Hydroquinone molecular imprinting photoelectrochemical sensor, preparation method and application thereof
By using molecular imprinted photoelectrochemical sensor based on the heterostructure of CdS nanoparticles/ZnIn2S4 nanosheets in hydroquinone detection, the sensitivity and response speed of hydroquinone detection in the prior art were solved, and high sensitivity and Highly accurate detection effect, suitable for rapid online detection of water bodies.
Patent Information
- Application Number
- CN202210972496.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-08-15
AI Technical Summary
The existing hydroquinone detection technology has the problems of high instrument cost, complex operation, slow response speed and low sensitivity, which cannot meet the actual use needs, especially the technical gap in high sensitivity detection for hydroquinone.
Using a molecular imprinted photoelectrochemical sensor based on visible light-driven heterostructure of CdS nanoparticles/ZnIn2S4 nanosheets, CdS nanoparticles/ZnIn2S4 nanosheets was prepared by hydrothermal synthesis, and molecular imprinted polymerization was modified on glass carbon electrodes by electropolymerization. The film layer forms a specific detection layer to achieve high sensitivity detection of hydroquinone.
The specific detection of hydroquinone is realized, with a wide response range and low detection limit, which is convenient to operate and high sensitivity. It is suitable for rapid online detection of water bodies, with a detection limit of 0.7nmol/L, meeting field analysis in the field Requirements and improve detection accuracy and accuracy.
Smart Images

Figure CN115343339B_ABST
Abstract
Description
Technical Field
[0001] The disclosed embodiments relate to the field of chemistry, and in particular to a hydroquinone molecular imprinting photoelectrochemical sensor, a preparation method thereof, and applications thereof. Background Art
[0002] Hydroquinone, also known as hydroquinone, is a derivative of the benzene molecule in which two hydrogen atoms 1 and 4 are replaced by two hydroxyl groups. It is widely used in photographic film developers, azo dyes, inhibitors, rubber antioxidants and synthetic cosmetics. Hydroquinone is also a decolorizing drug that can treat pigmented skin problems and has important applications in the medical field. However, hydroquinone is highly toxic, and trace amounts of hydroquinone will have adverse effects on the human body. When the human body ingests more than 1g, symptoms such as pale complexion, tinnitus and headache will appear. In severe cases, symptoms such as collapse, respiratory failure or coma will also occur. In addition, hydroquinone has low biodegradability in the environment. During production and use, it will be dispersed in soil and water bodies, causing pollution to water sources and groundwater, and causing irreversible effects on ecosystems and human health. Therefore, the specific detection of hydroquinone is of great significance.
[0003] In current technology, traditional detection technologies such as spectroscopy, high performance liquid chromatography, and capillary electrophoresis are usually used for detection. However, these methods have high instrument costs, complex operations, slow response speeds, and relatively low detection sensitivity and width, which cannot meet actual use needs.
[0004] In recent years, there are also methods for detecting molecular imprinting using photoelectrochemistry. Compared with traditional detection technologies such as spectroscopy, high performance liquid chromatography, and capillary electrophoresis, photoelectrochemical detection has the advantages of low instrument cost, simple operation, fast response, and easy miniaturization, which can meet the requirements of field analysis. However, there has always been a technical gap in the use of photoelectrochemical sensors with specific structures and compositions to detect molecular imprinting of hydroquinone with high sensitivity. Summary of the invention
[0005] The purpose of the present disclosure is to provide a hydroquinone molecular imprinting photoelectrochemical sensor based on a visible light driven CdS nanoparticle / ZnIn2S4 nanosheet heterostructure, and a preparation method and application thereof, so as to at least partially solve the problems existing in the current technology.
[0006] According to the first aspect of the present disclosure, the embodiment of the present disclosure provides a hydroquinone molecular imprinting photoelectrochemical sensor. The sensor includes a reference electrode, an auxiliary electrode and a working electrode, wherein the reference electrode, the auxiliary electrode and the working electrode form a three-electrode system, wherein the working electrode is a molecular imprinting modified electrode, and the molecular imprinting modified electrode includes a conductive substrate, a composite material loaded on the conductive substrate and a molecular imprinting polymer film layer; wherein the conductive substrate is an L-shaped glassy carbon electrode, the composite material is a CdS nanoparticle / ZnIn2S4 nanosheet heterostructure, and the molecular imprinting polymer film layer is prepared by an electropolymerization-elution method.
[0007] In some embodiments, the composite material is a CdS nanoparticle / ZnIn2S4 nanosheet heterostructure, which is a non-ion-doped heterostructure. In such an embodiment, detection errors caused by redundant doping ions can be avoided, thereby improving the precision and accuracy of detection.
[0008] According to a second aspect of the present disclosure, a method for preparing a hydroquinone molecular imprinting photoelectrochemical sensor according to the first aspect of the present disclosure is provided, the preparation method comprising the following steps:
[0009] S1. Determine the band structure of CdS nanoparticles and ZnIn2S4 nanosheets;
[0010] S2, preparing a CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material through hydrothermal synthesis, and vacuum drying the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material and sealing and storing it for later use;
[0011] S3, cleaning the glassy carbon electrode with acetone, ethanol, and ultrapure water ultrasonically in sequence, and drying it with nitrogen for later use;
[0012] S4, dispersing the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material prepared in step S2 in deionized water to obtain a uniform dispersion, taking 10 μL of the uniform dispersion and 10 μL of nafion solution to coat the surface of the glassy carbon electrode cleaned in step S3, and drying at room temperature to obtain the glassy carbon electrode modified with a CdS / ZnIn2S4 photoelectric conversion layer;
[0013] S5. Place the glassy carbon electrode modified with the CdS / ZnIn2S4 photoelectric conversion layer obtained in step S4 in a molecular imprinting polymerization solution containing hydroquinone, prepare the molecular imprinting polymer by an electropolymerization method, so that the molecular imprinting polymer is in situ modified on the surface of the glassy carbon electrode modified with the CdS / ZnIn2S4 photoelectric conversion layer to form a molecular imprinting polymer film layer, and use acetic acid eluent and ethanol eluent to elute the hydroquinone template molecules to obtain a glassy carbon electrode modified with a molecular imprinting polymer MI-CdS / ZnIn2S4 / GCE, and connect the glassy carbon electrode modified with the molecular imprinting polymer film layer as a working electrode to a photoelectrochemical sensing system to obtain the molecular imprinting photoelectrochemical sensor based on the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material.
