Improved SMA resin formulation
By using resin compositions containing styrene maleic anhydride copolymer, epoxy resin, crosslinking agent and filler, the problem of layering of printed circuit board prepreg and laminate at high temperature is solved, and their electrical and thermal are improved and mechanical properties meet the needs of low wicking and white glass characteristics.
Patent Information
- Application Number
- CN202210610920.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-07-25
- Filing Date
- 2017-07-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2037-07-25
AI Technical Summary
The prepregs and laminates of existing printed circuit boards are easily layered at high temperatures and are difficult to meet the needs of low wicking and white glass characteristics, affecting electrical and thermal performance.
Resin is prepared by compounding method using a resin composition containing styrene maleic anhydride copolymer, epoxy resin, crosslinking agent, talc and silica for the production of prepregs and laminates and on copper foil Coat the resin to improve its performance.
The electrical, thermal and mechanical properties of laminates and printed circuit boards are significantly improved, layering is reduced, and low expansion and white glass cracks are exhibited at high temperatures, improving wicking performance.
Smart Images

Figure SMS_2 
Figure SMS_3 
Figure SMS_4
Abstract
Description
[0001] This application is a divisional application of the invention patent application with the application date of July 25, 2017, application number: 2017800461902, and name “Improved SMA Resin Formulation”. Field of the Invention
[0002] The present invention relates to a resin composition, which is used to impregnate a woven material and then partially or completely cured to form a prepreg and a laminate for manufacturing a printed circuit board. The prepreg and the laminate prepared using the resin composition of the present invention have excellent electrical properties suitable for high-frequency applications in electronic devices, as well as excellent thermal and mechanical properties. Background of the Invention
[0003] Fillers such as talc can be an important component in resins used to make prepregs and laminates, which are then used in the manufacture of printed circuit boards. Talc provides thermal stability, fills voids, and improves PCB drilling. Styrene maleic anhydride (SMA) is a component of certain resins used to make prepregs and laminates. SMA can be included in resins to improve the glass transition temperature (T g ). When used together in a resin system for PCB applications, talc and SMA can provide prepregs with improved thermal reliability under reflow. However, as the thermal and electrical specifications of laminates and printed circuit boards continue to change, there remains a need for prepregs and laminates with improved thermal, electrical and mechanical properties. Summary of the invention
[0004] Laminates and prepregs for printed circuit boards form a stack and ultimately a printed circuit board (PCB), which includes multiple laminate layers bonded together. One problem that arises from PCBs is that adjacent laminate layers may delaminate, particularly when the stack or PCB is subjected to high temperatures. Delamination may result in circuit board failure. In addition, PCB manufacturers have also begun to require prepreg materials that can be used to make PCBs with low wicking and white glass properties. Therefore, there is a need for prepregs, laminates, resin-coated copper and similar resin-containing materials that can be used to form PCBs that are less prone to delamination and / or exhibit improved wicking and / or white glass properties.
[0005] In one aspect, we have discovered that the use of an unexpected combination of fillers - silica and talc - provides a synergistic combination that improves the electrical and / or thermal properties of certain laminates and / or PCBs better than using silica or talc alone. This is particularly true when using anhydride curing agents.
[0006] Another aspect is a resin composition comprising a styrene maleic anhydride copolymer; at least one epoxy resin; at least one crosslinking agent; talc; and silica.
[0007] Another aspect is a resin composition comprising: about 5 to about 40 wt % of a styrene maleic anhydride copolymer based on the dry solvent-free resin; about 10 to about 50 wt % of at least one epoxy resin selected from brominated bisphenol A, brominated bisphenol F, non-brominated bisphenol A, non-brominated bisphenol F, and combinations thereof based on the dry solvent-free resin; about greater than 0 to about 20 wt % of at least one crosslinker selected from tetrabromobisphenol A, tetrakis-DOPO-bisphenol A, and mixtures thereof based on the dry solvent-free resin; about 2.5 to about 15 wt % of talc based on the dry resin; and about 2.5 to about 15 wt % of fumed silica based on the dry resin.
[0008] Another aspect is a prepreg and / or laminate comprising a reinforcement material impregnated with a resin as described herein and a resin-coated copper foil; the copper foil comprising a copper foil sheet having a first planar surface and a second planar surface, and a B-stage or C-stage resin layer as described herein applied to at least one of the planar surfaces.
