High crystallinity copolyester and preparation method and product thereof

The high crystallinity copolyester prepared through the esterification-precondensation-polycondensation process solves the problem of insufficient performance of existing polyester materials, significantly improves the tensile, heat resistance and gas barrier properties, and expands its application fields.

CN115368545BActive Publication Date: 2024-10-01NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210884294.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-25
Publication Date
2024-10-01
Estimated Expiration
2042-07-25

AI Technical Summary

Technical Problem

Existing polyester materials have deficiencies in tensile properties, chemical solvent resistance, heat resistance and gas barrier properties, which limits their application scope.

Method used

A preparation method of high crystallinity copolyester is adopted, through esterification or transesterification reaction, precondensation polymerization and polycondensation reaction, using 2,5-thiophenedicarboxylic acid, 3,4-thiophenedicarboxylic acid and their esterified products and hexane dicarboxylic acid. Acids and aliphatic chain glycols, combined with specific catalysts and stabilizers, produce highly crystalline copolyesters with excellent properties.

Benefits of technology

The high crystallinity copolyester has been significantly improved in tensile properties, chemical solvent resistance, heat resistance and gas barrier properties, broadening its application scope in packaging bags, barrier films and fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115368545B_ABST
    Figure CN115368545B_ABST
Patent Text Reader

Abstract

The invention relates to a high-crystallinity copolyester and a preparation method and product thereof. The preparation method comprises the following steps: subjecting a first mixed reaction system comprising a dibasic acid or an esterification product thereof, an aliphatic chain diol and an esterification or transesterification catalyst to an esterification or transesterification reaction under a protective atmosphere to obtain an esterification or transesterification product, wherein the dibasic acid or the esterification product thereof comprises 2,5-thiophenedicarboxylic acid or an esterification product thereof, 3,4-thiophenedicarboxylic acid or an esterification product thereof and adipic acid or an esterification product thereof, and the carbon chain length of the aliphatic chain diol is 2-20; subjecting a second mixed reaction system comprising the esterification or transesterification product and a stabilizer to a pre-polycondensation reaction under vacuum conditions to obtain a pre-polymerization product; and subjecting the pre-polymerization product to a polycondensation reaction to obtain a high-crystallinity copolyester having excellent tensile properties, chemical solvent resistance, heat resistance, degradation properties and gas barrier properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a high-crystallinity copolyester and a preparation method and product thereof. Background Art

[0002] Polyester is a polymer containing an ester group on the main chain and is widely used in packaging bags, plastic bottles, films, fibers and other fields. Although polyesters such as polyethylene succinate, polybutylene succinate and polybutylene adipate have excellent degradation properties and are environmentally friendly, they have poor tensile properties, chemical solvent resistance, insufficient heat resistance and weak gas barrier properties, which greatly limit their applications. Summary of the invention

[0003] Based on this, it is necessary to provide a high-crystallinity copolyester and its preparation method and product to address the above problems. The high-crystallinity copolyester has excellent tensile properties, chemical solvent resistance, heat resistance, degradation performance and gas barrier properties.

[0004] The present invention provides a method for preparing a high-crystallinity copolyester, comprising the following steps:

[0005] A first mixed reaction system comprising a dibasic acid or an esterified product thereof, an aliphatic chain diol and an esterification or transesterification catalyst is subjected to an esterification or transesterification reaction under a protective atmosphere to obtain an esterification or transesterification product, wherein the dibasic acid or the esterified product thereof comprises 2,5-thiophenedicarboxylic acid or an esterified product thereof, 3,4-thiophenedicarboxylic acid or an esterified product thereof and adipic acid or an esterified product thereof, and the carbon chain length of the aliphatic chain diol is 2-20;

[0006] subjecting the second mixed reaction system comprising the esterification or transesterification product and the stabilizer to a pre-polycondensation reaction under vacuum conditions to obtain a pre-polymerized product; and

[0007] The prepolymer product is subjected to polycondensation reaction to obtain a high-crystallinity copolyester.

[0008] In one embodiment, in the dibasic acid or its ester, the molar ratio of the 3,4-thiophenedicarboxylic acid or its ester to the 2,5-thiophenedicarboxylic acid or its ester is 5:95-95:5, and the molar ratio of the adipic acid or its ester to the sum of the 2,5-thiophenedicarboxylic acid or its ester and the 3,4-thiophenedicarboxylic acid or its ester is 1:99-99:1.

[0009] In one embodiment, the 2,5-thiophenedicarboxylate is selected from dimethyl 2,5-thiophenedicarboxylate;

[0010] and / or, the 3,4-thiophenedicarboxylate is selected from dimethyl 3,4-thiophenedicarboxylate;

[0011] And / or, the adipic acid ester is at least one selected from dimethyl adipate, diethyl adipate, dipropyl adipate or dibutyl adipate.

[0012] In one embodiment, the molar ratio of the dibasic acid or its esterification product to the aliphatic chain diol is 1:1.1-1:3.0.

[0013] In one embodiment, the aliphatic chain diol is at least one selected from ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, butanediol, pentanediol, hexanediol, octanediol or decanediol.

[0014] In one embodiment, the esterification or transesterification catalyst is selected from at least one of a zinc-based catalyst, a titanium-based catalyst, a tin-based catalyst, or a germanium-based catalyst, and the mass of the esterification or transesterification catalyst is 0.01%-0.5% of the theoretical mass of the high crystallinity copolyester;

[0015] And / or, the stabilizer is selected from phosphorus-based stabilizers, and the mass of the stabilizer is 0.01%-0.5% of the theoretical mass of the high crystallinity copolyester.

