Bio-based polyurethane millstone coating and application thereof, bio-based polyurethane millstone floor and preparation method thereof
Through the use of bio-based polyurethane grindstone coating, the problems of high rigidity and high cost of terrazzo floor materials are solved, and a floor solution with crack resistance, high durability and high aesthetics is realized, which is suitable for a variety of places and is environmentally friendly. and carbon neutrality standards.
Patent Information
- Application Number
- CN202410955345.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The existing terrazzo floor material is rigid, easy to crack, difficult to construct, non-renewable, and costly, making it difficult to meet the needs of indoor entertainment venues with strong design and high update speed.
Bio-based polyurethane grindstone coating is used, including component A and component B. Component A is composed of bio-based polyester polyol, defoaming agent, pigment, quartz powder and coarse aggregate, and component B is modified polyisocyanate. , through strict control of the component ratio, a polyurethane grindstone floor that is resistant to cracking, weathering and wear is formed, and meets the national carbon neutral standard.
The polyurethane grindstone floor has high crack resistance, durability and aesthetics, long life cycle, seamless overall, light weight, meets the requirements of environmental protection and low cost, and is suitable for a variety of indoor and outdoor places.
Smart Images

Figure BDA0004948803650000071 
Figure BDA0004948803650000101 
Figure HDA0004948803710000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and specifically relates to a bio-based polyurethane terrazzo coating and an application thereof, a bio-based polyurethane terrazzo floor and a preparation method thereof. Background Art
[0002] Flooring refers to the floor that is constructed using specific materials and processes to present a certain decorative and functional floor, such as epoxy self-leveling floor, corundum wear-resistant floor, epoxy terrazzo floor, cement-based terrazzo, epoxy colored sand floor, epoxy anti-static floor, epoxy anti-slip floor, polyurea anti-corrosion floor, polyurethane floor, silicon PU floor, concrete sealing and curing agent floor, etc.
[0003] Terrazzo floor is a type of floor. Terrazzo is a product made by mixing crushed stone, glass, quartz stone and other aggregates into cement binder to form a concrete product, and then surface grinding and polishing. Terrazzo made of cement binder is called inorganic terrazzo, and terrazzo made of epoxy binder is called epoxy terrazzo or organic terrazzo. Terrazzo is divided into on-site cast terrazzo and prefabricated terrazzo floor according to the construction and production process.
[0004] However, the commonly used terrazzo floors mentioned above have the following problems: the base material is generally rigid cement or thermosetting epoxy resin, the material itself is very rigid / brittle, and is prone to cracking due to environmental changes and uneven force; it is very hard, and its poor flexibility when used in indoor public places affects the comfort experience, and it is easy to cause noise pollution; it is difficult to construct and non-renewable, and is not suitable for indoor entertainment venues with a strong sense of design and a high update speed.
[0005] Chinese patent CN113549389A discloses a renewable elastic polyurethane grinding stone material and its application, but the raw materials of the polyurethane grinding stone material disclosed in the patent are complex and the cost is high. Summary of the invention
[0006] The purpose of the present invention is to provide a bio-based polyurethane terrazzo coating and its application, a bio-based polyurethane terrazzo floor and its preparation method. The polyurethane terrazzo floor formed by the bio-based polyurethane terrazzo coating provided by the present invention has excellent anti-cracking performance, weather resistance, durability and wear resistance, and has a long life cycle, high aesthetics, seamless overall, resistant to concrete cracks, and no other anti-cracking layer is required, and the dead weight is light. At the same time, the bio-based polyurethane terrazzo coating provided by the present invention meets the national carbon neutrality standards and has the advantages of emission reduction, environmental protection and low cost.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] The present invention provides a bio-based polyurethane grinding stone coating, comprising component A and component B;
[0009] The A component includes the following components in percentage by weight:
[0010] Bio-based polyester polyol 60-80%, defoamer 4-5%, pigment 4-5%, quartz powder 7-18%, coarse aggregate 5-12%;
[0011] The B component is a curing agent, and the curing agent is a modified polyisocyanate.
[0012] Preferably, the mass ratio of component A to component B is (5-6):1.