[0014] In some embodiments, determining the band structure of CdS nanoparticles and ZnIn2S4 nanosheets in step S1 may include: combining the optical band gap Eg of CdS and ZnIn2S4 with the geometric mean of the absolute electronegativity of each atom in the semiconductor, calculating the positions of the conduction band and valence band of the semiconductor, and designing a heterostructure with matching band gaps.
[0015] In some embodiments, the energy band structures of the CdS nanoparticles and the ZnIn2S4 nanosheets determined in step S1 can be obtained by photoelectric characterization testing and calculation, specifically including:
[0016] The light absorption characteristics and optical band gap of CdS nanoparticles and ZnIn2S4 nanosheets can be obtained by UV-vis diffuse reflectance spectroscopy (DRS) testing. According to the relationship between Eg and incident photon energy hν: αhν=K(hν-Eg) n The optical band gap Eg of CdS and ZnIn2S4 can be calculated; and
[0017] Based on the following equation, the positions of the conduction band (CB) and valence band (VB) of the semiconductor are obtained by combining the optical band gap Eg of CdS and ZnIn2S4 with the geometric mean of the absolute electronegativity of each atom in the semiconductor, and a heterostructure with matching energy band gap is designed:
[0018] E VB =X–E0+0.5Eg;
[0019] E CB =E VB – Eg;
[0020] Where: E0 is a constant, which is the electron energy relative to the standard hydrogen electrode, E 0 =4.5eV; Eg is the band gap of the semiconductor, and X is the geometric mean of the absolute electronegativity of each atom in the semiconductor.
[0021] In some embodiments, in step S4, dispersing the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material prepared in step S2 in deionized water to obtain a uniform dispersion may include: dispersing the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material prepared in step S2 in deionized water, and ultrasonically cleaning with an ultrasonic cleaner to obtain a uniform CdS nanoparticle / ZnIn2S4 nanosheet heterostructure dispersion, wherein the concentration of the uniform CdS nanoparticle / ZnIn2S4 nanosheet heterostructure dispersion is 1 to 10 mg / mL.
[0022] In some embodiments, the specific steps of obtaining the glassy carbon electrode modified with the CdS / ZnIn2S4 photoelectric conversion layer in step S4 may include: dispersing the CdS / ZnIn2S4 composite material in deionized water to obtain a dispersion with a concentration of 1 to 10 mg / mL, measuring 10 μL of the dispersion with a pipette and coating it on the cleaned electrode surface, drying at room temperature, and then measuring 10 μL of nafion solution again and coating it on the modified electrode surface, and obtaining a CdS / ZnIn2S4 composite material modified electrode after drying at room temperature.
[0023] In some embodiments, the preparation of CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material in step S2 may include: dispersing ZnIn2S4 nanosheets in an aqueous solution, adding hexadecyltrimethylammonium bromide, CdCl2 and thiourea and stirring evenly to form a mixed solution, and then transferring it to a polytetrafluoroethylene-lined high-pressure reactor, sealing it and reacting it at 120°C to 140°C; and after it is naturally cooled to room temperature, centrifuging the dispersion, washing it with water and anhydrous ethanol several times in turn, and placing the precipitate in a vacuum drying oven to dry it, and grinding it to obtain the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material.
[0024] In some embodiments, the molar ratio of ZnIn2S4, CdCl2 and thiourea is 1:5:15, and the ratio of the mass of hexadecyltrimethylammonium bromide to the sum of the mass of ZnIn2S4 and CdCl2 is 2% to 5%:1; the sealed and reacted at 120°C to 140°C for 2 to 4 hours, and the precipitate is placed in a vacuum drying oven at a drying temperature of 60°C for 12 hours.
[0025] In some embodiments, the preparation of ZnIn2S4 nanosheets and CdS nanoparticles includes the following steps: using a hydrothermal synthesis method, ZnCl2, InCl3, hexadecyltrimethylammonium bromide and thiourea are added to a mixture of ethylene glycol and water, stirred evenly, heated at 180°C to 210°C for 24 to 36 hours, centrifuged after cooling, washed several times with water and anhydrous ethanol, and vacuum dried at 60°C for 12 hours, and then ground to obtain ZnIn2S4 nanosheets.
[0026] In some embodiments, hydrothermal synthesis may include adding ZnCl2 and InCl3 to a mixture of ethylene glycol and water, stirring to fully dissolve them, then adding hexadecyltrimethylammonium bromide and stirring evenly, and finally adding thiourea and stirring thoroughly; wherein the molar ratio of ZnCl2, InCl3 and thiourea is 1:2:6, and the ratio of the mass of hexadecyltrimethylammonium bromide to the sum of the mass of ZnCl2 and InCl3 is 2% to 5%:1; and using a hydrothermal synthesis method, CdCl2, hexadecyltrimethylammonium bromide and thiourea are added to ultrapure water, stirred evenly, heated at 120°C to 140°C for 2 to 4 hours, centrifuged after cooling, washed several times with water and anhydrous ethanol, and vacuum dried at 60°C for 12 hours, and then ground to obtain CdS nanoparticles.
