A self-produced electro-enzyme cascade microneedle patch and its preparation method and application

By using materials such as polydopamine-modified polypyrrole and hyaluronic acid combined with enzyme-linked reactions, the problem of existing conductive microneedle patches requiring an external power source and poor dispersion of conductive polymers has been solved, and self-produced electroenzymes without external power sources have been achieved. The cascaded microneedle patch has good biocompatibility and application prospects and is used for diabetic wound and nerve repair.

CN115337255BActive Publication Date: 2024-10-22LANZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211057304.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-30
Publication Date
2024-10-22
Estimated Expiration
2042-08-30

AI Technical Summary

Technical Problem

Existing conductive microneedle patches require an external power supply, are complicated to prepare, and the conductive polymer PPy has poor dispersion in water, making them difficult to make and inconvenient to use.

Method used

Polydopamine-modified polypyrrole, hyaluronic acid and polyvinyl alcohol are used as base materials, combined with glucose oxidase and horseradish peroxidase/catalase, and fixed on the metal-organic framework material ZIF-8 to form a self-produced The electro-enzyme cascade microneedle patch generates physiological current through enzyme cascade reaction.

Benefits of technology

A microneedle patch that does not require an external power supply is realized. It has good biocompatibility, safety, portability, low cost, and high efficiency. It can quickly respond to blood sugar concentration, promote wound healing and nerve repair, and has broad biomedical application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115337255B_ABST
    Figure CN115337255B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of biomedicine, and specifically discloses a self-generated enzyme cascade microneedle patch and a preparation method and application thereof. The microneedle patch is composed of a conductive substrate without a target drug and a microneedle array composed of at least one needle body containing the target drug. The substrate is prepared from polypyrrole modified with polydopamine, hyaluronic acid and polyvinyl alcohol, and the needle body is prepared from polypyrrole modified with polydopamine, hyaluronic acid and polyvinyl alcohol, glucose oxidase, and horseradish peroxidase / catalase. The self-generated enzyme cascade microneedle patch does not require an external power supply, can generate physiological current through an enzyme cascade reaction, and promotes the migration and growth of various cells. The patch has the advantages of safety, effectiveness, portability, low cost, high efficiency, simple operation, etc., has good biocompatibility and no in vivo toxicity, and has broad application prospects in the field of biomedicine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of biomedical materials, and in particular to a self-generated electroenzyme cascade microneedle patch and a preparation method and application thereof. Background Art

[0002] Microneedles are a new type of transdermal drug delivery system. When administering drugs, they can pierce the stratum corneum of the skin, thereby opening a microchannel from the stratum corneum to the epidermis or the superficial dermis for drug delivery. The microneedles are then absorbed by the capillaries, and the active drug molecules circulate in the blood to reach the lesion site of the human body to play a therapeutic role. Microneedle drug delivery has the advantages of being minimally invasive, painless, and convenient. In order to promote the release of drugs in microneedles, people add bioelectric conductive materials to microneedles. The prepared microneedles have good in vitro stability, excellent electrochemical properties and biocompatibility, and have attracted much attention in biomedical sensors, neural prostheses, wound dressings and drug controlled release devices.

[0003] For example, the invention patent CN110201296A discloses a conductive polymer microneedle patch for controlled drug release, wherein the microneedle is a conductive polymer microneedle, which is composed of a polymer solid microneedle, an inert metal layer and a drug-carrying conductive polymer film layer; controlled release of the drug is achieved by electrical stimulation. However, the above-mentioned microneedle needs to provide an external power supply, and the outer layer of the microneedle is provided with an inert metal layer and a drug-carrying conductive polymer film layer, the preparation method is complicated, and the coating is easy to fall off; in the preliminary research of the inventor's research group, a double-layer conductive microneedle patch for treating subcutaneous tumors and its preparation method and application (CN114848577A) were developed, and the conductive polymer material used in the substrate and the microneedle needle tip near the substrate provides an external power supply, which is conducive to electroporation to increase cell membrane permeability and increase the absorption rate of biological agents or drugs; however, the above-mentioned microneedle patch also needs to provide an external power supply, which is inconvenient to use. In addition, the inventors discovered during the research process that the existing conductive microneedle patches have the following problems: the conductive polymer PPy, which is most commonly used to prepare conductive microneedles, has poor dispersibility in water, making the production of conductive microneedles difficult.