[0009] Description of current implementation
[0010] The present disclosure generally relates to resins made from various components and to prepregs and laminates including partially or fully cured resins.
[0011] Resins are prepared by a "compounding" process in which resin ingredients are combined to form a thermosetting resin. In one example, the resin is used to make a laminate by "impregnating" a reinforcement material such as a woven glass fabric with the resin. In another example, the resin is used to coat a copper foil to form a resin-coated copper laminate. In another example, the resin is used to form a laminate that does not include reinforcement materials. One type of product made using these resins is a "prepreg," i.e., a sheet that may include a resin or a resin-impregnated reinforcement material in which the resin is only partially cured or "B-staged." Another type of product made from the resin is a C-stage laminate in which the resin is fully cured. The ingredients used to formulate the resins are discussed below. Unless otherwise noted, the component weight percentage ranges are reported on a "dry" solvent-free basis.
[0012] The resin of the present invention comprises: (1) at least one SMA copolymer; (2) at least one epoxy resin; (3) at least one co-crosslinking agent; (4) talc; (5) fused silica; and a catalyst. The resin may include various optional ingredients, including UV blockers, flame retardants, and solvents.
[0013] SMA copolymers
[0014] The first component of the resin of the present invention is one or more SMA copolymers. Copolymers of styrene and maleic anhydride are described in particular in Encyclopedia of Polymer Science and Engineering, Vol. 9 (1987), p. 225. Within the scope of the present invention, the term "copolymer" also refers to SMA or a mixture of SMAs.
[0015] Useful styrene and maleic anhydride (SMA) are type 1 SMA copolymers having a molecular weight in the range of about 1400 to about 50,000 and an anhydride content greater than 15 wt %. Preferred are SMA copolymers having a molecular weight in the range of 1400 to 10,000. Examples of such copolymers include commercially available SMA 1000, SMA 2000, SMA 3000, and SMA 4000. The styrene: maleic anhydride ratios of these copolymers are, for example, 1:1, 2:1, 3:1 and 4:1, 5:1, 6:1, 7:1; 8:1 and 9:1, respectively, and the molecular weight range is about 1400 to about 4000. Mixtures of these SMAs may also be used.
[0016] The amount of SMA copolymer used in the resin is from about 5 to about 40 wt %, and more suitably from about 5 to about 30 wt %, on a dry solids basis.
[0017] Epoxy resin
[0018] As used herein, the term "epoxy resin" refers to curable compositions of oxirane ring-containing compounds as described in CA, May, Epoxy Resins, 2nd Edition, (New York & Basle: Marcel Dekker Inc.), 1988.
[0019] Some examples of epoxy resins include: diglycidyl ethers based on bisphenol A; polyglycidyl ethers based on phenol-formaldehyde novolac or cresol-formaldehyde novolac; those based on triglycidyl ether of tri(p-hydroxyphenyl)methane or tetraglycidyl ether of tetraphenylethane; amines such as those based on tetraglycidyl-methylenedianiline or triglycidyl ether of p-aminoethylene glycol; alicyclic types, such as those based on 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate. The term "epoxy resin" also represents the reaction product of compounds containing an excess of an epoxy compound (e.g., the types described above) and an aromatic dihydroxy compound. These compounds may be halogen-substituted.
[0020] Preferred are epoxy resins which are derivatives of bisphenol A, in particular FR4, particularly due to their low price. FR4 is prepared by the propulsive reaction of an excess of bisphenol A diglycidyl ether with tetrabromobisphenol A. Mixtures of epoxy resins with bismaleimide resins, cyanate resins and / or bismaleimide triazine resins may also be used.
[0021] It should be noted that epoxy resins are usually represented by a single, clear structural formula. Those skilled in the art will appreciate that this should include deviation products resulting from side reactions occurring during the preparation of the epoxy resins. Since these by-products constitute normal components of cured epoxy resins, they also constitute normal components of the resins according to the present invention.
[0022] The resin comprises one or more epoxy resins in a total amount of about 5 wt% to about 50 wt%, and more narrowly about 10 wt% to about 40 wt%, on a dry weight basis. In one aspect of the invention, the resin comprises two different epoxy resins.