[0027] In some embodiments, hydrothermal synthesis may include: adding CdCl2 to ultrapure water, stirring to fully dissolve it, then adding hexadecyltrimethylammonium bromide and stirring evenly, and finally adding thiourea and stirring thoroughly; wherein the molar ratio of CdCl2 and thiourea is 1:3, and the ratio of the mass of hexadecyltrimethylammonium bromide to the mass of CdCl2 is 2% to 5%:1.
[0028] In some embodiments, the concentration of the molecular imprinting polymer solution in step S5 can be a PBS buffer solution containing 0.1-1.0 M phenylenediamine and 1-3 mM hydroquinone.
[0029] In some embodiments, the electropolymerization method in S5 may include: using the modified electrode coated with the photoelectric conversion layer as the working electrode, the platinum sheet as the counter electrode, and Ag / AgCl as the reference electrode, performing electrochemical cyclic voltammetry electropolymerization on a CHI660e workstation, and forming a molecular imprinting polymer film layer by electropolymerization, and then eluting the template molecules using acetic acid and ethanol solutions respectively.
[0030] In some embodiments, the molecular imprinting polymerization solution of hydroquinone in step S5 is a PBS buffer solution with a concentration of 0.1-1.0M phenylenediamine and 1-3mM hydroquinone; and / or the scanning voltage of the electropolymerization method is -0.2-0.8V, the scanning speed is 50mv / s, and the number of scanning circles is 10-30 circles; the concentration of the acetic acid eluent is 5%; and the time for acetic acid and ethanol to elute the template molecule hydroquinone is 10-20 minutes respectively. That is, the time for acetic acid to elute the template molecule hydroquinone is 10-20 minutes, and the time for ethanol to elute the template molecule hydroquinone is also 10-20 minutes.
[0031] According to a third aspect of the present disclosure, an application of a hydroquinone molecular imprinting photoelectrochemical sensor prepared according to the first aspect of the present disclosure or according to the second aspect of the present disclosure is provided, and the sensor is applied to the detection of hydroquinone.
[0032] In some embodiments, the detecting comprises the steps of:
[0033] S1. Incubation of molecular imprinting photoelectrochemical sensor: preparing hydroquinone standard solutions of different concentrations, and immersing the molecular imprinting photoelectrode in the hydroquinone standard solutions of different concentrations for incubation;
[0034] S2. Detecting the electrical signal of the photoelectrochemical sensor for hydroquinone: using an Ag / AgCl electrode as a reference electrode, a platinum electrode as an auxiliary electrode, and the prepared MI-CdS / ZnIn2S4 / GCE with molecular imprinting function as a working electrode to form a three-electrode system, connected to a photoelectrochemical detection device, using IT testing means, and drawing a working curve based on the relationship between the obtained photocurrent value and the concentration of the hydroquinone standard solution; and
[0035] S3. Determine the content of hydroquinone: replace the hydroquinone standard solution with the sample to be tested, and use the IT test method in the same way. Compare the intensity value of the response signal with the working curve to obtain the content of hydroquinone in the sample to be tested.
[0036] In some embodiments, the incubation time in step S1 is 10 to 20 minutes.
[0037] The various embodiments of the present disclosure can at least achieve the following beneficial effects:
[0038] 1. The present invention combines molecular imprinting with photoelectrochemistry, uses CdS / ZnIn2S4 composite material as the photoelectric conversion layer, and modifies the surface with molecular imprinting containing hydroquinone recognition sites to achieve specific detection of hydroquinone. It can be detected in the concentration range of 1 to 100 nmol / L, has a wide response range and a low detection limit, and is easy to operate, highly sensitive, has a stable response and high selectivity. It can be suitable for rapid online detection of water bodies, and provides a new method for rapid online detection of hydroquinone.
[0039] 2. The photoelectrochemical analysis method disclosed in the present invention realizes the detection of hydroquinone. The instrument has a fast signal response and high sensitivity. Its detection limit reaches 0.7nmol / L. In addition, the instrument is easy to carry and simple to operate, which can meet the analysis requirements of special occasions such as field sites.
[0040] 3. The present disclosure combines molecular imprinting technology with photoelectrochemical analysis methods, making full use of the material appearances of CdS and ZnIn2S4, which are nanoparticles and nanosheets, respectively. By fully combining CdS and ZnIn2S4, a reasonable composite photoelectric conversion layer is designed. In addition to effectively preventing the recombination of photogenerated electrons and hole pairs, the composite photoelectric conversion layer also serves the purpose of enriching analytes. And the composite photoelectric conversion layer with a specific structural appearance can be effectively applied to the detection of hydroquinone, making the detection accuracy and results significantly better than the current methods.
[0041] 4. The CdS / ZnIn2S4 composite material disclosed in the present invention can be prepared without ion doping, thereby avoiding detection errors caused by the adverse effects of doped ions on electrodes, improving the precision and accuracy of detection, and further expanding the detection limit.