[0004] In order to solve the above technical problems, the present invention has prepared an advanced self-generated enzyme cascade microneedle patch system. The self-generated enzyme cascade microneedle patch does not require an external power supply, can generate physiological current through enzyme cascade reaction, promote the migration and growth of various cells, has the advantages of safety, effectiveness, portability, low cost, high efficiency, easy operation, etc., has good biocompatibility and no in vivo toxicity, and has broad application prospects in the biomedical field. Summary of the invention

[0005] In order to achieve the above-mentioned purpose, the primary purpose of the present invention is to provide a self-produced electro-enzyme cascade microneedle patch, wherein the microneedle patch is composed of a conductive substrate without a target drug and a microneedle array composed of at least one needle body containing a target drug, wherein the substrate is prepared from polydopamine-modified polypyrrole (DA-PPy), hyaluronic acid (HA) and polyvinyl alcohol (PVA), and the needle body is prepared from polydopamine-modified polypyrrole (DA-PPy), hyaluronic acid (HA) and polyvinyl alcohol (PVA), glucose oxidase, and horseradish peroxidase / catalase.

[0006] Preferably, the glucose oxidase and horseradish peroxidase / catalase are immobilized on the metal organic framework material ZIF-8.

[0007] Preferably, in the substrate, the mass ratio of dopamine-modified polypyrrole (DA-PPy), hyaluronic acid (HA), and polyvinyl alcohol (PVA) is 0.01-1: 1-100: 0.5-50, and in the needle body, the mass ratio of dopamine-modified polypyrrole (DA-PPy), hyaluronic acid (HA), polyvinyl alcohol (PVA), glucose oxidase, horseradish peroxidase / catalase, and ZIF-8 is 0.01-1: 1-100: 0.5-50: 0.005-0.5: 0.005-0.5: 0.1-10.

[0008] The second object of the present invention is to provide a method for preparing the self-produced electro-enzyme cascade microneedle patch, comprising the following steps:

[0009] (1) under the conditions of a water bath and magnetic stirring, polydopamine-modified polypyrrole, hyaluronic acid, and polyvinyl alcohol are added to deionized water in proportion to obtain a microneedle patch base gel;

[0010] (2) mixing the microneedle patch base gel prepared in step (1) with glucose oxidase to obtain glucose oxidase needle body gel; and mixing with horseradish peroxidase / catalase to obtain horseradish peroxidase / catalase needle body gel;

[0011] (3) Using a pipette, take 5-20ul of the glucose oxidase needle gel prepared in step (2) and drop it onto half of the pinholes of the PDMS microneedle template. Place the template in a vacuum drying oven and perform negative pressure injection molding at -1 to -0.8MPa. Repeat the vacuuming 2 to 3 times for 3 to 5 minutes each time. After natural drying at room temperature, obtain a microneedle template loaded with glucose oxidase.

[0012] (4) Using a pipette, take 5-20ul of the horseradish peroxidase / catalase needle gel prepared in step (2) and drip it onto the other half of the pinholes in the microneedle template in step (3), and place it in a vacuum drying oven under a negative pressure of -1 to -0.8MPa for injection molding: repeatedly evacuate 2 to 3 times, each time for 3 to 5 minutes, and dry naturally at room temperature to obtain the conductive microneedle patch needle body loaded with glucose oxidase-horseradish peroxidase / catalase;

[0013] (5) placing the base gel prepared in step (1) on the microneedle body template obtained in step (4), placing it in a vacuum drying oven again, setting the vacuum to -1 to -0.8 MPa, vacuuming the negative pressure injection mold for 10 to 30 minutes, and naturally drying at room temperature to obtain the self-produced electro-enzyme cascade microneedle patch body;

[0014] (6) Spreading the conductive hydrogel prepared in step (1) onto the microneedle template in step (5) whose needle body is filled with conductive polymer matrix gel, and drying naturally to obtain a self-produced electro-enzyme cascade microneedle patch.

[0015] Preferably, the water bath temperature in step (1) is 0 to 90°C.

[0016] The third object of the present invention is to provide the use of the self-produced electro-enzyme cascade microneedle patch in preparing drugs for treating local diseases.

[0017] The fourth object of the present invention is to provide the use of the self-produced electro-enzyme cascade microneedle patch in the preparation of drugs for treating skin injuries.

[0018] The fifth object of the present invention is to provide the use of the self-produced electro-enzyme cascade microneedle patch in the preparation of drugs for treating nerve damage.

