A self-adhesive hydrogel and its preparation method and application

By preparing self-adhesive hydrogels with low initial viscosity and high consolidation strength, the problem of poor effectiveness of existing binders in coal dust suppression is solved, and efficient coal dust consolidation and safe production are achieved.

CN115651221BActive Publication Date: 2024-10-29TIANJIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211406478.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-10
Publication Date
2024-10-29
Estimated Expiration
2042-11-10

AI Technical Summary

Technical Problem

The existing binders have high initial viscosity and low consolidation strength, resulting in poor atomization effect and inability to effectively suppress coal dust and ensure safe production and worker health in the coal mining industry.

Method used

A method for preparing self-adhesive hydrogel is adopted, by reacting dopa or its derivatives with polyacrylic acid or polyacrylamide in a hydrochloric acid solution to form a cross-linked product, and adding reduced glutathione to adjust the pH value , forming self-adhesive hydrogels with low initial viscosity and high consolidation strength.

Benefits of technology

The dust suppression rate is greater than 95% when the wind speed is lower than 10m/s, and it can be sprayed into mist under a pressure of 0.2 to 0.3Mpa, which significantly improves the consolidation effect of coal dust and ensures safe production and worker health in coal mines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115651221B_ABST
    Figure CN115651221B_ABST
Patent Text Reader

Abstract

The present invention discloses a self-adhesive hydrogel and its preparation method and application. The preparation method comprises preparing a main chain solution, preparing a side chain solution and mixing the main chain solution with the side chain solution to form the self-adhesive hydrogel; the preparation of the side chain solution comprises mixing solute A with a hydrochloric acid solution to form a dissolving solution, adjusting the pH of the dissolving solution, reacting solute A with its oxidation product to form a cross-linked product, adding a reducing agent to form a side chain solution, the solute A is DOPA, droxidopa or carbidopa, and the main chain solution is a polyacrylic acid solution or a polyacrylamide solution. The polyacrylic acid and polyacrylamide in the self-adhesive hydrogel of the present invention have high viscosity. The presence of the catechol group on the surface of DOPA can lead to a decrease in the activity of polyacrylic acid free radicals, thereby significantly reducing the relative molecular mass of polyacrylic acid, so that the dust binder has low initial viscosity and easy atomization characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dust adsorption, and in particular to a self-adhesive hydrogel and a preparation method and application thereof. Background Art

[0002] As a non-renewable natural resource, coal mines are an important material basis for the development of social production. However, due to the widespread application of mechanized coal mining technology, the amount of coal dust generated underground has continued to increase. Working in a high-dust environment for a long time, the coal dust level exceeds the allowable value, which may cause underground miners to suffer from serious lung diseases. In addition, when the coal dust suspended in the air reaches a certain concentration and encounters a high-temperature heat source, an underground coal dust explosion is likely to occur. Therefore, effective coal dust suppression technology is urgently needed to reduce the coal dust concentration to ensure safe production in the coal mining industry and protect the life and health of coal miners.

[0003] Most of the research on binders involves high-viscosity polymers, such as chitosan, agarose, guar gum, etc. Due to the strong intermolecular hydrogen bonding between polar functional groups such as -OH, -NH2, -COOH on these polymers and coal dust particles, and due to the steric hindrance effect of macromolecular chain polymers, the initial viscosity of the solution is high, resulting in poor atomization effect in industrial applications. Therefore, a binder with low initial viscosity and high consolidation strength is the key to the invention. Summary of the invention

[0004] The purpose of the present invention is to provide a self-adhesive hydrogel in view of the high initial viscosity, low consolidation strength and poor atomization effect of the binder solution in the prior art.

[0005] Another object of the present invention is to provide a method for preparing the self-adhesive hydrogel.

[0006] Another aspect of the present invention provides a use of the self-adhesive hydrogel.

[0007] The technical solution adopted to achieve the purpose of the present invention is:

[0008] A method for preparing a self-adhesive hydrogel comprises the following steps:

[0009] (1) preparing a backbone solution;

[0010] (2) preparing a side chain solution;

[0011] (3) mixing the main chain solution prepared in step (1) and the side chain solution prepared in step (2) to form a self-adhesive hydrogel;

[0012] The method for preparing the side chain solution in step (2) is to mix solute A with a hydrochloric acid solution to form a dissolving solution, wherein part of the solute in the dissolving solution forms an oxidation product, and then the solute A reacts and polymerizes with the oxidation product to form a cross-linked product, and then a reducing agent is added to form a side chain solution;

[0013] The solute A is dopa, droxidopa or carbidopa; the main chain solution is a polyacrylic acid solution or a polyacrylamide solution.

