Dispersion liquid, composition, sealing component, light emitting device, lighting fixture, display device, and method for producing dispersion liquid
By using surface-modified metal oxide particles in methyl silicone resin, the problem of dispersion and aggregation in the sealing material is solved, and the light scattering efficiency and brightness of the light-emitting device are improved.
Patent Information
- Application Number
- CN202180024588.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-03-24
AI Technical Summary
When methyl silicone resin is used as a sealing material, it is difficult for the metal oxide particles to be uniformly dispersed, resulting in aggregation and a decrease in transparency, which affects the light scattering efficiency of the light-emitting device.
Using metal oxide particles surface-modified with silane compounds and silicone compounds, and using a specific dispersion manufacturing method to ensure that the metal oxide particles are evenly dispersed in the methyl silicone resin to avoid aggregation, combined with Fourier transform infrared Spectrophotometric measurement to optimize adhesion of surface modification materials.
The uniform dispersion of metal oxide particles is achieved, the transparency and light scattering efficiency of the sealing component are improved, and the brightness of the light-emitting device is enhanced.
Smart Images

Figure CN115335330B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a dispersion containing metal oxide particles whose surfaces are modified with a silane compound and a silicone compound, a composition, a sealing component, a light-emitting device, a lighting fixture, a display device, and a method for producing the dispersion.
[0002] This application claims priority based on Japanese Patent Application No. 2020-056492 filed in Japan on March 26, 2020, the contents of which are incorporated herein by reference. Background Art
[0003] As a light source with advantages such as small size, long life, and low voltage drive, light emitting diodes (LEDs) are widely used. The LED chip in the LED package is usually sealed with a sealing material containing resin to prevent contact with degradation factors present in the external environment such as oxygen or moisture. Therefore, the light emitted from the LED chip is emitted to the outside through the sealing material. Therefore, in order to increase the light beam emitted from the LED package, it is important to efficiently extract the light emitted from the LED chip to the outside of the LED package.
[0004] As a sealing material for improving the efficiency of extracting light emitted from an LED chip, a composition for forming a light-scattering composite containing metal oxide particles and a matrix resin composition is known, wherein the metal oxide particles are surface-modified by a surface modification material having one or more functional groups selected from an olefinic group, an H-Si group, and an alkoxy group (for example, Patent Document 1).
[0005] In the composition for forming a light scattering composite, a dispersion containing metal oxide particles with a small dispersed particle size and a high refractive index is mixed with a silicone resin in a state of relatively maintaining transparency. Thus, the light scattering composite obtained by curing the composition for forming a light scattering composite suppresses the decrease in light transmittance and improves light scattering.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2016 / 142992 Summary of the invention
[0009] Problem that the invention aims to solve
[0010] However, the inventors have found that by making the sealing material contain metal oxide particles with a high refractive index, not only the light scattering of the obtained sealing component is improved, but also the refractive index of the sealing component can be improved. When the refractive index of the sealing component is improved, the extraction efficiency of light from the sealed light-emitting element is usually improved. In the case of making the sealing material contain metal oxide particles for this purpose, from the viewpoint of improving the refractive index, the larger the content of the metal oxide particles, the more advantageous it is.
[0011] On the other hand, in recent years, for the high life of LED, as the sealing resin for sealing material, the demand of methyl silicone resin with high heat resistance is increasing. Compared with the phenyl silicone resin commonly used in the past, the methyl silicone resin has a large content of methyl and a large degree of hydrophobicity. Therefore, even if the metal oxide particles whose surface is hydrophobized as the invention described in patent document 1, when it is mixed with the methyl silicone resin, the metal oxide particles condense each other, and there is a problem of being unable to obtain a transparent composition. This problem becomes significant as the content of the metal oxide particles in the sealing material increases.
[0012] The present invention has been made to solve the above-mentioned problems, and its object is to provide a dispersion liquid containing metal oxide particles and suppressing the aggregation of the metal oxide particles when the metal oxide particles are dispersed in a methyl silicone resin, a composition containing the dispersion liquid, a sealing member formed using the composition, a light-emitting device having the sealing member, a lighting fixture and a display device having the light-emitting device, and a method for producing the dispersion liquid.
[0013] Solutions for solving problems
[0014] In order to solve the above-mentioned problems, a first aspect of the present invention provides a dispersion liquid comprising metal oxide particles whose surfaces are modified with a surface modification material and a hydrophobic solvent.
[0015] The surface modification material contains a silane compound and a silicone compound.
[0016] The metal oxide particles obtained by drying the dispersion liquid by vacuum drying were measured at 800 cm using a Fourier transform infrared spectrophotometer. -1 Above and 3800cm -1 The transmission spectrum in the following wave number range satisfies the following formula (1) when the spectrum value is normalized so that the maximum value of the spectrum in the above range is 100 and the minimum value is 0:
[0017] IA / IB ≤ 3.5(1)
[0018] (In the formula, “IA” means 3500cm -1Spectral values below, "IB" means 1100cm -1 Spectral values below. )
[0019] The dispersion and methylphenyl silicone were mixed to prepare a mixture in such a manner that the mass ratio of the total mass of the metal oxide particles and the surface modification material to the mass of methylphenyl silicone was 30:70, and the viscosity of the mixture after removing the hydrophobic solvent was 9 Pa·s or less.
[0020] In order to solve the above-mentioned problems, a second aspect of the present invention provides a composition which is a mixture of the above-mentioned dispersion and a resin component.
[0021] In order to solve the above-mentioned problems, a third aspect of the present invention provides a sealing member which is a cured product of the above-mentioned composition.
[0022] In order to solve the above-mentioned problems, a fourth aspect of the present invention provides a light-emitting device including the above-mentioned sealing member and a light-emitting element sealed by the above-mentioned sealing member.
[0023] In order to solve the above-mentioned problems, a fifth aspect of the present invention provides a lighting fixture including the above-mentioned light emitting device.
[0024] In order to solve the above-mentioned problems, a sixth aspect of the present invention provides a display device including the above-mentioned light-emitting device.
[0025] In order to solve the above-mentioned problems, a seventh aspect of the present invention provides a method for producing a dispersion liquid, comprising: step B, mixing a silane compound and metal oxide particles to obtain a mixed liquid;
[0026] Step C, dispersing the metal oxide particles in the mixed solution to obtain a first dispersion solution in which the metal oxide particles are dispersed;
[0027] Step D, adding a hydrophobic solvent to the first dispersion to obtain a second dispersion; and
[0028] Step E, adding a silicone compound to the second dispersion to obtain a third dispersion,
[0029] The content of the metal oxide particles in the mixed solution of the step B is 10 mass % or more and 49 mass % or less, and the total content of the silane compound and the metal oxide particles in the mixed solution of the step B is 65 mass % or more and 98 mass % or less,
[0030] The step D of adding the hydrophobic solvent is selected from any one of the following steps: step d1, heating the first dispersion and, after heating, adding the hydrophobic solvent at a rate at which the metal oxide particles do not aggregate; step d2, while heating the first dispersion, adding the hydrophobic solvent at a rate at which the metal oxide particles do not aggregate; and step d3, after adding the hydrophobic solvent at a rate at which the metal oxide particles do not aggregate, heating the first dispersion.
[0031] In the above-mentioned embodiment of the present invention, there is also a step A of mixing the above-mentioned silane compound and water to obtain a hydrolyzed solution containing the above-mentioned silane compound after hydrolysis, and in the step B of obtaining the above-mentioned mixed solution, the above-mentioned mixed solution can be obtained by mixing the above-mentioned hydrolyzed solution and the above-mentioned metal oxide particles.
[0032] Effects of the Invention
[0033] As described above, according to the present invention, there can be provided a dispersion liquid containing metal oxide particles and suppressing the aggregation of the metal oxide particles when the metal oxide particles are dispersed in a methyl silicone resin, a composition containing the dispersion liquid, a sealing member formed using the composition, a light-emitting device having the sealing member, a lighting fixture and a display device having the light-emitting device, and a method for producing the dispersion liquid. The method for producing the dispersion liquid of the present invention can provide a preferred dispersion liquid having an appropriate viscosity, particularly a low initial viscosity. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic cross-sectional view showing a preferred example of a light emitting device according to an embodiment of the present invention.
[0035] Figure 2 It is a schematic cross-sectional view showing another example of the light emitting device according to the embodiment of the present invention.
[0036] Figure 3 It is a schematic cross-sectional view showing another example of the light emitting device according to the embodiment of the present invention.
[0037] Figure 4 It is a schematic cross-sectional view showing another example of the light emitting device according to the embodiment of the present invention. DETAILED DESCRIPTION
[0038] Hereinafter, examples of preferred embodiments of the present invention will be described in detail with reference to the drawings.
[0039] In addition, the present embodiment is specifically described for a better understanding of the purpose of the invention, and does not limit the present invention unless otherwise specified. Within the scope of the purpose of the present invention, the amount, quantity, type, ratio, structure, position, order, ratio, etc. can be omitted, added, replaced or changed.
[0040] <1. Concept of the present inventors>
[0041] First, before describing the present invention in detail, the conception by which the inventors accomplished the present invention will be described.
[0042] Generally, in the manufacture of a sealing material (composition) as a raw material of a sealing component, metal oxide particles are modified by a surface modifying material and dispersed in a resin such as a silicone resin. However, compared with the phenyl silicone resins and the like commonly used in the past, methyl silicone resins have a large methyl content and a high degree of hydrophobicity. Therefore, as described above, even when metal oxide particles are modified by a surface modifying material, it is difficult for the metal oxide particles to be uniformly dispersed in the methyl silicone resin.
[0043] Therefore, the present inventors have conducted intensive studies to solve the problem and have found that the dispersibility of the metal oxide particles in the methyl silicone resin is not significantly improved even if the amount of the surface modification material used is simply increased.
[0044] After obtaining this result, the present inventors conducted further research and focused on the modification state of the surface modification material on the surface of the metal oxide particles. That is, even if a large amount of surface modification material is used to modify the metal oxide particles, when only a small amount of surface modification material is attached to the surface of the metal oxide particles, the surface of the metal oxide particles is not sufficiently hydrophobic. On the other hand, even if a small amount of surface modification material is used to modify the metal oxide particles, the attachment ratio of the surface modification material to the surface of the metal oxide particles is high, and when a large amount of surface modification material is attached to the surface of the metal oxide particles, the surface of the metal oxide particles is sufficiently hydrophobic.
[0045] Furthermore, the present inventors have found that when using silane compounds and silicone compounds as surface modification materials, the degree of adhesion of the surface modification materials to the above-mentioned metal oxide particles can be measured and observed using a Fourier transform infrared spectrophotometer (FT-IR). Furthermore, the present inventors have found that even by using the viscosity when mixed with a methyl silicone resin, the degree of adhesion of the surface modification materials to the metal oxide particles can be measured and observed. Furthermore, it has been found that by the excellent method described later, silane compounds and silicone compounds can be fully attached to the surface of the metal oxide particles.
[0046] <2. Dispersion liquid>
[0047] The dispersion liquid according to the present embodiment will be described. The dispersion liquid according to the present embodiment contains metal oxide particles whose surfaces are modified with a silane compound and a silicone compound, and a hydrophobic solvent.
[0048] In the present embodiment, the dispersion of the present embodiment is dried by vacuum drying the dispersion to obtain metal oxide particles, and the wavelength of the dispersion at 800 cm is measured by a Fourier transform infrared spectrophotometer. -1 Above and 3800cm -1 The transmission spectrum has the following wave number range, and when the spectrum value is normalized so that the maximum value of the spectrum in the above range is 100 and the minimum value is 0, the following formula (1) is satisfied.
[0049] IA / IB ≤ 3.5(1)
[0050] (In the formula, “IA” means 3500cm -1 Spectral values below, "IB" means 1100cm -1 Spectral values below. )
[0051] The dispersion of the present embodiment and methylphenyl silicone are mixed so that the mass ratio of the total mass of the metal oxide particles and the surface modification material to the mass of methylphenyl silicone is 30:70, and the viscosity after removing the hydrophobic solvent is 9 Pa·s or less.
[0052] Due to the above characteristics, when the dispersion liquid involved in the present embodiment is mixed with a methyl silicone resin to disperse the metal oxide particles in the methyl silicone resin, the aggregation of the metal oxide particles is suppressed. As a result, the turbidity of the composition (resin composition) obtained as the mixture is suppressed and becomes relatively transparent.
[0053] Specifically, in the transmission spectrum measured by Fourier transform infrared spectrophotometer, the wave number is 1100 cm -1 The position is attributed to the siloxane bond (Si-O-Si bond), with a wave number of 3500 cm -1 The position of 3500cm belongs to the silanol group (Si-OH group). Silane compounds and silicone compounds have Si-OH groups that can form Si-O-Si bonds and groups that can form Si-OH groups, respectively. -1 Spectral values at (IA) and 1100cm -1 The spectral value (IB) below can be used to observe the reaction degree of the Si—OH group of the silane compound and the silicone compound, or the group that can form the Si—OH group.
