A plate shape control method for 355MPa thick steel plate with a thickness greater than 60mm

By combining two-stage rolling, segmented cooling, and hot straightening with slow cooling treatment, the problem of shape control for steel plates with a thickness of 60mm or more and a yield strength of 355MPa was solved, achieving efficient production and low-cost processing of steel plates.

CN115351073BActive Publication Date: 2024-11-29ANGANG STEEL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210897029.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-28
Publication Date
2024-11-29
Estimated Expiration
2042-07-28

AI Technical Summary

Technical Problem

Existing technologies are unable to effectively control the shape of steel plates with a thickness of 60mm or more and a yield strength of 355MPa, which leads to problems such as waviness defects and rolling scrap during production, affecting the first pass rate and production efficiency, and increasing costs.

Method used

A combination of two-stage rolling process, segmented cooling control, hot straightening and slow cooling treatment is adopted, including billet heating, rolling, cooling and slow cooling of steel plate stacking. By controlling the heating temperature, rolling reduction rate, roller cooling and straightening parameters, the controlled cooling process is optimized to ensure good steel plate shape.

Benefits of technology

It has achieved shape control for steel plates with a thickness of 60mm or more, and the flatness of the finished steel plates has reached less than 10mm/2m, which has reduced the scrap rate, saved the cost of subsequent cold straightening equipment, and improved production efficiency and first pass rate of steel plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003769304030000071
    Figure BDA0003769304030000071
  • Figure BDA0003769304030000072
    Figure BDA0003769304030000072
  • Figure BDA0003769304030000081
    Figure BDA0003769304030000081
Patent Text Reader

Abstract

The invention relates to a plate shape control method for a 355MPa grade thick steel plate with a thickness greater than 60mm. The chemical composition of the steel plate is: C 0.13%-0.18%, Si 0.25%-0.3%, Mn 1.25%-1.40%, P≤0.03%, S≤0.025%, Al 0.015%-0.04%, Nb 0.03%-0.05%, N≤0.012%, Ceq≤0.40% and Ceq=C+Mn / 6; the remainder is Fe and unavoidable impurities; the steel plate is obtained by rolling a slab with a thickness of 250-360mm through a medium and thick plate reciprocating rolling mill; the production process includes heating, rolling, cooling, hot straightening and slow cooling of steel plate stacking; and the plate shape control requirements of the steel plate can be met without subsequent cold straightening treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel plate production, and in particular to a plate shape control method for a steel plate with a thickness specification greater than 60 mm and a yield strength of 355 MPa. Background Art

[0002] In order to improve the competitiveness of medium and thick plate products, some medium and thick plate products adopt the production process of replacing alloy with "water". However, with the increase of plate thickness and the use of TMCP process, the steel plate is prone to wave-breaking defects. At the same time, the plate shape control is difficult. For example, when producing high-rise steel, engineering structure steel and other products, the plate shape cannot meet the requirements of automatic welding, which seriously affects customer use and has a long delivery date. Other steel types also have serious wave-breaking problems. The characteristics of this type of steel plate are thick rolled pieces and are very sensitive to rolling force and temperature changes. Wave shape defects and rolling waste are very likely to occur during production. The scrap rate is high, and the rolled steel plate has a plate shape similar to that of corrugated plates, resulting in excessive flatness and difficulty in forming mass production capacity. Especially for products with a thickness of more than 60mm, the plate shape of most steel plates needs to be flattened by a flattening machine to save it. If it cannot be flattened, it has to be re-rolled, which wastes raw materials, affects production efficiency, increases production costs, and seriously affects the one-time pass rate of steel plates, resulting in a significant increase in the manufacturing cost of extra-thick steel plates and a prolonged delivery cycle.

[0003] It can be seen that how to solve the plate shape problem of the above-mentioned steel plates with a thickness of more than 60mm and a yield strength of 355MPa and improve the one-time pass rate of the steel plates are the key to the development and application of steel plates of this specification level.