[0013] Preferably, the bio-based polyester polyol is Savimo castor oil modified polyol.
[0014] Preferably, the mesh size of the quartz powder is 300-400 meshes; the average particle size of the coarse aggregate is 5-8 mm; the defoamer is a silicone defoamer; the coarse aggregate includes one or more of marble chips, glass, mine quartz, amethyst, turquoise, white marble, white crystal, colored glass, agate and shells.
[0015] The present invention provides the use of the bio-based polyurethane terrazzo coating described in the above technical solution in the preparation of polyurethane terrazzo flooring.
[0016] The present invention provides a method for preparing a bio-based polyurethane terrazzo floor, comprising the following steps:
[0017] Applying the terrazzo primer on the surface of the foundation to obtain a primer-treated foundation;
[0018] The components A and B of the bio-based polyurethane terrazzo coating described in the above technical solution are mixed to obtain a terrazzo mixture; the terrazzo mixture is coated on the surface of the foundation treated with the primer to obtain a bio-based polyurethane terrazzo surface layer, thereby obtaining the bio-based polyurethane terrazzo floor.
[0019] Preferably, the thickness of the bio-based polyurethane grindstone surface layer is 8 to 10 mm.
[0020] Preferably, after obtaining the primer-treated foundation and before coating the grindstone mixture, the method further comprises: preparing an elastic polyurethane leveling pad on the surface of the primer-treated foundation, wherein the thickness of the elastic polyurethane leveling pad is 3 to 5 mm.
[0021] Preferably, after obtaining the bio-based polyurethane terrazzo surface layer, the process further comprises sealing the bio-based polyurethane terrazzo surface layer with a covering material to obtain a covering layer, thereby obtaining the bio-based polyurethane terrazzo floor.
[0022] The present invention provides a bio-based polyurethane terrazzo floor prepared by the preparation method described in the above technical solution.
[0023] The present invention provides a bio-based polyurethane terrazzo coating, comprising component A and component B; the component A comprises the following components in percentage by mass: 60-80% of bio-based polyester polyol, 4-5% of defoamer, 4-5% of pigment, 7-18% of quartz powder, and 5-12% of coarse aggregate; the component B is a curing agent, and the curing agent is a modified polyisocyanate. The present invention uses bio-based polyester polyol as the main component of the polyurethane terrazzo coating, and auxiliary defoamer, pigment, quartz powder filler and coarse aggregate as auxiliary components. By strictly controlling the mass ratio of the above components, the obtained bio-based polyurethane terrazzo coating has a high solid content, and the formed polyurethane terrazzo floor has excellent crack resistance, weather resistance, durability and wear resistance, and has a long life cycle, high aesthetics, overall seamlessness, concrete crack resistance, and no other anti-cracking layer is required, and the dead weight is light.
[0024] At the same time, the present invention uses renewable bio-based polyester polyols as bio-based raw materials to replace traditional fossil raw materials. The bio-based polyester polyols are produced by processing biomass such as soybean oil or castor oil as raw materials. The bio-based content of the bio-based polyester polyols is as high as 65-100%. Therefore, the bio-based polyurethane grindstone coating provided by the present invention meets the national carbon neutrality standards and has the advantages of emission reduction, environmental protection and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a physical picture of the bio-based polyurethane terrazzo floor prepared according to an embodiment of the present invention. DETAILED DESCRIPTION
[0026] The present invention provides a bio-based polyurethane grinding stone coating, comprising component A and component B;
[0027] The A component includes the following components in percentage by weight:
[0028] Bio-based polyester polyol 60-80%, defoamer 4-5%, pigment 4-5%, quartz powder 7-18%, coarse aggregate 5-12%;
[0029] The B component is a curing agent, and the curing agent is a modified polyisocyanate.
[0030] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.
[0031] The bio-based polyurethane grinding stone coating provided by the present invention comprises an A component.
[0032] In terms of mass percentage, the A component comprises 60-80% of bio-based polyester polyol, preferably 65-75%. In the present invention, the bio-based polyester polyol is Savimore castor oil modified polyol. In a specific embodiment of the present invention, the bio-based polyester polyol is specifically Savimore castor oil modified polyol produced by BASF.