[0054] Furthermore, the inventors of the present invention have found that when IA / IB is less than 3.5, the silane compound and the silicone compound are sufficiently well attached to the surface of the metal oxide particles. Due to this feature, the metal oxide particles will not condense even when mixed with a methyl silicone resin, and can be dispersed in the methyl silicone resin. As a result, the turbidity of the composition obtained as a mixture is suppressed and becomes relatively transparent. Moreover, since the metal oxide particles are contained, when the sealing component for sealing a light-emitting element is obtained using the composition, the refractive index of the sealing component is improved compared to the case where a methyl silicone resin is used alone. Thus, a composition is obtained using the dispersion involved in the present embodiment, and when the light-emitting element is sealed using the composition, the brightness of the light-emitting device is improved due to the high refractive index and light transmittance of the sealing component.
[0055] On the other hand, when IA / IB exceeds 3.5, the silane compound and the silicone compound are not sufficiently attached to the surface of the metal oxide particles, and as a result, it is difficult to make the metal oxide particles have excellent dispersibility in the methyl silicone resin. As a result, when the dispersion and the methyl silicone resin are mixed, the metal oxide particles aggregate and turbidity is generated in the obtained composition. As described above, IA / IB is 3.5 or less, preferably 3.0 or less, more preferably 2.5 or less, further preferably 2.3 or less, and particularly preferably 2.0 or less.
[0056] Furthermore, the lower limit of IA / IB is preferably IA=0, and therefore 0. However, even if a small amount of silanol groups (Si-OH groups) remain, it can be mixed with the methyl silicone resin. Therefore, the lower limit of IA / IB can be 0, or 0.1, or 0.3, or 0.5, or 0.7, or 1.0, or 1.2, or 1.5, or 1.8.
[0057] Furthermore, the transmission spectrum of the metal oxide particles can be measured using a Fourier transform infrared spectrophotometer (FT-IR) as follows, to give a specific example.
[0058] First, the dispersion of the present embodiment is dried by vacuum drying. The drying conditions can be appropriately adjusted according to the amount and concentration of the dispersion. For example, if the solid content is 30% by mass, 10 g of the dispersion can be dried at 100° C. and 20 hPa or less for more than 2 hours. As a vacuum dryer, VACUUMOVEN VOS-201SD manufactured by EYELA TOKYO RIKAKIKAI CO, LTD. can be used.
[0059] Next, using 0.01 g to 0.05 g of the metal oxide particles obtained by drying, a transmission spectrum can be measured using a Fourier transform infrared spectrophotometer (for example, manufactured by JASCO Corporation, model: FT / IR-670Plus).
[0060] The dispersion of the present embodiment and methylphenyl silicone (methyl silicone resin) are mixed to form a mixture in such a manner that the mass ratio of the total mass of the metal oxide particles and the surface modification material (silane compound and silicone compound) to the mass of methylphenyl silicone is 30:70. Then, when the hydrophobic solvent is removed from the mixture, the viscosity thereof is 9 Pa·s or less.
[0061] The viscosity is 9.0 Pa·s or less, and may be 8.5 Pa·s or less, 8.0 Pa·s or less, 7.5 Pa·s or less, 7.0 Pa·s or less, 6.5 Pa·s or less, or 6.0 Pa·s or less.
[0062] The viscosity of the methylphenyl silicone used may be, for example, 1 to 10 Pa·s, 1 to 9 Pa·s, 2 to 5 Pa·s, or 2 to 3 Pa·s. As a specific example, methylphenyl silicone having a viscosity (23° C.) of 2.7 Pa·s can be preferably used.
[0063] As the methylphenyl silicone, for example, KER-2500-B manufactured by Shin-Etsu Chemical Co., Ltd. is preferably used.
[0064] The lower limit of the viscosity may be the viscosity of methylphenyl silicone itself, for example, the viscosity of KER-2500-B itself. The lower limit of the viscosity may be, for example, 1.0 Pa·s or more, 1.5 Pa·s or more, 2.0 Pa·s or more, 2.5 Pa·s or more, or 3.0 Pa·s or more.
[0065] It is preferred to completely remove the hydrophobic solvent from the mixture using an evaporator or the like. However, since it is difficult to completely remove the hydrophobic solvent, about 5% by mass may remain. That is, the hydrophobic solvent may contain 0 to 5.0% by mass, 0.1 to 3.0% by mass, or 0.5 to 1.0% by mass.
[0066] The viscosity is measured using a rheometer, for example, a rheometer (trade name: RheoStress RS-6000, manufactured by HAAKE) at 25° C. and a shear rate of 1 (1 / S).
[0067] When the hydrophobic solvent is removed from the composition containing the hydrophobic solvent (composition containing metal oxide particles, surface modification material and methyl silicone resin), the viscosity of the composition increases due to the proximity of the particles. That is, when the hydrophobic solvent is removed, the viscosity of the composition (composition containing metal oxide particles, surface modification material and methyl phenyl silicone) increases due to the proximity of the particles. The viscosity increases over time.
[0068] Therefore, the viscosity after the hydrophobic solvent is removed refers to the viscosity of the composition measured within 1 hour after the hydrophobic solvent is removed from the dispersion.
[0069] When the viscosity of the dispersion is 9 Pa·s or less, the viscosity of the composition obtained by mixing methylphenyl silicone with the dispersion and removing the hydrophobic solvent increases slowly, so that the composition can be easily handled and the quality stability of the sealing component can be improved.
[0070] There has been no finding so far that the IA / IB value of the metal oxide particles can be adjusted to a viscosity of 9 Pa·s or less when mixed with methylphenyl silicone. The present inventors have found for the first time that a dispersion having the above-mentioned excellent effect can be obtained by the method described below, and that the excellent effect can be achieved.
[0071] Hereinafter, each component contained in the dispersion liquid will be described.
[0072] (2.1 Metal oxide particles)
[0073] The metal oxide particles scatter the light emitted from the light emitting element in the sealing member described later. In addition, the metal oxide particles increase the refractive index of the sealing member depending on the type of the metal oxide particles. Thus, the metal oxide particles contribute to the improvement of the brightness of light in the light emitting device.
[0074] The metal oxide particles contained in the dispersion liquid involved in the present embodiment are not particularly limited. In the present embodiment, as the metal oxide particles, for example, zirconium oxide particles, titanium oxide particles, zinc oxide particles, iron oxide particles, copper oxide particles, tin oxide particles, cerium oxide particles, tantalum oxide particles, niobium oxide particles, tungsten oxide particles, europium oxide particles, yttrium oxide particles, molybdenum oxide particles, indium oxide particles, antimony oxide particles, germanium oxide particles, lead oxide particles, bismuth oxide particles and hafnium oxide particles, as well as potassium titanate particles, barium titanate particles, strontium titanate particles, potassium niobate particles, lithium niobate particles, calcium tungstate particles are preferably used. At least one or more selected from the group consisting of yttria-stabilized zirconia particles, cerium-stabilized zirconia particles, calcium-stabilized zirconia particles, magnesium-stabilized zirconia particles, scandium-stabilized zirconia particles, hafnium-stabilized zirconia particles, yttria-stabilized zirconia particles, cerium-stabilized zirconia particles, indium-stabilized zirconia particles, strontium-stabilized zirconia particles, samarium-stabilized zirconia particles, gadolinium-stabilized zirconia particles, antimony-added tin oxide particles, and indium-added tin oxide particles.
[0075] Among the above, the dispersion preferably contains at least one selected from the group consisting of zirconium oxide particles and titanium oxide particles from the viewpoint of improving transparency or compatibility (affinity) with the sealing resin (resin component).
[0076] Furthermore, from the viewpoint of increasing the refractive index of the sealing member, the metal oxide particles preferably have a refractive index of 1.7 or more.
[0077] The metal oxide particles are more preferably at least one of zirconium oxide particles and titanium oxide particles, and are particularly preferably zirconium oxide particles.
[0078] The metal oxide particles may be dispersed in the dispersion as primary particles or may be dispersed as secondary particles formed by agglomeration of primary particles. Usually, the metal oxide particles are dispersed as secondary particles.
[0079] The average dispersed particle size of the metal oxide particles in the dispersion is not particularly limited, for example, it is more than 10nm and less than 300nm, preferably more than 20nm and less than 250nm, and more preferably more than 30nm and less than 200nm. As needed, it can also be more than 30nm and less than 80nm, more than 30nm and less than 100nm, more than 80nm and less than 180nm, etc. The average dispersed particle size of the metal oxide particles is more than 10nm, and the brightness of the light of the light-emitting device described later manufactured using the dispersion is improved. In addition, the average dispersed particle size of the metal oxide particles is less than 300nm, which can suppress the dispersion or the dispersion The transmittance of the light of the composition and sealing component described later manufactured using the dispersion decreases. As a result, the brightness of the light of the light-emitting device is improved.
[0080] In addition, the average dispersed particle size of the metal oxide particles is the particle size D50 of the metal oxide particles when the cumulative percentage of the scattering intensity distribution obtained by the dynamic light scattering method is 50%. This value can be measured by a dynamic light scattering particle size distribution meter (for example, manufactured by HORIBA, Ltd., model: SZ-100SP). A quartz cell with an optical path length of 10 mm×10 mm can be used to measure a dispersion in which the solid content is adjusted to 5% by mass. In addition, in this specification, "solid content" refers to the residue when the volatile components are removed from the dispersion. For example, when a dispersion, such as 1.2 g of a dispersion, is placed in a magnetic crucible and heated at 100°C for 1 hour with a hot plate, the non-volatile and residual components (metal oxide particles or surface modification materials, etc.) can be used as solid components.
[0081] In addition, regardless of the state of the metal oxide particles being dispersed as primary particles or secondary particles, the average dispersed particle size of the metal oxide particles is measured and calculated based on the diameter of the metal oxide particles in the dispersed state. Moreover, in the present embodiment, the average dispersed particle size of the metal oxide particles can also be measured as the average dispersed particle size of the metal oxide particles with the surface modification material attached. In the dispersion, there may be metal oxide particles with the surface modification material attached and metal oxide particles without the surface modification material attached. Therefore, usually, the average dispersed particle size of the metal oxide particles is measured as a value in their mixed state.
[0082] The average primary particle size of the metal oxide particles contained in the dispersion and prepared as a material can be arbitrarily selected, for example, preferably 3 nm or more and 200 nm or less, more preferably 5 nm or more and 170 nm or less, and further preferably 10 nm or more and 100 nm or less. As required, the average primary particle size of the particles can also be 5 to 20 nm, 5 to 25 nm, 50 to 120 nm, 50 to 150 nm. By having the average primary particle size of the metal oxide particles within the above range, the transparency of the sealing component can be suppressed from decreasing. As a result, the brightness of the light of the light-emitting device can be further improved.
[0083] The average primary particle size of the metal oxide particles can be determined by any method selected. For example, it can be performed by observation with a transmission electron microscope. First, a collodion film obtained by extracting metal oxide particles from a dispersion is observed by a transmission electron microscope to obtain a transmission electron microscope image. Next, a specified number, for example, 100 metal oxide particles in the transmission electron microscope image are selected. In addition, the longest straight line amount (maximum long diameter) of each of these metal oxide particles is measured, and these measured values are arithmetic averaged to obtain the average primary particle size of the metal oxide particles.
[0084] Here, when the metal oxide particles are aggregated, the aggregate particle size of the aggregate is not measured. The maximum major diameter of a predetermined number of particles (primary particles) of the metal oxide particles constituting the aggregate is measured and taken as the average primary particle size.
[0085] Furthermore, as long as it can be mixed with the resin component described later, the content of the metal oxide particles in the dispersion is not particularly limited. The content of the metal oxide particles in the dispersion can be arbitrarily selected, for example, preferably 1% by mass or more and 70% by mass or less, more preferably 5% by mass or more and 50% by mass or less, further preferably 7% by mass or more and 40% by mass or less, and particularly preferably 10% by mass or more and 30% by mass or less. As required, it can also be 20% by mass or more and 40% by mass or less, 25% by mass or more and 35% by mass or less.
[0086] By using such an amount, the viscosity of the dispersion can be suppressed from being too large. Therefore, mixing with the resin component described later becomes easy. In addition, the excess amount of solvent (dispersion medium) after mixing with the resin component can be suppressed, and the removal of the solvent becomes easy. The metal oxide particles in the dispersion of the present embodiment can be metal oxide particles that are initially surface-modified by a silane compound and then surface-modified by a silicone compound.
[0087] The surface modification material described below is attached to the surface of the metal oxide particles described above. Due to this attachment, the metal oxide particles are stably dispersed in the dispersion liquid and the dispersion liquid produced using the dispersion liquid.
[0088] (2.2 Surface modification materials)
[0089] The dispersion liquid according to the present embodiment contains a silane compound and a silicone compound as the surface modification material. As the surface modification material, only a silane compound and a silicone compound may be used.
[0090] In the dispersion, at least a portion of the surface modifying material adheres to the surface of the metal oxide particles to modify the surface, thereby preventing the metal oxide particles from agglomerating. Furthermore, the adhesion improves the compatibility with the resin component.