[0016] In one embodiment, when the esterification or transesterification catalyst is selected from a zinc-based catalyst, the second mixed reaction system also includes a polycondensation catalyst, and the polycondensation catalyst includes at least one of an antimony-based catalyst, a titanium-based catalyst, a tin-based catalyst or a germanium-based catalyst; the mass of the polycondensation catalyst is 0.01%-0.5% of the theoretical mass of the high crystallinity copolyester.

[0017] In one embodiment, in the step of performing the esterification or transesterification reaction, the temperature is 140° C.-220° C. and the time is 1.5 h-8.0 h;

[0018] And / or, in the step of performing the pre-polycondensation reaction, the vacuum degree is 50Pa-700Pa, the temperature is 160°C-230°C, and the time is 0.5h-1.0h;

[0019] And / or, in the step of performing polycondensation reaction, the vacuum degree is within 50 Pa, the temperature is 200° C.-250° C., and the time is 1.5 h-10.0 h.

[0020] A high crystallinity copolyester is prepared by the above-mentioned preparation method of the high crystallinity copolyester.

[0021] An article is made of the high crystallinity copolyester as described above.

[0022] In the preparation method of the high-crystallinity copolyester provided by the present invention, 2,5-thiophene dicarboxylic acid or its ester, 3,4-thiophene dicarboxylic acid or its ester, adipic acid or its ester and aliphatic chain diol cooperate with each other to obtain the high-crystallinity copolyester, and the high-crystallinity copolyester has excellent tensile properties, chemical solvent resistance and heat resistance. In addition, both 2,5-thiophene dicarboxylic acid or its ester and 3,4-thiophene dicarboxylic acid or its ester contain a rigid aromatic five-membered ring structure, which enhances the rigidity of the molecular chain segment of the high-crystallinity copolyester and further improves the gas barrier property, heat resistance and tensile property of the high-crystallinity copolyester. Moreover, 2,5-thiophene dicarboxylic acid or its ester, 3,4-thiophene dicarboxylic acid or its ester, adipic acid or its ester cooperate with each other, so that the bio-based content in the high-crystallinity copolyester is high, which not only makes the high-crystallinity copolyester have good degradation performance, but also reduces the dependence on petrochemical resources.

[0023] Since the high crystallinity copolyester provided by the present invention has excellent tensile properties, chemical solvent resistance, heat resistance, degradation performance and gas barrier properties, the products prepared with the high crystallinity copolyester can be well used in the fields of packaging bags, barrier films, fibers, etc., which greatly broadens the use field and application range of the high crystallinity copolyester. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The poly(2,5-thiophenedicarboxylic acid, 3,4-thiophenedicarboxylic acid, adipate) glycol copolyester prepared in Example 1 is 1 H-NMR spectrum;

[0025] Figure 2 is a DSC curve diagram of the poly-2,5-thiophenedicarboxylic acid, 3,4-thiophenedicarboxylic acid, adipate, ethylene glycol copolyester prepared in Example 1;

[0026] Figure 3 is a TGA curve diagram of poly(2,5-thiophenedicarboxylic acid, 3,4-thiophenedicarboxylic acid, adipate) glycol copolyester prepared in Example 1;

[0027] Figure 4 It is a stress-strain curve diagram of the poly (2,5-thiophenedicarboxylic acid, 3,4-thiophenedicarboxylic acid, ethylene glycol adipate) copolyester prepared in Example 1. DETAILED DESCRIPTION

[0028] For ease of understanding of the present invention, the present invention will be described more fully below with reference to relevant embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0030] The applicant has found through a large number of experiments that if polyester is prepared directly using dibasic acids and diols containing aromatic groups, the prepared polyester not only has low crystallinity but is also non-biodegradable. In addition, due to the large variety of dibasic acids, aliphatic dibasic acids and diols containing aromatic groups, it is difficult to make the prepared copolyester have good crystallization properties, heat resistance, tensile properties, chemical solvent resistance, degradation properties and gas barrier properties.

[0031] The method for preparing a high crystallinity copolyester provided by the present invention comprises the following steps:

[0032] S10, subjecting a first mixed reaction system comprising a dibasic acid or an esterified product thereof, an aliphatic chain diol, and an esterification or transesterification catalyst to an esterification or transesterification reaction under a protective atmosphere to obtain an esterification or transesterification product;

[0033] S20, subjecting the second mixed reaction system comprising the esterification or transesterification product and the stabilizer to a pre-polycondensation reaction under vacuum conditions to obtain a pre-polymerized product; and

[0034] S30, subjecting the prepolymerized product to a condensation polymerization reaction to obtain a high-crystallinity copolyester.

[0035] In step S10, the dibasic acid or its ester includes 2,5-thiophenedicarboxylic acid or its ester, 3,4-thiophenedicarboxylic acid or its ester and adipic acid or its ester, and the carbon chain length of the aliphatic chain diol is 2-20. Therefore, 2,5-thiophenedicarboxylic acid or its ester, 3,4-thiophenedicarboxylic acid or its ester, adipic acid or its ester and aliphatic chain diol cooperate with each other to obtain a high-crystallinity copolyester, and the high-crystallinity copolyester has excellent tensile properties, chemical solvent resistance and heat resistance.