[0033] In terms of mass percentage, the component A includes 4-5%, preferably 4.2-4.5% of the defoamer. In the present invention, the defoamer is preferably an organosilicon defoamer.
[0034] In terms of mass percentage, the component A includes 4-5% of pigment, preferably 4.2-4.6%. In the present invention, the pigment is preferably polyurethane pigment.
[0035] In terms of mass percentage, the component A comprises 7-18% quartz powder, preferably 7.5-15%. In the present invention, the mesh size of the quartz powder is 300-400 meshes.
[0036] In terms of mass percentage, the A component includes 5-12% coarse aggregate, preferably 5-10%. In the present invention, the coarse aggregate preferably includes one or more of marble chips, glass, mine quartz, amethyst, turquoise, white marble, white crystal, colored glass, agate and shell. The average particle size of the coarse aggregate is preferably 5-8 mm.
[0037] The bio-based polyurethane grinding stone coating provided by the present invention comprises component B. The component B is a curing agent, and the curing agent is a modified polyisocyanate. In a specific embodiment of the present invention, the modified polyisocyanate is specifically purchased from BASF, and the product model is HI100 curing agent.
[0038] In the present invention, the mass ratio of the component A to the component B is preferably (5-6):1, more preferably 5:1.
[0039] The present invention provides the use of the bio-based polyurethane terrazzo coating described in the above technical solution in the preparation of polyurethane terrazzo flooring.
[0040] The bio-based polyurethane terrazzo coating provided by the present invention has light weight, low load, excellent resistance to foundation deformation, and UV resistance without yellowing. The bio-based polyurethane terrazzo coating provided by the present invention is preferably used in the ground of indoor and outdoor places such as ships, offices, medical treatment, education, entertainment, residences, exhibition halls or retail, such as luxury cruise ships, luxury CBD office spaces, hospitals, schools, hotels, commercial plazas, administrative offices, corporate exhibition halls, museums, libraries, art galleries, civic centers, research institutes, shops or private villas. The base surface of the application preferably includes: a cement-based base surface, a glass-top building base surface or a steel structure base surface.
[0041] The present invention provides a method for preparing a bio-based polyurethane terrazzo floor, comprising the following steps:
[0042] Applying the terrazzo primer on the surface of the foundation to obtain a primer-treated foundation;
[0043] The components A and B of the bio-based polyurethane terrazzo coating described in the above technical solution are mixed to obtain a terrazzo mixture; the terrazzo mixture is coated on the surface of the foundation treated with the primer to obtain a bio-based polyurethane terrazzo surface layer, thereby obtaining the bio-based polyurethane terrazzo floor.
[0044] The present invention applies a grindstone primer (hereinafter referred to as the first coating) on the surface of the foundation to obtain a foundation after primer treatment. In the present invention, the foundation includes a cement foundation, a glass foundation or a steel structure foundation. Before applying the grindstone primer, the present invention preferably performs pretreatment on the surface of the foundation. In the present invention, the pretreatment preferably includes sandblasting, and the sandblasting is preferably performed using a vacuum sandblasting machine. When there are cracks on the surface of the foundation, the pretreatment preferably also includes: repairing the cracks on the surface of the foundation after sandblasting, and the repair is preferably performed when the cracks are 1 to 5 mm. The material used for the repair is preferably a mixture of polyurethane primer and quartz sand. The mass ratio of the polyurethane primer and quartz sand is preferably 3:1. During the repair, the present invention preferably extends at least 600 mm along the length direction of the crack, or covers all the foundation surface. In the present invention, the roughness level of the foundation surface after pretreatment is ≥CSP-3 level. The moisture content of the foundation surface is ≤8%. The foundation surface is preferably oil-free.
[0045] In the present invention, the grindstone primer is preferably a polyurethane primer, and the polyurethane primer preferably includes a polyurethane resin primer component and a curing agent. The present invention has no special requirements on the source of the polyurethane resin primer. During the first coating, the coating amount of the grindstone primer is preferably 0.13 to 0.22 kg / m 2 The first coating preferably includes beach coating and roller coating. The temperature of the first coating is preferably 10-25° C., and the time of the first coating is ≤30 min.