[0023] Crosslinking agent
[0024] The resin will contain one or more crosslinking agents. Useful crosslinking agents include brominated and non-brominated bisphenol A, brominated and non-brominated bisphenol A diglycidyl ethers, tetrabromobisphenol A, and tetra-DOPO-bisphenol A. As described above, each crosslinking agent may optionally be brominated, i.e., substituted with one or more bromine atoms. Brominated co-crosslinking agents are useful for their flame retardant properties. Preferably, the aromatic moieties of BPA and BPADGE are each substituted with two bromine atoms to give tetrabromo-TBBPA and TBBPADGE, respectively. Optionally, brominated phenolic novolacs may also be used as crosslinking agents.
[0025] The amount of crosslinker used in the resin is greater than about 0 to about 20 wt %, and more narrowly about 0.05 to about 10 wt % on a solvent-free or solids basis.
[0026] filler
[0027] The resin of the present invention comprises two or more different fillers. Typically, the filler can be selected from fused silica, amorphous fused silica, crystalline silica, fumed silica, talc, core-shell particles, One or more of quartz, ceramic, amorphous or crystalline particulate metal oxides such as silica, titania, alumina, ceria, clay, calcined clay, boron nitride, wollastonite, granular rubber, polyphenylene ether, and mixtures thereof. Other examples of useful fillers include calcined clay, fused silica, and combinations thereof.
[0028] Particularly useful fillers are talc and silica, with fused silica and talc being a particularly useful combination. The first filler and the second filler are present in the resin in an amount of about 5 wt % to about 50 wt % based on dry resin, and more narrowly in an amount of about 5 wt % to about 37.5 wt % based on dry resin, and finally more narrowly in an amount of about 5 wt % to about 25 wt % based on dry resin.
[0029] When a combination of talc and silica is used in the resin, the talc should be present in an amount of about 2.5 wt% to about 25 wt%, and the silica should be present in an amount of about 2.5 wt% to about 25 wt%. More narrowly, the talc should be present in an amount of about 2.5 wt% to about 15 wt%, and the silica should be present in an amount of about 2.5 wt% to about 15 wt%, both based on dry resin. In alternative embodiments, the weight ratio of silica or fumed silica to talc in the resin is about 1:2.5 to about 5:1, and more narrowly about 1:1 to about 2.5:1.
[0030] An example of a useful talc is Microtuff AGD manufactured by Barretts Minerals, Inc. The talc can be silane treated or unsilane treated. In addition, the average talc particle size will be less than about 1.2 microns, preferably less than about 0.9 microns. Smaller talc particles can fill the resin voids in smaller amounts, so the resin is less likely to expand when heated.
[0031] An example of a useful silica filler is amorphous fused silica, particularly D 50 Amorphous fused silica having a particle size of less than about 6.0 microns and more narrowly less than 4.0. In another example, the silica has a percolation threshold of 2-4 microns. It has been found that silica with a percolation amount of 2-4 microns can enhance prepreg or PCB properties, such as electrical properties, while these properties, as well as mechanical properties, begin to degrade when silica with a percolation threshold outside of this range is used. The silica can be silanized (silane treated) or non-silanized (not silane treated). Silane treatment uses silanes and silazanes to chemically modify the surface of silica (or talc) to make the surface hydrophobic.
[0032] Flame retardants
[0033] The compounded resin of the present invention may contain one or more flame retardants. Any flame retardant known to be useful in a resin composition for making composite materials and laminates for making printed circuit boards may be used. Flame retardants may contain halogens or they may be halogen-free. Examples of useful flame retardants include, but are not limited to, halides of glycidyl-etherified difunctional alcohols; halides of novolac resins such as bisphenol A, bisphenol F, polyvinylphenol or phenol, cresol, alkylphenol, catechol and novolac resins; inorganic flame retardants such as antimony trioxide, red phosphorus, zirconium hydroxide, barium metaborate, aluminum hydroxide and magnesium hydroxide; and phosphorus-based flame retardants such as tetraphenylphosphine, tricresyl diphenyl phosphate, triethyl phosphate, cresyl diphenyl phosphate, ditolyl diphenyl phosphate, acid phosphates, ammonium phosphate, ammonium polyphosphate, ammonium cyanurate, nitrogen-containing phosphate compounds and phosphates containing halides.
