalt composite diquaternary phosphonium salt of the present invention;
[0025] Figure 8 It is a standard curve diagram of the tetrachlorocobalt composite diquaternary phosphonium salt of the present invention;
[0026] Fig. 9 The graph is an in vitro sustained release curve of the fiber film material of the tetrachlorocobalt composite diquaternary phosphonium salt of the present invention. DETAILED DESCRIPTION
[0027] In order to better understand the present invention, the technical solution of the present invention is described below through specific examples.
[0028] Example 1
[0029] A method for preparing a tetrachlorocobalt composite diquaternary phosphonium salt fiber film material comprises the following steps:
[0030] (1) Preparation of diquaternary phosphonium salt [T(4Me)PPBzT(4Me)PP]Cl2: Weigh 1 mmol of 1, 4-dichlorobenzyl and 2 mmol of tri(p-methyl)phenylphosphine into a 100 mL ground-mouth conical flask, add 30 mL of acetone to dissolve, stir and reflux at 65-70°C for 20 hours, a white precipitate is generated, filter under reduced pressure, wash three times with a small amount of acetone, and vacuum dry to obtain a white solid powder as the target product diquaternary phosphonium salt.
[0031] (2) Preparation of tetrachlorocobalt complex diquaternary phosphonium salt [T(4Me)PPBzT(4Me)PP][CoCl4]: 1 mmol of diquaternary phosphonium salt and 1 mmol of cobalt chloride hexahydrate were dissolved in methanol, mixed evenly, and an appropriate amount of concentrated hydrochloric acid was added to react at 65-70°C to generate a dark blue solution. After the reaction was completed, the solid and liquid were separated, and the liquid was allowed to stand and evaporate naturally. Blue crystals were precipitated in about 1-2 weeks. The main crystallographic data are shown in Table 1.
[0032] (3) Preparation of fiber film material: Weigh 1.5 g of polyacrylonitrile (PAN) and add it to a mixed solvent with a volume ratio of DMSO:DMF of 1:1. Stir at 80°C until completely dissolved. Weigh 20% of the mass of PAN blue crystals and add them to the bottle. Cover the bottle with a lid and place it on a magnetic stirrer for constant heating and stirring for 1 h. After standing to defoam, spin the tetrachlorocobalt composite diquaternary phosphonium salt fiber film material. The optimal electrospinning conditions are: voltage 16 kV, receiving distance 5 cm, liquid supply rate 0.8 mL·h -1 , the slide speed is 15.0 mm·s -1 , the ambient temperature was 22℃, and the relative humidity was 40%-70%. Finally, a light blue fiber film was obtained. The structure of PAN and drug-loaded film was clear, the fibers were evenly distributed, and there was no obvious agglomeration phenomenon, indicating that the electrospinning was relatively successful. The macroscopic and microscopic images are shown in Figure 2. Figure 2 , Figure 3 .
[0033] Table 1 Main crystallographic data of tetrachlorocobalt complex diquaternary phosphonium salt
[0034] .