[0036] Specifically, the carbon chain length of the aliphatic chain diol is 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20; in one embodiment, the aliphatic chain diol is selected from at least one of ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, butanediol, pentanediol, hexanediol, octanediol or decanediol; in one embodiment, the molar ratio of the dibasic acid or its esterification product to the aliphatic chain diol is 1:1.1-1:3.0, including but not limited to, the molar ratio of the dibasic acid or its esterification product to the aliphatic chain diol is 1:1.1, 1:1.4, 1:1.7, 1:2.0, 1:2.3, 1:2.6 or 1:3.0.

[0037] In addition, both 2,5-thiophenedicarboxylic acid or its esters and 3,4-thiophenedicarboxylic acid or its esters contain a relatively rigid aromatic five-membered ring structure, which enhances the rigidity of the molecular chain segments of the high-crystalline copolyester and further improves the gas barrier properties, heat resistance and tensile properties of the high-crystalline copolyester; and, 2,5-thiophenedicarboxylic acid or its esters, 3,4-thiophenedicarboxylic acid or its esters, and adipic acid or its esters work synergistically with each other, resulting in a high bio-based content in the high-crystalline copolyester, which not only makes the high-crystalline copolyester have good degradation properties, but also reduces dependence on petrochemical resources.

[0038] In one embodiment, the 2,5-thiophene dicarboxylic acid ester is selected from dimethyl 2,5-thiophene dicarboxylate; and the 3,4-thiophene dicarboxylic acid ester is selected from dimethyl 3,4-thiophene dicarboxylate.

[0039] It should be noted that adipic acid refers to 1,6-adipic acid. In one embodiment, the adipic acid ester is at least one selected from dimethyl adipate, diethyl adipate, dipropyl adipate, dibutyl adipate, and the like.

[0040] In order to avoid too high a melting temperature, in one embodiment, in the dibasic acid or its ester, the molar ratio of 3,4-thiophenedicarboxylic acid or its ester to 2,5-thiophenedicarboxylic acid or its ester is 50:50-95:5, including but not limited to, the molar ratio of 3,4-thiophenedicarboxylic acid or its ester to 2,5-thiophenedicarboxylic acid or its ester is 50:50, 55:45, 60:40, 65:35, 70:30, 75:25, 80:20, 85:15, 90:10 or 95:5.

[0041] In order to better balance the tensile properties, chemical solvent resistance, heat resistance, degradation properties and gas barrier properties, the molar ratio of adipic acid or its ester to the sum of the 2,5-thiophenedicarboxylic acid or its ester and the 3,4-thiophenedicarboxylic acid or its ester is 1:99-99:1. Preferably, the molar ratio of adipic acid or its ester to the sum of the 2,5-thiophenedicarboxylic acid or its ester and the 3,4-thiophenedicarboxylic acid or its ester is 85:15-10:90, including but not limited to 85:15, 80:20, 75:25, 70:30, 65:35, 60:40, 55:45, 50:50, 45:55, 40:60, 35:65, 30:70, 25:75, 20:80, 15:85 or 10:90.

[0042] In one embodiment, the esterification or transesterification catalyst in the first mixed reaction system of step S10 is selected from at least one of a zinc-based catalyst, a titanium-based catalyst, a tin-based catalyst or a germanium-based catalyst, and the mass of the esterification or transesterification catalyst is 0.01%-0.5% of the theoretical mass of the high crystallinity copolyester.

[0043] In one embodiment, zinc-based catalysts include but are not limited to zinc acetate; manganese-based catalysts include but are not limited to manganese acetate; titanium-based catalysts include but are not limited to at least one of tetrabutyl titanate, isopropyl titanate, titanium dioxide or an inorganic supported titanium catalyst; tin-based catalysts include but are not limited to at least one of dibutyl tin oxide, stannous isooctanoate, monobutyl tin triisooctoate, and dioctyl tin oxide.

[0044] In one embodiment, in the step of performing esterification or transesterification reaction of the first mixed reaction system under a protective atmosphere, the temperature is 140° C.-220° C. and the time is 1.5 h-8.0 h, wherein the protective atmosphere can be a nitrogen atmosphere or an inert gas atmosphere.

[0045] In the second mixed reaction system of step S20, the stabilizer is selected from a phosphorus-based stabilizer, and the phosphorus-based stabilizer includes but is not limited to at least one of phosphorous acid, hypophosphorous acid, pyrophosphoric acid, ammonium phosphate, trimethyl phosphate, dimethyl phosphate, triphenyl phosphate, diphenyl phosphate, triphenyl phosphite, diphenyl phosphite, ammonium phosphite, and diammonium phosphate, and the mass of the stabilizer is 0.01%-0.5% of the theoretical mass of the high crystallinity copolyester.

[0046] In one embodiment, especially when the esterification or transesterification catalyst is selected from a zinc-based catalyst, the second mixed reaction system also includes a condensation catalyst, and the condensation catalyst includes at least one of an antimony-based catalyst, a titanium-based catalyst, a tin-based catalyst, and a germanium-based catalyst. It can be understood that the selection of the titanium-based catalyst and the tin-based catalyst can refer to the selection of the titanium-based catalyst and the tin-based catalyst in the esterification or transesterification catalyst. The mass of the condensation catalyst is 0.01%-0.5% of the theoretical mass of the high crystallinity copolyester.

[0047] In one embodiment, the antimony-based catalyst includes but is not limited to at least one of antimony trioxide, ethylene glycol antimony, antimony acetate, and polyethylene glycol antimony; the germanium-based catalyst includes but is not limited to germanium oxide.