[0034] Phosphorus-based flame retardants may include, for example, those disclosed in US Pat. Nos. 6,645,631, 7,687,556, and 8,129,456, the specifications of each of which are incorporated herein by reference.
[0035] The flame retardant is present in the resin composition of the present invention in an amount sufficient to allow a laminate made from the resin composition to pass the UL-94 flammability test. More narrowly, the flame retardant or a combination thereof may be present in the resin in an amount of about 5 wt % to about 50 wt %, or about 10 wt % to about 30 wt %, based on dry weight.
[0036] In a preferred embodiment, the flame retardant is a solid flame retardant decabromodiphenylethane having the following structure:
[0037]
[0038] Decabromodiphenylethane is commercially available from, for example, Albemarle Corporation (451 Florida St., Baton Rouge, LA 70801). Albemarle products are available under the trade name Saytex TM Decabromodiphenylethane is sold as 8010. Decabromodiphenylethane also unexpectedly improves the dielectric properties of the cured resin composition. Thus, decabromodiphenylethane can be included in the resin composition in an amount much greater than that required as a flame retardant so as to also improve the dielectric properties of the cured resin. Another useful high bromine content insoluble flame retardant is ethylene bistetrabromophthalimide, which is sold as Saytex BT93W by Albemarle Corporation. Other similar useful flame retardants include decabromodiphenyl ether and brominated polystyrene.
[0039] Initiator / Catalyst
[0040] The resin also contains an initiator / catalyst, which promotes crosslinking of the resin components, for example by performing various functions, such as promoting homopolymerization and / or crosslinking of the resin components, and can be used to increase the rate of resin curing during resin thermal curing. The initiator / catalyst selected can be any compound known to be useful in resin synthesis or curing, whether or not it performs any of these functions.
[0041] Examples of useful initiators are azo-type initiators / catalysts such as azobisisobutyronitrile (AIBN), 2-propylimidazole (2-PI), tetrabutylphosphonium acetate (TBPAAc), and 2-methylimidazole (2-MI).
[0042] The amount of initiator used depends on the application. When used in a resin, the initiator is present in an amount ranging from about 0.01 to about 3.0 wt%, more narrowly from about 0.05 to about 1 wt%.
[0043] In certain aspects, the resin generally comprises the ingredients in the amounts reported in Table 1 below, where the amounts are reported as parts by weight on a solvent-free basis or on a solids basis only.
[0044] Table 1
[0045]
[0046] Alternative resin compositions are summarized in Table 2 below, where the amounts of ingredients are reported in parts by weight including solvent.
[0047] Table 2
[0048]
[0049] In one aspect, the invention includes a resin having the following composition, wherein weight percent amounts are reported on a total solids (solvent-free) basis:
[0050] 1. 10-40wt% styrene maleic anhydride copolymer (SMA);
[0051] 2. 5-40 wt% epoxy resin (combination of brominated or non-brominated bisphenol A or bisphenol F);
[0052] 3. 0-20 wt% of tetrabromobisphenol A or tetra-DOPO-bisphenol A;
[0053] 4. 5-20% of halogen-containing or halogen-free flame retardants, such as bromine- or phosphorus-based monomers or resins;
[0054] 5. 5-40 wt% of a filler combination (combining two or more fillers) with the following possibilities: fused silica, crystalline silica, fumed silica, talc, clay, core-shell rubber particles or granular flame retardants.
[0055] In another aspect, the invention includes a resin having the following composition, wherein the weight percent amounts are reported based on the total weight including solvent:
[0056] 1. A solvent combination package of 30%-40% low-boiling point and high-boiling point solvents: methyl ethyl ketone, cyclohexanone;
[0057] 2. 15%-30% styrene maleic anhydride copolymer (SMA)
[0058] 3. 10%-20% of epoxy resin combination of brominated or non-brominated epoxy resin;
[0059] 4. 0.5%-10% of tetrabromobisphenol A or tetra-DOPO-bisphenol A;
[0060] 5. 5%-12.5% talc
[0061] 6. 5%-25% fused silica
[0062] 7. 0.01%-0.03% Tinopal OB (UV blocking agent) (optional)
[0063] 8. 0.01-0.13% tetrabutylphosphonium acetate (TBPAAc), 2-methylimidazole (2-MI)
[0064] or 2-phenylimidazole (2-PI).