[0035] The tetrachlorocobalt complex diquaternary phosphonium salt crystal material was used for antibacterial test, and the minimum inhibitory concentration (MIC) was determined by filter paper method and 96 plate method. The specific implementation method is: take the activated Escherichia coli and Staphylococcus aureus, inoculate them on the agar slant, put them in a 37℃ constant temperature box for culture, and after 24 hours, inoculate the bacteria in liquid culture medium. Dilute the Staphylococcus aureus liquid to a concentration of about 6.0×10 6 CFU·mL -1 , the concentration of E. coli is about 2.0×107 CFU·mL -1 . Prepare 0.01 mol / L monoquaternary phosphonium salt, diquaternary phosphonium salt, and tetrachlorocobalt complex diquaternary phosphonium salt solutions. Take a batch of agar culture dishes, inject 80 µL of Staphylococcus aureus into them, and inject 80 µL of Escherichia coli into another batch of culture dishes. Use a spreading rod to evenly spread the bacterial solution in the culture dishes. Use sterile tweezers to stick the sterilized and dried filter paper (0.60 cm in diameter) to the surface of each agar culture dish. Inject 10 µL of antibacterial solution into each filter paper, and seal the culture dish with plastic wrap. Place it in a constant temperature and humidity incubator at 37°C for 24 h, and measure the diameter of the inhibition zone, see Table 2, Figure 4 It can be seen that both the diquaternary phosphonium salt and the tetrachlorocobalt complex diquaternary phosphonium salt exhibit good antibacterial activity. The D row of the 96-plate was divided into four equal parts, the first part was the negative control, the second part was the positive control, the third part was the solvent control, and the fourth part was the blank control; while the AC row was used to determine the minimum inhibitory concentration of the diquaternary phosphonium salt, and the FH row was used to determine the minimum inhibitory concentration of the tetrachlorocobalt complex diquaternary phosphonium salt. First, 100 µL of liquid culture medium was transferred to the required wells of the two 96-plates, the negative control was kanamycin solution, the positive control was without antibacterial agent, and the solvent control was DMSO. 100 µL of 0.01mol·L was added to the first wells of the AC and FH rows, respectively. -1 The monoquaternary phosphonium salt solution, tetrachlorocobalt complex diquaternary phosphonium salt, and diquaternary phosphonium salt solution were diluted twice in each row until the 100 µL solution in the last well was discarded; secondly, 100 µL of bacterial suspension was transferred to each of the two 96 plates, except for the blank control without Escherichia coli or Staphylococcus aureus, and then aspirated and sealed the 96 plates with sealing film and placed them in a constant temperature and humidity incubator at 37°C for 16-20 h; finally, 20 µL of TTC dye was added to the 96 plates to detect the minimum inhibitory concentration of antibacterial substances, and the minimum inhibitory concentrations of monoquaternary phosphonium salts against Escherichia coli and Staphylococcus aureus were measured to be 7.8125×10 -4 mol·L -1 , 1.5625×10 -3 mol·L -1 The minimum inhibitory concentrations of diquaternary phosphonium salts against Escherichia coli and Staphylococcus aureus were 1.95×10 -5 mol·L -1 , 9.77×10 -6 mol·L -1 The minimum inhibitory concentrations of tetrachlorocobalt complex diquaternary phosphonium salt against Escherichia coli and Staphylococcus aureus were 1.95×10 -5 mol·L -1 , 9.77×10 -6 mol·L -1,See Figure 5 .
[0036] Table 2 Antibacterial effect of antibacterial materials
[0037] .
[0038] The UV absorption spectrum of the tetrachlorocobalt composite diquaternary phosphonium salt crystal obtained in Example 1 is shown in Figure 6 The absorption peak at 281 nm belongs to the π→π on the benzene ring of the diquaternary phosphonium salt cation. * The absorption peak at 527 nm belongs to the d→d transition of the metal cobalt ion. * Transition.
[0039] The infrared spectrum of the tetrachlorocobalt complex diquaternary phosphonium salt obtained in Example 1 is as follows: Figure 7 In the infrared spectrum, the CH stretching vibration on the benzene ring is located at 3027 cm -1 The CH asymmetric and symmetric stretching vibrations on the methylene group are at 2982 cm -1 and 2893 cm -1 The stretching vibration of C=C of benzene ring appears at 1631, 1596 cm -1 The CC stretching vibration of methylene is at 1194 cm -1 The stretching vibration of the CP bond appears at 1110 cm -1 806 cm -1 、705 cm -1 The nearby absorption peaks all belong to the C─H out-of-plane bending vibration of the benzene ring.
[0040] The tetrachlorocobalt complex diquaternary phosphonium salt film material obtained in Example 1 was used for sustained release test. 0.0050 g of the tetrachlorocobalt complex diquaternary phosphonium salt was weighed and diluted to different concentration gradients using PBS solution as solvent to prepare a standard curve. Figure 8 ; Place 0.900 g of tetrachlorocobalt composite diquaternary phosphonium salt film material with a content of 0.30 g in 50 mL PBS buffer solution, take a sample once every hour, and then add an equal volume of fresh PBS buffer solution to calculate its sustained release amount. Fig. 9 The release rate is faster in the first 5 hours and slower in the next 7 hours, which has a certain antibacterial time effect.