[0004] So far, there has been little research on the shape control of steel plates with a thickness greater than 60 mm and a yield strength of 355 MPa at home and abroad. The Chinese patent application with publication number CN103722023A discloses "a TMCP high-strength ship plate shape control method", which is effective for the shape control of high-strength ship plates after rolling. However, this method is applicable to steel plates with a thickness of 30-60 mm, and does not involve the shape control of steel plates with a thickness of more than 60 mm. The Chinese patent application with publication number CN101069896A discloses "a medium and thick plate shape control method", which can reduce the wave shape of 30 mm thick steel plates after rolling. However, this method cannot completely eliminate the wave shape of the steel plate because there is no reduction in the last pass; and because the rolling mill only has two upper and lower rollers in contact with the steel plate, when there is no reduction in the last pass, the shape defects such as warping caused by the previous rolling pass cannot be eliminated.

[0005] In the journal article "Optimization Control of Hot-rolled Thin-gauge Plate Production Process" ("Henan Metallurgy" 2020.8), the problem of plate shape control of thin-gauge steel plates with a thickness of 6-10mm was solved by optimizing the heating, rolling and pressing procedures. However, its production method cannot meet the plate shape control requirements of steel plates with a thickness of more than 60mm. Summary of the invention

[0006] The present invention provides a plate shape control method for 355MPa grade thick steel plates with a thickness greater than 60mm, which can meet the plate shape control requirements of the steel plates without subsequent cold straightening treatment, and solves the problems that such steel plates are prone to wave shapes during production due to thin rolled pieces and rapid temperature drop, affecting the first-time pass rate and cost reduction rate of the steel plates.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A method for controlling the shape of a 355MPa thick steel plate with a thickness greater than 60mm, wherein the steel plate production process includes heating of the ingot, rolling, cooling, hot straightening and slow cooling of the steel plate stacking; the specific steps are as follows:

[0009] 1) Heating of the ingot: The ingot is sent into a walking beam heating furnace and heated to 1245-1270°C. The total heating time of the soaking section and the heating section is 4-5.5 hours, and the total time in the furnace is 6-7 hours. The temperature difference between the upper and lower surfaces of the ingot after heating is ensured to be less than 30°C.

[0010] 2) Rolling; Rolling is divided into two stages: the first stage is the rough rolling stage, the final rolling temperature is greater than 1020℃, and at least the first two passes of the rough rolling stage adopt a large reduction rate, and the reduction rate of each pass is not less than 15%; in the rough rolling stage, the sled plate coefficient SKI value of the rolling widening stage is controlled, and the SKI value is set to +5~+9; the second stage is the non-recrystallization rolling, i.e. the finishing rolling stage, the start rolling temperature is 930~960℃, the final rolling temperature is 830~860℃, and at least the last two passes of the finishing rolling stage adopt a small reduction rate, and the reduction rate of each pass is controlled at 1%~1.5%; the intermediate billet bite speed is 1.5~2.5m / s; the rough rolling stage and the finishing rolling stage are both controlled by segmented cooling of the rolls; when rolling the 1 / 4L length section of the head of the cast billet, the roll cooling water is not turned on; when rolling the 1 / 4L length section of the tail of the continuous casting billet, the roll cooling water volume is controlled at 35~50m 3 / h; when rolling the remaining length of the middle section of the billet, the roller cooling water volume is controlled at 50~80m 3 / h; where L is the length of the ingot in the rolling direction during each rolling pass; at the same time, the roller cooling water volume from the rolling mill to the pre-straightening machine is adjusted to 180-230m 3 / h;

[0011] 3) Cooling; the cooling temperature is 780~810℃, the return temperature is 580~610℃, the cooling system is shielded at the head and tail; the upper header opening correction value is -400~-600mm, the lower header opening correction value is -500~-800mm; fully automatic cooling control is adopted: the header opening water volume is 180~220m 3 / h, 2 to 4 water groups are opened in the header, the water volume ratio of the lower header to the upper header is 2 to 2.5; the roller speed is 2.0 to 3 m / s;

[0012] 4) Hot straightening: the position of the lead-in roller is -1.1 to -1.5 mm, the position of the lead-out roller is -3.1 to -4.2 mm, the final straightening temperature is not more than 520°C, and the straightening force is 6000 to 8000 kN;

[0013] 5) Slow cooling of steel plates stacking: After hot straightening, the steel plates are immediately transported to the slow cooling area for stacking. The temperature of the stacked steel plates is greater than 450°C, and the stacking slow cooling rate is 5-10°C / h, and the time is 24-48h.