[0042] 5. The hydroquinone molecular imprinting photoelectrochemical sensor prepared in the present invention adopts an electrodeposition method to obtain a molecular imprinting film, which is simple and easy to operate; at the same time, the bias voltage used in the photoelectric test is relatively low, which is conducive to protecting the sensor and signal stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0044] Figure 1 This is an X-ray diffraction pattern of the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure prepared in Example 1 of the present disclosure;
[0045] Figure 2 The SEM image and TEM image of the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure prepared in Example 2 of the present disclosure;
[0046] Figure 3 The energy band position of the heterostructure and the composition of the heterostructure of the exemplary embodiment 3 of the present disclosure;
[0047] Figure 4 A comparison diagram of the photoelectric response of a molecularly imprinted photoelectrochemical sensor of a CdS nanoparticle / ZnIn2S4 nanosheet heterostructure prepared in Example 4 of the present disclosure;
[0048] Figure 5This is a selectivity test diagram of the hydroquinone molecular imprinting photoelectrochemical sensor prepared in Example 5 of the present disclosure, where the concentration of hydroquinone is 0.1 μmol·L -1 , the concentration of other interfering substances was 1 μmol·L -1 ;
[0049] Figure 6 The photocurrent response diagram and the corresponding linear relationship diagram of the photoelectrochemical sensor prepared by the exemplary embodiment 6 of the present disclosure for detecting hydroquinone, wherein the concentration of hydroquinone is 1 nmol·L -1 , 3nmol·L -1 , 5nmol·L -1 , 8nmol·L -1 , 10nmol·L -1 、30nmol·L -1 , 50nmol·L -1 、80nmol·L -1 , 100nmol·L -1 . DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings in the embodiments of the present disclosure. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.
[0051] The purpose of the present disclosure is to provide a molecular imprinting photoelectrochemical sensor for hydroquinone based on a visible light driven CdS nanoparticle / ZnIn2S4 nanosheet heterostructure, and its preparation method and application. In order to improve the performance of the photoelectrochemical sensor, the present disclosure selects a heterostructure with a matching energy band structure as a photoelectric conversion layer through photoelectric characterization testing and calculation to accelerate the separation of photogenerated electrons and holes; on the other hand, the molecular imprinting technology is combined with photoelectrochemistry to improve the sensor's selectivity for hydroquinone, thereby achieving high-sensitivity detection. Based on the above research ideas, the present disclosure is directed to an ultra-sensitive analytical detection of hydroquinone-a molecular imprinting photoelectrochemical sensor based on a CdS nanoparticle / ZnIn2S4 nanosheet heterostructure is prepared. The sensor according to the present disclosure can simply and quickly realize the detection of a wide range of hydroquinone, and the scheme has sensitive detection and high detection accuracy.
[0052] The preparation method of the hydroquinone molecular imprinting photoelectrochemical sensor disclosed in the present invention may include the following steps: S1, determining the energy band structure of CdS nanoparticles and ZnIn2S4 nanosheets; S2, preparing CdS nanoparticles / ZnIn2S4 nanosheets heterostructure composite materials by hydrothermal synthesis, and vacuum drying the CdS nanoparticles / ZnIn2S4 nanosheets heterostructure composite materials and sealing and storing them for later use; S3, cleaning the glassy carbon electrode by ultrasonic washing with acetone, ethanol, and ultrapure water in sequence, and drying it with nitrogen for later use; S4, dispersing the CdS nanoparticles / ZnIn2S4 nanosheets heterostructure composite materials prepared in step S2 in deionized water to obtain a uniform dispersion, taking 10 μL of the uniform dispersion and 10 μL of The nafion solution is coated on the surface of the glassy carbon electrode cleaned in step S3, and dried at room temperature to obtain the glassy carbon electrode modified with a CdS / ZnIn2S4 photoelectric conversion layer; S5, the glassy carbon electrode modified with a CdS / ZnIn2S4 photoelectric conversion layer obtained in step S4 is placed in a molecular imprinting polymerization solution containing hydroquinone, and a molecular imprinting polymer is prepared by an electropolymerization method, so that the molecular imprinting polymer is in situ modified on the surface of the glassy carbon electrode modified with the CdS / ZnIn2S4 photoelectric conversion layer to form a molecular imprinting polymer film layer, and the hydroquinone template molecules are eluted with acetic acid eluent and ethanol eluent to obtain a glassy carbon electrode modified with a molecular imprinting polymer MI-CdS / ZnIn2S4 / GCE, and the glassy carbon electrode modified with the molecular imprinting polymer film layer is connected as a working electrode to a photoelectrochemical sensing system to obtain the molecular imprinting photoelectrochemical sensor based on the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material.
[0053] In combination with the attached embodiment of the present disclosure Figures 1 to 6 , used for preferred embodiments and drawings with detailed description.
[0054] Example 1
[0055] Example 1 provides an exemplary method for preparing ZnIn2S4 nanosheets, CdS nanoparticles, and CdS nanoparticle / ZnIn2S4 nanosheet heterostructures, respectively.
[0056] In this embodiment, ZnIn2S4 nanosheets can be prepared by the following method:
[0057] Using the solvent thermal synthesis method, ZnCl2 and InCl3 are first added to a mixture of ethylene glycol and water, stirred to fully dissolve, and then the surfactant hexadecyl trimethyl ammonium bromide is added and stirred evenly, and finally thiourea is added and stirred fully, and then transferred to a polytetrafluoroethylene-lined autoclave, heated at 180°C for 24 hours, centrifuged after cooling, washed with water and anhydrous ethanol several times, and vacuum dried at 60°C for 12 hours, and then ground to obtain ZnIn2S4 nanosheets. Among them, the volume ratio of ethylene glycol to water is 3:1, the molar ratio of ZnCl2, InCl3 and thiourea is 1:2:6, and the ratio of the mass of hexadecyl trimethyl ammonium bromide to the mass sum of ZnCl2 and InCl3 is 2%:1.
[0058] In this embodiment, CdS nanoparticles can be prepared by the following method:
[0059] The hydrothermal synthesis method is adopted. First, CdCl2 is added to ultrapure water, stirred to fully dissolve, and then the surfactant hexadecyl trimethyl ammonium bromide is added and stirred evenly. Finally, thiourea is added and stirred thoroughly, and then transferred to a polytetrafluoroethylene-lined autoclave, heated at 120°C for 2h, centrifuged after cooling, washed with water and anhydrous ethanol for 3 times, and vacuum dried at 60°C for 12h, and then ground to obtain CdS nanoparticles. Among them, the molar ratio of CdCl2 and thiourea is 1:3, and the mass ratio of hexadecyl trimethyl ammonium bromide to the mass of CdCl2 is 2%:1.