[0014] In the above technical solution, the concentration of the hydrochloric acid solution is 1% to 2%, the mass ratio of the solute A to the hydrochloric acid solution is 1:12 to 17, the molar ratio of the reducing agent to the solute A is 1:1, and the reducing agent is reduced glutathione or ascorbic acid, preferably reduced glutathione.

[0015] In the above technical scheme, after solute A and hydrochloric acid solution are mixed to form a dissolving solution in step (2), the pH of the dissolving solution is adjusted; the method for adjusting the pH of the dissolving solution is to stir the dissolving solution and dropwise add a 30% concentration alkaline solution until the pH of the dissolving solution is 4.2 to 4.5; the alkaline solution is a NaOH solution or a KOH solution.

[0016] In the above technical solution, the step (1) is specifically as follows: dissolving solute B in water at a concentration of 5% to 15%, adding an initiator, and dialyzing for 24 to 48 hours after the reaction is complete to obtain a main chain solution.

[0017] In the above technical solution, in step (1), the solute B is acrylic acid or acrylamide, the mass concentration of the solute B is 5% to 15%, and the initiator is a persulfate, preferably ammonium persulfate or potassium persulfate.

[0018] In the above technical solution, the step (3) is specifically: mixing the side chain solution and the main chain solution in a mass ratio of 1:1 to 5, stirring for 1 to 2 hours, and then adjusting the pH to obtain the self-adhesive hydrogel.

[0019] In the above technical solution, the pH is adjusted in step (3) by the following steps: NaOH solution is added dropwise to adjust the pH to 7.2-7.5.

[0020] Another aspect of the present invention provides a self-adhesive hydrogel prepared by the preparation method, wherein the density of the self-adhesive hydrogel is 0.965-0.975 g / ml; and the viscosity of the self-adhesive hydrogel is 2-2.2 Pa·s.

[0021] Another aspect of the present invention provides a use of the self-adhesive hydrogel in dust adsorption, characterized in that when the wind speed is lower than 10 m / s, the dust suppression rate is greater than 95%.

[0022] In the above technical solution, the self-adhesive hydrogel can be sprayed into mist for use at a pressure of 0.2-0.3 MPa.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The polyacrylic acid and polyacrylamide in the self-adhesive hydrogel of the present invention have high viscosity. The presence of catechol groups on the surface of DOPA can reduce the free radical activity of polyacrylic acid, thereby significantly reducing the relative molecular weight of polyacrylic acid, so that the dust binder has low initial viscosity and easy atomization characteristics.

[0025] 2. The N-(NL-γ-glutamyl-L-cysteinyl)glycine (reduced glutathione) in the self-adhesive hydrogel of the present invention is a strong reducing antioxidant. In the catechol redox system, the reducing effect of glutathione and the oxidizing effect of air can reach a dynamic balance. In addition, the catechol group will generate a large number of free radicals during the oxidation process, which will trigger the self-gelation of the hydrogel, thereby giving the hydrogel long-term self-adhesion ability and good mechanical properties.

[0026] 3. The -COOH groups on the surface of polyacrylic acid and the -OH, -COOH, -NH2 groups on the surface of DOPA and the -COOH, -SH, carbonyl groups on the surface of glutathione in the self-adhesive hydrogel of the present invention can be cross-linked through strong hydrogen bonds to form an interpenetrating network structure, giving it high toughness. Moreover, when the water evaporates, the contact between polyacrylic acid and DOPA-glutathione becomes closer, thereby consolidating the coal dust. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Shown is a schematic diagram of the reaction process of the present invention.

[0028] Figure 2 Shown is a physical picture of the self-adhesive hydrogel of the present invention after freeze drying.

[0029] Figure 3 Shown is the gelation diagram of the self-adhesive hydrogel of the present invention.

[0030] Figure 4 Shown is the infrared spectrum of the self-adhesive hydrogel of Examples 1-2 of the present invention.

[0031] Figure 5 The figure shows a coal pile after the self-adhesive hydrogel of the present invention is sprayed on the surface of the coal dust and air-dried. (a) in the figure is a coal dust pile without the addition of the self-adhesive hydrogel; (b) is a coal dust pile after the self-adhesive hydrogel is added and solidified, and a layer of gel shell formed by the self-adhesive hydrogel on the surface of the coal dust.