[0014] The chemical composition of the steel plate is calculated by weight percentage as follows: C 0.13% to 0.18%, Si 0.25% to 0.3%, Mn 1.25% to 1.40%, P≤0.03%, S≤0.025%, Al 0.015% to 0.04%, Nb 0.03% to 0.05%, N≤0.012%, Ceq≤0.40% and Ceq=C+Mn / 6; the remainder is Fe and unavoidable impurities, among which O≤0.0050%, and the total amount of other impurities is less than 0.05%.

[0015] The steel plate is obtained by rolling a cast billet with a thickness of 250 to 360 mm through a medium and thick plate reciprocating rolling mill.

[0016] In the step 2), before rolling, high-pressure water is used to descale the ingot after it leaves the heating furnace. The descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa.

[0017] In the step 2), the thickness of the rolled intermediate billet is 2 to 3 times the thickness of the finished steel plate.

[0018] In the step 4), the side spraying is started after the steel plate is cooled, the side spraying pressure is 2-5 MPa, and the side spraying water volume is 25-50 m 3 / h.

[0019] The straightness of the finished steel plate is below 10mm / 2m.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1) Use a higher heating temperature and ensure that the soaking section and heating section are in the furnace for a certain time, so that the temperature difference between the upper and lower surfaces of the ingot after heating is controlled within 30°C, shortening the temperature difference between the surface and the core of the ingot, and improving the uniformity of the metal flow in the horizontal and vertical directions on the surface of the steel plate; control the total time in the furnace, effectively inhibit the excessive growth of austenite grains, and ensure the performance of the steel plate.

[0022] 2) A two-stage controlled rolling process is adopted to control the reduction rate of the last two passes in the rough rolling stage and the last two passes in the finishing rolling stage, as well as the thickness of the intermediate billet, which effectively ensures the initial plate shape of the rolled steel plate and reduces the internal stress of the steel plate. At the same time, the SKI value of the rolling mill sled plate coefficient in the control rolling widening stage of the rough rolling stage is limited to keep the intermediate billet horizontal or slightly upturned; in addition, the roller cooling water flow rate and the segmented cooling process of the roller are controlled to avoid a large amount of cooling water flowing on the surface of the steel plate, causing uncontrolled temperature drop on the surface of the steel plate and increasing the number of rolling passes; the cooling water volume of the roller is reasonably controlled, and the roller shape is effectively controlled, which greatly improves the problem of irregular deviation and sickle bend during rolling due to uneven temperature distribution of the head, middle and tail of the steel billet.

[0023] 3) By optimizing the controlled cooling process, the temperature uniformity of the head, middle and tail of the steel plate is achieved, which suppresses the warping of the steel plate due to uneven temperature at different positions after controlled cooling; three-pass hot straightening is adopted, and the initial lead-in roller position, lead-out roller position, straightening temperature and pressure are set to ensure that the steel plate is straight and has a good shape after straightening; at the same time, a lower final straightening temperature is set to reduce the temperature drop range of the steel plate during the cooling process, avoiding large internal stress due to rapid phase change; side spraying is beneficial to the control of the steel plate shape, reducing the probability of buckle head and buckle tail shape problems, and saving the subsequent cold straightening equipment investment cost.

[0024] 4) The hot straightened steel plates are immediately transported to the slow cooling area for stacking, and the steel plates are slowly cooled and insulated with asbestos. At the same time, the slow cooling temperature and stacking speed of the steel plates are strictly limited to ensure that the temperature drop of the steel plates tends to be consistent. At the same time, the phase change interval with large internal stress at 450°C is avoided to ensure that the final straightness of the finished steel plates meets the requirement of less than 10mm / 2m, saving the cost of subsequent flattening and straightening processes. DETAILED DESCRIPTION

[0025] The present invention discloses a method for controlling the shape of a 355MPa thick steel plate with a thickness greater than 60mm. The steel plate production process includes heating of the ingot, rolling, cooling, hot straightening and slow cooling of the steel plate stacking. The specific steps are as follows:

[0026] 1) Heating of the ingot: The ingot is sent into a walking beam heating furnace and heated to 1245-1270°C. The total heating time of the soaking section and the heating section is 4-5.5 hours, and the total time in the furnace is 6-7 hours. The temperature difference between the upper and lower surfaces of the ingot after heating is ensured to be less than 30°C.