[0065] Solvents
[0066] One or more solvents are typically incorporated into the resin composition of the present invention to dissolve suitable resin composition ingredients, and / or to control resin viscosity, and / or to maintain the ingredients in a suspended dispersion. Any solvent known to those skilled in the art that can be used in conjunction with a thermosetting resin system can be used. Particularly useful solvents include methyl ethyl ketone (MEK), toluene, dimethylformamide (DMF), acetone, propyl acetate, cyclohexanone, and combinations thereof.
[0067] When used, the solvent is present in the resin in an amount of about 20 wt% to about 50 wt% (weight percent) based on the total weight of the resin composition including the solvent. Useful solvents are combinations of low boiling point solvents and high boiling point solvents, such as methyl ethyl ketone and cyclohexane.
[0068] Optional Ingredients
[0069] (a) Toughening agent
[0070] The thermosetting resin composition of the present invention may contain one or more toughening agents. Toughening agents are added to the resin composition to improve the drilling performance of the resulting composite material and laminate. Useful toughening agents include copolymers of methyl methacrylate / butadiene / styrene, methacrylate butadiene styrene core-shell particles, and mixtures thereof. A preferred toughening agent is methacrylate butadiene styrene core-shell particles, which are available under the trade name Available from Rohm & Haas (100 Independence Mall West, Philadelphia, PA). When used, the toughening agent is present in the thermosetting resin composition of the present invention in an amount of about 1% to about 5%, preferably about 2% to about 4%, based on 100% by weight solids of the composition.
[0071] (b) Other optional ingredients
[0072] Optionally, the compounded resin may also contain other additives such as defoamers, leveling agents, dyes and pigments. For example, fluorescent dyes may be added to the resin composition in trace amounts so that when exposed to light, the laminate prepared therefrom is fluorescent when examined with optical equipment. Useful fluorescent dyes are highly conjugated diene dyes. An example of such a dye is OB (2,5-thiophenediylbis(5-tert-butyl-1,3-benzoxazole) was purchased from Ciba Specialty Chemicals, Tarrytown, New York.
[0073] Other optional ingredients known to those skilled in the art as being useful in the manufacture of printed circuit board laminates may also be included in the resin composition of the present invention.
[0074] Prepregs and laminates of the present invention prepared with a resin system comprising a combination of fumed silica and talc synergistically exhibit lower expansion under thermal stress and reflow, particularly when the amount of styrene in the SMA is increased proportionally with the anhydride. The improvement in expansion caused by the filler combination is even greater as the ratio of SMA space to anhydride increases; particularly useful when the ratio of anhydride to styrene is 1:1; 1:2; 1:3; 1:4; 1:5; 1:6, 1:7, 1:8 and 1:9.
[0075] In another aspect of the present invention, the resin may include different combinations of SMA and SMA in different proportions. For example, a combination including two or more anhydrides and styrene ratios (1:3, 1:4, 1:5, 1:6) and a filler combination with talc and fumed silica may be used. Extensions of these filler combinations include any filler type similar to talc, which is composed of a thin sheet combined with a spherical or elliptical or even porous silica filler. This will include a combination of any of these shaped fillers, such as shell rubber core particles that are generally spherical. The resin including this filler combination is more uniform, thereby improving the thermal properties unique to the laminate and prepreg materials used in the PCB industry. The industry has long-term thermal requirements, which help prevent any delamination of the laminate in the printed circuit board. When incorporated into a laminate for a PCB, the resin including the combination of fillers disclosed above prevents PCB delamination in addition to reducing laminate expansion under thermal stress.
[0076] The combination of resin components including two different fillers produces a product that exhibits increased expansion with a greater spatial volume ratio in an SMA system. This greater ratio is ideal for low dielectric constant performance, but this advantage produces increased expansion and thermal instability, which has been addressed in recent history by using a separate silica filler. The combination of two fillers in the resin described herein helps reduce expansion and thermal stability, especially under thermal stress and reflow, and reduces the threat of delamination and / or white glass cracking and / or wicking.
[0077] Prepregs and Laminates
[0078] The above resins can be used to prepare prepregs and / or laminates for use in the manufacture of printed circuit boards. For use in the manufacture of printed circuit boards, the laminates can be partially cured or B-staged (in which case they are called prepregs), in which state they can be stacked with other sheets of material and fully cured ("C-staged") to form a stack or PCB. Alternatively, the resin can be incorporated into a C-stage laminate, resin-coated copper sheet or interlayer sheet.