[0046] In the present invention, after obtaining the primer-treated foundation and before applying the grindstone mixture, the present invention further comprises: preparing an elastic polyurethane leveling pad on the primer-treated foundation surface, and the thickness of the elastic polyurethane leveling pad is preferably 3 to 5 mm. In the present invention, the polyurethane paint used for the elastic polyurethane leveling pad preferably includes a polyurethane resin component and a curing agent. The present invention has no special requirements for the preparation method of the elastic polyurethane leveling pad.
[0047] After obtaining the primer-treated foundation or the elastic polyurethane leveling cushion, the present invention mixes the A component and the B component of the bio-based polyurethane grindstone coating described in the above technical solution to obtain a grindstone mixture; the grindstone mixture is coated (hereinafter referred to as the second coating) on the primer-treated foundation or the elastic polyurethane leveling cushion surface to obtain a bio-based polyurethane grindstone surface layer, and the bio-based polyurethane grindstone floor is obtained. In the present invention, the mixing preferably includes the following steps: the bio-based polyester polyol in the A component and the B component are mixed for the first time to obtain a first mixture; the first mixture, the defoamer, the pigment and the quartz powder are mixed for the second time to obtain a second mixture; the second mixture and the coarse aggregate are mixed for the third time. The first mixing is preferably carried out in a drum mixer, the first mixing is preferably carried out under stirring conditions, and the first mixing time is preferably 2 minutes. The second mixing is preferably carried out under stirring conditions, and the second mixing is preferably carried out in a drum mixer. The present invention has no special requirements for the time of the second mixing, and it is sufficient to ensure that the above components are mixed evenly. The third mixing is preferably carried out under stirring conditions, and the third mixing time is preferably 3 to 4 minutes. In the present invention, the temperature of the second coating is preferably 10-35°C, and the time of the second coating is preferably ≤50min. The second coating is preferably performed by spreading the grindstone mixture along a straight line, and then flattening it with a straight-edged trowel to a suitable thickness with the maximum particle size of the aggregate, and using the trowel to flatten the aggregate. In the present invention, in order to improve the density of the bio-based polyurethane grindstone surface layer, the present invention preferably uses a mechanical troweling method for the final troweling construction. In the present invention, the initial grindstone surface layer is directly obtained after the second coating is completed. The present invention preferably cures the initial grindstone surface layer to obtain the bio-based polyurethane grindstone surface layer. The curing time is preferably 12-16h, and the temperature of the foundation during the curing is preferably 20-21°C.
[0048] In the present invention, the thickness of the bio-based polyurethane grindstone surface layer is preferably 8 to 10 mm.
[0049] A bio-based polyurethane grindstone surface layer is obtained. The present invention preferably performs post-treatment on the bio-based polyurethane grindstone surface layer, and the post-treatment preferably includes the following steps: grinding, slurry filling and polishing. The grinding preferably includes primary grinding and intermediate grinding. The primary grinding is preferably performed using a 24-56 mesh diamond grinding disc. When the coarse aggregate in the A component is preferably glass, the primary grinding is preferably wet grinding, and the wet grinding is specifically preferably: wet grinding using a diamond grinding head and coarse grinding using a lightweight grinder. The intermediate grinding is preferably performed using 80 mesh diamond sand or a diamond grinding disc.
[0050] After the grinding is completed, the present invention preferably cleans the grinding surface and then performs grouting. The grouting is preferably performed using the above-mentioned bio-based polyurethane grindstone coating. The grouting is preferably performed using a straight-edge trowel to scrape the grindstone mixed slurry on the surface and fill the slurry into the holes. After the grouting, the present invention preferably polishes the grouting surface within 18 to 24 hours at a foundation temperature of 24°C.
[0051] In the present invention, the polishing is preferably performed using a diamond grinding disc or a resin grinding disc with a mesh size of ≥120.
[0052] In the present invention, after the post-treatment is completed, the present invention preferably further comprises sealing the post-treated bio-based polyurethane terrazzo surface layer to obtain a topcoat layer to obtain the bio-based polyurethane terrazzo floor. The sealing is preferably performed using a topcoat material, and the topcoat material preferably includes a polyurethane terrazzo topcoat material or wax water. The sealing is preferably performed using a short-nap roller for roller coating. The number of times of roller coating is preferably ≥2 times.