[0027] 2) Rolling; Rolling is divided into two stages: the first stage is the rough rolling stage, the final rolling temperature is greater than 1020℃, and at least the first two passes of the rough rolling stage adopt a large reduction rate, and the reduction rate of each pass is not less than 15%; in the rough rolling stage, the sled plate coefficient SKI value of the rolling widening stage is controlled, and the SKI value is set to +5~+9; the second stage is the non-recrystallization rolling, i.e. the finishing rolling stage, the start rolling temperature is 930~960℃, the final rolling temperature is 830~860℃, and at least the last two passes of the finishing rolling stage adopt a small reduction rate, and the reduction rate of each pass is controlled at 1%~1.5%; the intermediate billet bite speed is 1.5~2.5m / s; the rough rolling stage and the finishing rolling stage are both controlled by segmented cooling of the rolls; when rolling the 1 / 4L length section of the head of the cast billet, the roll cooling water is not turned on; when rolling the 1 / 4L length section of the tail of the continuous casting billet, the roll cooling water volume is controlled at 35~50m 3 / h; when rolling the remaining length of the middle section of the billet, the roller cooling water volume is controlled at 50~80m 3 / h; where L is the length of the ingot in the rolling direction during each rolling pass; at the same time, the roller cooling water volume from the rolling mill to the pre-straightening machine is adjusted to 180-230m 3 / h;

[0028] 3) Cooling; the cooling temperature is 780~810℃, the return temperature is 580~610℃, the cooling system is shielded at the head and tail; the upper header opening correction value is -400~-600mm, the lower header opening correction value is -500~-800mm; fully automatic cooling control is adopted: the header opening water volume is 180~220m 3 / h, 2 to 4 water groups are opened in the header, the water volume ratio of the lower header to the upper header is 2 to 2.5; the roller speed is 2.0 to 3 m / s;

[0029] 4) Hot straightening: the position of the lead-in roller is -1.1 to -1.5 mm, the position of the lead-out roller is -3.1 to -4.2 mm, the final straightening temperature is not more than 520°C, and the straightening force is 6000 to 8000 kN;

[0030] 5) Slow cooling of steel plates stacking: After hot straightening, the steel plates are immediately transported to the slow cooling area for stacking. The temperature of the stacked steel plates is greater than 450°C, and the stacking slow cooling rate is 5-10°C / h, and the time is 24-48h.

[0031] The chemical composition of the steel plate is calculated by weight percentage as follows: C 0.13%-0.18%, Si 0.25%-0.3%, Mn 1.25%-1.40%, P≤0.03%, S≤0.025%, Al 0.015%-0.04%, Nb 0.03%-0.05%, N≤0.012%, Ceq≤0.40% and Ceq=C+Mn / 6; the remainder is Fe and unavoidable impurities, among which O≤0.0050%, and the total amount of other impurities is less than 0.05%.

[0032] The steel plate is obtained by rolling a cast billet with a thickness of 250 to 360 mm through a medium and thick plate reciprocating rolling mill.

[0033] In the step 2), before rolling, high-pressure water is used to descale the ingot after it leaves the heating furnace. The descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa.

[0034] In the step 2), the thickness of the rolled intermediate billet is 2 to 3 times the thickness of the finished steel plate.

[0035] In the step 4), the side spraying is started after the steel plate is cooled, the side spraying pressure is 2-5 MPa, and the side spraying water volume is 25-50 m 3 / h.

[0036] The straightness of the finished steel plate is below 10mm / 2m.