[0041] Example 2
[0042] A method for preparing a tetrachlorocobalt composite diquaternary phosphonium salt fiber film material comprises the following steps:
[0043] (1) Preparation of diquaternary phosphonium salt [T(4Me)PPBzT(4Me)PP]Cl2: Weigh 1 mmol of 1, 4-dichlorobenzyl and 1.5 mmol of tri(p-methyl)phenylphosphine into a 100 mL ground-mouth conical flask, add 30 mL of acetone to dissolve, stir and reflux at 65-70°C for 24 hours, a white precipitate is generated, filter under reduced pressure, wash three times with a small amount of acetone, and vacuum dry to obtain a white solid powder as the target product diquaternary phosphonium salt.
[0044] (2) Preparation of tetrachlorocobalt complex diquaternary phosphonium salt [T(4Me)PPBzT(4Me)PP][CoCl4]: 1 mmol of diquaternary phosphonium salt and 0.8 mmol of cobalt chloride hexahydrate were dissolved in methanol, mixed evenly, and an appropriate amount of concentrated hydrochloric acid was added to react at 65-70°C to generate a dark blue solution. After the reaction was completed, the solid and liquid were separated, and the liquid was allowed to stand and evaporate naturally. Blue crystals were precipitated in about 1-2 weeks. The main crystallographic data are shown in Table 1.
[0045] (3) Preparation of fiber film material: Weigh 1.5 g of polyacrylonitrile (PAN) and add it to a mixed solvent with a volume ratio of DMSO:DMF of 1:0.8. Stir at 80°C until completely dissolved. Weigh 15% of the mass of PAN blue crystals and add them to the bottle. Cover the bottle with a lid and place it on a magnetic stirrer for constant heating and stirring for 0.5 h. After standing to defoam, spin the tetrachlorocobalt composite diquaternary phosphonium salt fiber film material. The optimal electrospinning conditions are: voltage 16 kV, receiving distance 5 cm, liquid supply rate 0.8 mL·h -1 , the slide speed is 15.0 mm·s -1 , the ambient temperature is 22℃ and the relative humidity is 40%-70%.
[0046] Example 3
[0047] A method for preparing a tetrachlorocobalt composite diquaternary phosphonium salt fiber film material comprises the following steps:
[0048] (1) Preparation of diquaternary phosphonium salt [T(4Me)PPBzT(4Me)PP]Cl2: Weigh 1 mmol of 1, 4-dichlorobenzyl and 1.8 mmol of tri(p-methyl)phenylphosphine into a 100 mL ground-mouth conical flask, add 30 mL of acetone to dissolve, stir and reflux at 65-70°C for 18 hours, a white precipitate is generated, filter under reduced pressure, wash three times with a small amount of acetone, and vacuum dry to obtain a white solid powder as the target product diquaternary phosphonium salt.
[0049] (2) Preparation of tetrachlorocobalt diquaternary phosphonium salt [T(4Me)PPBzT(4Me)PP][CoCl4]: 1 mmol of diquaternary phosphonium salt and 1.2 mmol of cobalt chloride hexahydrate were dissolved in methanol, mixed evenly, and an appropriate amount of concentrated hydrochloric acid was added to react at 65-70°C to generate a dark blue solution. After the reaction was completed, the solid and liquid were separated, and the liquid was allowed to stand and evaporate naturally. Blue crystals were precipitated in about 1-2 weeks. The main crystallographic data are shown in Table 1.