[0053] The present invention provides a bio-based polyurethane terrazzo floor prepared by the preparation method described in the above technical solution. The bio-based polyurethane terrazzo floor provided by the present invention includes a bio-based polyurethane terrazzo surface layer arranged on the surface of the foundation after the primer treatment, and the thickness of the bio-based polyurethane terrazzo surface layer is preferably 8 to 10 mm. The bio-based polyurethane terrazzo floor provided by the present invention preferably also includes an elastic polyurethane leveling pad layer arranged between the foundation after the primer treatment and the bio-based polyurethane terrazzo surface layer, and the thickness of the elastic polyurethane leveling pad layer is preferably 3 to 5 mm. The bio-based polyurethane terrazzo floor provided by the present invention preferably also includes a topcoat layer arranged on the surface of the bio-based polyurethane terrazzo surface layer.
[0054] The bio-based polyurethane terrazzo floor provided by the present invention does not crack, is seamless as a whole, has quiet noise reduction, is comfortable to the feet, has Class A fire protection, is relatively non-slip, can be renewable and repeatedly renewed, is weather-resistant and aging-resistant, and does not yellow. It can be used in outdoor environments, and the applicable areas include: ships, high-end administrative office areas, medical institutions, education and entertainment, and other public spaces or private spaces indoor and outdoor fields. For example: luxury cruise ships, hospitals, schools, hotels, commercial plazas, administrative offices (including luxury CBD office spaces), corporate exhibition halls, museums, libraries, art galleries, civic centers, research institutes, shops, private villas, etc. It can be heavily pressed and can be used for outdoor or glass-top building areas, steel structures and other base surfaces.
[0055] The properties of the bio-based polyurethane terrazzo floor provided by the present invention and the epoxy terrazzo / inorganic terrazzo in the prior art are compared as shown in Table 1.
[0056] Table 1 Comparison of properties of the bio-based polyurethane terrazzo floor provided by the present invention and the epoxy terrazzo / inorganic terrazzo in the prior art
[0057]
[0058] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0059] Example 1
[0060] This embodiment provides a bio-based polyurethane grinding stone coating, including component A and component B; component A includes the following components in percentage by weight:
[0061] Bio-based polyester polyol (Savymo castor oil modified polyol produced by BASF) 80%, defoamer 4%, pigment 4%, quartz powder (300 mesh) 7%, coarse aggregate (average particle size of 5-8mm, marble chips and glass chips) 5%; the B component is a curing agent, and the curing agent is a modified polyisocyanate. The mass ratio of bio-based polyester polyol to modified polyisocyanate is 5:1.
[0062] This embodiment provides a bio-based polyurethane terrazzo floor, and the preparation method thereof specifically includes:
[0063] 1. Base surface treatment
[0064] 1) All base surfaces must be properly prepared to achieve a surface roughness requirement of at least CSP-3.
[0065] 2) The area where the floor is constructed must be closed and protected to avoid temperature fluctuations, be oil-free, and have a moisture content below 8%, otherwise the floor system may be damaged.
[0066] 3) Check the temperature of the area where the floor system needs to be constructed. The most suitable temperature for the construction of polyurethane is 10-25℃.
[0067] 2. Moisture meter test method: base moisture content test
[0068] The moisture content of the concrete base layer is determined by the moisture meter test method, and the moisture content cannot exceed 8%.
[0069] 3. Crack repair (if necessary)
[0070] 1) 1mm~5mm cracks: Use polyurethane primer and add quartz sand for repair (extending at least 600mm along the length of the seam, or covering all base surfaces).
[0071] 4. Separator setting (separator seam)
[0072] 1) Use separators: If you choose to use separators, you need to install separators. 2) If you need to have no separator effect, you can use other separation methods and remove the separators after the color separation is completed.
[0073] 5. Construction of special primer for grinding stone
[0074] If a water vapor barrier is required, it should be installed before the terrazzo-specific primer is applied.