[0091] Here, the surface modification material "attaches" to the metal oxide particles means that the surface modification material contacts or bonds with the metal oxide particles through interaction or reaction between the surface modification materials. As contact, for example, physical adsorption can be cited. And as bonding, for example, ionic bonding, hydrogen bonding, covalent bonding, etc. can be cited.
[0092] The dispersion liquid according to the present embodiment contains at least a silane compound and a silicone compound as surface modification materials. That is, in the present embodiment, the metal oxide particles are surface-modified by at least a silane compound and a silicone compound.
[0093] Silane compounds are easily attached to the surface of metal oxide particles. On the other hand, silicone compounds have a relatively large molecular weight and mainly contribute to improving affinity with the dispersion medium or the resin component described later. By using such silane compounds and silicone compounds at the same time, the dispersion stability of metal oxide particles in methyl silicone resin is improved.
[0094] On the other hand, when the dispersion does not contain any of the silane compound and the silicone compound, the excellent effect described above cannot be obtained. For example, when the dispersion does not contain the silane compound, the silicone compound is not easy to adhere to the surface of the metal oxide particles, and the dispersibility of the metal oxide particles in the methyl silicone resin is poor. On the other hand, when the dispersion does not contain the silicone compound, the affinity of the metal oxide particles and the methyl silicone resin is not large enough, and the dispersibility of the metal oxide particles in the methyl silicone resin is poor.
[0095] (Silane compound)
[0096] The silane compound can be arbitrarily selected, and examples thereof include silane compounds containing an alkyl group and an alkoxy group such as methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, ethyltrimethoxysilane, ethyltripropoxysilane, isobutyltrimethoxysilane, methylphenyldimethoxysilane, and methylphenyldiethoxysilane; silane compounds containing an alkenyl group and an alkoxy group such as vinyltrimethoxysilane, methacryloxypropyltrimethoxysilane, and acryloxypropyltrimethoxysilane; Diethoxymonomethylsilane, monoethoxydimethylsilane, diphenylmonomethoxysilane, diphenylmonoethoxysilane etc. contain H-Si group and alkoxy silane compounds, phenyltrimethoxysilane etc. contain other alkoxy silane compounds and dimethylchlorosilane, methyldichlorosilane, diethylchlorosilane, ethyldichlorosilane, methylphenylchlorosilane, diphenylchlorosilane, phenyldichlorosilane, trimethoxysilane, dimethoxysilane, monomethoxysilane, triethoxysilane etc. contain H-Si group silane compounds etc. These silane compounds can be used alone or in combination of more than two kinds. Wherein, silane compounds with alkoxy, especially methoxy, are easily attached to metal oxide particles, so it is preferred.
[0097] Among the above, the silane compound preferably contains a silane compound having an alkyl group and an alkoxy group, since the viscosity is low and the dispersion of the metal oxide particles in the dispersion step described later is easy.
[0098] The number of alkoxy groups in the silane compound containing an alkyl group and an alkoxy group is preferably 1 to 3, and the number of alkoxy groups is more preferably 3. The number of alkoxy groups may be 1 or 2 as required. The number of carbon atoms in the alkoxy group can be arbitrarily selected, and is preferably 1 to 5. The number of carbon atoms may also be 1 to 3, or 2 to 4.
[0099] The number of alkyl groups in the silane compound containing an alkyl group and an alkoxy group is preferably 1 to 3, more preferably 1. In addition, as required, the number of alkyl groups may be 2 or 3. The number of carbon atoms in the alkyl group is preferably 1 to 5, more preferably 1 to 3, and further preferably 1 to 2.
[0100] The total number of the alkoxy group and the alkyl group in the silane compound containing an alkyl group and an alkoxy group is preferably 2 or more and 4 or less, and preferably 4.
[0101] Examples of the silane compound as the surface modification material include methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane and ethyltripropoxysilane. It is preferred that at least one selected from the group consisting of these compounds be contained.
[0102] The content of the silane compound in the dispersion can be arbitrarily selected, and is not particularly limited. Relative to the amount of 100 mass % of the metal oxide particles, for example, preferably 50 mass % or more and 500 mass % or less, more preferably 70 mass % or more and 400 mass % or less, and further preferably 90 mass % or more and 300 mass % or less. As required, it can also be 80 mass % or more and 350 mass % or less, 150 mass % or more and 250 mass % or less. Thus, a sufficient amount of silicone compound can be attached to the surface of the metal oxide particles through the silane compound, and while the dispersion stability of the metal oxide particles can be improved, the dispersibility in the methyl silicone resin can be improved.
[0103] (Silicone compound)
[0104] The silicone compound can be arbitrarily selected, and examples thereof include alkoxy-containing phenyl silicone, dimethyl silicone, methyl phenyl silicone, methyl hydrogen silicone, methyl phenyl hydrogen silicone, diphenyl hydrogen silicone, alkoxy-terminated phenyl silicone, alkoxy-terminated methyl phenyl silicone, alkoxy-containing methyl phenyl silicone, alkoxy-containing dimethyl silicone, alkoxy-terminated trimethyl-terminated (methyl-terminated) dimethyl silicone, and alkoxy-containing phenyl silicone. These silicone compounds may be used alone or in combination of two or more.
[0105] The silicone compound may be a monomer, an oligomer, or a resin (polymer). Since surface modification is easy, it is preferable to use a monomer or an oligomer.
[0106] Among the above, from the viewpoint of the ease of reaction and the high degree of hydrophobicity, the silicone compound preferably includes alkoxy-containing phenyl silicone, dimethyl silicone, methyl phenyl silicone, alkoxy-terminated phenyl silicone, alkoxy-terminated methyl phenyl silicone, alkoxy-containing methyl phenyl silicone, alkoxy-containing dimethyl silicone, alkoxy-terminated trimethyl-terminated (methyl-terminated) dimethyl silicone, and alkoxy-containing phenyl silicone. It can contain at least one selected from the group consisting of these compounds. More preferably, the silicone compound contains at least one selected from the group consisting of methoxy-containing phenyl silicone, dimethyl silicone, and methoxy-containing dimethyl silicone.
[0107] The content of the silicone compound in the dispersion can be arbitrarily selected and is not particularly limited. For example, relative to the amount of 100% by mass of the metal oxide particles, for example, preferably 50% by mass or more and 500% by mass or less, more preferably 80% by mass or more and 400% by mass or less, and further preferably 100% by mass or more and 300% by mass or less. As required, the amount may also be 50% by mass or more and 200% by mass or less, 50% by mass or more and 150% by mass or less. Thus, a sufficient amount of silicone compounds can be attached to the surface of the metal oxide particles, and while the dispersion stability of the metal oxide particles can be improved, the dispersibility in the methyl silicone resin can be improved. Moreover, the amount of free silicone compounds can be reduced, and the unintentional agglomeration of the metal oxide particles in the methyl silicone resin can be suppressed.
[0108] (Other compounds)
[0109] Furthermore, the dispersion may contain components other than the silane compound and the silicone compound as a surface modification material. Examples of such components include carbon-carbon unsaturated bond-containing fatty acids, specifically, methacrylic acid, acrylic acid, and the like.
[0110] (Total content of silane compounds and silicone compounds)
[0111] The amount of the surface modification material relative to the metal oxide particles, that is, the total content of the silane compound and the silicone compound is not particularly limited and can be selected arbitrarily. Relative to the amount of the metal oxide particles, for example, it is preferably 100% by mass or more and 1000% by mass or less, more preferably 150% by mass or more and 800% by mass or less, and further preferably 190% by mass or more and 600% by mass or less. The amount may also be 200% by mass or more and 900% by mass or less, 250% by mass or more and 850% by mass or less. When the amount of the surface modification material is within the above range, the amount of the free surface modification material can be reduced, and the dispersibility of the metal oxide particles can be fully improved.
[0112] (2.3 Hydrophobic solvent)
[0113] The dispersion liquid according to the present embodiment contains a hydrophobic solvent as a dispersion medium for dispersing metal oxide particles. The hydrophobic solvent is not particularly limited as long as it can disperse the metal oxide particles to which the surface modification material is attached and can be mixed with the resin component described below.
[0114] Examples of such hydrophobic solvents include aromatic solvents, saturated hydrocarbons, and unsaturated hydrocarbons. These hydrophobic solvents may be used alone or in combination of two or more.
[0115] Among the above, the hydrophobic solvent is preferably an aromatic solvent, and an aromatic hydrocarbon is particularly preferred. Aromatic solvents have excellent compatibility with the methyl silicone resin described below, and contribute to improving the viscosity characteristics of the resulting composition and the quality (transparency, shape, etc.) of the resulting sealing component.
[0116] As such aromatic hydrocarbons, for example, benzene, toluene, ethylbenzene, 1-phenylpropane, isopropylbenzene, n-butylbenzene, tert-butylbenzene, sec-butylbenzene, o-xylene, m-xylene or p-xylene, 2-ethyltoluene, 3-ethyltoluene or 4-ethyltoluene, etc., can be mentioned. These aromatic hydrocarbons can be used alone or in combination of two or more.
[0117] Among the above, from the viewpoint of the stability of the dispersion and the ease of handling such as removal of the hydrophobic solvent during the preparation of the composition described below, it is particularly preferred to use at least one selected from the group consisting of toluene, o-xylene, m-xylene or p-xylene, and benzene as the hydrophobic solvent.
[0118] The content of the hydrophobic solvent contained in the dispersion can be arbitrarily selected, as long as it is appropriately adjusted to the desired solid content. The content of the hydrophobic solvent is, for example, preferably 40% by mass or more and 95% by mass or less, more preferably 50% by mass or more and 90% by mass or less, and further preferably 60% by mass or more and 80% by mass or less. Thus, the dispersion and the resin component described later, especially the mixing of the methyl silicone resin, becomes easier. As required, the amount can also be 60% by mass or more and 90% by mass or less, 65% by mass or more and 85% by mass or less, 70% by mass or more and 80% by mass or less.
[0119] (Hydrophilic solvent)
[0120] The dispersion of the present embodiment may contain a hydrophilic solvent. For example, due to the method described later, the hydrophilic solvent may be included in the dispersion. As such a hydrophilic solvent, for example, an alcohol solvent, a ketone solvent, a nitrile solvent, etc. may be cited. These hydrophilic solvents may be used alone or in combination of two or more.
[0121] As the alcohol solvent, for example, branched or linear alcohol compounds having 1 to 4 carbon atoms and ether condensates thereof can be cited. These alcohol solvents can be used alone or in combination of two or more. In addition, the alcohol compound contained in the alcohol solvent can also be any one of a primary alcohol, a secondary alcohol, and a tertiary alcohol. In addition, the alcohol compound contained in the alcohol solvent can be any one of a monohydric alcohol, a dihydric alcohol, and a trihydric alcohol. More specifically, examples of the alcohol solvent include methanol, ethanol, 1-propanol, isopropanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, methylene glycol, 1,2-ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2-butene-1,4-diol, 1,4-butynediol, glycerol, diethylene glycol, and 3-methoxy-1,2-propanediol.
[0122] Examples of the ketone solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone.
[0123] Examples of the nitrile solvent include acetonitrile and the like.
[0124] The hydrophilic solvent preferably contains an alcohol solvent from the viewpoint of excellent affinity with both water and the hydrophobic solvent and promoting their mixing. In this case, the number of carbon atoms of the alcohol compound constituting the alcohol solvent is preferably 1 to 3, more preferably 1 to 2.
[0125] Among the above, methanol and ethanol, especially methanol, can fully demonstrate the effect of the above alcohol solvent and can therefore be preferably used.
[0126] The content of the hydrophilic solvent in the dispersion is, for example, preferably 10% by mass or less, more preferably 7% by mass or less, further preferably 5% by mass or less, and particularly preferably 3% by mass or less. The content of the hydrophilic solvent may be 0% by mass.
[0127] (2.4 Other ingredients)
[0128] The dispersion liquid involved in the present embodiment may also contain ingredients other than the above. For example, the dispersion liquid involved in the present embodiment may also contain ingredients other than the above as needed, for example, common additives such as dispersants, dispersing aids, antioxidants, flow regulators, thickeners, pH regulators, preservatives, etc.
[0129] Furthermore, the dispersion liquid according to the present embodiment may contain components obtainable by the method described later, for example, acid, water, alcohol, and the like.
[0130] In addition, in this specification, the dispersion involved in the present embodiment is distinguished from the composition involved in the present embodiment, and the composition involved in the present embodiment contains a resin component and can form a sealing component by curing. That is, even if the dispersion involved in the present embodiment contains a resin component described later, when simply cured, the amount of the resin component described later is not contained in the amount of the degree of the sealing component. More specifically, the mass ratio of the resin component to the metal oxide particles in the dispersion involved in the present embodiment is preferably in the range of 0:100 to 40:60, more preferably in the range of 0:100 to 30:70, and further preferably in the range of 0:100 to 20:80 in terms of resin component: metal oxide particles. The dispersion involved in the present embodiment is particularly preferably essentially free of the resin component described later, and most preferably completely free of the resin component described later.