[0048] In one embodiment, in the step of performing a pre-polycondensation reaction of the second mixed reaction system under vacuum conditions, the vacuum degree is 50Pa-700Pa, the temperature is 160°C-230°C, and the time is 0.5h-1.0h.

[0049] In step S30, in the step of subjecting the prepolymerized product to a condensation reaction, the vacuum degree is within 50 Pa, the temperature is 200° C.-250° C., and the time is 1.5 h-10.0 h.

[0050] The preparation method of the high-crystallinity copolyester of the present invention adopts an esterification-prepolymerization-polycondensation process for preparation. The preparation method is simple, easy to operate, highly controllable, easy to implement, suitable for large-scale industrial production, and realizes the simple preparation of copolyester with good crystallinity, heat resistance, tensile properties, degradation properties and gas barrier properties.

[0051] The present invention also provides a high-crystallinity copolyester, which is prepared by the preparation method of the high-crystallinity copolyester.

[0052] The high-crystallinity copolyester provided by the present invention has excellent tensile properties, chemical solvent resistance, heat resistance, degradation performance and gas barrier properties. Products prepared with the high-crystallinity copolyester can be well applied to packaging bags, barrier films, fibers and other fields, greatly broadening the use field and application range of the high-crystallinity copolyester.

[0053] The present invention also provides an article, which is made of the high crystallinity copolyester.

[0054] In one embodiment, the step of preparing the high crystallinity copolyester into an article comprises: first preparing the high crystallinity copolyester into polyester particles, and then further preparing the article.

[0055] In one embodiment, the step of preparing the high crystallinity copolyester into polyester particles comprises the following steps: melt-extruding and pelletizing the high crystallinity copolyester.

[0056] In one embodiment, the step of preparing the polyester particles into products includes melt-extruding the polyester particles and casting the molten fluid onto a roller to obtain a cast thick sheet; and then longitudinally and transversely stretching the cast thick sheet to obtain a polyester film or sheet.

[0057] The products prepared by using the high crystallinity copolyester provided by the present invention can be well applied to the fields of packaging materials, films, fibers, etc., which greatly broadens the use field and application range of the high crystallinity copolyester.

[0058] In the following examples, a nuclear magnetic resonance spectrometer (Bruker, 400 MHz AVANCE III) was used to measure the hydrogen nuclear magnetic resonance spectrum ( 1 H-NMR), deuterated trifluoroacetic acid (CF3COOD) as solvent.

[0059] In the following examples, a differential scanning calorimeter (NETZSCH DSC 214) was used to test the thermal transition performance in a N2 atmosphere, with a temperature range of -100°C to 280°C and a heating rate of 10°C / min.

[0060] In the following examples, thermal stability tests were performed using a thermogravimetric analyzer (PerkinElmer TGA 8000) in a N2 atmosphere at a temperature range of 30°C-800°C and a heating rate of 20°C / min.

[0061] In the following examples, a universal material testing machine (Zwicki 1 kN) was used to perform tensile property tests, the sample size was 20.0 mm×2.0 mm×1.0 mm (length×width×thickness), and the tensile speed was 50 mm / min.

[0062] In the following examples, the barrier properties of oxygen and carbon dioxide were measured using a differential pressure gas permeameter (Labthink VAC-V2), with CO2 and O2 as gas sources, respectively. The test temperature was 23°C, the humidity was 50% RH, the sample diameter was 97 mm, and the permeation area was 38.5 cm 2 .

[0063] In the following examples, a phosphate buffer solution containing 0.2 mg / ml lipase was used as a degradation solvent, and the biodegradation test was carried out at a constant temperature of 37° C. The sample size was 20.0 mm×20.0 mm×0.5 mm (length×width×thickness).

[0064] Example 1

[0065] 0.1 mol of 2,5-thiophenedicarboxylic acid, 0.05 mol of 3,4-thiophenedicarboxylic acid, 0.6 mol of adipic acid, 1.5 mol of ethylene glycol and 0.1% of the theoretical mass of the high crystallinity copolyester product tetrabutyl titanate are put into a reactor to obtain a first mixed reaction system. The first mixed reaction system is evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system is gradually increased to 180° C. and the reaction is carried out for 4.0 hours to obtain an esterification product.

[0066] 0.12% of the theoretical mass of the high crystallinity copolyester product triphenyl phosphate was added into the reactor, the temperature was raised to 200° C., the vacuum was evacuated to 300 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0067] The temperature was further increased to 220° C., the vacuum was evacuated to 20 Pa, and the reaction was carried out for 4.0 hours to obtain polyethylene 2,5-thiophenedicarboxylic acid 3,4-thiophenedicarboxylic acid adipate glycol copolyester.

[0068] like Figure 1 The poly(2,5-thiophenedicarboxylic acid, 3,4-thiophenedicarboxylic acid, ethylene glycol adipate) copolyester prepared in this embodiment is shown in FIG. 1 H-NMR spectrum, where 11.63ppm is the peak of the solvent trifluoroacetic acid, 8.69ppm is the H peak on the five-membered thiophene ring of 3,4-thiophenedicarboxylic acid (2H), 7.93ppm is the H peak on the five-membered thiophene ring of 2,5-thiophenedicarboxylic acid (2H), 2.57ppm is the H peak on CH2 close to the carboxyl group on the adipic acid chain (4H), 1.79ppm is the H peak of CH2 in the middle position of the adipic acid chain (4H), and 4.50ppm-4.86ppm are the H peaks on ethylene glycol (4H).