[0075] 1) Mixing
[0076] The grindstone-specific primer A (polyurethane resin primer) component (resin) and component B (curing agent) are mixed according to a mass ratio, and mixed evenly using a low-speed agitator and a high-speed mixer.
[0077] Pour the mixed primer on the ground immediately and use it up within 30 minutes (spread and roll back and forth).
[0078] 2) Construction
[0079] Pour the primer onto a properly prepared concrete base.
[0080] Use a straight-edged trowel or rubber scraper to spread evenly, and use a short-haired roller to roll back and forth, making sure not to allow the primer to accumulate.
[0081] 6. Bio-based polyurethane grinding stone construction
[0082] 1) Mixing:
[0083] The bio-based polyester polyol in component A of the bio-based polyurethane grindstone coating and component B (curing agent) of the bio-based polyurethane grindstone coating were mixed according to a mass ratio and stirred at a low speed for 2 minutes in a drum mixer.
[0084] The defoamer, pigment and quartz powder are slowly added into the elastic polyurethane formed by mixing the above bio-based polyester polyol and curing agent, and stirred in a mixer until the filler is completely impregnated with the resin.
[0085] Continue stirring and add coarse aggregate, resin and ground stone aggregate and continue mixing for 3 to 4 minutes until there are no lumps and a uniform mixture is obtained.
[0086] After thorough mixing, use a cart or bucket to transport the material to the construction area. Note: The elastic polyurethane masterbatch must be mixed by mechanical stirring. The mixer must be thoroughly cleaned during mixing breaks or before adjusting the color of the elastic polyurethane resin mortar. Use alcohol to clean the equipment. If the construction time interval exceeds 40 to 50 minutes, the material should not be stirred too much. The construction temperature of the elastic polyurethane resin mortar should be between 10 and 35°C.
[0087] 2) Construction:
[0088] Carry out construction on the base surface after primer treatment and spread the material along a straight line.
[0089] Use a straight-edged trowel to level the surface, taking the maximum aggregate size as the appropriate thickness, and use the trowel to flatten the aggregate. To increase the volume and density of the elastic polyurethane resin mortar, a mechanical trowel method can be used for the final troweling construction. Common finishing machines: trowels with four 91 cm wide blades.
[0090] Ensure that the polyurethane resin mortar is cured for at least 12 to 16 hours (substrate temperature is 21°C)
[0091] 8. Sanding and grouting
[0092] 1) Primary grinding: Use a 24-56 mesh diamond grinding disc for grinding. If the aggregate ratio is 100% glass, use a diamond grinding head for wet grinding and a lightweight grinder for coarse grinding.
[0093] 2) Intermediate grinding: Before filling, use 80 mesh diamond sand or diamond grinding disc for intermediate grinding. Note: The machine should always be in motion, moving parallel at first and then across the ground in a diagonal direction.
[0094] 3) Cleaning: Clean the floor after sanding. Before filling, make sure the floor is clean and dry.
[0095] 4) Grouting: When filling, elastic polyurethane masterbatch of the same color must be used. After filling, it can be polished after 18 to 24 hours (the base surface temperature is 24°C).
[0096] 5) Mixing of elastic polyurethane masterbatch for grouting
[0097] Each component of the elastic polyurethane masterbatch should be thoroughly stirred before mixing.
[0098] The elastic polyurethane masterbatch component A (main agent) and component B (curing agent) were mixed according to the mass ratio and mixed for 3 minutes using a low-speed electric stirrer. The bio-based polyurethane millstone filler was added to the mixed bio-based polyurethane millstone slurry to form a paste slurry suitable for slurrying.
[0099] If the usage time exceeds 30 minutes, the materials should not be stirred too much.
[0100] Use a straight-edged trowel to firmly apply the elastic polyurethane masterbatch mortar to the surface and fill the mortar into the holes. Allow it to cure overnight before polishing. When filling the mortar, sprinkle the mortar filler on the filled surface to facilitate the absorption of excess resin mortar on the surface.
[0101] Finally, use a 120-mesh or higher diamond or resin grinding disc for polishing.