[0019] The beneficial effects of the present invention are as follows: (1) the present invention provides a self-generated enzyme cascade microneedle patch, which can generate physiological current through enzyme cascade reaction without adding external electrical stimulation equipment; (2) the self-generated enzyme cascade microneedle patch, the base material of which is polydopamine-modified (DA) polypyrrole (PPy) added to hyaluronic acid (HA) and polyvinyl alcohol (PVA) gel to prepare a polymer (DPPH) with good conductive properties, half of the needle body is doped with ZG nanoparticles of glucose oxidase fixed by ZIF-8, and the other half is ZH nanoparticles of horseradish peroxidase fixed by ZIF-8, ZIF-8 can protect the activity and stability of the enzyme, and ZIF-8 solves the problem that the free enzyme is easily inactivated and denatured under strong acid, strong alkali and high temperature, thereby affecting its catalytic effect; the reuse rate of the free enzyme is not high, the purification and separation process is relatively complicated, and the use cost is relatively high. (3) After the self-generated enzyme-cascade microneedle patch acts on the human body, it absorbs body fluids and swells to release ZG, which can quickly undergo redox reactions when it encounters substrates. The generated hydrogen peroxide can be reduced to water and oxygen by ZH released from the other half of the needle body. The electrons generated in this process can be transmitted through the DPPH hydrogel to form a complete current pathway, promoting the migration and growth of various cells; (4) The prepared self-generated enzyme-cascade microneedle patch is sensitive to the blood glucose concentration of diabetic wounds, can respond quickly, undergo enzyme cascade reactions, reduce local blood glucose, and output physiological microcurrents, thereby better promoting wound healing; the ZGH-MN microneedle patch group achieved scar-free healing at 21 days, while the other groups still had smaller wounds on the skin surface or obvious scars on the skin surface after healing. (5) The self-produced electro-enzyme-linked microneedle patch has good antibacterial properties; (6) The self-produced electro-enzyme-linked microneedle patch has a good effect on the repair of sciatic nerve; (7) The microneedle patch has the advantages of safety, effectiveness, portability, low cost, high efficiency, and easy operation. It has broad application prospects in the biomedical field such as chronic wounds such as diabetes, nerve repair, myocardial repair, body fluid testing, and diagnosis and detection of various physiological indicators. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Self-produced electro-enzyme cascade microneedle patch

[0021] Figure 2 Differences in dispersibility and solubility of PPy and DA-PPy in water

[0022] Figure 3 SEM images of PPy and DAPPy

[0023] Figure 4 Self-generated electrical performance diagram of the self-generated electroenzyme cascade microneedle patch

[0024] Figure 5Antibacterial results of ZG / ZH nanoparticles at different concentrations

[0025] Figure 6 Self-produced electro-enzyme cascade microneedle patch for wound treatment in diabetic rats

[0026] Figure 7 Repair of sciatic nerve with self-produced electro-enzyme cascade microneedle patch

[0027] Figure 8 HE staining of gastrocnemius muscle slices with self-produced electro-enzyme cascade microneedle patch DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] In the following examples, glucose oxidase immobilized on the metal organic framework material ZIF-8 is abbreviated as ZG nanoparticles, and horseradish peroxidase immobilized on the metal organic framework material ZIF-8 is abbreviated as ZH nanoparticles.

[0030] Example 1. Preparation of microneedle template

[0031] (1) Prepare microneedle molds using PDMS transfer technology, with a PDMS solid-liquid mass ratio of 10:3;

[0032] (2) Place the poured mold in a vacuum drying oven and dry it for later use.

[0033] Example 2. Preparation of ZIF-8, ZG and ZH Nanoparticles

[0034] (1) A mixture of Zn(NO3)2·6H2O (40 mg) and 2-methylimidazole (0.77 g) was dissolved in 5 mL of deionized (DI) water. They were then stirred at room temperature for 5 min and centrifuged to obtain pale yellow nanocrystals, which were washed several times with DI water and dried to obtain ZIF-8 nanoparticles.

[0035] (2) A mixture of Zn(NO3)2·6H2O (40 mg), 2-methylimidazole (0.77 g) and glucose oxidase (GOX) was dissolved in 5 mL of deionized (DI) water. They were then stirred at room temperature for 5 min, centrifuged to obtain pale yellow nanocrystals, washed several times with DI water, and dried to obtain ZG nanoparticles.

