A high-strength, toughened zirconium oxide sizing nozzle for continuous casting and its manufacturing method

Through a combination of nano-scale raw materials and fine processing, the performance problems of the zirconia sizing nozzle under mechanical erosion and thermal shock have been solved, and a high-strength and high-toughness zirconia sizing nozzle has been achieved, which significantly extends the service life.

CN115353382BActive Publication Date: 2024-10-01SHANGHAI LIER REFRACTORY MATERIAL +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211107650.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-13
Publication Date
2024-10-01
Estimated Expiration
2042-09-13

AI Technical Summary

Technical Problem

The zirconia sizing nozzle is subjected to mechanical erosion, chemical erosion and stress spalling during use, resulting in a decrease in performance. It is difficult to improve its strength and thermal shock resistance at the same time, affecting its service life.

Method used

Using a combination of nano-scale raw materials, including yttrium oxide, basic magnesium carbonate, boron nitride nanosheets, nano-magnesium oxide, nano-alumina and PVA glue, through processes such as ball milling, roasting, wet grinding, stirring and hydraulic molding, it forms a high-strength , Toughened zirconia sizing nozzle to control the generation of nanocrystal grains and the distribution of liquid phase.

Benefits of technology

The anti-erosion and thermal shock resistance of the zirconia sizing nozzle is significantly improved, the service life is extended, and the formation of nodules is avoided, achieving a combination of high strength and high toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115353382B_ABST
    Figure CN115353382B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of refractory materials, in particular to a high-strength and toughened zirconium oxide sizing nozzle for continuous casting and a manufacturing method thereof. The raw material components are as follows by mass percentage: yttrium oxide is 1.8-2.4%, basic magnesium carbonate is 2.5-4%, boron nitride nanosheets are 0.08-0.1%, nano magnesium oxide is 0.3-0.5%, nano aluminum oxide is 0.5-0.8%, PVA glue is 8-9%, and the balance is zirconium oxide. The invention adopts nano-grade raw materials by design so that the nano characteristics still partially exist after firing. The crystal size, content and liquid phase distribution generated by the additive components have a great influence on the high strength, toughening and ultra-microporous structure effect of the zirconium product. The mixing, granulation and firing are controlled so that the nano crystal grains are generated and diffused within a proper liquid phase range, so that the scouring resistance and thermal shock resistance of the zirconium product can be effectively enhanced, and the formation of nodules can be effectively avoided. At the same time, a set of perfect and feasible preparation schemes of zirconium products doped with nano raw materials are designed to improve the stability and scouring resistance of the liquid phase.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of refractory materials, in particular to a high-strength and toughened zirconia sizing nozzle for continuous casting and a manufacturing method thereof. Background Art

[0002] Zirconia sizing nozzle is a very critical functional refractory product for continuous casting process. It plays a flow control role during use, controls the continuous and stable flow of molten steel in the tundish to the crystallizer, stabilizes the molten steel level in the crystallizer, and thus maintains the billet drawing speed and improves the continuous casting efficiency and product quality, extending the number of continuous casting furnaces while increasing the service life of the tundish.

[0003] During use, the zirconia sizing nozzle is subjected to severe mechanical scouring, chemical erosion and stress spalling. The performance is often evaluated by the second thermal stress fracture resistance factor R'. The theoretical core is that the lower the porosity of the zirconia sizing nozzle material, the smaller the grain size, the greater the strength of the material, and the better the performance. At the same time, it is necessary to have good thermal shock resistance to slow down the instantaneous thermal shock and scouring of the molten steel on the contact surface of the sizing nozzle, avoid the formation of microcracks on the contact surface, and the expansion of microcracks during use or even partial shedding. Therefore, high strength, low porosity, small grains, and high toughness are the key to significantly improving the service life of zirconia sizing nozzles.

[0004] In summary, the present invention solves the existing problems by designing a high-strength, toughened zirconia sizing nozzle for continuous casting and a manufacturing method thereof. Summary of the invention

[0005] The object of the present invention is to provide a high-strength, toughened zirconia sizing nozzle for continuous casting and a manufacturing method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A high-strength and toughened zirconium oxide sizing nozzle for continuous casting, the raw material components of which are as follows by mass percentage: yttrium oxide is 1.8-2.4%, basic magnesium carbonate is 2.5-4%, boron nitride nanosheets are 0.08-0.1%, nano magnesium oxide is 0.3-0.5%, nano aluminum oxide is 0.5-0.8%, PVA glue is 8-9%, and the balance is zirconium oxide, yttrium oxide is of industrial grade; basic magnesium carbonate is of industrial grade; boron nitride nanosheets have a sheet diameter of 0.1-0.4 μm, and a BN content of 98 wt%; nano magnesium oxide has an average particle diameter of 20 nm, is nearly spherical, and has a specific surface area of ​​more than 42 m 2 / g, MgO content is 98wt%; the average particle size of nano-alumina is 10-15nm, γ phase, specific surface area>120m 2 / g, Al2O3 content is 99.9wt%; the concentration of dry basis PVA in PVA glue is 5wt%.