[0050] (3) Preparation of fiber film material: Weigh 1.5 g of polyacrylonitrile (PAN) and add it to a mixed solvent with a volume ratio of DMSO:DMF of 1:1.2. Stir at 80°C until completely dissolved. Weigh 25% of the mass of PAN blue crystals and add them to the bottle. Cover the bottle with a lid and place it on a magnetic stirrer for constant heating and stirring for 1.5 h. After standing to defoam, spin the fiber film material of tetrachlorocobalt composite diquaternary phosphonium salt. Optimized electrospinning conditions: voltage 16 kV, receiving distance 5 cm, liquid supply rate 0.8 mL·h -1 , the slide speed is 15.0 mm·s -1 , the ambient temperature is 22℃ and the relative humidity is 40%-70%.
[0051] The above implementation cases only describe several specific implementation schemes of the present invention, rather than limiting the scope of the patent of the present invention. It should be that for ordinary technicians in this field, different improvements can be made based on these drawings without creative work to obtain other drawings, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.
Claims
1. A tetrachlorocobalt composite diquaternary phosphonium salt, characterized in that: With cobalt tetrachloride as anion and diquaternary phosphonium salt as cation, the specific chemical structure is shown in formula (I): (I); The tetrachlorocobalt complex diquaternary phosphonium salt is in the form of a single crystal, and the single crystal is of the triclinic system and the P-1 space group; The unit cell parameters of the single crystal are: a is 10.520-10.528Å, b is 11.228-11.236Å, c is 13.978-13.988Å, α is 97.265-97.289°, β is 104.284-104.310°, and γ is 104.234-104.258°.
2. The method for preparing the tetrachlorocobalt composite diquaternary phosphonium salt according to claim 1, characterized in that: The following steps are involved: (1) placing a certain proportion of 1, 4-dichlorobenzyl and tri(p-methyl)phenylphosphine in a container, adding an appropriate amount of acetone to dissolve, heating to react, separating the solid and the liquid after the reaction is completed, washing and drying the solid phase product to obtain a diquaternary phosphonium salt; (2) A certain amount of diquaternary phosphonium salt and cobalt chloride hexahydrate are placed in a container, an appropriate amount of methanol is used as a solvent, and an appropriate amount of concentrated hydrochloric acid is added to react at 65-70° C. After the reaction is completed, the solid and liquid are separated, and the liquid is naturally evaporated and crystallized to obtain a crystalline material, which is tetrachlorocobalt complex diquaternary phosphonium salt.
3. The preparation method according to claim 2, characterized in that: The molar ratio of 1,4-dichlorobenzyl to tri(p-methyl)phenylphosphine in step (1) is 1:1.5-2.
4. The preparation method according to claim 2, characterized in that: The reaction conditions of step (1) are stirring and reflux at 65-70° C. for 18-24 hours.
5. The preparation method according to claim 2, characterized in that: The molar ratio of the diquaternary phosphonium salt to cobalt chloride hexahydrate in step (2) is 1:0.8-1.
2.
6. A method for preparing a tetrachlorocobalt composite diquaternary phosphonium salt fiber film material, characterized in that: The following steps are involved: A certain amount of polyacrylonitrile is added to a mixed solvent of dimethyl sulfoxide and N, N-dimethylformamide, and then 15-25% of the mass of the polyacrylonitrile used of the tetrachlorocobalt complex diquaternary phosphonium salt described in claim 1 is weighed and added to the mixed solvent, heated and stirred for 30-100 min, and then allowed to stand for defoaming and then electrostatic spinning is performed to obtain the tetrachlorocobalt complex diquaternary phosphonium salt fiber film material.
7. The preparation method according to claim 6, characterized in that: The volume ratio of DMSO to DMF in the mixed solvent is 1: 0.8-1.2; the electrospinning conditions are as follows: the voltage of the high-voltage power supply of the instrument is adjusted to 15-18 kV, the receiving distance is 4-6 cm, and the liquid supply rate is 0.6-1.0 mL·h -1 , slide speed is 12-18 mm·s -1 , the ambient temperature is 20-25℃, and the relative humidity is 40-70%.
8. Use of the tetrachlorocobalt complex diquaternary phosphonium salt according to claim 1 in the preparation of antibacterial materials.