[0131] In the dispersion liquid involved in this embodiment, the surface of the metal oxide particles is fully modified by the silane compound and the silicone compound. In addition, the metal oxide particles modified in this way have excellent affinity with the methyl silicone resin and can be dispersed relatively uniformly in the methyl silicone resin. Therefore, even when the metal oxide particles are dispersed in the methyl silicone resin, the generation of turbidity such as white turbidity is suppressed. In addition, the viscosity change of the methyl silicone resin containing the metal oxide particles is also suppressed.
[0132] <3. Method for producing dispersion>
[0133] Next, a method for producing the dispersion liquid according to the present embodiment will be described.
[0134] The method for producing a dispersion liquid according to the present embodiment comprises: step B of mixing a silane compound and metal oxide particles to obtain a mixed liquid;
[0135] Step C, dispersing the metal oxide particles in the mixed solution to obtain a first dispersion solution in which the metal oxide particles are dispersed;
[0136] Step D, adding a hydrophobic solvent to the first dispersion to obtain a second dispersion; and
[0137] In step E, a silicone compound is added to the second dispersion to obtain a third dispersion.
[0138] The content of the metal oxide particles in the mixed solution of the step B is 10% by mass or more and 49% by mass or less, and the total content of the silane compound and the metal oxide particles in the mixed solution is 65% by mass or more and 98% by mass or less.
[0139] Step D of adding the hydrophobic solvent is any one of the following steps: step d1, after heating the first dispersion, adding the hydrophobic solvent at a rate at which the metal oxide particles do not aggregate; step d2, while heating the first dispersion, adding the hydrophobic solvent at a rate at which the metal oxide particles do not aggregate; or step d3, after adding the hydrophobic solvent at a rate at which the metal oxide particles do not aggregate, heating the first dispersion.
[0140] In addition, the total content of the silane compound and the metal oxide particles can also be evaluated based on the solid content.
[0141] Furthermore, the total content of the silane compound and the metal oxide particles does not contain alcohol generated during the hydrolysis of the silane compound described later. That is, the total content of the silane compound and the metal oxide particles refers to the total content of the silane compound, the hydrolyzed silane compound, and the metal oxide particles. In addition, of course, the total content is a value including the content of the metal oxide particles attached to the silane compound.
[0142] Furthermore, in the present embodiment, before the above-mentioned steps, a step A (hydrolysis step) may be included in which a silane compound and water are mixed to obtain a hydrolyzed liquid containing a hydrolyzed silane compound.
[0143] Hereinafter, each step will be described in detail.
[0144] (Step A (Hydrolysis Step))
[0145] In the hydrolysis step, at least the silane compound and water are mixed to obtain a hydrolyzed solution containing the hydrolyzed silane compound. Thus, by using a mixed solution in which at least a part of the silane compound is hydrolyzed in advance, the silane compound is easily attached to the metal oxide particles in the dispersion step described later.
[0146] As the silane compound, one of the above-mentioned silane compounds may be used alone, or two or more of them may be used in combination.
[0147] Furthermore, the content of the silane compound in the hydrolyzed solution is not particularly limited. It can be the remainder after removing other components from the hydrolyzed solution, for example, preferably 60% by mass or more and 99% by mass or less, more preferably 70% by mass or more and 97% by mass or less, and further preferably 80% by mass or more and 95% by mass or less. It can also be 85% by mass or more and 95% by mass or 87% by mass or more and 93% by mass or less as required.
[0148] Furthermore, in the hydrolysis step, a surface modification material other than the silane compound may be contained in the hydrolysis liquid.
[0149] Furthermore, in the hydrolysis step, the hydrolysis liquid includes water, and water serves as a substrate for the hydrolysis reaction of the surface modification material such as the silane compound.
[0150] The content of water in the hydrolyzate is not particularly limited and can be arbitrarily selected. For example, the content of water can be appropriately set corresponding to the amount of the silane compound. For example, relative to 1 mol of the silane compound, the amount of water added to the hydrolyzate is preferably 0.5 mol or more and 5 mol or less, more preferably 0.6 mol or more and 3 mol or less, and further preferably 0.7 mol or more and 2 mol or less. Thus, the hydrolysis reaction of the silane compound can be fully carried out, and the aggregation of metal oxide particles in the dispersion made of excess water can be more reliably prevented.
[0151] Alternatively, the water content in the hydrolysis liquid is, for example, preferably 1 mass % to 20 mass %, more preferably 1 mass % to 15 mass %, and further preferably 1 mass % to 10 mass %.
[0152] Furthermore, a catalyst may be added to the hydrolysis solution together with the silane compound and water. As the catalyst, for example, an acid or a base may be used.
[0153] In the hydrolysis solution, the acid catalyzes the hydrolysis reaction of the silane compound. On the other hand, the base catalyzes the condensation reaction between the hydrolyzed silane compound and the functional groups on the surface of the metal oxide particles, such as hydroxyl groups or silanol groups. Through these reactions, in the dispersion step (step C) described later, the silane compound represented by the silane compound is easily attached to the metal oxide particles, and the dispersion stability of the metal oxide particles is improved.
[0154] Here, the above-mentioned "acid" refers to an acid based on the so-called Bronsted-Lowry definition, and refers to a substance that donates protons in the hydrolysis reaction of a surface modification material such as a silane compound. In addition, the above-mentioned "base" refers to a base based on the so-called Bronsted-Lowry definition, and refers to a substance that accepts protons in the hydrolysis reaction of a surface modification material such as a silane compound and the subsequent condensation reaction.
[0155] As the acid, there is no particular limitation as long as it can supply protons in the hydrolysis reaction of the silane compound, and it can be arbitrarily selected. For example, as the acid, inorganic acids such as hydrochloric acid, hydrobromic acid, hydroiodic acid, sulfuric acid, nitric acid, boric acid, phosphoric acid, or organic acids such as acetic acid, citric acid, and formic acid can be cited. These acids can be used alone or in combination of two or more.
[0156] As the base, there is no particular limitation as long as it can accept protons in the hydrolysis reaction of the silane compound, and it can be arbitrarily selected. For example, sodium hydroxide, potassium hydroxide, barium hydroxide, calcium hydroxide, ammonia, amines, etc. can be mentioned. These bases can be used alone or in combination of two or more.
[0157] Among the above, it is preferable to use an acid as the catalyst. As the acid, from the viewpoint of acidity, an inorganic acid is preferable, and hydrochloric acid is more preferable.
[0158] The content of the catalyst in the hydrolyzed solution is not particularly limited, for example, preferably more than 10ppm and less than 1000ppm, more preferably more than 20ppm and less than 800ppm, further preferably more than 30ppm and less than 600ppm. Thus, the hydrolysis of the silane compound can be fully promoted, and the side reaction of the silane compound can be suppressed. In addition, as required, it can also be more than 0.1ppm and less than 100ppm, more than 1ppm and less than 10ppm. And, for example, when using an acid such as hydrochloric acid (1N) as a catalyst, relative to 100 mass parts of the hydrolyzed solution, the amount of the acid can be more than 0.001 mass parts and less than 5 mass parts, it can also be more than 0.001 mass parts and less than 3 mass parts, it can also be more than 0.005 mass parts and less than 1 mass part, it can also be more than 0.005 mass parts and less than 0.1 mass part.
[0159] Furthermore, the hydrolysis solution may contain a hydrophilic solvent as required. The hydrophilic solvent can promote the mixing of water and the silane compound in the hydrolysis solution, and further promote the hydrolysis reaction of the silane compound.
[0160] Examples of such a hydrophilic solvent include various hydrophilic solvents that can be contained in the above-mentioned dispersion.
[0161] Among the above, the hydrophilic solvent preferably contains at least one selected from the group consisting of alcohol solvents, and more preferably contains at least one selected from the group consisting of methanol and ethanol, from the viewpoint of having excellent affinity with both water and the hydrophobic solvent and promoting their mixing.
[0162] Furthermore, the content of the hydrophilic solvent in the hydrolyzed solution is not particularly limited, for example, it is preferably 60% by mass or less, and more preferably 50% by mass or less. When within this range, the content of the silane compound and water in the hydrolyzed solution can be sufficiently increased. The content of the hydrophilic solvent can also be 40% by mass or less or 20% by mass or less. Furthermore, the content of the hydrophilic solvent in the hydrolyzed solution is, for example, preferably 10% by mass or more, and more preferably 15% by mass or more. When within this range, the mixing of the surface modification material and water can be further promoted, and as a result, the hydrolysis reaction of the surface modification material can be efficiently carried out. In addition, the hydrolyzed solution may not contain any hydrophilic solvent other than the compound derived from the hydrolysis reaction. That is, it may also contain only a hydrophilic solvent as a compound derived from the hydrolysis reaction.
[0163] In the present embodiment, when a silane compound having an alkoxy group is used as the silane compound, an alcohol compound derived from the alkoxy group is contained in the mixed solution due to its hydrolysis. Since the hydrolysis reaction also proceeds in the adsorbed water of the metal oxide particles, it may occur in any of the steps A to E. Therefore, in this case, the obtained dispersion will contain the alcohol compound unless there is a step of removing the alcohol compound.
[0164] In the hydrolysis step, after the hydrolysis solution is prepared, it may be maintained at an arbitrarily selected constant temperature for a predetermined time, thereby further promoting the hydrolysis of the silane compound.
[0165] In this treatment, the temperature of the hydrolysis solution is not particularly limited and can be arbitrarily selected and can be appropriately changed according to the type of the silane compound. For example, it is preferably 5°C to 65°C, more preferably 20°C to 65°C, and further preferably 30°C to 60°C. It can also be 40°C to 75°C, or 50°C to 70°C as required.
[0166] The holding time at the above temperature is not particularly limited, but is preferably 10 minutes to 180 minutes, more preferably 30 minutes to 120 minutes, and may be 15 minutes to 60 minutes, or 20 minutes to 40 minutes, as required.
[0167] Furthermore, while the hydrolyzed liquid is being maintained, the hydrolyzed liquid may be stirred appropriately.
[0168] (Process B (Mixing process))
[0169] In the mixing step, the silane compound and the metal oxide particles are mixed to obtain a mixed solution. In the mixing step, water or a catalyst may be mixed in addition to the silane compound and the metal oxide particles. In addition, in the case where a hydrolyzed solution is obtained by the above-mentioned hydrolysis step, the mixed solution can be obtained by mixing the hydrolyzed solution and the metal oxide particles.
[0170] Furthermore, the mixture is mixed so that the content of the metal oxide particles in the mixed solution is 10 mass % to 49 mass % and the total content of the silane compound and the metal oxide particles is 65 mass % to 98 mass %.
[0171] Thus, in the present embodiment, the total content of the silane compound and the metal oxide particles in the mixed solution is very large. In addition, the dispersion medium such as organic solvent and water, which was previously considered to be necessary, is not included in the mixed solution, or is only mixed in a very small amount compared to the past. Or, by hydrolysis, a small amount of inevitable alcohol compound is contained. Even in this case, by passing through the dispersion process, the metal oxide particles can be uniformly dispersed in the mixed solution, and the uniform attachment (surface modification) of the silane compound to the metal oxide particles is achieved.
[0172] In detail, when the surface of metal oxide particles is modified by a surface modification material in a liquid phase, usually, not only the metal oxide particles and the surface modification material are mixed, but also a dispersion medium is mixed to obtain a mixed solution, and the mixed solution is dispersed using a disperser. In addition, when the metal oxide particles surface-modified by this method are mixed with a methyl silicone resin, they cannot be fully dispersed in the methyl silicone resin and agglomerate, and as a result, there is a problem of turbidity such as white turbidity in the methyl silicone resin. In this case, the added metal oxide particles cannot fully exert the desired performance.
[0173] The dispersion medium is usually added for the purpose of reducing the viscosity of the mixed solution, uniformly dispersing the metal oxide particles, and uniformly modifying the surface of the metal oxide particles by the surface modification material. In the past, it was believed that, without the use of a dispersion medium, the viscosity of the dispersion solution increased, and the surface modification material could not be fully attached to the surface of the metal oxide particles. The inventors of the present invention surprisingly found that by not using or only using a small amount of such a dispersion medium that was previously considered to be necessary, the metal oxide particles are directly dispersed in a high concentration of a silane compound, and in the resulting dispersion solution, the uniform dispersion of the metal oxide particles can be achieved, and the uniform modification of the metal oxide particles by the silane compound can be performed.
[0174] Silane compounds are low molecular weight and relatively low in viscosity. Moreover, by being hydrolyzed in the above-mentioned hydrolysis step, they have good adhesion to metal oxide particles. Therefore, silane compounds are extremely suitable for dispersing metal oxide particles in high-concentration surface modification materials.