[0008] As a preferred solution of the present invention, the raw material components of the sizing nozzle include 2.1% yttrium oxide, 3.1% basic magnesium carbonate, 0.09% boron nitride nanosheets, 0.4% nano magnesium oxide, 0.61% nano aluminum oxide, 8.7% PVA glue, and the balance is zirconium oxide.

[0009] A method for manufacturing a high-strength, toughened zirconia sizing nozzle for continuous casting, the specific steps of which are as follows:

[0010] Step 1, weighing yttrium oxide, basic magnesium carbonate, and zirconium oxide as ball milling materials according to weight percentage, loading them into a polyurethane ball mill, adding zirconium oxide grinding balls, and grinding them to 325-400 meshes at a rotation speed of 160±10 r / min to form a premix A, wherein the mixing uniformity coefficient of the premix A is less than 2.5%;

[0011] Step 2, calcining the premix A at a temperature of 1470±25° C. for a time of 8±0.5 h, and ball-milling the premix A to 325-400 meshes after cooling to form a premix B;

[0012] Step 3, weighing 45% of the premix B by weight and anhydrous ethanol, wet grinding and drying, grinding to a particle size of 8000-10000 mesh, to form a premix C;

[0013] Step 4, weighing boron nitride nanosheets, nano magnesium oxide, nano aluminum oxide, and PVA glue according to weight percentage, mixing and first stirring at a low speed, the stirring speed is 1000 r / min, the stirring time is 15 min, and then stirring at a high speed, the stirring speed is 3500 r / min, and the stirring time is 45 min, to form a premix D;

[0014] Step 5, the remaining premix B, premix C, and premix D are fully mixed and granulated, and then loaded into a mold, and pressed by a 150t hydraulic press to form a sizing nozzle blank;

[0015] Step 6, after the green billet is naturally dried for 24 hours, it is placed in an oven at 110°C for drying for 20±2 hours, and then placed in an electric furnace at 1725±5°C for sintering for 7 hours to form a sizing nozzle;

[0016] Step 7: After cooling, carry out local polishing, testing, packaging, warehousing and sales.

[0017] As a preferred solution of the present invention, in step 5, ultrasonic vibration is performed while mixing.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. In the present invention, nano-grade raw materials are used to make their nano-properties still partially exist after firing. The crystal size, content and liquid phase distribution of the additive components have a great influence on the high strength, toughening and ultra-microporous structure effects of zirconium products. Controlling the blending, granulation, firing, etc. to make the nano-grains generate and diffuse within the appropriate liquid phase range can effectively enhance the anti-erosion and thermal shock resistance of zirconium products and effectively avoid the formation of nodules.

[0020] 2. In the present invention, by designing a complete and feasible preparation scheme for zirconium products doped with nano-raw materials, the product structure and the liquid phase structural morphology can be effectively controlled and designed, which solves the problem that the strength and thermal shock resistance of zirconium products are difficult to improve at the same time, improves the stability and erosion resistance of the liquid phase, and thus has high strength and toughness characteristics, good thermal shock resistance, and can significantly extend the service life of the nozzle. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the structure of the liquid phase region and nano-grains in the zirconium oxide of the present invention. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] To facilitate understanding of the present invention, the present invention will be described more comprehensively below with reference to the relevant drawings, and several embodiments of the present invention are given. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0024] It should be noted that when an element is referred to as being "fixed on" another element, it may be directly on the other element or there may also be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used in this article are for illustrative purposes only.

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0026] For examples, see Figure 1 , the present invention provides a technical solution:

[0027] A high-strength and toughened zirconium oxide sizing nozzle for continuous casting, the raw material components of which are as follows by mass percentage: yttrium oxide is 1.8-2.4%, basic magnesium carbonate is 2.5-4%, boron nitride nanosheets are 0.08-0.1%, nano magnesium oxide is 0.3-0.5%, nano aluminum oxide is 0.5-0.8%, PVA glue is 8-9%, and the balance is zirconium oxide, yttrium oxide is of industrial grade; basic magnesium carbonate is of industrial grade; boron nitride nanosheets have a sheet diameter of 0.1-0.4 μm, and a BN content of 98 wt%; nano magnesium oxide has an average particle diameter of 20 nm, is nearly spherical, and has a specific surface area of ​​more than 42 m 2 / g, MgO content is 98wt%; the average particle size of nano-alumina is 10-15nm, γ phase, specific surface area>120m 2 / g, Al2O3 content is 99.9wt%; the concentration of dry basis PVA in PVA glue is 5wt%.