[0036] (3) A mixture of Zn(NO3)2·6H2O (40 mg), 2-methylimidazole (0.77 g) and horseradish peroxidase (HRP) was dissolved in 5 mL of deionized (DI) water. They were then stirred at room temperature for 5 min, centrifuged to obtain pale yellow nanocrystals, washed several times with DI water, and dried to obtain ZH nanoparticles.

[0037] Example 3: Preparation of self-produced electro-enzyme cascade microneedle patch (ZGH-MN)

[0038] (1) Using the PDMS microneedle template prepared in Example 1;

[0039] (2) 0.01 g DA-PPy, 1 g hyaluronic acid (HA), and 0.5 g polyvinyl alcohol (PVA) were weighed and dissolved in 10 ml deionized water and stirred under magnetic stirring for 24 h to ensure sufficient swelling to obtain the DPPH microneedle substrate gel;

[0040] (3) The hydrogel polymer matrix solution was mixed with ZG and ZH nanoparticles to obtain drug-loaded syringe gel, wherein the weight of the added ZG and ZH was 5 mg each.

[0041] (4) Use a pipette to absorb 5-20ul of the ZG needle gel prepared in step (3), drop it onto half of the pinholes of the PDMS microneedle template, and place it in a vacuum drying oven for vacuum-1MPa negative pressure injection molding: repeatedly evacuate 3 times, each time for 5 minutes, and naturally dry at room temperature to obtain the ZG-loaded microneedle template;

[0042] (5) Use a pipette to absorb 10ul of the ZH needle gel prepared in step (3) and drop it onto the other half of the pinholes in the microneedle template in step (4). Place it in a vacuum drying oven and perform vacuum-1MPa negative pressure injection molding: Repeat the vacuuming for 3 times, each time for 3 to 5 minutes, and dry it naturally at room temperature to obtain a needle-tip-loaded ZG-ZH conductive microneedle patch (such as Figure 1 );

[0043] (6) placing the gel solution prepared in step (2) on the microneedle template with ZG-ZH nanoparticles loaded on the needle tip in step (5), placing it in a vacuum drying oven again, setting the vacuum to -1 MPa negative pressure injection molding and evacuating for 30 min, and drying naturally at room temperature to obtain a self-produced electro-enzyme cascade microneedle patch with the needle tip full of ZG-ZH nanoparticles loaded;

[0044] (7) spreading the soluble polymer matrix solution prepared in step (2) onto the microneedle template whose needle tip is filled with the conductive polymer matrix gel in step (6), and drying naturally to obtain a molded self-produced electro-enzyme cascade microneedle patch;

[0045] Example 4. Preparation of Conductive Microneedle Patch (ZIF-MN) Loaded with ZIF-8 Nanoparticles

[0046] (1) Using the PDMS microneedle template prepared in Example 1;

[0047] (2) 0.01 g DA-PPy, 1 g hyaluronic acid (HA), and 0.5 g polyvinyl alcohol (PVA) were weighed and dissolved in 10 ml deionized water and stirred under magnetic stirring for 24 h to ensure sufficient swelling to obtain the DPPH microneedle substrate gel;

[0048] (3) The hydrogel polymer matrix solution was mixed with ZIF-8 nanoparticles to obtain drug-loaded needle gel, wherein the mass of ZIF-8 was 5 mg.

[0049] (4) Use a pipette to take 10ul of the ZIF-8 needle gel prepared in step (3), drop it onto the micropores of the PDMS microneedle template, and place it in a vacuum drying oven under vacuum -1MPa negative pressure injection molding: repeatedly evacuate 3 times, each time for 5min, and naturally dry at room temperature to obtain the ZIF-8 loaded microneedle template;

[0050] (5) placing the gel solution prepared in step (2) on the microneedle template with ZIF-8 nanoparticles loaded on the needle tip in step (4), placing it in a vacuum drying oven again, setting the vacuum to -1 MPa negative pressure injection molding and evacuating for 30 min, and naturally drying at room temperature to obtain a conductive microneedle patch with ZIF-8 nanoparticles loaded on the needle tip;

[0051] (6) spreading the soluble polymer matrix solution prepared in step (2) onto the microneedle template whose needle tip is filled with the conductive polymer matrix gel in step (5), and obtaining a conductive microneedle patch loaded with ZIF-8 nanoparticles after natural drying;

[0052] Example 5. Preparation of Conductive Microneedle Patch Carrying ZG Nanoparticles (ZG-MN)

[0053] (1) Using the PDMS microneedle template prepared in Example 1;

[0054] (2) 0.01 g DA-PPy, 1 g hyaluronic acid (HA), and 0.5 g polyvinyl alcohol (PVA) were weighed and dissolved in 10 ml deionized water and stirred under magnetic stirring for 24 h to ensure sufficient swelling to obtain the DPPH microneedle substrate gel;

[0055] (3) The above hydrogel polymer matrix solution was mixed with ZG nanoparticles to obtain drug-loaded syringe gel, wherein the mass of ZG was 5 mg.