[0037] The working principle of the plate shape control method of a 355MPa grade thick steel plate with a thickness greater than 60mm described in the present invention is as follows:

[0038] 1. Billet heating process;

[0039] The ingot (thickness of 250-360mm, preferably continuous casting ingot) is sent into a walking beam heating furnace for heating, and the ingot is heated to 1245-1270℃. The total heating time of the soaking section and the heating section is 4-5.5 hours, and the total furnace time is 6-7 hours. A higher heating temperature is used to ensure that the temperature difference between the upper and lower surfaces of the ingot after heating is less than 30℃, shorten the temperature difference between the surface and the core of the ingot, and improve the uniformity of the metal flow in the horizontal and vertical directions on the surface of the steel plate. Control the total furnace time to effectively inhibit the excessive growth of austenite grains and ensure the mechanical properties of the steel plate.

[0040] 2. High-pressure water descaling and rolling process;

[0041] Before rolling, high-pressure water is used to descale the ingot after leaving the heating furnace. The descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa.

[0042] In the rough rolling stage, the roller cooling water in the rough rolling to pre-straightening section is reduced to 180-230m 3 / h; avoid a large amount of cooling water flowing under the steel plate surface to cause uncontrolled temperature drop on the steel plate surface, increase the rolling pass, and also help to control the intermediate billet to maintain a horizontal or slightly upturned state; in the rough rolling and finishing rolling stages, the rollers are cooled in sections. When the length section of the billet head is set, the roller cooling water is not turned on; when the length section of the middle part of the billet is set, the roller cooling water volume is 50-80m 3 / h; when rolling the tail of the billet to set the length, the roller cooling water volume is 35~50m 3 / h. By adjusting the water volume of the rolls, the roll shape is effectively controlled, which greatly improves the irregular deviation and sickle bend caused by uneven temperature distribution in the head, middle and tail of the billet during the rolling process.

[0043] The rolling process is divided into two stages: the final rolling temperature in the first stage is greater than 1020℃, the first two passes of the rough rolling stage use a large reduction rate, and the reduction rate of each pass is not less than 15%, and the thickness of the intermediate billet is 2 to 3 times the thickness of the finished steel plate. In the rough rolling stage, the sled plate coefficient SKI value of the rolling widening stage is controlled, and the SKI value is set to +5 to +9 to keep the intermediate billet horizontal or slightly upturned, which is conducive to the rapid bite of the intermediate billet during the finishing rolling stage. The second stage is non-recrystallization rolling (finishing rolling), the starting rolling temperature is 930-960℃, the final rolling temperature is 830-860℃, and the reduction rate of the two passes after the finishing rolling stage is controlled within 1%-1.5%; through two-stage rolling, the grain structure of different stages is refined and has a certain degree of pre-deformation to reduce the grain size after phase transformation; in addition, the first two passes of the rough rolling stage use the rolling mill capacity as much as possible, and adopt a large reduction rate rolling. The last two passes of the finishing rolling stage adopt a small reduction rate rolling due to the increase of the uncontrolled temperature drop deformation resistance of the steel plate to flatten the plate shape and reduce the internal stress of the steel plate. In order to ensure the shape of the steel plate after finishing rolling, the intermediate billet bite speed and the maximum rolling speed are set to the same value, and the value is 1.5-2.5m / s.

[0044] 3. Cooling and heat straightening process;

[0045] Initial cooling temperature is 780~810℃, return to red temperature is 580~610℃, and the cooling system is shielded at the head and tail. The upper header opening correction value is -400~-600mm, and the lower header opening correction value is -500~-800mm. Fully automatic cooling control is adopted: the header opening water volume is 180~220m 3 / h, 2 to 4 groups of water are opened in the header, the roller speed is 2.0 to 3m / s, and the water volume ratio between the lower header and the upper header is 2 to 2.5.

[0046] After the steel plate is cooled, the side spray is turned on, with a pressure of 2-5 MPa and a water volume of 25-50 m 3 / h.