[0069] like Figure 2 The DSC curve of the poly(2,5-thiophenedicarboxylic acid, 3,4-thiophenedicarboxylic acid, ethylene glycol adipate) copolyester prepared in this embodiment is shown in the figure. g It is -29.2°C and the melting enthalpy is 20.95 J / g.

[0070] like Figure 3 The TGA curve of the poly (2,5-thiophenedicarboxylic acid, 3,4-thiophenedicarboxylic acid, adipate) copolyester prepared in this embodiment is shown in the figure. It can be seen from the figure that the temperature (T d,5% ) is 335℃.

[0071] like Figure 4 The stress-strain curve of the poly (2,5-thiophenedicarboxylic acid, 3,4-thiophenedicarboxylic acid, ethylene glycol adipate) copolyester prepared in this embodiment is shown. As can be seen from the figure, the tensile modulus is 38 MPa, the tensile strength is 12.6 MPa, and the elongation at break is 779%.

[0072] After testing, the CO2 permeability coefficient of the poly (2,5-thiophenedicarboxylic acid, 3,4-thiophenedicarboxylic acid, ethylene glycol adipate) copolyester prepared in this embodiment is 9.64×10 -11 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 7.36×10 -11 cm 3 cm / cm 2 ·s·cmHg, can be biodegraded, and the mass loss in 30 days is 76.3%.

[0073] Example 2

[0074] 0.05 mol of 2,5-thiophenedicarboxylic acid, 0.05 mol of 3,4-thiophenedicarboxylic acid, 0.4 mol of adipic acid, 0.8 mol of 1,3-propylene glycol and 0.1% of the theoretical mass of the high crystallinity copolyester product tetrabutyl titanate are put into a reactor to obtain a first mixed reaction system. The first mixed reaction system is evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system is gradually increased to 180° C., and the reaction is carried out for 4.0 hours to obtain an esterification product.

[0075] 0.12% of triphenyl phosphate of the theoretical mass of high crystallinity copolyester product was added to the reactor, the temperature was raised to 200°C, the vacuum was pumped to 300Pa, and the reaction was carried out for 0.5h to obtain a prepolymer product. The temperature was further raised to 220°C, the vacuum was pumped to 20Pa, and the reaction was carried out for 4.0h to obtain a high crystallinity copolyester.

[0076] After testing, the T of the high crystallinity copolyester obtained in this embodiment is g The temperature (T d,5% ) is 344℃, the tensile modulus is 35MPa, the tensile strength is 14.1MPa, the elongation at break is 720%, and the CO2 permeability coefficient is 9.06×10 -11 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 5.29×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0077] Example 3

[0078] 0.005 mol of 2,5-thiophenedicarboxylic acid, 0.095 mol of 3,4-thiophenedicarboxylic acid, 0.4 mol of adipic acid, 0.8 mol of 2-methyl-1,3-propanediol and 0.05% of the theoretical mass of the high-crystallinity copolyester product isopropyl titanate are put into a reactor to obtain a first mixed reaction system. The first mixed reaction system is evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system is gradually increased to 170° C., and the reaction is carried out for 6.0 hours to obtain an esterification product.

[0079] 0.1% of phosphorous acid based on the theoretical mass of the high crystallinity copolyester product was added to the reactor, the temperature was raised to 180° C., the vacuum was evacuated to 300 Pa, and the reaction was carried out for 1.0 h to obtain a prepolymerized product.

[0080] The temperature was further increased to 220° C., the vacuum was evacuated to 20 Pa, and the reaction was carried out for 4.0 hours to obtain a high-crystallinity copolyester.

[0081] After testing, the T of the high crystallinity copolyester obtained in this embodiment is g is -37.0℃, the melting enthalpy is 27.44J / g, and the temperature at which the mass loss is 5% (T d,5% ) is 356℃, the tensile modulus is 44MPa, the tensile strength is 16.8MPa, the elongation at break is 622%, and the CO2 permeability coefficient is 8.37×10 -11 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 5.64×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0082] Example 4

[0083] 0.095 mol of 2,5-thiophenedicarboxylic acid, 0.005 mol of 3,4-thiophenedicarboxylic acid, 0.4 mol of adipic acid, 0.8 mol of 2,2-dimethyl-1,3-propanediol and 0.01% of the theoretical mass of the high-crystallinity copolyester product isopropyl titanate are put into a reactor to obtain a first mixed reaction system. The first mixed reaction system is evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system is gradually increased to 180° C., and the reaction is carried out for 4.0 hours to obtain an esterification product.

[0084] 0.01% of hypophosphorous acid of the theoretical mass of the high crystallinity copolyester product was added to the reactor, the temperature was raised to 200° C., the vacuum was evacuated to 50 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0085] The temperature was further increased to 220° C., the vacuum was evacuated to 20 Pa, and the reaction was carried out for 1.5 hours to obtain a high-crystallinity copolyester.

[0086] After testing, the T of the high crystallinity copolyester obtained in this embodiment is g The temperature (T d,5% ) is 367℃, the tensile modulus is 48MPa, the tensile strength is 20.8MPa, the elongation at break is 586%, and the CO2 permeability coefficient is 1.01×10 -10 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 6.50×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0087] Example 5

[0088] 0.004 mol of 2,5-thiophenedicarboxylic acid, 0.001 mol of 3,4-thiophenedicarboxylic acid, 0.495 mol of adipic acid, 0.8 mol of 1,4-butanediol and 0.5% of the theoretical mass of the high crystallinity copolyester product of dibutyltin oxide were put into a reactor to obtain a first mixed reaction system. The first mixed reaction system was evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system was gradually increased to 140° C., and the reaction was carried out for 8.0 hours to obtain an esterification product.