[0175] When the total content of the silane compound and the metal oxide particles is less than 65% by mass, the components other than the above two components, such as the dispersion medium, become too much, so that in the dispersion process (process C) described later, the silane compound cannot be fully attached to the surface of the metal oxide particles. As a result, a large amount of hydroxyl groups remain on the surface of the metal oxide particles, and then when the obtained dispersion is mixed with a hydrophobic material, the metal oxide particles condense and produce turbidity in the hydrophobic material. The total content of the silane compound and the metal oxide particles can be more than 65% by mass, preferably more than 70% by mass, and more preferably more than 75% by mass. As required, it can also be more than 80% by mass, more than 85% by mass, more than 90% by mass, and more than 92% by mass.
[0176] In contrast, when the total content of the silane compound and the metal oxide particles exceeds 98% by mass, the viscosity of the mixed solution becomes too high, and in the dispersion step (step C) described later, the silane compound cannot be fully attached to the surface of the metal oxide particles. The total content of the silane compound and the metal oxide particles can be as long as it is less than 98% by mass, preferably less than 97% by mass, and more preferably less than 95% by mass. As required, it can also be less than 90% by mass, less than 85% by mass, less than 80% by mass, or less than 75% by mass.
[0177] Furthermore, as described above, the content of the metal oxide particles in the mixed solution is 10 mass % or more and 49 mass % or less. By using this range, the amount of the silane compound relative to the metal oxide particles can be within an appropriate range, and the silane compound can be uniformly attached to the surface of the metal oxide particles while suppressing the increase in the viscosity of the mixed solution.
[0178] On the other hand, when the content of the metal oxide particles in the mixed solution is less than 10% by mass, the silane compound is excessive relative to the amount of the metal oxide particles, and the excess silane compound in the obtained dispersion induces aggregation of the metal oxide particles. The content of the metal oxide particles in the mixed solution is preferably 20% by mass or more, more preferably 23% by mass or more, more preferably 26% by mass or more, and particularly preferably 30% by mass or more.
[0179] Furthermore, when the content of metal oxide particles exceeds 49% by mass, the amount of silane compound relative to the metal oxide particles is insufficient, and a sufficient amount of silane compound is not attached to the metal oxide particles. Furthermore, the content of metal oxide particles becomes too much, and as a result, the viscosity of the mixed solution increases too much, and the metal oxide particles cannot be fully dispersed in the dispersion step (step C) described later. The content of metal oxide particles in the mixed solution is preferably 45% by mass or less, and more preferably 40% by mass or less. The amount is further preferably 38% by mass or less, and particularly preferably 36% by mass or less. It can also be 34% by mass or less.
[0180] The content of the silane compound relative to the content of the metal oxide particles in the mixed solution is not particularly limited, and is, for example, preferably 100% by mass or more and 800% by mass or less, more preferably 140% by mass or more and 600% by mass or less, further preferably 180% by mass or more and 400% by mass or less, and particularly preferably 200% by mass or more and 270% by mass or less, relative to the amount of the metal oxide particles. Thus, the amount of the silane compound relative to the metal oxide particles can be within an appropriate range, and the silane compound can be uniformly attached to the surface of the metal oxide particles.
[0181] Furthermore, in the mixing step, an organic solvent may be further mixed in the mixed solution. By mixing the organic solvent in the mixed solution, the reactivity of the surface modification material can be controlled, and the degree of adhesion of the surface modification material to the surface of the metal oxide particles can be controlled. Furthermore, the viscosity of the mixed solution can be adjusted by the organic solvent.
[0182] Examples of such an organic solvent include the hydrophobic solvent or the hydrophilic solvent mentioned as the dispersion medium of the dispersion liquid according to the present embodiment. These organic solvents may be used alone or in combination of two or more.
[0183] The content of the organic solvent in the mixed liquid is not particularly limited as long as it satisfies the above-mentioned contents of the metal oxide particles and the silane compound. In addition, it is a matter of course that the mixed liquid does not need to contain an organic solvent.
[0184] The mixing time and mixing temperature in the mixing step can be arbitrarily selected. For example, the mixing may be performed at room temperature, or the materials may be stirred for about 0 to 600 seconds after mixing.
[0185] (Process C (dispersion process))
[0186] In the dispersing step, the metal oxide particles are dispersed in the mixed solution to obtain a first dispersion in which the metal oxide particles are dispersed. In this embodiment, the metal oxide particles are dispersed in a high concentration of a hydrolyzed silane compound. Therefore, in the obtained first dispersion, the silane compound is relatively uniformly attached to the surface of the metal oxide particles, and the metal oxide particles are relatively uniformly dispersed.
[0187] The dispersion of the metal oxide particles can be carried out by a known dispersion method, for example, using a disperser. As a disperser, for example, a bead mill, a ball mill, a homogenizer, a disperser, a stirrer, etc. are preferably used. Step C is preferably a step in which only the mixture obtained in step B is dispersed.
[0188] Here, in the dispersing step, it is preferred to disperse the metal oxide particles in the mixed liquid by applying the minimum energy required without applying excessive energy so that the particle size (dispersed particle size) of the metal oxide particles in the dispersion liquid becomes substantially uniform.
[0189] The dispersion time can be arbitrarily selected according to the conditions, and may be, for example, 3 to 15 hours, preferably 4 to 12 hours, and more preferably 5 to 10 hours, but is not limited thereto.
[0190] The dispersion temperature can be arbitrarily selected, and may be, for example, 10 to 50° C., preferably 20 to 40° C., and more preferably 30 to 40° C. However, the present invention is not limited thereto.
[0191] In addition, the dispersion step C may be different from the mixing step B in that the dispersion is performed continuously for a certain period of time.
[0192] (Step D (Adding Step (First Adding Step)))
[0193] In the adding step, a hydrophobic solvent is added to the first dispersion obtained in step C (dispersion step) to adjust the first dispersion to a desired solid content (concentration).
[0194] The solid content (concentration) of the first dispersion obtained in the dispersion step is high. Therefore, the viscosity is high and the operability is poor. However, in order to reduce the solid content, if a hydrophobic solvent is simply added to the obtained first dispersion, the hydrophobicity of the particle surface is low, so the particles are aggregated and a uniform dispersion cannot be obtained.
[0195] Therefore, the present inventors conducted research and found that a dispersion having a low solid content can be prepared by heating the obtained first dispersion and slowly adding a hydrophobic solvent. This operation can achieve very excellent effects.
[0196] The above mechanism is presumed as follows.
[0197] By heating the first dispersion liquid, the silane compound attached to the metal oxide particles is polymerized, and the hydrophobicity of the particle surface is improved. In addition, even if the polymerization reaction of the silane compound is excessively carried out, the metal oxide particles will also condense. Therefore, the hydrophobic solvent is slowly added to the first dispersion liquid in which the polymerization reaction is being carried out. By carrying out this addition, excessive polymerization reaction is suppressed, and the surface is slowly hydrophobized, and the hydrophobic solvent can be slowly mixed.
[0198] That is, a hydrophobic solvent is added in an amount that does not cause the metal oxide particles to aggregate, and the polymerization reaction of the silane compound is allowed to proceed to an extent that the silane compound is compatible with the added amount of the hydrophobic solvent. Thus, a dispersion adjusted to a desired solid content can be obtained.
[0199] As described above, the hydrophobic solvent may be added slowly to prevent the metal oxide particles from agglomerating. Therefore, the hydrophobic solvent may be added after the first dispersion obtained in the above-mentioned dispersing step is heated, or the first dispersion may be heated after the hydrophobic solvent is added, or the first dispersion may be heated and the hydrophobic solvent may be added simultaneously.
[0200] That is, more specifically, the adding step may be a step d1 of adding the hydrophobic solvent at a rate at which the metal oxide particles do not aggregate after heating the first dispersion, a step d2 of adding the hydrophobic solvent at a rate at which the metal oxide particles do not aggregate while heating the first dispersion, or a step d3 of heating the first dispersion after adding the hydrophobic solvent at a rate at which the metal oxide particles do not aggregate.
[0201] In addition, in step d1, when adding the metal oxide particles, the heating of the dispersion may be continued or stopped. The temperature of the dispersion may be constant or may be changed. Preferably, the temperature is maintained constant. In step d2, when adding the metal oxide particles, the temperature of the dispersion may be constant or may be changed.
[0202] The hydrophobic solvent may be added continuously or intermittently in two or more times. In the case of intermittent addition, the number of times is not limited, for example, it can be added in 2 to 6 times or 3 to 5 times. In the case of adding the hydrophobic solvent in multiple times, the amount of the hydrophobic solvent may be the same or may be varied.
[0203] The speed at which the metal oxide particles do not condense is not particularly limited. The addition rate or ratio of the hydrophobic solvent can be arbitrarily selected. For example, the hydrophobic solvent can be added continuously at an addition rate at which the solid content is reduced within a range of more than 3% by mass and less than 20% by mass within 1 hour. In other words, after continuously adding the hydrophobic solvent for 1 hour, the difference in the solid content in the dispersion before and after the addition can be within a range of more than 3% by mass and less than 20% by mass. The addition amount of the hydrophobic solvent can be appropriately adjusted so that the addition amount of the hydrophobic solvent is increased when the heating temperature is high, and the addition amount of the hydrophobic solvent is reduced when the heating temperature is low.
[0204] As mentioned above, the addition speed or ratio of the hydrophobic solvent can be arbitrarily selected.For example, the hydrophobic solvent can be added in stages, so that every 30 minutes, every 1 hour or every 2 hours, more than 3 mass % and 20 mass % below the scope of reducing solid content.The addition of the hydrophobic solvent can be appropriately adjusted, so that when the heating temperature is high, the addition of the hydrophobic solvent once added is increased, and when the heating temperature is low, the addition of the hydrophobic solvent once added is reduced.In this case, the addition time or the number of additions of the hydrophobic solvent can also be preferably adjusted.
[0205] The heating temperature is not particularly limited as long as it is a temperature at which the polymerization reaction of the silane compound is carried out. The heating temperature is preferably, for example, 35°C or more and 80°C or less. The heating temperature may be 40°C or more and 75°C or more, or 45°C or more and 70°C or less, or 50°C or more and 65°C or less. By making the heating temperature 35°C or more, the polymerization reaction of the silane compound can be carried out. On the other hand, by making the heating temperature 80°C or less, the aggregation of the metal oxide particles caused by the rapid reaction of the silane compound can be suppressed.
[0206] The heating time can be appropriately implemented until the adjustment of the solid component is completed. For example, it is preferably more than 4 hours and less than 12 hours. By heating time being more than 4 hours, the polymerization reaction of the silane compound can be carried out and can be mixed with a hydrophobic solvent. On the other hand, by heating time being less than 12 hours, the agglomeration of the metal oxide particles caused by the excessive polymerization reaction of the silane compound can be suppressed.
[0207] As long as the hydrophobic solvent is a solvent that is compatible with the material that is intended to be mixed with the dispersion of the present embodiment, it is not particularly limited. As the hydrophobic solvent, for example, aromatics, saturated hydrocarbons, unsaturated hydrocarbons, etc. can be cited. These hydrophobic solvents can be used alone or in combination. Two or more kinds can also be used. Among them, aromatics are preferred, and aromatic hydrocarbons are particularly preferred. The compatibility of aromatics and methyl silicone resins is excellent, which contributes to the improvement of the viscosity characteristics of the composition thus obtained and the improvement of the quality (transparency, shape, etc.) of the formed sealing component.
[0208] As the aromatic hydrocarbon, for example, benzene, toluene, ethylbenzene, 1-phenylpropane, isopropylbenzene, n-butylbenzene, tert-butylbenzene, sec-butylbenzene, o-xylene, m-xylene, p-xylene, 2-ethyltoluene, 3-ethyltoluene or 4-ethyltoluene, etc., can be mentioned. These aromatic hydrocarbons can be used alone or in combination of two or more.
[0209] Among them, from the viewpoint of the stability of the dispersion or the ease of workability such as removal of the dispersion medium when preparing the composition described below, it is particularly preferred to use at least one selected from the group consisting of toluene, o-xylene, m-xylene, p-xylene and benzene as the aromatic hydrocarbon.
[0210] The content of the hydrophobic solvent contained in the final dispersion can be appropriately adjusted to the desired solid content. The content of the hydrophobic solvent is, for example, preferably 40% by mass or more and 95% by mass or less, more preferably 50% by mass or more and 90% by mass or less, and further preferably 60% by mass or more and 80% by mass or less.
[0211] The second dispersion adjusted to a desired solid content can be obtained by the first addition step. By using the second dispersion, the handling properties of the dispersion in the following steps are improved.
[0212] (Process F (removal process))
[0213] In the present embodiment, a step F of removing alcohol generated by hydrolysis may be provided between the step D and the step E.
[0214] It is presumed that providing the removal step improves the production efficiency of the steps described below.
[0215] The removal method is not particularly limited, and for example, an evaporator can be used. The removal step may be performed until the alcohol is completely removed, or until about 5% by mass remains.
[0216] (Step E (Second Addition Step))
[0217] Next, the metal oxide particles are treated with a silicone compound to obtain a third dispersion. As described above, in the dispersion step, the silane compound is relatively uniformly attached to the surface of the metal oxide particles. Therefore, the silicone compound can be relatively uniformly attached to the surface of the metal oxide particles through the silane compound.