[0047] Hot straightening is carried out in three passes, with the position of the lead-in roller at -1.1 to -1.5 mm, the position of the lead-out roller at -3.1 to -4.2 mm, the final straightening temperature not exceeding 520°C, and the straightening force between 6000 and 8000 kN. By limiting the cooling control parameters and injecting side sprays, it is beneficial to control the shape of the steel plate. By setting the appropriate roller gap, straightening force and number of straightening passes, the steel plate is guaranteed to be straight and in good shape after straightening. At the same time, a lower final straightening temperature is set to reduce the temperature drop range of the steel plate during the cooling process, avoid large internal stress due to rapid phase change, reduce the probability of buckle head and buckle tail shape problems of the steel plate, and save the subsequent cold straightening equipment investment cost.

[0048] 4) Steel plate stacking and slow cooling: The hot straightened steel plates are immediately transported to the slow cooling area for stacking. The temperature of the stacked steel plates should be greater than 450°C, and the number of stacked steel plates should be no less than 8. At the same time, the stacked steel plates are insulated with asbestos on the top, bottom and both sides. The steel plate stacking time is 24 to 48 hours, and then plasma cutting is performed. Since the cooling speed of the lower surface, upper surface and both sides of thick-gauge steel plates is different, the use of steel plate stacking and slow cooling and asbestos insulation can ensure that the temperature drop of the steel plates tends to be consistent, while also avoiding the phase change interval with large internal stress at 450°C, ensuring the final plate shape of the finished steel plate.

[0049] The present invention combines chemical composition with controlled rolling and controlled cooling technology to overcome the shortcomings of the prior art and solve the problem of plate shape control for steel plates with a thickness of more than 60 mm and a yield strength of 355 MPa. The straightness of the steel plate is less than 10 mm / 2 m, meeting the technical requirements.

[0050] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0051] [Example]

[0052] In this embodiment, Table 1 is the chemical composition of the steel plate, Table 2 is the heating system of the ingot and the high-pressure water descaling process parameters before rolling; Table 3 is the rolling process parameters of the steel plate; Table 4 is the controlled cooling process parameters of the steel plate, and Table 5 is the hot straightening process parameters of the steel plate and the straightness of the finished steel plate.

[0053] Table 1 Chemical composition of steel plates (wt, %)

[0054] Example C Si Mn Al Nb N Ceq 1 0.13 0.30 1.35 0.016 0.031 0.009 0.355 2 0.14 0.27 1.38 0.035 0.042 0.011 0.370 3 0.18 0.25 1.25 0.040 0.049 0.007 0.388 4 0.17 0.26 1.36 0.038 0.037 0.012 0.397 5 0.16 0.28 1.27 0.026 0.046 0.010 0.372 6 0.15 0.29 1.40 0.015 0.035 0.008 0.383

[0055] Note: Impurity elements in steel are P≤0.03%, S≤0.025%; 0≤0.0050%, and the total amount of other impurity elements is less than 0.05%.

[0056] Table 2 Billet heating system and pre-rolling high pressure water descaling process parameters

[0057]

[0058] Table 3 Rolling process parameters of steel plates

[0059]

[0060]

[0061] Table 4 Steel plate controlled cooling process parameters

[0062]

[0063] Table 5 Steel plate hot straightening process parameters and finished steel plate straightness

[0064]

[0065] It can be seen that the method of the present invention solves the plate shape problem of producing hot-rolled steel plates with a thickness of more than 60 mm and a yield strength of 355 MPa using 300-360 mm thick ingots, and the straightness of the steel plates meets the technical requirements of less than 10 mm / 2 m.