[0089] 0.5% pyrophosphoric acid of the theoretical mass of the high crystallinity copolyester product was added to the reactor, the temperature was raised to 180° C., the vacuum was evacuated to 300 Pa, and the reaction was carried out for 1.0 h to obtain a prepolymerized product.

[0090] The temperature was further increased to 200° C., the vacuum was evacuated to 20 Pa, and the reaction was carried out for 10.0 h to obtain a high-crystallinity copolyester.

[0091] After testing, the T of the high crystallinity copolyester obtained in this embodiment is g The temperature (T d,5% ) is 353℃, the tensile modulus is 31MPa, the tensile strength is 25.7MPa, the elongation at break is 826%, and the CO2 permeability coefficient is 1.08×10 -10 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 8.22×10 -11 cm 3 cm / cm 2·s·cmHg, biodegradable.

[0092] Example 6

[0093] 0.06 mol of 2,5-thiophenedicarboxylic acid, 0.04 mol of 3,4-thiophenedicarboxylic acid, 0.4 mol of adipic acid, 0.8 mol of 1,5-pentanediol and 0.1% of the theoretical mass of the high-crystallinity copolyester product in anhydrous zinc acetate were put into a reactor to obtain a first mixed reaction system. The first mixed reaction system was evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system was gradually increased to 180° C., and the reaction was carried out for 4.0 hours to obtain an esterification product.

[0094] 0.1% antimony trioxide and 0.12% trimethyl phosphate of the theoretical mass of the high crystallinity copolyester product were added to the reactor, the temperature was raised to 200° C., the vacuum was evacuated to 300 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0095] The temperature was further increased to 220° C., the vacuum was evacuated to 20 Pa, and the reaction was carried out for 4.0 hours to obtain a high-crystallinity copolyester.

[0096] After testing, the T of the high crystallinity copolyester obtained in this embodiment is g The temperature (T d,5% ) is 348℃, the tensile modulus is 110MPa, the tensile strength is 24.3MPa, the elongation at break is 483%, and the CO2 permeability coefficient is 6.38×10 -11 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 4.60×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0097] Example 7

[0098] 0.03 mol of 2,5-thiophenedicarboxylic acid, 0.07 mol of 3,4-thiophenedicarboxylic acid, 0.4 mol of adipic acid, 0.8 mol of 1,6-hexanediol and 0.1% of the theoretical mass of the high crystallinity copolyester product tetrabutyl titanate are put into a reactor to obtain a first mixed reaction system. The first mixed reaction system is evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system is gradually increased to 180° C., and the reaction is carried out for 4.0 hours to obtain an esterification product.

[0099] 0.12% of the theoretical mass of triphenyl phosphate of the high crystallinity copolyester product was added to the reactor, the temperature was raised to 200° C., the vacuum was evacuated to 700 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0100] The temperature was further increased to 220° C., the vacuum was evacuated to 20 Pa, and the reaction was carried out for 4.0 hours to obtain a high-crystallinity copolyester.

[0101] After testing, the T of the high crystallinity copolyester obtained in this embodiment is g is -51.0℃, the melting enthalpy is 29.17J / g, and the temperature at which the mass loss is 5% (T d,5% ) is 353℃, the tensile modulus is 86MPa, the tensile strength is 18.8MPa, the elongation at break is 862%, and the CO2 permeability coefficient is 8.19×10 -11 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 6.34×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0102] Example 8

[0103] 0.02 mol of 2,5-thiophenedicarboxylic acid, 0.08 mol of 3,4-thiophenedicarboxylic acid, 0.4 mol of adipic acid, 0.8 mol of 1,8-octanediol and 0.1% of the theoretical mass of the high-crystallinity copolyester product in germanium oxide were put into a reactor to obtain a first mixed reaction system. The first mixed reaction system was evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system was gradually increased to 180° C., and the reaction was carried out for 4.0 hours to obtain an esterification product.

[0104] 0.12% of the theoretical mass of triphenyl phosphate of the high crystallinity copolyester product was added to the reactor, the temperature was raised to 200° C., the vacuum was evacuated to 300 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0105] The temperature was further increased to 220° C., the vacuum was evacuated to 20 Pa, and the reaction was carried out for 4.0 hours to obtain a high-crystallinity copolyester.

[0106] After testing, the T of the high crystallinity copolyester obtained in this embodiment is g is -58.2°C, the melting enthalpy is 37.80 J / g, and the temperature at which the mass loss is 5% (T d,5% ) is 334℃, the tensile modulus is 62MPa, the tensile strength is 15.2MPa, the elongation at break is 649%, and the CO2 permeability coefficient is 9.34×10 -11 cm 3 cm / cm2 ·s·cmHg, O2 permeability coefficient is 7.81×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0107] Example 9

[0108] 0.0495 mol of dimethyl 2,5-thiophenedicarboxylate, 0.4455 mol of dimethyl 3,4-thiophenedicarboxylate, 0.005 mol of dimethyl adipate, 1.5 mol of 1,10-decanediol and 0.1% of the theoretical mass of the high crystallinity copolyester product tetrabutyl titanate were put into a reactor to obtain a first mixed reaction system. The first mixed reaction system was evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system was gradually increased to 180° C., and the reaction was carried out for 4.0 hours to obtain an esterification product.