[0056] (4) Use a pipette to absorb 10ul of the ZG needle gel prepared in step (3), drop it onto the micropores of the PDMS microneedle template, and place it in a vacuum drying oven under vacuum -1MPa negative pressure injection molding: repeatedly evacuate 3 times, each time for 5min, and naturally dry at room temperature to obtain the ZG-loaded microneedle template;

[0057] (5) placing the gel solution prepared in step (2) on the microneedle template with ZG nanoparticles loaded on the needle tip in step (4), placing it in a vacuum drying oven again, setting the vacuum to -1 MPa negative pressure injection molding and evacuating for 30 min, and drying naturally at room temperature to obtain a conductive microneedle patch with ZG nanoparticles loaded on the needle tip;

[0058] (6) spreading the soluble polymer matrix solution prepared in step (2) onto the microneedle template whose needle tip is filled with the conductive polymer matrix gel in step (5), and obtaining a molded conductive microneedle patch loaded with ZG nanoparticles after natural drying;

[0059] Example 6. Preparation of Conductive Microneedle Patch (ZH-MN) Carrying ZH Nanoparticles

[0060] (1) performing the first step of operation: using the PDMS microneedle template prepared in Example 1;

[0061] (2) 0.01 g DA-PPy, 1 g hyaluronic acid (HA), and 0.5 g polyvinyl alcohol (PVA) were weighed and dissolved in 10 ml deionized water and stirred under magnetic stirring for 24 h to ensure sufficient swelling to obtain the DPPH microneedle substrate gel;

[0062] (3) The above hydrogel polymer matrix solution was mixed with ZH nanoparticles to obtain a drug-loaded syringe gel, wherein the mass of ZH was 5 mg.

[0063] (4) Use a pipette to absorb 10ul of the ZH needle gel prepared in step (3), drop it onto the micropores of the PDMS microneedle template, and place it in a vacuum drying oven under vacuum -1MPa negative pressure injection molding: repeatedly evacuate 3 times, 5min each time, and dry it naturally at room temperature to obtain the ZH-loaded microneedle template;

[0064] (5) placing the gel polymer matrix solution prepared in step (2) on the microneedle template with ZH nanoparticles loaded on the needle tip in step (4), placing it in a vacuum drying oven again, setting the vacuum to -1 MPa negative pressure injection molding and evacuating for 30 min, and drying naturally at room temperature to obtain a conductive microneedle patch with ZH nanoparticles loaded on the needle tip;

[0065] (6) spreading the hydrogel polymer matrix solution prepared in step (2) onto the microneedle template whose needle tip is filled with the conductive polymer matrix gel in step (5), and obtaining a molded conductive microneedle patch loaded with ZH nanoparticles after natural drying;

[0066] Example 7. Preparation of DPPH conductive microneedle patch (DPPH-MN)

[0067] (1) Using the PDMS microneedle template prepared in Example 1;

[0068] (2) 0.01 g DA-PPy, 1 g hyaluronic acid (HA), and 0.5 g polyvinyl alcohol (PVA) were weighed and dissolved in 10 ml deionized water and stirred under magnetic stirring for 24 h to ensure sufficient swelling to obtain a blank microneedle substrate gel;

[0069] (3) Use a pipette to take 10ul of the needle gel prepared in step (2), drop it onto the micropores of the PDMS microneedle template, and place it in a vacuum drying oven for vacuum-1MPa negative pressure injection molding: repeatedly evacuate 3 times, each time for 5 minutes, and dry it naturally at room temperature to obtain the DPPH conductive microneedle template;

[0070] (4) placing the gel polymer matrix solution prepared in step (3) on the microneedle template with the needle tip filled with DPPH in step (3), placing it in a vacuum drying oven again, setting the vacuum to -1 MPa negative pressure injection molding and evacuating for 30 minutes, and drying naturally at room temperature to obtain a conductive microneedle patch with the needle tip filled with the conductive polymer matrix solution;