[0218] In the second adding step, first, the second dispersion and the silicone compound are mixed to obtain a treatment liquid. Then, the treatment liquid may be kept at a constant temperature for a predetermined time. This can further promote the adhesion of the silicone compound to the metal oxide particles.
[0219] Examples of the silicone compound include the above-mentioned silicone compounds. These silicone compounds may be used alone or in combination of two or more.
[0220] The silicone compound can be mixed with the second dispersion so that the content of the silicone compound in the third dispersion is preferably 50% by mass or more and 500% by mass or less, more preferably 80% by mass or more and 400% by mass or less, and further preferably 100% by mass or more and 300% by mass or less relative to the metal oxide particles. Thus, a sufficient amount of the silicone compound can be attached to the surface of the metal oxide particles, which can improve the dispersion stability of the metal oxide particles and improve the dispersibility in the methyl silicone resin. In addition, the amount of free silicone compound can be reduced, and the unintentional aggregation of the metal oxide particles in the methyl silicone resin can be suppressed.
[0221] In the second adding step, the holding temperature is not particularly limited and can be appropriately changed depending on the type of silicone compound, but is preferably 40° C. or higher and 130° C. or lower, and more preferably 50° C. or higher and 120° C. or lower.
[0222] The retention time is not particularly limited, but is, for example, preferably 1 hour to 24 hours, and more preferably 2 hours to 20 hours.
[0223] In addition, during the above-mentioned maintaining process, the second dispersion liquid may be stirred appropriately.
[0224] Furthermore, in the second adding step, the treatment with the silicone compound may be performed multiple times. For example, by using different types of silicone compounds and performing the treatment with the silicone compound multiple times, it becomes easier to control the surface state of the metal oxide particles corresponding to the type of methyl silicone resin.
[0225] Furthermore, in the second adding step, the solid content may be measured after the treatment with the silicone compound, and a hydrophobic solvent may be added to obtain a desired solid content. By reducing the solid content, mixing with the sealing resin described later becomes easier.
[0226] In this way, the metal oxide particles can be treated with the silicone compound to obtain the third dispersion.
[0227] In the dispersion liquid manufactured by the manufacturing method of the dispersion liquid involved in the present embodiment, the metal oxide particles are uniformly dispersed, and the surfaces of the metal oxide particles are uniformly and fully modified by the silane compound and the silicone compound. In addition, the metal oxide particles modified in this way have excellent affinity with the methyl silicone resin and can be relatively uniformly dispersed in the methyl silicone resin. Therefore, even when the metal oxide particles are dispersed in the methyl silicone resin, the generation of turbidity such as white turbidity is also suppressed. In addition, the viscosity change of the methyl silicone resin containing the metal oxide particles is also suppressed.
[0228] In addition, the dispersion liquid involved in this embodiment may also be mixed with components other than the above as needed, for example, common additives such as dispersants, dispersing aids, antioxidants, flow regulators, thickeners, pH regulators, preservatives, etc. These may also be added to any process as needed.
[0229] As described above, the dispersion of the present embodiment can mix the metal oxide particles with the hydrophobic material by directly dispersing the metal oxide particles in the silane compound. It is estimated that the silane compound adheres to the metal oxide particles in a larger amount and covers them densely compared to conventional dispersions.
[0230] In addition, it is not clear whether the dispersion can be mixed with the hydrophobic material depending on the state of the surface of the metal oxide particles. Therefore, it is difficult to directly determine the characteristics of the dispersion of the present embodiment based on the state of the surface of the metal oxide particles modified with the silane compound and the silicone compound.
[0231] In the case where the dispersion contains metal oxide particles, at least a portion of one or more silane compounds and one or more silicone compounds attached to the metal oxide particles, and a hydrophobic solvent, it is not simple to determine the state of the surface for enabling the metal oxide particles to be mixed with the hydrophobic material by language. The reason why the metal oxide particles can be well mixed with the hydrophobic material is speculated to be due to the complex interweaving of many factors such as the structure of the silane compound and the silicone compound, the degree of polymerization in the dispersion, and the characteristics of the metal oxide particles. However, according to the present invention, a dispersion with excellent effect can be provided.
[0232] <4. Composition>
[0233] Next, the composition according to the present embodiment will be described.
[0234] The composition according to the present embodiment is a mixture of the above dispersion and a resin component. Therefore, the composition according to the present embodiment contains, in addition to the metal oxide particles whose surfaces are modified with the above silane compound and silicone compound, a resin component, that is, at least one of a resin and a precursor thereof.
[0235] The composition according to this embodiment can be cured as described below and used as a sealing member of a light-emitting element. The composition according to this embodiment contains metal oxide particles that contribute to improving the refractive index and transparency, and can improve the brightness of light of a light-emitting device when used as a sealing member.
[0236] Furthermore, the composition according to the present embodiment contains metal oxide particles whose surface is modified by the above-mentioned silane compound and silicone compound. Therefore, even when a methyl silicone resin is contained as a resin component, the aggregation of the metal oxide particles is suppressed, and the decrease in transparency is suppressed. Therefore, when the composition according to the present embodiment is used for a sealing component, the brightness of the light of the light-emitting device can be increased.
[0237] The content of the metal oxide particles in the composition of the present embodiment can be arbitrarily selected. From the viewpoint of obtaining a composition with high transparency, the amount is preferably 5% by mass or more and 50% by mass or less, more preferably 5% by mass or more and 40% by mass or less, and further preferably 10% by mass or more and 35% by mass or less. As required, it can also be 1% by mass or more and 20% by mass or less, 3% by mass or more and 15% by mass or less.
[0238] Furthermore, the content of the surface modification material such as the silane compound and the silicone compound in the composition can correspond to the content in the dispersion liquid according to the present embodiment.
[0239] The resin component is the main component in the composition involved in this embodiment. When the composition involved in this embodiment is used as a sealing material, the resin component is cured to seal the light-emitting element. As a result, deterioration factors from the external environment such as moisture and oxygen are prevented from reaching the light-emitting element. In addition, in this embodiment, the cured product obtained from the resin component is basically transparent and can transmit light emitted from the light-emitting element.
[0240] As such a resin component, there is no particular limitation as long as it can be used as a sealing material. For example, a single silicone resin or epoxy resin or other resin may be used alone, or two or more resins may be used in combination. In particular, from the viewpoint of durability, silicone resins are preferred, and methyl silicone resins are particularly preferred.
[0241] As the methyl silicone resin, for example, dimethyl silicone resin, methylphenyl silicone resin, etc. can be used.
[0242] The content of the methyl silicone resin in the resin component can be adjusted according to the desired characteristics, and is not particularly limited. For example, it can be 100% by mass, or more than 20% by mass and less than 80% by mass, or more than 30% by mass and less than 70% by mass, or more than 40% by mass and less than 60% by mass. In the past, if metal oxide particles were contained in the methyl silicone resin, the metal oxide particles would condense, and while the transparency decreased, the refractive index was not fully improved. In contrast, the composition involved in the present embodiment contains metal oxide particles surface-modified by the above-mentioned silane compound and silicone compound. Therefore, even in the case of such a large amount of methyl silicone resin as a resin component, the condensation of the metal oxide particles is also suppressed, and the transparency is suppressed. In addition, since the methyl silicone resin can be used, the durability of the sealing component formed using the composition is improved.
[0243] The structure of the resin component may be a two-dimensional chain structure, a three-dimensional network structure, or a cage structure.
[0244] The resin component can be in the form of a polymer that cures when used as a sealing component. In the composition, the resin component can also be in a state before curing, i.e., a precursor. Therefore, the resin component present in the composition can be, for example, a monomer, an oligomer, or a polymer.
[0245] As the resin component, an addition reaction type resin component, a condensation reaction type resin component, or a radical polymerization reaction type resin component may be used.
[0246] The viscosity of the resin component at 25° C. measured in accordance with JIS Z 8803:2011 is, for example, preferably 10 mPa·s to 100,000 mPa·s, more preferably 100 mPa·s to 10,000 mPa·s, and further preferably 1,000 mPa·s to 7,000 mPa·s.
[0247] Furthermore, the content of the resin component in the composition according to the present embodiment may be the remainder of other components, and is preferably, for example, 10% by mass or more and 70% by mass or less.
[0248] The mass ratio of the resin component to the surface-modified metal oxide particles in the composition of this embodiment can be arbitrarily selected. For example, the resin component: surface-modified metal oxide particles is preferably in the range of 50:50 to 90:10, and more preferably in the range of 60:40 to 80:20.
[0249] The composition according to the present embodiment may contain a dispersion medium derived from the dispersion liquid according to the present embodiment, or may remove the dispersion medium. That is, the dispersion medium derived from the dispersion liquid may be completely removed. The dispersion medium may remain in the composition at a level of 1% by mass or more and 10% by mass or less, or at a level of 2% by mass or more and 5% by mass or less.
[0250] Furthermore, within the scope of not hindering the purpose of the present invention, the composition involved in this embodiment may also contain phosphor particles. The phosphor particles absorb light of a specific wavelength emitted from the light-emitting element and emit light of a specified wavelength. That is, the wavelength of light can be converted by the phosphor particles and the color tone can be adjusted.
[0251] The phosphor particles are not particularly limited as long as they can be used in a light-emitting device as described below, and can be arbitrarily selected. They can be appropriately selected and used so that the light-emitting device emits a desired color.
[0252] The content of the phosphor particles in the composition of the present embodiment can be appropriately adjusted so as to obtain a desired brightness.
[0253] Furthermore, the composition of the present embodiment may contain commonly used additives such as preservatives, polymerization initiators, polymerization inhibitors, curing catalysts, and light diffusing agents within the scope of not hindering the purpose of the present invention. As the light diffusing agent, silica particles having an average particle size of 1 μm to 30 μm are preferably used.
[0254] The composition according to the present embodiment can be produced by mixing the dispersion according to the present embodiment and the resin component. After mixing, the dispersion medium contained in the dispersion may be removed by an evaporator or the like as needed.
[0255] The composition according to the present embodiment contains metal oxide particles whose surfaces are modified by the above-mentioned silane compound and silicone compound. As a result, even when a methyl silicone resin is contained as a resin component, the aggregation of the metal oxide particles is suppressed, and the decrease in transparency is suppressed. Therefore, using the composition according to the present embodiment, a sealing component that improves the brightness of light of a light-emitting device can be formed.
[0256] In addition, the methyl silicone resin used in the above description may refer to a resin having, as a main skeleton, siloxane bonds in which silicon and oxygen are alternately bonded, and most of the functional groups bonded to Si atoms, for example, 60% or more, preferably 80% or more, are methyl groups. However, the present invention is not limited to this example.
[0257] <5. Sealing parts>
[0258] The sealing member according to this embodiment is a cured product of the composition according to this embodiment. The sealing member according to this embodiment is generally used as a sealing member disposed on a light emitting element or a part thereof.
[0259] The thickness and shape of the sealing member according to the present embodiment can be appropriately adjusted according to the desired use or characteristics, and are not particularly limited.
[0260] As described above, the sealing component involved in the present embodiment can be manufactured by curing the composition involved in the present embodiment. The curing method of the composition can be selected according to the characteristics of the resin component in the composition involved in the present embodiment. For example, thermal curing or electron beam curing can be cited. More specifically, the resin component in the composition of the present embodiment is cured by an addition reaction or a polymerization reaction, so that the sealing component of the present embodiment can be obtained.
[0261] The average dispersed particle size of the metal oxide particles in the sealing member is preferably 10 nm to 300 nm, more preferably 20 nm to 250 nm, and even more preferably 30 nm to 200 nm.
[0262] In addition, the average dispersed particle size of the metal oxide particles in the sealing component is the average particle size (median particle size) of the number distribution benchmark measured by transmission electron microscopy (TEM) of the sealing component. Furthermore, the average dispersed particle size of the metal oxide particles in the sealing component involved in the present embodiment is a value measured and calculated based on the dispersed particle size of the metal oxide particles in the sealing component. Regardless of the state in which the metal oxide particles are dispersed as primary particles or secondary particles, the average dispersed particle size is measured and calculated based on the diameter of the metal oxide particles in the dispersed state. Furthermore, in the present embodiment, the average particle size of the metal oxide particles in the sealing component can also be measured as the average particle size of the metal oxide particles attached with the surface modification material described later. In the sealing component, there may be metal oxide particles attached with the surface modification material and metal oxide particles not attached with the surface modification material. Therefore, usually, the average particle size of the metal oxide particles in the sealing component is measured as a value in their mixed state.
[0263] The sealing member according to this embodiment is a cured product of the composition according to this embodiment, and therefore has excellent refractive index and transparency. Therefore, according to this embodiment, a sealing member having excellent light extraction efficiency that improves the brightness of light in a light-emitting device can be obtained.
[0264] <6. Light-emitting device>
[0265] Next, a light emitting device according to this embodiment is described. The light emitting device according to this embodiment includes the above-mentioned sealing member and a light emitting element sealed by the sealing member.