[0109] 0.12% of the theoretical mass of triphenyl phosphate of the high crystallinity copolyester product was added to the reactor, the temperature was raised to 200° C., the vacuum was evacuated to 300 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0110] The temperature was further increased to 220° C., the vacuum was evacuated to 5 Pa, and the reaction was carried out for 4.0 h to obtain a high-crystallinity copolyester.

[0111] After testing, the T of the high crystallinity copolyester obtained in this embodiment is g The temperature at which the mass loss is 5% (T d,5% ) is 382℃, the tensile modulus is 136MPa, the tensile strength is 5.7MPa, the elongation at break is 320%, and the CO2 permeability coefficient is 8.95×10 -13 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 2.55×10 -12 cm 3 cm / cm 2 ·s·cmHg, biodegradation can occur, but the degradation rate is extremely slow.

[0112] Example 10

[0113] 0.09 mol of dimethyl 2,5-thiophenedicarboxylate, 0.01 mol of dimethyl 3,4-thiophenedicarboxylate, 0.4 mol of dibutyl adipate, 0.4 mol of ethylene glycol, 0.4 mol of 1,5-pentanediol and 0.1% of the theoretical mass of the high crystallinity copolyester product tetrabutyl titanate were put into a reactor to obtain a first mixed reaction system. The first mixed reaction system was evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system was gradually increased to 180° C. and the reaction was carried out for 4.0 hours to obtain an esterification product.

[0114] 0.5% of the theoretical mass of the high crystallinity copolyester product triphenyl phosphate was added into the reactor, the temperature was raised to 200° C., the vacuum was evacuated to 300 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0115] The temperature was further increased to 220° C., the vacuum was evacuated to 20 Pa, and the reaction was carried out for 4.0 hours to obtain a high-crystallinity copolyester.

[0116] After testing, the T of the high crystallinity copolyester obtained in this embodiment is g The temperature at which the mass loss is 5% (T d,5% ) is 344℃, the tensile modulus is 58MPa, the tensile strength is 19.3MPa, the elongation at break is 658%, and the CO2 permeability coefficient is 8.53×10 -11 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 6.23×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0117] Embodiment 11

[0118] 0.08 mol of 2,5-thiophenedicarboxylic acid, 0.02 mol of 3,4-thiophenedicarboxylic acid, 0.4 mol of adipic acid, 0.7 mol of ethylene glycol, 0.1 mol of 1,4-cyclohexanedimethanol and 0.1% of the theoretical mass of the high-crystallinity copolyester product tetrabutyl titanate were put into a reactor to obtain a first mixed reaction system. The first mixed reaction system was evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system was gradually increased to 180° C. and the reaction was carried out for 4.0 hours to obtain an esterification product.

[0119] 0.12% of the theoretical mass of the high crystallinity copolyester product triphenyl phosphate was added into the reactor, the temperature was raised to 200° C., the vacuum was evacuated to 300 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0120] The temperature was further increased to 220° C., the vacuum was evacuated to 20 Pa, and the reaction was carried out for 4.0 hours to obtain a high-crystallinity copolyester.

[0121] After testing, the T of the high crystallinity copolyester obtained in this embodiment is g is -27.1°C, the melting enthalpy is 34.09 J / g, and the temperature at which the mass loss is 5% (T d,5% ) is 343℃, the tensile modulus is 51MPa, the tensile strength is 14.4MPa, the elongation at break is 672%, and the CO2 permeability coefficient is 8.95×10 -11 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 6.07×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0122] Example 12

[0123] Some embodiments of the present invention also provide uses of the high crystallinity copolyester, such as preparing packaging bags, barrier films, fibers, etc.

[0124] Comparative Example 1

[0125] 0.5 mol of 2,5-thiophenedicarboxylic acid, 0.8 mol of ethylene glycol and 0.1% of the theoretical mass of the polyester product in anhydrous zinc acetate were added into a reactor to obtain a first mixed reaction system. The first mixed reaction system was evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system was gradually increased to 180° C. and the reaction was carried out for 4.0 hours to obtain an esterification product.

[0126] 0.1% antimony trioxide and 0.1% triphenyl phosphate of the theoretical mass of the polyester product were added into the reactor, the temperature was raised to 220° C., the vacuum was evacuated to 400 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0127] The temperature was further increased to 240° C., the vacuum was evacuated to 15 Pa, and the reaction was carried out for 4.0 h to obtain poly(ethylene thiophene dicarboxylate).

[0128] After testing, the T of the polythiophene dicarboxylic acid glycol ester obtained in this comparative example is g is 64.6℃, melting enthalpy is 1.40J / g, T d,5% The temperature is 409℃, the tensile modulus is 1775MPa, the tensile strength is 66.2MPa, the elongation at break is 380%, and the CO2 permeability coefficient is 7.50×10 -13 cm 3 cm / cm 2·s·cmHg, O2 permeability coefficient is 9.02×10 -13 cm 3 cm / cm 2 ·s·cmHg, cannot be biodegraded.

[0129] Comparative Example 2

[0130] 0.5 mol of adipic acid, 0.8 mol of ethylene glycol and 0.1% of the theoretical mass of the polyester product of tetrabutyl titanate are put into a reactor to obtain a first mixed reaction system. The first mixed reaction system is evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system is gradually increased to 180°C and reacted for 4.0 hours to obtain an esterification product.

[0131] 0.1% of triphenyl phosphate based on the theoretical mass of the polyester product was added into the reactor, the temperature was raised to 200° C., the vacuum was evacuated to 500 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0132] The temperature was further increased to 210° C., the mixture was evacuated to 10 Pa, and the reaction was carried out for 7.0 h to obtain polyethylene adipate.