[0028] The raw material components of the sizing nozzle include 2.1% yttrium oxide, 3.1% basic magnesium carbonate, 0.09% boron nitride nanosheets, 0.4% nano magnesium oxide, 0.61% nano aluminum oxide, 8.7% PVA glue, and the balance zirconium oxide.

[0029] A method for manufacturing a high-strength, toughened zirconia sizing nozzle for continuous casting, comprising the following steps:

[0030] (1) Weighing yttrium oxide, basic magnesium carbonate, and zirconium oxide as ball milling materials according to weight percentage, loading them into a polyurethane ball mill, adding zirconium oxide grinding balls, and grinding them to 325-400 meshes at a rotation speed of 160±10 r / min to form a premix A, wherein the coefficient of variation of the mixing uniformity of the premix A is less than 2.5%;

[0031] (2) calcining the premix A at a temperature of 1470±25° C. for a time of 8±0.5 h, and then ball-milling the premix A to a size of 325-400 meshes after cooling to form a premix B;

[0032] (3) Weighing 45% of the premix B by weight and mixing with anhydrous ethanol, wet grinding the mixture and drying the mixture to a particle size of 8000 to 10000 mesh to form a premix C;

[0033] (4) Weighing boron nitride nanosheets, nano magnesium oxide, nano aluminum oxide, and PVA glue according to weight percentage, mixing, first stirring at a low speed of 1000 r / min for 15 min, and then stirring at a high speed of 3500 r / min for 45 min to form a premix D;

[0034] (5) The remaining premix B, premix C, and premix D are fully mixed and granulated, and then loaded into a mold and pressed using a 150t hydraulic press to form a sizing nozzle blank;

[0035] (6) After the green billet is naturally dried for 24 hours, it is placed in an oven at 110°C for 20±2 hours, and then placed in an electric furnace at 1725±5°C for sintering for 7 hours to form a sizing nozzle;

[0036] (7) After cooling, local polishing, testing, packaging, warehousing and sales are carried out.

[0037] In the method for preparing the sizing nozzle, in step (5), ultrasonic vibration is performed while mixing.

[0038] The qualified product inspection index range of the zirconia sizing nozzle of the present invention is: compressive strength ≥400MPa; thermal shock number ≥20 times, service life ≥15h;

[0039] Specific implementation cases:

[0040] Please see attached Figure 1 The raw material components of high-strength, toughened zirconia sizing nozzles for continuous casting in Examples 1 to 6 and Comparative Examples 1 to 4 are shown in Table 1 by mass fraction.

[0041] Table 1 Raw material composition of Examples 1 to 6 and Comparative Examples 1 to 4, wt%

[0042]

[0043]

[0044] A method for manufacturing a high-strength, toughened zirconia sizing nozzle for continuous casting, comprising the following steps:

[0045] (1) Weighing yttrium oxide, basic magnesium carbonate, and zirconium oxide as ball milling materials according to weight percentage, loading them into a polyurethane ball mill, adding zirconium oxide grinding balls, and grinding them to 325-400 meshes at a rotation speed of 160±10 r / min to form a premix A, wherein the coefficient of variation of the mixing uniformity of the premix A is less than 2.5%;

[0046] (2) calcining the premix A at a temperature of 1470±25° C. for a time of 8±0.5 h, and then ball-milling the premix A to a size of 325-400 meshes after cooling to form a premix B;

[0047] (3) Weighing 45% of the premix B by weight and mixing with anhydrous ethanol, wet grinding the mixture and drying the mixture to a particle size of 8000 to 10000 mesh to form a premix C;

[0048] (4) Weighing boron nitride nanosheets, nano magnesium oxide, nano aluminum oxide, and PVA glue according to weight percentage, mixing, first stirring at a low speed of 1000 r / min for 15 min, and then stirring at a high speed of 3500 r / min for 45 min to form a premix D;

[0049] (5) The remaining premix B, premix C, and premix D are fully mixed and granulated, and then loaded into a mold and pressed using a 150t hydraulic press to form a sizing nozzle blank;

[0050] (6) After the green billet is naturally dried for 24 hours, it is placed in an oven at 110°C for 20±2 hours, and then placed in an electric furnace at 1725±5°C for sintering for 7 hours to form a sizing nozzle;

[0051] (7) After cooling, local polishing, testing, packaging, warehousing and sales are carried out.