[0060] In this embodiment, further, the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure can be prepared by the following method:
[0061] The ZnIn2S4 nanosheets were dispersed in ultrapure water by hydrothermal synthesis, a certain amount of surfactant hexadecyl trimethyl ammonium bromide was added, stirred to fully dissolve, CdCl2 was added to mix well, and finally thiourea was added to mix well to form a mixed solution and transferred to a polytetrafluoroethylene lined autoclave, heated at 120°C for 2h, cooled naturally to room temperature, centrifuged, washed with water and anhydrous ethanol several times in turn, and vacuum dried at 60°C for 12h, and then ground to obtain a CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material. Among them, the molar ratio of ZnIn2S4, CdCl2 and thiourea is 1:5:15, and the mass ratio of hexadecyl trimethyl ammonium bromide to the mass sum of ZnIn2S4 and CdCl2 is 2%:1.
[0062] Figure 1It is the X-ray diffraction pattern (XRD) of three materials of ZnIn2S4 nanosheet, CdS nanoparticle and CdS nanoparticle / ZnIn2S4 nanosheet heterostructure prepared in this embodiment 1. As can be seen from the figure, ZnIn2S4 nanosheet and CdS nanoparticle have good crystallinity, and their XRD patterns correspond to the patterns of ZnIn2S4 (JCPDS: 65-2023) with hexagonal phase structure and CdS (JCPDS: 65-3414) with cubic sphalerite structure. In the XRD pattern of CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material, the characteristic diffraction peaks of ZnIn2S4 and CdS can be seen, but the diffraction peak intensity has a certain reduction, which is due to the insertion of CdS nanoparticles destroying the crystal form of ZnIn2S4 nanosheet and making its diffraction peak relatively widened and shorter. These information show the successful preparation of heterostructure, and the composite material is not simply mixed.
[0063] Example 2
[0064] Example 2 provides another exemplary method for preparing ZnIn2S4 nanosheets and CdS nanoparticles / ZnIn2S4 nanosheet heterostructures, respectively.
[0065] In this embodiment, ZnIn2S4 nanosheets can be prepared by the following method:
[0066] Using the solvent thermal synthesis method, ZnCl2 and InCl3 are first added to a mixture of ethylene glycol and water, stirred to fully dissolve, and then the surfactant hexadecyl trimethyl ammonium bromide is added and stirred evenly, and finally thiourea is added and stirred fully, and then transferred to a polytetrafluoroethylene-lined autoclave, heated at 210°C for 24 hours, centrifuged after cooling, washed with water and anhydrous ethanol several times, and vacuum dried at 60°C for 12 hours, and then ground to obtain ZnIn2S4 nanosheets. Among them, the volume ratio of ethylene glycol to water is 2:1, the molar ratio of ZnCl2, InCl3 and thiourea is 1:2:6, and the ratio of the mass of hexadecyl trimethyl ammonium bromide to the mass sum of ZnCl2 and InCl3 is 5%:1.
[0067] In this embodiment, the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure can be prepared by the following method:
[0068] The ZnIn2S4 nanosheets were dispersed in ultrapure water by hydrothermal synthesis, a certain amount of surfactant hexadecyl trimethyl ammonium bromide was added, stirred to fully dissolve, CdCl2 was added to mix well, and finally thiourea was added to stir well to form a mixed solution and transferred to a polytetrafluoroethylene lined autoclave, heated at 140°C for 2h, cooled naturally to room temperature, centrifuged, washed with water and anhydrous ethanol several times, and vacuum dried at 60°C for 12h, and then ground to obtain a CdS nanoparticle / ZnIn2S4 nanosheet heterostructure composite material. Among them, the molar ratio of ZnIn2S4, CdCl2 and thiourea is 1:5:15, and the mass ratio of hexadecyl trimethyl ammonium bromide to the mass sum of ZnIn2S4 and CdCl2 is 5%:1.
[0069] Figure 2 These are the scanning electron microscope (SEM) and transmission electron microscope (TEM) images of the ZnIn2S4 nanosheets and CdS nanoparticle / ZnIn2S4 nanosheet heterostructures prepared in Example 2. Figure 2 a and Figure 2 b are the SEM and TEM images of ZnIn2S4 nanosheets, respectively, showing the lamellar structure of ZnIn2S4; Figure 2 c and Figure 2 d are the SEM and TEM images of the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure, respectively. It can be seen that small granular CdS is loaded on the ZnIn2S4 nanosheets. The ZnIn2S4 nanosheets with a large specific surface area provide a large number of attachment sites for the loading of CdS particles, which is more conducive to the formation of a heterostructure.