[0266] Examples of the light emitting element include a light emitting diode (LED), an organic light emitting diode (OLED), etc. In particular, the sealing member according to the present embodiment is suitable for sealing a light emitting diode.
[0267] Hereinafter, the light-emitting device according to the present embodiment will be described by taking an example in which the light-emitting element is a light-emitting diode on a chip, that is, an LED chip, and the light-emitting device is an LED package.
[0268] Figure 1 to Figure 4 Each of them is a schematic diagram (cross-sectional view) showing an example of a light emitting device according to an embodiment of the present invention.
[0269] In addition, for the sake of convenience, the size of each component in the figure is appropriately emphasized and does not represent the actual size or ratio between components. In addition, in this specification and the drawings, the same symbols are marked for components with substantially the same functional structure, thereby omitting repeated descriptions.
[0270] Figure 1 The light emitting device (LED package) 1A shown includes: a substrate 2 having a recess 21; a light emitting element (LED chip) 3 arranged on the bottom surface of the recess 21 of the substrate 2; and a sealing member 4A for sealing the recess 21 by covering the light emitting element 3.
[0271] The sealing member 4A is composed of the sealing member involved in the present embodiment described above. Therefore, metal oxide particles derived from the composition involved in the present embodiment described above are dispersed in the sealing member 4A, and as a result, the light extraction efficiency in the light emitting device 1A is improved. In addition, phosphor particles 5 are dispersed in the sealing member 4A. The phosphor particles 5 convert the wavelength of at least a part of the light emitted by the light emitting element 3.
[0272] Figure 2 The light-emitting device 1B shown is different from the light-emitting device 1A in that the sealing member 4B is two layers. That is, the sealing member 4B has a first layer 41B that directly covers the light-emitting element 3 and a second layer 43B that covers the first layer 41B. The first layer 41B and the second layer 43B are both sealing members involved in this embodiment. In the first layer 41B, phosphor particles 5 are dispersed. On the other hand, the second layer 43B does not contain phosphor particles 5. The light-emitting device 1B improves the brightness of light by dispersing metal oxide particles derived from the composition involved in the above-mentioned present embodiment in the first layer 41B and the second layer 43B constituting the sealing member 4B.
[0273] Figure 3 The light-emitting device 1C shown is different from the light-emitting device 1A in that the structure of the sealing member 4C is different from that of the sealing member 4A. The sealing member 4C has a first layer 41C that directly covers the light-emitting element 3 and a second layer 43C that covers the first layer 41C. The first layer 41C is not the sealing member involved in the present embodiment, but is a sealing member of a resin that does not contain the above-mentioned metal oxide particles, and is composed of a resin that can be used for a sealing member. In addition, phosphor particles 5 are dispersed in the first layer 41C. On the other hand, the second layer 43C is the sealing member involved in the present embodiment. The light-emitting device 1C improves the light extraction efficiency by dispersing metal oxide particles derived from the composition involved in the above-mentioned present embodiment in the second layer 43C constituting the sealing member 4C.
[0274] exist Figure 4 In the light-emitting device 1D shown, the sealing member 4D has a first layer 41D directly covering the light-emitting element 3, a second layer 43D covering the first layer 41D, and a third layer 45D further covering the second layer 43D. The first layer 41D and the second layer 43D are not the sealing members involved in this embodiment, but are sealing members of a resin that does not contain the above-mentioned metal oxide particles, and are composed of a resin that can be used for a sealing member. In addition, phosphor particles 5 are dispersed in the second layer 43D. On the other hand, the third layer 45D is the sealing member involved in this embodiment. The light-emitting device 1D improves the brightness of light by dispersing metal oxide particles derived from the composition involved in the above-mentioned present embodiment in the third layer 45D constituting the sealing member 4D.
[0275] In addition, the light-emitting device of this embodiment is not limited to the illustrated embodiment. For example, the light-emitting device of this embodiment may not contain fluorescent particles in the sealing component. Furthermore, the sealing component of this embodiment may exist at any position in the sealing component.
[0276] As described above, in the light emitting device according to the present embodiment, since the light emitting element is sealed by the sealing member of the present embodiment, the brightness of light is improved.
[0277] Furthermore, the light-emitting device according to this embodiment uses the composition according to this embodiment as described above to seal the light-emitting element. Therefore, the present invention also relates to a method for manufacturing a light-emitting device, which in one embodiment has a step of sealing the light-emitting element using the composition according to this embodiment. In the same manner, the manufacturing method may also have a step of mixing the dispersion according to this embodiment and a resin component to obtain the composition.
[0278] The sealing of the light emitting element can be performed by applying the composition according to this embodiment to the light emitting element using a dispenser or the like, and then curing the composition.
[0279] <7. Lighting equipment and display devices>
[0280] The light emitting device according to the present embodiment described above can be used, for example, in a lighting fixture or a display device. Therefore, one aspect of the present invention relates to a lighting fixture or a display device including the light emitting device according to the present embodiment.
[0281] Examples of the lighting fixture include general lighting devices such as indoor lamps and outdoor lamps, and lighting for switch parts of electronic devices such as mobile phones and OA equipment.
[0282] The lighting fixture according to the present embodiment includes the light emitting device according to the present embodiment. Therefore, even if the same light emitting element is used, the emitted light beam becomes larger than before, and the surrounding environment can be brighter.
[0283] Examples of the display device include mobile phones, mobile information terminals, electronic dictionaries, digital cameras, computers, televisions, and peripheral devices thereof.
[0284] The display device according to this embodiment includes the light emitting device according to this embodiment. Therefore, even if the same light emitting element is used, the emitted light beam becomes larger than before, and for example, a clearer and higher-brightness display can be performed.
[0285] Example
[0286] Hereinafter, the present invention will be described in further detail by way of examples and comparative examples. In addition, the examples described below are merely examples of the present invention and do not limit the present invention.
[0287] [Example 1]
[0288] (1. Preparation of dispersion)
[0289] (i) Hydrolysis process
[0290] 90.78 parts by mass of methyltrimethoxysilane (product name KBM-13, manufactured by Shin-Etsu Chemical Co., Ltd.), 9.21 parts by mass of water, and 0.01 parts by mass of hydrochloric acid (1N) were prepared. These were added to a container and mixed to obtain a hydrolyzed solution. Next, the hydrolyzed solution was stirred at 60° C. for 30 minutes to hydrolyze the methyltrimethoxysilane to obtain a hydrolyzed solution.
[0291] (ii) Mixing process (process B)
[0292] 30 parts by mass of zirconium oxide (ZrO2) particles (manufactured by Sumitomo Osaka Cement Co., Ltd.) having an average primary particle size of 12 nm and 70 parts by mass of the above hydrolyzed solution were mixed to obtain a mixed solution. The content of zirconium oxide particles in the mixed solution was 30% by mass, the content of methyltrimethoxysilane was 63.5% by mass, and the total content of zirconium oxide particles and methyltrimethoxysilane was 93.5% by mass.
[0293] (iii) Dispersion process (process C)
[0294] After the mixed liquid was dispersed using a bead mill for 6 hours, the beads were removed to obtain a first dispersion liquid.
[0295] The solid content of the first dispersion liquid (the residual content after heating at 100° C. for 1 hour) was measured and found to be 70% by mass.
[0296] (iv) First Addition Step (Step D)
[0297] The obtained first dispersion was heated at 60° C. for 2 hours. Next, toluene was added to the dispersion so that the solid content was 40% by mass, and the dispersion was heated at 60° C. for 2 hours.
[0298] Next, toluene was added to the dispersion liquid so that the solid content became 30% by mass, and the dispersion liquid was heated at 60° C. for 1 hour.
[0299] Next, toluene was added to the dispersion liquid so that the solid content became 20 mass %, and the dispersion liquid was heated at 60° C. for 1 hour to obtain a second dispersion liquid.
[0300] (v) Second Addition Step (Step E)
[0301] After mixing 88.1 parts by mass of the second dispersion whose solid content was adjusted to 20% by mass with toluene and 11.9 parts by mass of a methoxy-containing phenyl silicone resin (trade name: KR217, manufactured by Shin-Etsu Chemical Co., Ltd.) to obtain a treatment liquid, the treatment liquid was heated at 110° C. for 1 hour to obtain the dispersion liquid (third dispersion liquid) involved in Example 1.
[0302] (2. Evaluation of dispersion)
[0303] (i) Particle size distribution
[0304] A portion of the obtained dispersion involved in Example 1 was extracted, and the D10, D50 and D90 of the zirconium oxide particles in the dispersion adjusted to 5% by mass of solid content with toluene were measured using a particle size distribution meter (model: SZ-100SP, manufactured by HORIBA, Ltd.). As a result, D10 was 104nm, D50 was 122nm, and D90 was 143nm. In addition, it is believed that the particles contained in the dispersion are basically only zirconium oxide particles with surface modification materials (methyltrimethoxysilane, methoxy-containing phenyl silicone resin) attached. Therefore, it is believed that the measured D10, D50, and D90 are D10, D50, and D90 of surface-modified zirconium oxide particles.
[0305] (ii)FT-IR analysis
[0306] 10 g of the dispersion of Example 1 adjusted to 30% by mass of solid content with toluene was dried at 100° C. and 20 hPa for 2 hours using a vacuum dryer (EYELA TOKYO RIKAKIKAI CO, LTD., device name: VACUUM OVENVOS-201SD). Next, 0.01 g to 0.05 g of the obtained metal oxide particles were used to measure the 800 cm-1 dispersion using a Fourier transform infrared spectrophotometer (model: FT / IR-670Plus, manufactured by JASCO Corporation). -1 Above and 3800cm -1 The transmission spectrum of the following wave number range was obtained. The spectrum values were normalized so that the maximum value of the spectrum in the measurement range was 100 and the minimum value was 0. Based on this, the 3500cm -1 The value (IA) and 1100cm -1 The results are shown in Table 1.
[0307] (3. Preparation of Composition)
[0308] 5.0 g of the dispersion of Example 1 adjusted to 30% by mass of solid content with toluene and 3.5 g of methylphenyl silicone (trade name: KER-2500-B, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed so that the total mass of zirconium oxide and the surface modification material and the mass ratio of methylphenyl silicone were 30:70.
[0309] Next, toluene was removed from the mixed liquid by an evaporator, thereby obtaining a composition according to Example 1.
[0310] The appearance of the obtained composition of Example 1 was observed with the naked eye. As a result, the composition was transparent. As a result, it was confirmed that the aggregation of zirconium oxide particles was suppressed in the composition and the zirconium oxide particles were relatively uniformly dispersed.
[0311] (Evaluation of Stability of Composition)
[0312] The viscosity of the composition according to Example 1 was measured using a rheometer (trade name: RheoStress RS-6000, manufactured by HAAKE) at 25° C. and a shear rate of 1 (1 / s).
[0313] As a result, the viscosity was 6.5 Pa·s.
[0314] The composition was stored at room temperature (25°C) and the viscosity was measured after one month. The result showed that the viscosity of the composition was 85.4 Pa·s. Although the viscosity was increased, it was at a level that could withstand practical use. This also confirmed that the zirconium oxide particles were dispersed stably in the composition for a long period of time.
[0315] (4. Fabrication of LED Package and Evaluation of Brightness)
[0316] In 1 mass part of the composition involved in Example 1, 14 mass parts of methylphenyl silicone resin (trade name: KER-2500-A / B, manufactured by Shin-Etsu Chemical Co., Ltd.) are added, and the composition is adjusted to contain 2 mass% of surface-modified zirconium oxide particles, and mixed. A composition (total amount of surface-modified zirconium oxide particles and resin: phosphor particles = 100:38) mixed with 1 mass part of the composition is filled into the LED lead frame with a thickness of 300 μm. Then, it is kept at room temperature for 3 hours. Next, the composition is slowly heated and cured to form a sealing component to make a white LED package.
[0317] The brightness of the obtained white LED package was measured by applying a voltage of 3 V and a current of 150 mA to the LED package using a full beam measurement system (manufactured by Otsuka Electronics Co., Ltd.) to measure the light. As a result, the brightness of the white LED package was 74.2 lm.
[0318] [Example 2]
[0319] (1. Preparation of dispersion)
[0320] A dispersion liquid (third dispersion liquid) according to Example 2 was obtained in the same manner as in Example 1, except that zirconium oxide particles having an average primary particle size of 90 nm (manufactured by Sumitomo Osaka Cement Co., Ltd.) were used instead of zirconium oxide particles having an average primary particle size of 12 nm. The content of zirconium oxide particles in the mixed solution obtained in the mixing step was 30% by mass, the content of methyltrimethoxysilane was 63.5% by mass, and the total content of zirconium oxide particles and methyltrimethoxysilane was 93.5% by mass.
[0321] The solid content of the first dispersion (the residual content after heating at 100° C. for 1 hour) was measured and found to be 70% by mass.
[0322] (Particle Size Distribution of the First Dispersion Liquid)
[0323] (i) Particle size distribution
[0324] The particle size distribution of the zirconium oxide particles in the dispersion of Example 2 was evaluated by adjusting the solid content to 5% by mass with toluene in the same manner as in Example 1. As a result, D10 was 118 nm, D50 was 151 nm, and D90 was 298 nm.