[0071] (5) spreading the polymer gel matrix solution prepared in step (2) onto the microneedle template whose needle tip is filled with the conductive polymer matrix gel in step (4), and drying naturally to obtain a molded DPPH conductive microneedle patch, namely BLANK-MN in the experimental example below;

[0072] Experimental Example 1: Comparison of dispersibility and solubility of PPy and DA-PPy in water

[0073] The prepared PPy and DA-PPy were dispersed in deionized water at the same concentration (10 mg / mL) by shaking, and then allowed to stand to observe the differences immediately after standing, after standing for 1 minute, and after standing for 5 minutes. At the same time, the micromorphology of PPy and DA-PPy was characterized by scanning electron microscopy to observe the changes in the micromorphology before and after polydopamine modification.

[0074] The experimental results show that: Figure 2 As shown in the figure, PPy has poor solubility in aqueous solution and its dispersion is unstable and soon becomes uneven; while DAPPy has good solubility in aqueous solution and good stability and can be dispersed evenly for a long time. Figure 3As shown, (a) and (b) are PPy, (c) and (d) are DAPPy, the scale bar in (a, c) is 1 μm, and the scale bar in (b, d) is 100 nm. It can be seen that DA modification can change the morphology of PPy from aggregated particles to short fibrous structures, which will improve its hydrophilic dispersibility and facilitate the preparation of microneedles.

[0075] Experimental Example 2: Test of the effect of self-produced electroenzyme cascade microneedle patch in generating current

[0076] The prepared self-produced electro-enzyme cascade microneedle patch ZGH-MN was placed in a culture dish, and glucose solutions of different concentrations (0 / 18 / 20 / 24 / 26 mmol / L) were added every 1 minute to simulate the body fluid environment with different blood glucose concentrations. The solution was measured with a high-precision desktop digital multimeter and the output current was recorded simultaneously.

[0077] Experimental results: Figure 4 As shown in the figure, when the glucose concentration increases, the output current of the microneedle also increases. When the glucose concentration is 0 / 18 / 20 / 24 / 26mmol / L, the output current generated by the microneedle patch through the enzyme cascade reaction is 1.01μA, 1.74μA, 2.01μA, 2.32μA, 2.64μA, and 3.53μA. The results show that the homemade electric microneedle patch is sensitive to the blood glucose concentration of the diabetic wound surface and can respond quickly. The enzyme cascade reaction occurs, and while reducing local blood sugar, it can output physiological microcurrent, thereby better promoting wound healing.

[0078] Experimental Example 3: Efficacy of self-produced electro-enzyme cascade microneedle patch in treating diabetic wounds

[0079] Since bacterial infection is prone to occur at wounds after skin damage, which affects wound healing, it is necessary to test the antibacterial properties of microneedle patches with different concentrations of ZIF-8, ZG, and ZH nanoparticles. The experimental method is to co-culture the microneedle patches with Escherichia coli and Staphylococcus aureus, and then use the plate count method for evaluation.

[0080] In the animal experiment, 6-week-old male Wister rats weighing 180-220g were selected and purchased from the Animal Experiment Center of Lanzhou University. STZ was prepared into a 10mg / mL STZ solution with PBS solution and sterilized with a 0.22μm filter. Note that the preparation should be kept away from light and used immediately. Fasting was performed for 12 hours before surgery. The rats in the model group were intraperitoneally injected with 60mg / kg STZ. Fasting blood sugar was measured 3 and 7 days after STZ injection. If the rats showed mental depression, slow reaction, increased appetite, significantly increased urine volume, weight loss and blood sugar concentration greater than 13.5-25mmol / L, the type I diabetes model was successfully established. The anesthetized diabetic rats were fixed on the rat rack, and two square full-thickness wounds of equal size of 1×1cm were prepared after shaving, skin preparation and disinfection on both sides of the back spine.

[0081] Experimental groups and treatment plans: The established diabetic wound animal model was divided into 6 groups, with 6 animals in each group. The wounds in 5 groups were treated with Blank-MN patch, ZIF-MN patch, ZG-MN patch, ZH-MN patch, and ZGH-MN patch, respectively, and the remaining group was a blank control group.

[0082] Evaluation of therapeutic efficacy: The wound was grossly observed on days 7, 14 and 21, and the wound size was measured and recorded.

[0083] Experimental results:

[0084] Depend on Figure 5 The results of the antibacterial experiment show that when the concentration of ZIF-8, ZG, and ZH nanoparticles reaches 0.5 mg / ml, the antibacterial rate is almost 100%, which has good antibacterial properties.