[0079] In a useful method, resin is used to make prepreg in an intermittent or continuous method. Prepreg is usually made of reinforcing materials, such as woven glass mesh (fabric), which is unfolded into a series of drive rollers. Then, the mesh is transported to the coating area, in which the mesh is immersed in a groove containing a thermosetting resin containing a solvent, and the glass mesh is now saturated with resin. Then, the resin-saturated glass mesh is passed through a pair of metering rods or rollers to remove excess resin from the saturated glass mesh, and then the resin-coated mesh is advanced for a selected period of time on the length of the drying tower until the solvent evaporates from the mesh. By repeating these steps, the optional second and subsequent resin coatings can be applied to the net until the preparation of the prepreg is completed, and the prepreg is now wound. The woven glass mesh can be replaced with woven fabric material, paper, plastic sheet, felt and / or granular material such as glass fiber particles or granular material.
[0080] In another method of making prepregs or laminates, the thermosetting resins of the present invention are premixed in a mixing vessel at ambient temperature and pressure. The viscosity of the premix is about 600-1000 cps, and the viscosity can be adjusted by adding solvent or removing solvent from the resin. The fabric substrate (usually but not limited to E-glass) is pulled through an impregnation tank containing the premixed resin, through an oven tower, where excess solvent is removed and the prepreg is rolled or sheeted to size, stacked between Cu foils in various configurations (depending on the style of glass weave, resin content & thickness requirements).
[0081] Thermosetting resin (resin) mixtures can also be applied in a thin layer onto Cu foil substrates (RCC - Resin Coated Cu) using a slot die or other related coating techniques.
[0082] Prepregs, laminates, resin-coated copper foils, and the like prepared using the resins described herein can be used to manufacture printed circuit boards (PCBs) using manufacturing techniques known in the art.
[0083] In summary, the embodiments of the present application include the following:
[0084] 1. A resin composition comprising:
[0085] Styrene maleic anhydride copolymer;
[0086] at least one epoxy resin;
[0087] at least one cross-linking agent;
[0088] Talc; and
[0089] Silicon dioxide.
[0090] 2. The resin composition of item 1, wherein the talc is present in the resin composition in an amount of about 2.5 to about 15 wt% on a dry weight basis.
[0091] 3. The resin composition of any one of items 1-2, wherein the silica is present in the resin composition in an amount of about 2.5 to about 25 wt% on a dry weight basis.
[0092] 4. The resin composition according to any one of items 1 to 3, wherein the silica is fused silica.
[0093] 5. The resin composition according to any one of items 1 to 4, wherein the silica is silanized silica.
[0094] 6. The resin composition according to any one of items 1 to 5, wherein the talc is a silanized talc.
[0095] 7. The resin composition of any one of items 1 to 6, comprising about 5 to about 12.5 wt% of talc and about 5 to about 25 wt% of silanized fused silica, each on a dry weight basis.
[0096] 8. The resin composition of any one of items 1-7, wherein the styrene maleic anhydride copolymer is present in the resin composition in an amount of about 5 to about 40 wt% on a dry weight basis.
[0097] 9. The resin composition of any one of items 1-8, wherein the at least one epoxy resin is present in the resin composition in an amount of about 10 to about 50 wt% on a dry weight basis.
[0098] 10. The resin composition of any one of items 1-9, wherein the at least one epoxy resin is selected from brominated bisphenol A, brominated bisphenol F, non-brominated bisphenol A, non-brominated bisphenol F, and combinations thereof.
[0099] 11. The resin composition of any one of items 1-10, wherein the at least one crosslinking agent is present in the resin composition in an amount of greater than 0 to about 20 wt% on a dry weight basis.
[0100] 12. The resin composition of any one of items 1-11, wherein the at least one crosslinking agent is selected from tetrabromobisphenol A, tetrakis-DOPO-bisphenol A, and mixtures thereof.
[0101] 13. The resin composition of any one of items 1-12, comprising from about 0.01 to about 3.0 wt% on a dry weight basis of at least one azo-type catalyst.