[0325] (ii)FT-IR analysis
[0326] Furthermore, the dispersion liquid according to Example 2 was subjected to FT-IR analysis in the same manner as in Example 1. As a result, IA was 48.4, IB was 24.8, and IA / IB was 2.0.
[0327] (3. Preparation of Composition)
[0328] The dispersion of Example 2 adjusted to 30% by mass of solid content with toluene was mixed with methylphenyl silicone in the same manner as in Example 1, and the toluene was removed to obtain a composition of Example 2. The appearance of the obtained composition was visually observed to be a transparent composition.
[0329] (Evaluation of Stability of Composition)
[0330] The viscosity of the composition was measured in the same manner as in Example 1. As a result, the viscosity immediately after the preparation was 5.5 Pa·s.
[0331] The composition was stored at room temperature (25°C) and the viscosity was measured after one month. The viscosity of the composition was 69.7 Pa·s, which was thick but at a level that could be tolerated in practical use.
[0332] A white LED package was produced in the same manner as in Example 1, except that the composition according to Example 2 was used instead of the composition according to Example 1. As a result, the luminance of the white LED package was 73.9 lm.
[0333] [Comparative Example 1]
[0334] (1. Preparation of dispersion)
[0335] The mixing step (step B) and the dispersing step (step C) were performed in the same manner as in Example 1, except that 20 parts by mass of the hydrolyzed liquid and 50 parts by mass of isopropyl alcohol (IPA) were used in the mixing step (step B) instead of using 70 parts by mass of the hydrolyzed liquid for mixing, to obtain a dispersion (first dispersion).
[0336] The solid content of the dispersion was measured (at 100° C. for 1 hour) and found to be 38% by mass.
[0337] (iv) First Addition Step
[0338] Toluene was added to the obtained dispersion (first dispersion) so that the solid content was 20% by mass, and the mixture was heated at 60°C for 2 hours. Next, toluene was added to the dispersion in an amount equal to the amount volatilized, and the mixture was heated at 60°C for 2 hours. Next, toluene was added to the dispersion in an amount equal to the amount volatilized, and the mixture was heated at 60°C for 1 hour. Next, toluene was added to the dispersion in an amount equal to the amount volatilized, and the mixture was heated at 60°C for 1 hour. In this way, surface modification was promoted by heating for 6 hours, and a dispersion in which isopropyl alcohol was replaced by toluene was obtained (second dispersion).
[0339] (v) Second Addition Step
[0340] A treatment liquid was obtained by mixing 88.1 parts by mass of the second dispersion liquid having a solid content adjusted to 20% by mass and 11.9 parts by mass of a methoxy-containing phenyl silicone resin (trade name: KR217, manufactured by Shin-Etsu Chemical Co., Ltd.). The treatment liquid was heated at 110° C. for 1 hour to obtain a dispersion liquid (third dispersion liquid) involved in Comparative Example 1.
[0341] The particle size distribution of the zirconium oxide particles in the dispersion of Comparative Example 1 was evaluated using a dispersion adjusted to 5% by mass of solid content with toluene in the same manner as in Example 1. As a result, D10 was 91 nm, D50 was 112 nm, and D90 was 136 nm.
[0342] Furthermore, the dispersion liquid according to Comparative Example 1 whose solid content was adjusted to 30% by mass with toluene was subjected to FT-IR analysis in the same manner as in Example 1. As a result, IA was 42.1, IB was 10.0, and IA / IB was 4.2.
[0343] In the same manner as in Example 1, the dispersion liquid of Comparative Example 1 adjusted to 30% by mass of solid content with toluene was mixed with methylphenyl silicone, and the toluene was removed to obtain a composition of Comparative Example 1. As a result, the composition of Comparative Example 1 became turbid, and a composition capable of sealing an LED could not be obtained.
[0344] Table 1 summarizes the conditions for producing the dispersions, the dispersions, and the evaluations of the compositions in Example 1, Example 2, and Comparative Example 1.
[0345] [Table 1]
[0346]
[0347] [Reference example]
[0348] A white LED package not containing surface-modified zirconium oxide particles was prepared, and the brightness was measured. That is, in the preparation of the LED package of Example 1, the total amount of resin: phosphor particles = 100:38 was replaced with the total amount of surface-modified zirconium oxide particles and resin: phosphor particles = 100:38, and the white LED package of the reference example was prepared in the same manner as in Example 1.
[0349] The obtained white package was measured in the same manner as in Example 1. As a result, the luminance of the white LED package was 72.5 lm.
[0350] As shown above, in the dispersions of Examples 1 and 2 in which zirconium oxide particles were dispersed in a high concentration of a silane compound, the zirconium oxide particles were properly dispersed even when methylphenyl silicone was mixed with the dispersion, and no turbidity or excessive increase in viscosity was observed. In addition, it was confirmed that the brightness of the white LED package could be improved.
[0351] On the other hand, in the dispersion of Comparative Example 1, when methylphenyl silicone was mixed with the dispersion, the obtained composition gelled and was not suitable as a composition for sealing a light-emitting element.
[0352] The preferred embodiments of the present invention are described in detail with reference to the accompanying drawings, but the present invention is not limited to these examples. It should be understood by those skilled in the art that various variations or modifications can be thought of within the scope of the technical ideas described in the claims, and these also belong to the technical scope of the present invention.
[0353] Industrial Applicability
[0354] Provided are a dispersion containing metal oxide particles, wherein when the metal oxide particles are dispersed in a methyl silicone resin, aggregation of the metal oxide particles is suppressed; a composition containing the dispersion; a sealing component formed using the composition; a light-emitting device having the sealing component; a lighting fixture and a display device having the light-emitting device; and a method for producing the dispersion.
[0355] Description of symbols
[0356] 1A, 1B, 1C, 1D - Light emitting device
[0357] 2-Substrate
[0358] 2a-upper part of substrate
[0359] 2b-lower part of base plate
[0360] 21-Concave
[0361] 21a-Bottom of recess
[0362] 3-Light-emitting element
[0363] 4A, 4B, 4C, 4D - Sealing parts
[0364] 41B, 41C, 41D - 1st floor
[0365] 43B, 43C, 43D - 2nd floor
[0366] 45D - 3rd floor
[0367] 5-Phosphor particles
Claims
1. A dispersion comprising metal oxide particles surface-modified with a surface modification material and a hydrophobic solvent, The surface modification material contains a silane compound and a silicone compound, The metal oxide particles obtained by drying the dispersion liquid by vacuum drying were measured at 800 cm using a Fourier transform infrared spectrophotometer. -1 Above and 3800cm -1 The transmission spectrum in the following wave number range satisfies the following formula (1) when the spectrum value is normalized so that the maximum value of the spectrum in the above range is 100 and the minimum value is 0: IA / IB≤3.5 (1) Where, “IA” means 3500cm -1 Spectral values below, "IB" means 1100cm -1 The spectral value of The dispersion and methylphenyl silicone were mixed to prepare a mixture in such a manner that the mass ratio of the total mass of the metal oxide particles and the surface modification material to the mass of methylphenyl silicone was 30:70, and the viscosity after removing the hydrophobic solvent was 9 Pa·s or less.
2. The dispersion according to claim 1, wherein The IA / IB is 2.0 or less.
3. The dispersion according to claim 1, wherein The metal oxide particles contain at least one of zirconium oxide particles and titanium oxide particles. The content of the metal oxide particles in the dispersion is 1 mass % or more and 70 mass % or less.
4. The dispersion according to claim 1, wherein The metal oxide particles have an average primary particle size of 3 nm or more and 200 nm or less.
5. The dispersion according to claim 1, wherein The metal oxide particles have an average dispersed particle size of 10 nm or more and 300 nm or less.
6. The dispersion according to claim 1, wherein The hydrophobic solvent is at least one selected from the group consisting of benzene, toluene, ethylbenzene, 1-phenylpropane, isopropylbenzene, n-butylbenzene, tert-butylbenzene, sec-butylbenzene, o-xylene, m-xylene, p-xylene, 2-ethyltoluene, 3-ethyltoluene or 4-ethyltoluene, The content of the hydrophobic solvent is 40% by mass or more and 95% by mass or less relative to the amount of the dispersion liquid.
7. The dispersion according to claim 1, wherein The silane compound is a silane compound having an alkyl group having 1 to 5 carbon atoms and 1 to 3 carbon atoms and an alkoxy group having 1 to 5 carbon atoms and 1 to 3 carbon atoms. The content of the silane compound is 50% by mass or more and 500% by mass or less relative to the amount of the metal oxide particles.
8. The dispersion according to claim 1, wherein The silicone compound contains at least one selected from the group consisting of methoxy-containing phenyl silicone, dimethyl silicone, and methoxy-containing dimethyl silicone, The content of the silicone compound is 50% by mass or more and 500% by mass or less relative to the amount of the metal oxide particles.
9. The dispersion according to claim 1, wherein The viscosity when the hydrophobic solvent is removed is 1 Pa·s or more.
10. A composition which is a mixture of the dispersion according to claim 1 and a resin component. 11 . A sealing member, which is a cured product of the composition according to claim 10 . 12 . A light-emitting device comprising the sealing member according to claim 11 and a light-emitting element sealed by the sealing member.
13. A lighting fixture comprising the light emitting device according to claim 12.
14. A display device comprising the light emitting device according to claim 12.
15. A method for producing the dispersion according to claim 1, comprising: Step B, mixing a silane compound and metal oxide particles to obtain a mixed solution; Step C, dispersing the metal oxide particles in the mixed solution to obtain a first dispersion solution in which the metal oxide particles are dispersed; Step D, adding a hydrophobic solvent to the first dispersion to obtain a second dispersion; and Step E, adding a silicone compound to the second dispersion to obtain a third dispersion, The content of the metal oxide particles in the mixed solution of the step B is 10 mass % or more and 49 mass % or less, The total content of the silane compound and the metal oxide particles in the mixed solution of the step B is 65 mass % or more and 98 mass % or less, The step D of adding the hydrophobic solvent is selected from any one of the following steps: Step d1, heating the first dispersion, and after heating, adding the hydrophobic solvent at a speed at which the metal oxide particles do not aggregate; Step d2, while heating the first dispersion, adding the hydrophobic solvent at a speed at which the metal oxide particles do not aggregate; and In step d3, after adding the hydrophobic solvent at a rate at which the metal oxide particles do not aggregate, the first dispersion is heated.
16. The method for producing a dispersion according to claim 15, wherein: In the step B, a dispersion medium is further mixed. The amount of the dispersion medium in the mixed liquid is 2 mass % or more and 35 mass % or less.
17. The method for producing a dispersion according to claim 15, wherein: In the step B, the amount of the inevitable alcohol compound generated by hydrolysis is 2% by mass or more and 35% by mass or less.
18. The method for producing a dispersion according to claim 15, comprising: Step A, before step B, mixing a silane compound and water to prepare a hydrolyzed solution containing the hydrolyzed silane compound, In the step B, the hydrolysis solution containing the silane compound and the metal oxide particles are mixed.
19. The method for producing a dispersion according to claim 18, wherein: The hydrolysis solution further contains at least one of a catalyst and a hydrophilic solvent.
20. The method for producing a dispersion according to claim 15, wherein: The metal oxide particles contain at least one of zirconium oxide particles and titanium oxide particles. The content of the metal oxide particles in the third dispersion is 1 mass % or more and 70 mass % or less, The average primary particle size of the metal oxide particles is 3 nm or more and 200 nm or less, The average dispersed particle size of the metal oxide particles in the third dispersion is 10 nm or more and 300 nm or less, The hydrophobic solvent is at least one selected from the group consisting of benzene, toluene, ethylbenzene, 1-phenylpropane, isopropylbenzene, n-butylbenzene, tert-butylbenzene, sec-butylbenzene, o-xylene, m-xylene, p-xylene, 2-ethyltoluene, 3-ethyltoluene or 4-ethyltoluene, The content of the hydrophobic solvent is 40% by mass or more and 95% by mass or less relative to the amount of the third dispersion liquid.
21. The method for producing a dispersion according to claim 15, wherein: The silane compound is a silane compound having an alkyl group having 1 to 5 carbon atoms and 1 to 3 carbon atoms and an alkoxy group having 1 to 5 carbon atoms and 1 to 3 carbon atoms. The content of the silane compound is 50% by mass or more and 500% by mass or less relative to the amount of the metal oxide particles, The silicone compound contains at least one selected from the group consisting of methoxy-containing phenyl silicone, dimethyl silicone, and methoxy-containing dimethyl silicone, The content of the silicone compound is 50% by mass or more and 500% by mass or less relative to the amount of the metal oxide particles.
Citation Information
Patent Citations
Composition for forming light scattering composite body, light scattering composite body and method for producing same
WO2016142992A1
Silicone-coated metal oxide ultrafine particle
JP2009149454A
Inorganic oxide particle dispersion liquid, resin composition, master batch, resin composite, and optical semiconductor light-emitting device
JP2016175804A