[0070] Example 3
[0071] The CdS nanoparticles and ZnIn2S4 nanosheets prepared in Example 1 were subjected to UV-vis diffuse reflectance spectroscopy (DRS) testing to obtain the light absorption characteristics and optical band gap of the CdS nanoparticles and ZnIn2S4 nanosheets. According to the relationship between Eg and the incident photon energy hv: αhv = K(hv-Eg) n The optical band gaps Eg of CdS and ZnIn2S4 can be calculated to be 2.32eV and 2.58eV respectively. Secondly, according to the equation:
[0072] E VB =X–E0+0.5Eg
[0073] E CB =E VB -Eg
[0074] Where: E0 is a constant, which is the electron energy relative to the standard hydrogen electrode, E 0=4.5eV; Eg is the bandgap width of the semiconductor; X is the geometric mean of the absolute electronegativity of each atom in the semiconductor. Finally, combining the optical band gap Eg of CdS and ZnIn2S4 with the geometric mean of the absolute electronegativity of each atom in the semiconductor, the positions of the conduction band (CB) and valence band (VB) of the semiconductor can be calculated. From the above levels, the CB and VB of CdS can be calculated as -0.48 and 1.84eV, respectively, and the CB and VB of ZnIn2S4 can be calculated as -0.92 and 1.66eV, respectively. Figure 3 The heterostructure shown. In the CdS / ZnIn2S4 heterostructure, both ZnIn2S4 and CdS are excited to generate photogenerated electrons and holes under visible light irradiation. Since the CB of ZnIn2S4 is more negative than that of CdS, and the VB of CdS is more positive than that of ZnIn2S4, ZnIn2S4 / CdS constructs a type II heterojunction. During the photoelectrocatalytic reaction, the photogenerated electrons in the CB of ZnIn2S4 are rapidly transferred to the CB of CdS, while the holes in the VB of CdS can be transferred to the VB of ZnIn2S4, realizing the separation and transfer of photogenerated electrons and holes.
[0075] Example 4
[0076] Heterostructure modified electrodes can be prepared by the following methods:
[0077] The CdS nanoparticles, ZnIn2S4 nanosheets and ZnIn2S4 composite materials prepared in Example 1 were respectively dispersed in deionized water to obtain a dispersion with a concentration of 1 mg / mL. 10 μL of the dispersion was measured with a pipette and coated on the cleaned surface of the L-type GCE electrode. After drying at room temperature, 10 μL of nafion solution was measured again and coated on the surface of the modified electrode. After drying at room temperature, modified electrodes were obtained, which were named CdS / GCE, ZnIn2S4 / GCE, and CdS / ZnIn2S4 / GCE, respectively.
[0078] Furthermore, the preparation method of the molecular imprinting photoelectrochemical sensor of the CdS nanoparticle / ZnIn2S4 nanosheet heterostructure is as follows:
[0079] The modified electrode (CdS / ZnIn2S4 / GCE) with CdS nanoparticles / ZnIn2S4 nanosheet heterostructure photoelectric material was used as the working electrode, platinum sheet as the counter electrode, Ag / AgCl as the reference electrode, and the electrolyte was a PBS buffer solution with a concentration of 0.1M phenylenediamine and 3mM hydroquinone. The three-electrode system was assembled and electrochemical cyclic voltammetry electropolymerization was performed on the CHI660e workstation. The electrochemical cyclic voltammetry electropolymerization parameters can be: scanning voltage of -0.2 to 0.8V, scanning speed of 50mV / s, and 10 cycles of scanning. The molecular imprinting polymer film layer was formed by electropolymerization, and then the template molecules were eluted by soaking in 5% acetic acid and ethanol solutions for 10 minutes respectively. Finally, the modified electrode prepared was named MI-CdS / ZnIn2S4 / GCE.
[0080] Furthermore, the concentration was 100 nmol·L -1 The prepared CdS / GCE, ZnIn2S4 / GCE, CdS / ZnIn2S4 / GCE and MI-CdS / ZnIn2S4 / GCE modified electrodes were immersed in the PBS blank solution and the hydroquinone PBS target solution for incubation for 15 min. Then, the Ag / AgCl electrode was used as the reference electrode, the platinum sheet electrode was used as the auxiliary electrode, and the prepared modified electrode formed a three-electrode system, which was connected to the photoelectrochemical detection device, and the photoelectric signal was recorded by IT testing.
[0081] Figure 4 The photocurrent diagrams of CdS / GCE, ZnIn2S4 / GCE, CdS / ZnIn2S4 / GCE and MI-CdS / ZnIn2S4 / GCE electrodes prepared in Example 4 in hydroquinone PBS target solution and PBS blank solution. It can be seen that the photocurrent of all electrodes in the hydroquinone target solution is significantly increased relative to the blank PBS, which may be due to the fact that the photogenerated holes generated by the photoelectrode are consumed to oxidize hydroquinone, thereby hindering the recombination of photogenerated electrons and holes, accelerating the transfer of photogenerated electrons, and generating increased photocurrent. Among them, the photocurrent generated by CdS / ZnIn2S4 / GCE is significantly increased compared to that of simple CdS / GCE and ZnIn2S4 / GCE, indicating that the formation of the CdS / ZnIn2S4 heterostructure is conducive to the transfer and separation of photogenerated electrons and holes. After the formation of molecular imprinting, MI-CdS / ZnIn2S4 / GCE has the ability to quickly recognize hydroquinone, which accelerates the utilization of photogenerated holes and generates a larger photocurrent.
[0082] Example 5
[0083] PBS target solutions and PBS blank solutions of different phenolic substances were prepared: hydroquinone (HQ), catechol (CC), resorcinol (RC), bisphenol B (BPB), bisphenol S (BPS) and bisphenol A (BPA). The concentration of HQ was 0.1 μmol·L -1 , the concentration of other phenols was 1 μmol·L -1 ; The MI-CdS / ZnIn2S4 / GCE modified electrode prepared in Example 4 was immersed in a PBS blank solution and a PBS target solution of different phenolic substances for incubation for 15 minutes. Then, an Ag / AgCl electrode was used as a reference electrode, a platinum sheet electrode was used as an auxiliary electrode, and the prepared modified electrode formed a three-electrode system, which was connected to a photoelectrochemical detection device, and the photoelectric signal was recorded by IT testing.