[0102] 14. The resin composition according to any one of items 1 to 13, comprising a catalyst selected from azobisisobutyronitrile, 2-propylimidazole, tetrabutylphosphonium acetate, 2-methylimidazole, and combinations thereof.
[0103] 15. A resin composition comprising:
[0104] From about 5 to about 40 weight percent, based on the dry solvent-free resin, of a styrene maleic anhydride copolymer;
[0105] From about 10 to about 50 weight percent, based on the dry solvent-free resin, of at least one epoxy resin selected from the group consisting of brominated bisphenol A, brominated bisphenol F, non-brominated bisphenol A, non-brominated bisphenol F, and combinations thereof;
[0106] From about greater than 0 to about 20 wt % of at least one crosslinking agent, based on the dry solvent-free resin, the at least one crosslinking agent being selected from tetrabromobisphenol A, tetrakis-DOPO-bisphenol A, and mixtures thereof;
[0107] about 2.5 to about 15 wt % talc; and
[0108] About 2.5 to about 15 wt % fumed silica.
[0109] 16. The resin composition according to item 15, wherein the weight ratio of the fumed silica to talc is 1:2.5 to 5:1.
[0110] 17. The resin composition according to item 15, wherein the weight ratio of the fumed silica to talc is 1:1 to 2.5:1.
[0111] 18. The resin composition according to item 15, wherein the fumed silica is amorphous silanized fumed silica.
[0112] 19. The resin composition according to item 15, wherein the talc is silanized talc.
[0113] 20. The resin composition of item 15, wherein the crosslinking agent is a mixture of tetrabromobisphenol A and tetrakis-DOPO-bisphenol A.
[0114] 21. The resin composition of item 15, wherein the catalyst is tetrabutylphosphonium acetate.
[0115] 22. A prepreg comprising a reinforcing material impregnated with the resin composition according to any one of items 1 to 21.
[0116] 23. A laminate comprising a reinforcing material and the resin composition of any one of items 1 to 21, wherein the resin is C-staged.
[0117] 24. A resin coated copper foil comprising a copper foil sheet having a first planar surface and a second planar surface, wherein a layer of the resin of any one of items 1-21 is applied to at least one of the planar surfaces, and wherein the resin is B-staged or C-staged.
[0118] 25. The prepreg of clause 22, wherein the prepreg is incorporated into a printed circuit board, and wherein the printed circuit board does not delaminate in the area of the prepreg.
[0119] 26. The printed circuit board of item 25, wherein the IR 260°C reflow wicking is 40 microns or less. Example
[0120] Resins with a single talc filler (ISE-S4) and with a filler comprising silica and talc (ISE-S3) were prepared according to the following recipes. The resins were used to prepare prepregs and laminates, which included glass fabric impregnated with the same type of resin. The prepregs and laminates were then used to prepare 24-layer multilayer printed circuit test boards having the specifications listed in Table 3 below; various properties were then tested, including their ability to withstand delamination, their ability to withstand wicking, and their ability to withstand white glass cracking.
[0121] Table 3
[0122]
[0123] In Table 3, 1×2116RC57.8% refers to, for example, a prepreg with 1 layer of 2116 woven glass with a resin content (RC) of 57.8%. 4mil [2×106] H / H refers to a fully cured 4mm laminate made of 106 glass cloth with two resin coatings.
[0124] In addition to the two resins listed above, IS415, a commercially available SMA / epoxy prepreg (without any filler) was also used to prepare the test panels as described in Table 3 above.
[0125] The ISE-S3 resin has the formulation listed in Table 4 below.
[0126] Table 4
[0127]
[0128] Including optional latex binder - 1.7 wt%
[0129] UV Blocker - 0.02wt%
[0130] The printed circuit board under test is a test carrier, which includes:
[0131] ■Various pitch sizes and BGA designs;
[0132] ■24 layers, about 3mm thick, with 4 layers of 2oz copper;
[0133] ■The resin content is adjusted according to the density of both variants, with the goal of maintaining the same volume of resin;
[0134] The ISE-S4 resin has a similar formulation except that talc (11.6 wt%) is used throughout.
[0135] IS415 resin has a similar formulation except that the filler is omitted entirely.
[0136] The test results on the test carrier show that:
[0137] ■After 6×260℃ IR reflow, both ISE-S3 and ISE-S4 performed well in thermal performance.