[0133] After testing, the polyethylene adipate T obtained in this comparative example g is -46.7℃, melting enthalpy is 15.83J / g, T d,5% The temperature is 301℃, the tensile modulus is 302MPa, the tensile strength is 13.5MPa, the elongation at break is 384%, and the CO2 permeability coefficient is 1.19×10 -10 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 8.50×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0134] Comparative Example 3

[0135] 0.1 mol of 2,5-thiophenedicarboxylic acid, 0.4 mol of 1,4-succinic acid, 0.8 mol of ethylene glycol and 0.15% of the theoretical mass of the polyester product of anhydrous zinc acetate are put into a reactor to obtain a first mixed reaction system. The first mixed reaction system is evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system is gradually increased to 180° C., and the reaction is carried out for 4.0 hours to obtain an esterification product.

[0136] 0.1% antimony trioxide and 0.12% triphenyl phosphate of the theoretical mass of the polyester product were added into the reactor, the temperature was raised to 210° C., the vacuum was evacuated to 500 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0137] The temperature was further increased to 230° C., the vacuum was evacuated to 20 Pa, and the reaction was carried out for 5.0 h to obtain polythiophenedicarboxylic acid succinate.

[0138] After testing, the T of the polythiophene dicarboxylic acid succinic acid glycol ester obtained in this embodiment is g The temperature (T d,5% ) is 350℃, the tensile modulus is 64MPa, the tensile strength is 15.4MPa, the elongation at break is 506%, and the CO2 permeability coefficient is 7.03×10 -11 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 2.62×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradation can occur, but the degradation rate is slower than that in Example 1.

[0139] Comparative Example 4

[0140] Comparative Example 4 was carried out with reference to Example 8, except that 3,4-thiophenedicarboxylic acid was replaced by 2,5-thiophenedicarboxylic acid.

[0141] After testing, the T of the polyester obtained in this embodiment is g The temperature at which the mass loss is 5% (T d,5% ) is 341℃, the tensile modulus is 78MPa, the tensile strength is 17.0MPa, the elongation at break is 507%, and the CO2 permeability coefficient is 5.35×10 -11 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 4.72×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0142] Comparative Example 5

[0143] Comparative Example 4 was carried out with reference to Example 8, except that 2,5-thiophenedicarboxylic acid was replaced by 3,4-thiophenedicarboxylic acid.

[0144] After testing, the T of the polyester obtained in this embodiment is gThe temperature at which the mass loss is 5% (T d,5% ) is 330℃, the tensile modulus is 54MPa, the tensile strength is 12.7MPa, the elongation at break is 726%, and the CO2 permeability coefficient is 2.35×10 -10 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 8.68×10 -11 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0145] Comparative Example 6

[0146] 0.05 mol of 2,5-thiophenedicarboxylic acid, 0.05 mol of 3,4-thiophenedicarboxylic acid, 0.4 mol of adipic acid, 0.2 mol of 1,4-cyclohexanedimethanol, 0.5 mol of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 0.1% of the theoretical mass of the polyester product tetrabutyl titanate are put into a reactor to obtain a first mixed reaction system. The first mixed reaction system is evacuated and replaced with nitrogen three times. Under nitrogen protection, the temperature of the first mixed reaction system is gradually increased to 180° C. and the reaction is carried out for 4.0 hours to obtain an esterification product.

[0147] 0.12% of triphenyl phosphate based on the theoretical mass of the polyester product was added into the reactor, the temperature was raised to 200° C., the vacuum was evacuated to 300 Pa, and the reaction was carried out for 0.5 h to obtain a prepolymerized product.

[0148] The temperature was further raised to 220° C., the vacuum was evacuated to 20 Pa, and the reaction was carried out for 4.0 hours to obtain copolyester.

[0149] After testing, the T of the copolyester obtained in this embodiment is g The temperature at which the mass loss is 5% (T d,5% ) is 379℃, the tensile modulus is 839MPa, the tensile strength is 49.1MPa, the elongation at break is 111%, and the CO2 permeability coefficient is 7.33×10 -12 cm 3 cm / cm 2 ·s·cmHg, O2 permeability coefficient is 6.85×10 -12 cm 3 cm / cm 2 ·s·cmHg, biodegradable.

[0150] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0151] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a high crystallinity copolyester, characterized in that: The following steps are involved: 0.0495 mol of dimethyl 2,5-thiophenedicarboxylate, 0.4455 mol of dimethyl 3,4-thiophenedicarboxylate, 0.005 mol of dimethyl adipate, 1.5 mol of 1,10-decanediol, and 0.1% of the theoretical mass of the high-crystallinity copolyester product tetrabutyl titanate are added into a reactor to obtain a first mixed reaction system, the first mixed reaction system is evacuated and replaced with nitrogen three times, and under nitrogen protection, the temperature of the first mixed reaction system is gradually increased to 180° C., and the reaction is carried out for 4.0 hours to obtain an esterification product; Add 0.12% of triphenyl phosphate based on the theoretical mass of the high crystallinity copolyester product into the reactor, raise the temperature to 200° C., evacuate to 300 Pa, and react for 0.5 h to obtain a prepolymer product; The temperature was further increased to 220° C., the vacuum was evacuated to 5 Pa, and the reaction was carried out for 4.0 h to obtain a high-crystallinity copolyester.

2. A high crystallinity copolyester, characterized in that: The high crystallinity copolyester is prepared by the preparation method of claim 1.