[0085] Depend on Figure 6 The results show that the diabetic wounds in the self-produced electro-enzyme-linked microneedle patch group gradually became smaller. The ZGH-MN microneedle patch group achieved scar-free healing at 21 days, while the other groups still had smaller wounds on the skin surface or obvious scars on the skin surface after healing. The experiment shows that the self-produced electro-enzyme-linked microneedle patch provided by the present invention has a significant healing effect on diabetic wounds and achieves scar-free healing of diabetic wounds.

[0086] Experimental Example 4: Efficacy of self-produced electro-enzyme cascade microneedle patch in treating sciatic nerve

[0087] 6-week-old male Wister rats, weighing 180-220g, were purchased from the Animal Experiment Center of Lanzhou University. 10% chloral hydrate was injected intraperitoneally (3ml / kg) and the skin was prepared after the rats were anesthetized to expose the skin around the right sciatic tuberosity of each rat. The right side was selected as the experimental side and the left side as the control side. The operation was carried out according to the principle of sterility. The position of the sciatic tuberosity was touched with a finger. The skin was cut back along the sciatic tuberosity in the superficial layer of the femur. The white line of the intermuscular fascia was clearly visible. The sciatic nerve trunk was exposed by blunt separation along the white line with a vascular clamp. The sciatic nerve trunk at the lower end of the right sciatic tuberosity of the rat was freed and exposed. A 10mm nerve segment was cut in the middle. The prepared microneedle nerve tube was placed at the free end of the nerve to replace the repaired missing nerve and sutured in layers.

[0088] Experimental grouping and treatment plan: The established sciatic nerve rat model was divided into 7 groups, with 3 rats in each group. The nerve stumps in 5 groups were treated with Blank-MN patch, ZIF-MNs patch, ZG-MN patch, ZH-MN patch, and ZGH-MN patch, respectively. The remaining group was a blank control group, and the other group was an autologous transplantation group, that is, the nerves of normal rats were transplanted to the free ends of the sciatic nerve model rats.

[0089] Evaluation of therapeutic effect: The rats were killed at the 6th and 12th weeks, and the sciatic nerve and gastrocnemius muscle after treatment were observed grossly. The gastrocnemius muscle tissue was fixed with fixative and used for HE section staining to compare the muscle fiber conditions.

[0090] Experimental results:

[0091] Depend on Figure 7 The results show that from the gross photos of the gastrocnemius muscle at week 6, the volume of the gastrocnemius muscle after treatment with the conductive microneedle patch was significantly larger than that of the blank control group, among which the volume of the gastrocnemius muscle in the ZGH self-produced electro-enzyme cascade microneedle patch group was the largest; Figure 8 The HE staining results of the gastrocnemius muscle sections show that the gastrocnemius muscle fibers in the self-produced electro-enzyme-linked microneedle patch treatment group were significantly larger than those in the ZG, ZH and Blank conductive microneedle patch groups at the 6th and 12th weeks, especially the size and arrangement of the gastrocnemius muscle fibers in the ZGH self-produced electro-enzyme-linked microneedle patch group were close to those in the autologous transplantation group; indicating that the self-produced electro-enzyme-linked conductive microneedle patch has a good effect on the repair of the sciatic nerve. Animal experiments show that the self-produced electro-enzyme-linked conductive microneedle patch provided by the present invention has a good repair effect on the damage of peripheral nerves such as the sciatic nerve, and the therapeutic effect is significant.

[0092] In summary, the present invention has prepared a self-generated enzyme-cascade microneedle patch, which is sensitive to the blood sugar concentration of diabetic wounds and can respond quickly. Enzyme cascade reaction occurs, and while lowering local blood sugar, physiological microcurrent can be output, thereby better promoting wound healing and having good antibacterial properties; the ZGH-MN microneedle patch group achieved scar-free healing at 21 days, while the other groups still had smaller wounds on the skin surface or obvious scars on the skin surface after healing. Experiments show that the self-generated enzyme-cascade microneedle patch provided by the present invention has a significant healing effect on diabetic wounds, achieving scar-free healing of diabetic wounds. From the gross photos of the gastrocnemius at week 6, it can be seen that the volume of the gastrocnemius muscle after treatment with the conductive microneedle patch is significantly larger than that of the blank control group, among which the volume of the gastrocnemius muscle in the ZGH self-produced electroenzyme-linked microneedle patch group is the largest; the gastrocnemius muscle fibers in the self-produced electroenzyme-linked microneedle patch treatment group are significantly larger than those in the ZG, ZH and Blank conductive microneedle patch groups at week 6 and week 12, especially the size and arrangement of the gastrocnemius muscle fibers in the ZGH self-produced electroenzyme-linked microneedle patch group are close to those in the autologous transplantation group; indicating that the self-produced electroenzyme-linked conductive microneedle patch has a good effect on the repair of the sciatic nerve. Animal experiments show that the self-produced electroenzyme-linked conductive microneedle patch provided by the present invention has a good repair effect on the damage of peripheral nerves such as the sciatic nerve, and has a significant therapeutic effect.