[0084] Figure 5 This is a test diagram of the selectivity of the MI-CdS / ZnIn2S4 / GCE electrode to hydroquinone prepared in Example 4. As can be seen from the figure, the photoelectric response of different interferents in this photoelectrochemical sensor is very small, and it can be considered that the presence of these interferents has little effect on the test of hydroquinone, which can explain that the prepared molecular imprinting photoelectrochemical sensor for hydroquinone has high selectivity and strong anti-interference ability, and can achieve selective detection of hydroquinone.
[0085] Example 6
[0086] Prepare the concentrations of 1 nmol·L -1 , 3nmol·L -1 , 5nmol·L -1 , 8nmol·L -1 , 10nmol·L -1 、30nmol·L -1 , 50nmol·L -1 、80nmol·L -1 , 100nmol·L -1 The MI-CdS / ZnIn2S4 / GCE modified electrode prepared in Example 4 was immersed in PBS blank solution and PBS target solution of different concentrations of hydroquinone for incubation for 15 minutes. Then, the Ag / AgCl electrode was used as the reference electrode, the platinum sheet electrode was used as the auxiliary electrode, and the prepared modified electrode formed a three-electrode system, which was connected to the photoelectrochemical detection device, and the photoelectric signal was recorded by IT testing.
[0087] Figure 6a is the photocurrent response diagram of MI-CdS / ZnIn2S4 / GCE prepared in Example 4 to different concentrations of hydroquinone, Figure 6 b is a linear graph of different concentrations and photocurrents. It can be seen from the figure that as the concentration of hydroquinone increases, the photocurrent gradually increases. The corresponding linear relationship is also very good, I = 0.66 + 0.072 × C (nmol·L -1 ), R 2 The detection limit was 0.7 nmol·L -1 .
[0088] In summary, the present disclosure provides a molecular imprinting photoelectrochemical sensor based on a visible light-driven CdS nanoparticle / ZnIn2S4 nanosheet heterostructure, and its preparation and application. The present disclosure uses a CdS nanoparticle / ZnIn2S4 nanosheet heterostructure as a photoelectric conversion layer, and modifies a molecular imprinting membrane capable of recognizing hydroquinone through electropolymerization technology to achieve analytical detection of hydroquinone. The various embodiments of the present disclosure can at least have the following beneficial technical effects that are superior to the prior art: The present disclosure combines molecular imprinting with photoelectrochemistry, uses a CdS / ZnIn2S4 composite material as a photoelectric conversion layer, and modifies the surface with a molecular imprint containing a hydroquinone recognition site to achieve specific detection of hydroquinone, and can detect in a concentration range of 1 to 100 nmol / L, has a wide response range and a low detection limit, and is easy to operate, highly sensitive, stable in response, and highly selective, and can be applied to rapid online detection of water bodies, providing a new method for rapid online detection of hydroquinone. The instrument has a fast signal response and high sensitivity, with a detection limit of 0.7 nmol / L. The instrument is easy to carry and simple to operate, and can meet the analysis requirements of special occasions such as field sites. The molecular imprinting technology is combined with the photoelectrochemical analysis method, and the material appearances of CdS and ZnIn2S4, which are nanoparticles and nanosheets respectively, are fully utilized. By fully combining CdS and ZnIn2S4, a reasonable composite material photoelectric conversion layer is designed. In addition to effectively preventing the recombination of photogenerated electrons and hole pairs, the composite material photoelectric conversion layer also serves the purpose of enriching the analyte. Moreover, the photoelectric conversion layer of the composite material with a specific structural appearance can be effectively applied to the detection of hydroquinone, making the detection accuracy and results significantly better than the current methods; the CdS / ZnIn2S4 composite material can avoid the detection error caused by the adverse effects of doped ions on the electrodes without ion doping, thereby improving the detection accuracy and precision and further expanding the detection limit; the hydroquinone molecular imprinting photoelectrochemical sensor adopts an electrodeposition method to obtain a molecular imprinting film, which is simple and easy to operate; at the same time, the bias voltage used in the photoelectric test is relatively low, which is conducive to protecting the sensor and the stability of the signal.
[0089] The disclosures of the references, patents, and published patent applications disclosed herein are each incorporated herein by reference in their entirety. In the event of a conflict between a definition herein and a definition provided in a patent or publication incorporated herein by reference, the definition provided herein shall prevail. Although the present disclosure is shown and described in conjunction with exemplary embodiments thereof, it will be appreciated by those of ordinary skill in the art that various changes in form and detail may be made without departing from the spirit and scope of the present disclosure.
Claims
1. A hydroquinone molecular imprinting photoelectrochemical sensor, It is characterized in that The sensor comprises a reference electrode, an auxiliary electrode and a working electrode, wherein the reference electrode, the auxiliary electrode and the working electrode form a three-electrode system, wherein the working electrode is a molecularly imprinted modified electrode, and the molecularly imprinted modified electrode comprises a conductive substrate, a composite material supported on the conductive substrate and a molecularly imprinted polymer film layer; wherein the conductive substrate is an L-shaped glassy carbon electrode, and the composite material is CdS nanoparticles / ZnIn 2 S 4 The nanosheet heterogeneous structure is prepared by an electropolymerization-elution method.