[0066] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for controlling the shape of a 355MPa thick steel plate with a thickness greater than 60mm, characterized in that: The chemical composition of the steel plate is as follows by weight percentage: C 0.13% to 0.18%, Si 0.25% to 0.3%, Mn 1.25% to 1.40%, P≤0.03%, S≤0.025%, Al 0.015% to 0.04%, Nb 0.03% to 0.05%, N≤0.012%, Ceq≤0.40% and Ceq=C+Mn / 6; the remainder is Fe and unavoidable impurities, O in the impurities is ≤0.0050%, and the total amount of other impurities is less than 0.05%; the steel plate is obtained by rolling a slab with a thickness of 250 to 360 mm through a medium and thick plate reciprocating rolling mill; the straightness of the finished steel plate is less than 10 mm / 2 m; The steel plate production process includes billet heating, rolling, cooling, hot straightening and steel plate stacking and slow cooling; the specific steps are as follows: 1) Heating of the ingot: The ingot is sent into a walking beam heating furnace and heated to 1245-1270°C. The total heating time of the soaking section and the heating section is 4-5.5 hours, and the total furnace time is 6-7 hours. The temperature difference between the upper and lower surfaces of the ingot after heating is ensured to be less than 30°C. 2) Rolling; Rolling is divided into two stages: the first stage is the rough rolling stage, the final rolling temperature is greater than 1020℃, and at least the first two passes of the rough rolling stage adopt a large reduction rate, and the reduction rate of each pass is not less than 15%; in the rough rolling stage, the sled plate coefficient SKI value of the rolling widening stage is controlled, and the SKI value is set to +5~+9; the second stage is the non-recrystallization rolling, that is, the finishing rolling stage, the starting rolling temperature is 930~960℃, the final rolling temperature is 830~860℃, and at least the last two passes of the finishing rolling stage adopt a small reduction rate, and the reduction rate of each pass is controlled at 1%~1.5%; the intermediate billet bite speed is 1.5~2.5m / s; the rough rolling stage and the finishing rolling stage are both controlled by segmented cooling of the rolls; when rolling the 1 / 4L length section of the head of the cast billet, the roll cooling water is not turned on; when rolling the 1 / 4L length section of the tail of the continuous casting billet, the roll cooling water volume is controlled at 35~50m 3 / h; when rolling the remaining length of the middle section of the billet, the roller cooling water volume is controlled at 50~80m 3 / h; where L is the length of the ingot in the rolling direction during each rolling pass; at the same time, the roller cooling water volume from the rolling mill to the pre-straightening machine is adjusted to 180-230m 3 / h; 3) Cooling; the cooling temperature is 780~810℃, the return temperature is 580~610℃, the cooling system is shielded at the head and tail; the upper header opening correction value is -400~-600mm, the lower header opening correction value is -500~-800mm; fully automatic cooling control is adopted: the header opening water volume is 180~220m 3 / h, 2 to 4 water groups are opened in the header, the water volume ratio of the lower header to the upper header is 2 to 2.5; the roller speed is 2.0 to 3 m / s; 4) Hot straightening; the position of the lead-in roller is -1.1 to -1.5 mm, the position of the lead-out roller is -3.1 to -4.2 mm, the final straightening temperature is not more than 520 ° C, and the straightening force is 6000 to 8000 kN; 5) Slow cooling of steel plates stacking: After hot straightening, the steel plates are immediately transported to the slow cooling area for stacking. The temperature of the stacked steel plates is greater than 450°C, and the stacking slow cooling rate is 5-10°C / h, and the time is 24-48h.

2. The method for controlling the shape of a 355MPa thick steel plate with a thickness greater than 60mm according to claim 1, characterized in that: In the step 2), before rolling, high-pressure water is used to descale the ingot after it leaves the heating furnace. The descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa.

3. The method for controlling the shape of a 355MPa thick steel plate with a thickness greater than 60mm according to claim 1, characterized in that: In the step 2), the thickness of the rolled intermediate billet is 2 to 3 times the thickness of the finished steel plate.

4. The method for controlling the shape of a 355MPa thick steel plate with a thickness greater than 60mm according to claim 1, characterized in that: In the step 4), the side spraying is started after the steel plate is cooled, the side spraying pressure is 2-5 MPa, and the side spraying water volume is 25-50 m 3 / h.

Citation Information

Patent Citations

  • Middle-thickness board-shape control method

    CN101069896A

  • Method for controlling plate shape of TMCP (thermal mechanical control processing) high-strength ship plate

    CN103722023A

  • Medium plate surface longitudinal edge crack control method

    CN103736742A

  • Method for controlling shape of thick steel plate with thickness greater than 50mm

    CN103817155A

  • Low-carbon extra-thick low-yield-ratio steel S355NL for reel and manufacturing method of low-carbon extra-thick low-yield-ratio steel S355NL

    CN106119713A