[0093] Finally, it should be noted that: although this specification is described according to implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.

Claims

1. A self-produced electro-enzyme cascade microneedle patch, characterized in that: The microneedle patch is composed of a conductive substrate without a target drug and a microneedle array composed of at least one needle body containing the target drug. The substrate is prepared from polypyrrole modified with polydopamine, hyaluronic acid and polyvinyl alcohol, and the needle body is prepared from polypyrrole modified with polydopamine, hyaluronic acid, polyvinyl alcohol, glucose oxidase and horseradish peroxidase. Half of the needle body is doped with ZG nanoparticles of glucose oxidase fixed by metal organic framework material ZIF-8, and the other half is ZH nanoparticles of horseradish peroxidase fixed by metal organic framework material ZIF-8.

2. The self-produced electro-enzyme cascade microneedle patch according to claim 1, characterized in that: In the substrate, the mass ratio of dopamine-modified polypyrrole, hyaluronic acid and polyvinyl alcohol is 0.01~1:1~100:0.5~50; in the needle body, the mass ratio of dopamine-modified polypyrrole, hyaluronic acid, polyvinyl alcohol, glucose oxidase, horseradish peroxidase and ZIF-8 is 0.01~1:1~100:0.5~50:0.005~0.5:0.005~0.5:0.1~10.

3. The method for preparing a self-produced electro-enzyme cascade microneedle patch according to any one of claims 1 to 2, characterized in that: The steps include: (1) In a water bath and under magnetic stirring, polydopamine-modified polypyrrole, hyaluronic acid and polyvinyl alcohol are added to deionized water in proportion to obtain a microneedle patch base gel; (2) mixing the microneedle patch base gel prepared in step (1) with glucose oxidase to obtain glucose oxidase needle body gel; mixing the microneedle patch base gel prepared in step (1) with horseradish peroxidase to obtain horseradish peroxidase needle body gel; (3) Use a pipette to absorb 5-20ul of the glucose oxidase needle gel prepared in step (2), drop it onto half of the pinhole of the PDMS microneedle template, and place it in a vacuum drying oven for negative pressure injection molding at -1~-0.8MPa: Repeat the vacuuming 2~3 times, each time for 3~5min, and obtain the microneedle template loaded with glucose oxidase after natural drying at room temperature; (4) Use a pipette to absorb 5-20ul of the horseradish peroxidase needle gel prepared in step (2), and drop it onto the other half of the needle hole of the microneedle template in step (3), and place it in a vacuum drying oven under a negative pressure of -1 to -0.8MPa for injection molding: Repeat the vacuuming 2 to 3 times, each time for 3 to 5 minutes, and dry it naturally at room temperature to obtain the conductive microneedle patch needle body loaded with glucose oxidase-horseradish peroxidase; (5) placing the base gel prepared in step (1) on the microneedle body template obtained in step (4), placing it in a vacuum drying oven again, setting the vacuum to -1 to -0.8 MPa, vacuuming the negative pressure injection mold for 10 to 30 minutes, and drying naturally at room temperature to obtain the self-produced electro-enzyme cascade microneedle patch body; (6) Spread the base gel prepared in step (1) onto the microneedle template in step (5) whose needle body is filled with conductive polymer matrix gel, and after natural drying, obtain a self-produced electro-enzyme cascade microneedle patch.

4. The preparation method according to claim 3, characterized in that: The water bath temperature in step (1) is 0-90°C.

5. Use of the self-produced electro-enzyme cascade microneedle patch as claimed in claim 1 or 2 in preparing medicine for treating diabetic wounds.

6. Use of the self-produced electro-enzyme cascade microneedle patch as claimed in claim 1 or 2 in the preparation of a drug for treating sciatic nerve injury.