2. A method for preparing the hydroquinone molecular imprinted photoelectrochemical sensor according to claim 1, It is characterized in that The preparation method comprises the following steps: S1. Determine the CdS nanoparticles and ZnIn 2 S 4 The band structure of the nanosheet; S2. Preparation of CdS nanoparticles / ZnIn by hydrothermal synthesis 2 S 4 Nanosheet heterostructure composite material, and the CdS nanoparticles / ZnIn 2 S 4 The nanosheet heterostructure composite material is vacuum dried and sealed for future use; S3, cleaning the glassy carbon electrode with acetone, ethanol, and ultrapure water ultrasonically in sequence, and drying it with nitrogen for later use; S4, the CdS nanoparticles / ZnIn prepared in step S2 2 S 4 The nanosheet heterostructure composite material is dispersed in deionized water to obtain a uniform dispersion, 10 μL of the uniform dispersion and 10 μL of nafion solution are coated on the surface of the glassy carbon electrode cleaned in step S3, and dried at room temperature to obtain CdS / ZnIn 2 S 4 The glassy carbon electrode modified with a photoelectric conversion layer; S5, the CdS / ZnIn obtained in step S4 2 S 4 The glassy carbon electrode modified with the photoelectric conversion layer is placed in a molecular imprinting polymerization solution containing hydroquinone, and the molecular imprinting polymer is prepared by an electropolymerization method, so that the molecular imprinting polymer is in situ modified on the CdS / ZnIn 2 S 4 The surface of the glassy carbon electrode modified with the photoelectric conversion layer forms a molecular imprinting polymer film layer, and the hydroquinone template molecules are eluted with acetic acid eluent and ethanol eluent to obtain a glassy carbon electrode modified with a molecular imprinting polymer MI-CdS / ZnIn 2 S 4 / GCE, and the glassy carbon electrode modified with the molecular imprinting polymer film layer is connected as a working electrode to a photoelectrochemical sensing system to obtain a CdS nanoparticle / ZnIn 2 S 4 The molecularly imprinted photoelectrochemical sensor based on nanosheet heterostructure composites.
3. The preparation method according to claim 2, It is characterized in that In step S1, the CdS nanoparticles and ZnIn 2 S 4 The band structure of the nanosheet includes: Combining CdS and ZnIn 2 S 4 The optical band gap Eg and the geometric mean of the absolute electronegativity of each atom in the semiconductor are used to calculate the positions of the conduction band and valence band of the semiconductor and design heterostructures with matching energy band gaps.
4. The preparation method according to claim 2, It is characterized in that Preparation of CdS nanoparticles / ZnIn by hydrothermal synthesis in step S2 2 S 4 Nanosheet heterostructure composites include: ZnIn 2 S 4 The nanosheets were dispersed in aqueous solution and hexadecyltrimethylammonium bromide, CdCl 2 and thiourea to form a mixed solution, which is then transferred to a polytetrafluoroethylene-lined autoclave, sealed and placed at 120°C to 140°C for reaction; and After cooling naturally to room temperature, the dispersion was centrifuged, washed with water and anhydrous ethanol for several times, and the precipitate was dried in a vacuum drying oven, and the CdS nanoparticles / ZnIn were obtained by grinding. 2 S 4 Nanosheet heterostructure composites.
5. The preparation method according to claim 4, It is characterized in that The ZnIn 2 S 4 , CdCl 2 The molar ratio of the hexadecyl trimethyl ammonium bromide to the thiourea is 1:5:
15. 2 S 4 and CdCl 2 The mass ratio is 2%~5%:1; the reaction time is 2~4h after sealing and placed at 120℃~140℃; the drying temperature of the precipitate in a vacuum drying oven is 60℃ and the drying time is 12h.
6. The preparation method according to claim 2, It is characterized in that In step S4, the CdS nanoparticles / ZnIn prepared in step S2 are 2 S 4 The nanosheet heterogeneous structure composite material is dispersed in deionized water to obtain a uniform dispersion comprising: The CdS nanoparticles / ZnIn prepared in step S2 2 S 4 The nanosheet heterostructure composite material was dispersed in deionized water and ultrasonically cleaned to obtain uniform CdS nanoparticles / ZnIn 2 S 4 Nanosheet heterostructure dispersion, the uniform CdS nanoparticles / ZnIn 2 S 4 The concentration of the nanosheet heterostructure dispersion is 1~10 mg / mL.
7. The preparation method according to claim 2, It is characterized in that In step S5, the molecular imprinting polymerization solution of hydroquinone is a PBS buffer solution with a concentration of 0.1-1.0 M phenylenediamine and 1-3 mM hydroquinone; and / or The scanning voltage of the electropolymerization method is -0.2~0.8 V, the scanning speed is 50 mv / s, and the number of scanning circles is 10~30 circles; the concentration of the acetic acid eluent is 5%; and the time for eluting the template molecule hydroquinone with acetic acid and ethanol is 10~20 minutes respectively.
8. An application of the hydroquinone molecular imprinted photoelectrochemical sensor according to claim 1 or an application of the hydroquinone molecular imprinted photoelectrochemical sensor prepared by the preparation method of the hydroquinone molecular imprinted photoelectrochemical sensor according to any one of claims 2 to 7, Features: The sensor is applied to the detection of hydroquinone.
9. The use according to claim 8, It is characterized in that The detection comprises the following steps: S1. Incubation of molecular imprinting photoelectrochemical sensor: preparing hydroquinone standard solutions of different concentrations, and immersing the molecular imprinting photoelectrode in the hydroquinone standard solutions of different concentrations for incubation; S2. Detection of electrical signals of photoelectrochemical sensor for hydroquinone: Ag / AgCl electrode was used as reference electrode, platinum electrode was used as auxiliary electrode, and the prepared MI-CdS / ZnIn with molecular imprinting function was used as reference electrode. 2 S 4 / GCE is the working electrode to form a three-electrode system, which is connected to the photoelectrochemical detection equipment. The IT test method is used to draw a working curve based on the relationship between the obtained photocurrent value and the concentration of the hydroquinone standard solution; as well as S3. Determine the content of hydroquinone: replace the hydroquinone standard solution with the sample to be tested, and use the IT test method in the same way. Compare the intensity value of the response signal with the working curve to obtain the content of hydroquinone in the sample to be tested.
10. The use according to claim 9, It is characterized in that The incubation time in step S1 is 10 to 20 minutes.