[0032] Figure 6Shown are SEM morphology images of the gel shell formed on the surface of coal dust by the self-adhesive hydrogel of the present invention, wherein (a) is the microscopic morphology of coal dust without the addition of self-adhesive hydrogel; (b) is the microscopic morphology of the gel shell formed on the surface of coal with the addition of self-adhesive hydrogel. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0034] Example 1

[0035] A self-adhesive hydrogel, such as Figure 1 As shown, it is prepared by the following steps:

[0036] Step 1, dissolving acrylic acid in a certain amount of ultrapure water at a concentration of 12%; adding initiator ammonium persulfate in an amount of 13% of the mass of the acrylic acid to control the low initial viscosity of the solution. After the reaction is complete, dialyzing in ultrapure water for 24 hours (changing the dialysate every 6 hours) to remove unreacted residues to prevent affecting the next step reaction, and obtaining a polyacrylic acid solution.

[0037] Step 2, in a certain amount of ultrapure water, prepare a hydrochloric acid solution with a concentration of 2%. DOPA and hydrochloric acid solution are mixed in a mass ratio of 1:15 to form a dissolving solution. NaOH solution is added dropwise to the dissolving solution until the pH of the dissolving solution is 4.2, at which time DOPA in the dissolving solution is partially oxidized, and DOPA and the oxidation product dopaquinone are cross-linked to form a cross-linked product to obtain a dissolving solution. A certain amount of ultrapure water is added to completely dissolve the reduced glutathione in the dissolving solution, and the molar ratio of DOPA to reduced glutathione is 1:1. At this time, the reducing effect of the reduced glutathione and the oxidizing effect of the air reach a dynamic equilibrium to obtain a side chain solution.

[0038] Step 3, mixing the side chain solution and the polyacrylic acid solution in a mass ratio of 1:4, stirring with a magnetic stirrer for 1 hour to mix evenly, and then dropping a NaOH solution to adjust the pH to 7.2 to obtain the self-adhesive hydrogel.

[0039] The self-adhesive hydrogel was freeze-dried to obtain Figure 2 The product shown can form a cross-linked network structure during the preparation process of the self-adhesive hydrogel, giving the self-adhesive hydrogel good toughness and water absorption.

[0040] Example 2

[0041] A self-adhesive hydrogel, such as Figure 1 As shown, it is prepared by the following steps:

[0042] Step 1, dissolving acrylic acid in a certain amount of ultrapure water at a concentration of 12%; adding initiator ammonium persulfate in an amount of 13% of the mass of the acrylic acid to control the low initial viscosity of the solution. After the reaction is complete, dialyzing in ultrapure water for 24 hours (changing the dialysate every 6 hours) to remove unreacted residues to prevent affecting the next step reaction, and obtaining a polyacrylic acid solution.

[0043] Step 2, in a certain amount of ultrapure water, prepare a hydrochloric acid solution with a concentration of 2%. DOPA and hydrochloric acid solution are mixed in a mass ratio of 1:15 to form a dissolving solution. NaOH solution is added dropwise to the dissolving solution until the pH of the dissolving solution is 4.2, at which time DOPA in the dissolving solution is partially oxidized, and DOPA and the oxidation product dopaquinone are cross-linked to form a cross-linked product to obtain a dissolving solution. A certain amount of ultrapure water is added to completely dissolve the reduced glutathione in the dissolving solution, and the molar ratio of DOPA to reduced glutathione is 1:1. At this time, the reducing effect of the reduced glutathione and the oxidizing effect of the air reach a dynamic equilibrium to obtain a side chain solution.

[0044] Step 3, mixing the side chain solution and the polyacrylic acid solution in a mass ratio of 1:4, stirring with a magnetic stirrer for 1 hour to mix evenly, and then dropping a NaOH solution to adjust the pH to 7.5 to obtain the self-adhesive hydrogel.

[0045] Example 3

[0046] On the basis of Examples 1-2, in order to further verify the property that the adhesive increases in viscosity after dehydration, as Figure 3 As shown, when the solid content of the binder is increased to 30% and the moisture content is reduced, the dopa-glutathione and polyacrylic acid polymer chains in the binder can self-adhere into larger molecules through intermolecular hydrogen bonding, the viscosity is improved, and a flexible self-adhesive hydrogel is formed.