[0052] In the method for preparing the sizing nozzle, in step (5), ultrasonic vibration is performed while mixing.

[0053] The qualified product detection index range of the zirconia sizing nozzle of the present invention is: compressive strength ≥400MPa; thermal shock times ≥20 times, and service life ≥15h.

[0054] The high-strength, toughened zirconia sizing nozzle for continuous casting of Examples 1 to 6 and Comparative Examples 1 to 4 was tested for bulk density and apparent porosity by drainage method according to GB / T2997-2000, the compressive strength was tested according to GB / T 5072-2008 refractory material room temperature compressive strength test method, and the thermal shock resistance was tested according to YB / T376.3-2004 refractory product thermal shock test detection method, and the service life was obtained when used in the production site. The test results are listed in Table 2.

[0055] Table 2 Test results of Examples 1 to 6 and Comparative Examples 1 to 4

[0056]

[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-strength, toughened zirconia sizing nozzle for continuous casting, characterized in that: The raw material components are as follows: 1.8-2.4% yttrium oxide, 2.5-4% basic magnesium carbonate, 0.08-0.1% boron nitride nanosheets, 0.3-0.5% nano magnesium oxide, 0.5-0.8% nano aluminum oxide, 8-9% PVA glue, and the balance is zirconium oxide. The yttrium oxide is of industrial grade; the basic magnesium carbonate is of industrial grade; the boron nitride nanosheet has a sheet diameter of 0.1-0.4 μm and a BN content of 98 wt%; the nano magnesium oxide has an average particle diameter of 20 nm, is nearly spherical, and has a specific surface area of ​​more than 42 m 2 / g, MgO content is 98wt%; the average particle size of nano-alumina is 10-15nm, γ phase, specific surface area>120m 2 / g, Al2O3 content is 99.9wt%; the concentration of dry basis PVA in PVA glue is 5wt%.

2. The high-strength, toughened zirconia sizing nozzle for continuous casting according to claim 1, characterized in that: The raw material components of the sizing nozzle include 2.1% yttrium oxide, 3.1% basic magnesium carbonate, 0.09% boron nitride nanosheets, 0.4% nano magnesium oxide, 0.61% nano aluminum oxide, 8.7% PVA glue, and the balance zirconium oxide.

3. The method for manufacturing a high-strength, toughened zirconia sizing nozzle for continuous casting according to claim 1, wherein the specific steps are as follows: Step 1, weighing yttrium oxide, basic magnesium carbonate, and zirconium oxide as ball milling materials according to weight percentage, loading them into a polyurethane ball mill, adding zirconium oxide grinding balls, and grinding them to 325-400 meshes at a rotation speed of 160±10 r / min to form a premix A, wherein the mixing uniformity coefficient of the premix A is less than 2.5%; Step 2, calcining the premix A at a temperature of 1470±25° C. for a time of 8±0.5 h, and ball-milling the premix A to 325-400 meshes after cooling to form a premix B; Step 3, weighing 45% of the premix B by weight and anhydrous ethanol, wet grinding and drying, grinding to a particle size of 8000-10000 mesh, to form a premix C; Step 4, weighing boron nitride nanosheets, nano magnesium oxide, nano aluminum oxide, and PVA glue according to weight percentage, mixing and first stirring at a low speed, the stirring speed is 1000 r / min, the stirring time is 15 min, and then stirring at a high speed, the stirring speed is 3500 r / min, and the stirring time is 45 min, to form a premix D; Step 5, the remaining premix B, premix C, and premix D are fully mixed and granulated, and then loaded into a mold, and pressed by a 150t hydraulic press to form a sizing nozzle blank; Step 6, after the green billet is naturally dried for 24 hours, it is placed in an oven at 110°C for drying for 20±2 hours, and then placed in an electric furnace at 1725±5°C for sintering for 7 hours to form a sizing nozzle; Step 7: After cooling, carry out local polishing, testing, packaging, warehousing and sales.

4. The method for manufacturing a high-strength, toughened zirconia sizing nozzle for continuous casting according to claim 3, characterized in that: In step 5, ultrasonic vibration is performed while mixing.

Citation Information

Cited By

  • Preparation method of composite layer reinforced long-life zirconia metering nozzle

    CN122254904A