[0138] However, ISE-S3 outperforms ISE-S4 in several important areas. ISE-S3 has:
[0139] ■Stronger resistance to delamination
[0140] ■Reduce white glass / crack
[0141] ■Higher Tg under T288
[0142] ■ISE-S4 exhibits interconnect defect ICD, while ISE-S3 does not have this defect.
[0143] The results of the mechanical, thermal and electrical tests performed on each of the three test panels are listed below in Tables 5-7.
[0144] Table 5
[0145]
[0146] Table 6
[0147]
[0148] Table 7
[0149]
[0150] Tables 6-7 detail the IR reflow test results at 260 degrees Celsius. IR Reflow Testing of Through-hole and Ball Grid Arrays (Infrared Reflow Soldering). Reflow testing showed that boards made with ISE-S3 prepreg and laminate exhibited consistently better wicking and white glass cracking results than boards made with IS415 and ISE-S4 prepreg and laminate.
[0151] It should be noted that wicking is a measure of how far the copper migrates into the glass strands adjacent to the plated through hole. Additionally, the "cracking" or "white glass" mentioned in the table above refers to the amount of separation (distance) between the epoxy system and the individual glass fibers. Cracking produces a silver or white sheen that flows down the individual glass fibers when viewed in cross-section with a microscope. The silver sheen is produced by air gaps around the individual glass fibers that reflect light.
[0152] Additionally, after the 6×IR reflow test at 260° C., the boards were cut open and their cross-sections observed to visually inspect for delamination, ie, areas where adjacent layers of prepreg or laminate had separated. The visual inspection results are reported in Table 8 below.
[0153] Table 8 - Layered inspection results
[0154]
[0155] BGA = Ball Grid Array
[0156] The results in Table 8 above indicate that boards made with laminates including the silica / talc filler combination did not exhibit delamination after reflow testing in BGA and thermal via applications.
[0157] Resins and articles containing resins have been described in detail above and with reference to the specific embodiments above; it will be apparent that modifications and variations may be made without departing from the scope of the present disclosure as defined in the appended claims. More specifically, although certain aspects of the present invention are considered herein to be particularly advantageous, it is contemplated that the present invention is not necessarily limited to these specific aspects of the present disclosure.
Claims
1. A resin composition comprising: 5 to 40 wt % of styrene maleic anhydride copolymer, based on dry solvent-free resin; 10 to 50 wt % of at least one epoxy resin, based on the dry solvent-free resin; the at least one epoxy resin is selected from brominated bisphenol A epoxy resin, brominated bisphenol F epoxy resin, non-brominated bisphenol A epoxy resin, non-brominated bisphenol F epoxy resin, and combinations thereof; greater than 0 to 20 wt % of at least one crosslinking agent, based on the dry solvent-free resin, the at least one crosslinking agent being selected from tetrabromobisphenol A, tetrakis-DOPO-bisphenol A, and mixtures thereof; Talc; wherein the talc is present in the resin composition in an amount of 5 to 25 wt% on a dry weight basis, and Silica, wherein the silica is present in the resin composition in an amount of 5 to 25 wt% on a dry weight basis.
2. The resin composition according to claim 1, wherein the silica is fused silica.
3. The resin composition according to claim 1, wherein the silicon dioxide is silanized silicon dioxide.
4. The resin composition according to claim 1 or 2, wherein the talc is silanized talc.
5. A prepreg comprising a reinforcing material impregnated with the resin composition according to any one of claims 1 to 4.
6. A laminate comprising a reinforcing material and the resin composition of any one of claims 1 to 4, wherein the resin is C-staged.
7. A resin coated copper foil comprising a copper foil sheet having a first planar surface and a second planar surface, wherein a layer of the resin composition of any one of claims 1 to 4 is applied to at least one of the planar surfaces, and wherein the resin is B-staged or C-staged.
Citation Information
Patent Citations
Flame retardant phosphorus element-containing epoxy resin compositions
US6645631B2
Flame retardant compositions
US7687556B2
Flame retardant compositions with a phosphorated compound
US8129456B2
Thermosetting resin composition and prepreg and laminate for printed circuits thereby
CN101643571A
Halogen-free fire resistance epoxy resin composite as well as prepreg material and printed circuit board therefrom
CN102250447A