[0047] In order to verify whether the self-adhesive hydrogel was successfully prepared, the self-adhesive hydrogel of Example 1-2 was characterized by infrared spectroscopy. Figure 4 The functional group peaks of the hydrogel binders at the two pH values ​​are at the same position, at 750 cm -1 、1450cm -1 and 3391cm -1 The stretching vibration peaks of disubstituted phthalate, aromatic ring C=C and -NH2 appeared at 1722cm -1 The stretching vibration peak of the C=O bond appears and moves to a lower wave number, which is affected by the hydrogen bond between the carboxyl groups of L-DOPA and polyacrylic acid. -1 and 3509cm -1The strong absorption peak at is the multi-molecular association peak of hydroxyl groups. This absorption peak is formed when two OH bonds form intermolecular hydrogen bonds, which proves the existence of strong hydrogen bonding between L-DOPA and polyacrylic acid.

[0048] Example 4

[0049] On the basis of Example 1, in order to simulate the coal dust environment of an actual coal yard, the coal was crushed into small particles by a crusher and piled into a cone shape, such as Figure 5 As shown in (a), the hydrogel binder with a viscosity of 2 Pa·s prepared in Example 1 is sprayed uniformly on the surface of the coal pile in a mist form under a pressure of 0.2 MPa. After air-drying for 24 hours, the adhesion state of the coal surface is observed. Figure 5 (b) As shown. By comparison, it can be seen that the coal particles are completely adhered by the binder, and the surface of the coal dust is bonded into a soft and strong gel shell structure. In addition, the surface of the coal shell layer was continuously blown by a fan at different wind speeds. At a wind speed of 10m / s, no dust loss was observed in the coal pile, proving that the binder has a significant effect in suppressing coal dust.

[0050] The microscopic morphology of the original coal dust and the gel shell on the surface of the coal after adding the binder were photographed by scanning electron microscope. Figure 6 As shown in the figure, it can be seen that the distance between the original coal dust particles is relatively dispersed, while the coal surface after adding the binder is covered by the binder, and the coal particles are tightly adhered and agglomerated together, which further proves that the binder can effectively consolidate the coal dust.

[0051] The above is only a preferred embodiment of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a self-adhesive hydrogel, characterized in that: The following steps are involved: (1) Prepare the backbone solution; (2) preparing a side chain solution; (3) mixing the main chain solution prepared in step (1) and the side chain solution prepared in step (2) to form a self-adhesive hydrogel; The method for preparing the side chain solution in step (2) is to mix solute A with hydrochloric acid solution to form a dissolving solution, wherein part of the solute in the dissolving solution forms an oxidation product, and then the solute A reacts and polymerizes with the oxidation product to form a cross-linked product, and then a reducing agent is added to form a side chain solution; The solute A is DOPA, droxidopa or carbidopa; the main chain solution is a polyacrylic acid solution, the molar ratio of the reducing agent to the solute A is 1:1, and the reducing agent is reduced glutathione.

2. The preparation method according to claim 1, characterized in that The concentration of the hydrochloric acid solution is 1%-2%, and the mass ratio of the solute A to the hydrochloric acid solution is 1:12-17.

3. The preparation method according to claim 1, characterized in that: After solute A and hydrochloric acid solution are mixed to form a solution in step (2), the pH of the solution is adjusted; the pH of the solution is adjusted by stirring the solution and adding a 30% alkaline solution dropwise until the pH of the solution is 4.2-4.5; the alkaline solution is a NaOH solution or a KOH solution.

4. The preparation method according to claim 1, characterized in that: The step (1) specifically comprises: dissolving solute B in water at a concentration of 5% to 15%, adding an initiator, and dialyzing for 24 to 48 hours after the reaction is complete to obtain a main chain solution.

5. The preparation method according to claim 4, characterized in that: In the step (1), the solute B is acrylic acid, the mass concentration of the solute B is 5% to 15%, and the initiator is persulfate.

6. The preparation method according to claim 5, characterized in that: The initiator is ammonium persulfate or potassium persulfate.

7. The preparation method according to claim 1, characterized in that: The step (3) is specifically as follows: mixing the side chain solution and the main chain solution in a mass ratio of 1:1-5, stirring for 1-2 hours, and then adjusting the pH to obtain the self-adhesive hydrogel.

8. The preparation method according to claim 7, characterized in that: The pH in step (3) is adjusted by the following steps: NaOH solution is added dropwise to adjust the pH to 7.2-7.

5.

9. A self-adhesive hydrogel prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The density of the self-adhesive hydrogel is 0.965-0.975 g / ml; the viscosity of the self-adhesive hydrogel is 2-2.2 pa·s.

10. An application of the self-adhesive hydrogel according to claim 9 in dust adsorption, characterized in that: When the wind speed is lower than 10m / s, the dust suppression rate is greater than 95%.

11. The use according to claim 10, characterized in that The self-adhesive hydrogel can be sprayed into mist for use at a pressure of 0.2-0.3 MPa.