[0102] 9. Sealing
[0103] Bio-based polyurethane terrazzo floor should be sealed with polyurethane terrazzo topcoat or wax water and other topcoat materials. Note: If the polished floor has met the design requirements and the aesthetic requirements, there is no need to seal the floor surface. If sealing is required, please consult with the floor construction party.
[0104] 1) Mixing and application
[0105] Stir the liquid in the can thoroughly before use.
[0106] Use a short nap roller for application. Avoid material accumulation. Two or more coats are required to achieve the desired gloss level as in the approved sample or panel appearance. If multiple coats are required, allow each coat to dry completely before applying the next coat. Maintenance for 24 hours (substrate temperature 24°C).
[0107] The properties of the bio-based polyurethane terrazzo floor prepared in this embodiment are shown in Table 2. The actual picture of the bio-based polyurethane terrazzo floor prepared in this embodiment is as shown in Table 2. Figure 1 shown.
[0108] Table 2 Properties of bio-based polyurethane terrazzo floor prepared in Example 1
[0109]
[0110] Example 2
[0111] This embodiment provides a bio-based polyurethane grinding stone coating, including component A and component B; component A includes the following components in percentage by weight:
[0112] Bio-based polyester polyol (Savymo castor oil modified polyol produced by BASF) 72%, defoamer 5%, pigment 5%, quartz powder (300 mesh) 10%, coarse aggregate (average particle size of 5-8mm, marble chips and glass chips) 8%; the B component is a curing agent, and the curing agent is a modified polyisocyanate. The mass ratio of bio-based polyester polyol to modified polyisocyanate is 5:1.
[0113] The preparation method of the bio-based polyurethane terrazzo floor provided in this embodiment is the same as that in Example 1.
[0114] Example 3
[0115] This embodiment provides a bio-based polyurethane grinding stone coating, including component A and component B; component A includes the following components in percentage by weight:
[0116] Bio-based polyester polyol (Savymo castor oil modified polyol produced by BASF) 70%, defoamer 5%, pigment 5%, quartz powder (300 mesh) 10%, coarse aggregate (average particle size of 5-8mm, marble chips and glass chips) 10%; the B component is a curing agent, and the curing agent is a modified polyisocyanate. The mass ratio of bio-based polyester polyol to modified polyisocyanate is 5:1.
[0117] The preparation method of the bio-based polyurethane terrazzo floor provided in this embodiment is the same as that in Example 1.
[0118] Example 4
[0119] This embodiment provides a bio-based polyurethane grinding stone coating, including component A and component B; component A includes the following components in percentage by weight:
[0120] Bio-based polyester polyol (Savymo castor oil modified polyol produced by BASF) 63%, defoamer 5%, pigment 5%, quartz powder (300 mesh) 15%, coarse aggregate (average particle size of 5-8mm, marble chips and glass chips) 12%; the B component is a curing agent, and the curing agent is a modified polyisocyanate. The mass ratio of bio-based polyester polyol to modified polyisocyanate is 5:1.
[0121] The preparation method of the bio-based polyurethane terrazzo floor provided in this embodiment is the same as that in Example 1.
[0122] It can be seen from the above embodiments that the bio-based polyurethane terrazzo coating provided by the present invention includes component A and component B; the component A includes the following components in percentage by mass: 60-80% bio-based polyester polyol, 4-5% defoamer, 4-5% pigment, 7-18% quartz powder, 5-12% coarse aggregate, wherein the coarse aggregate is marble chips and / or glass; the component B is a curing agent, and the curing agent is a modified polyisocyanate. The present invention uses bio-based polyester polyol as the main component of the polyurethane terrazzo coating, and auxiliary defoamer, pigment, quartz powder filler and coarse aggregate as auxiliary components. By strictly controlling the mass ratio of the above components, the obtained bio-based polyurethane terrazzo coating has a high solid content, and the formed polyurethane terrazzo floor has excellent crack resistance, weather resistance, durability and wear resistance, and has a long life cycle, high aesthetics, seamless overall, anti-concrete crack resistance, and no other anti-cracking layer is required, and the deadweight is light.
[0123] At the same time, the present invention uses renewable bio-based polyester polyols as bio-based raw materials to replace traditional fossil raw materials. The bio-based polyester polyols are produced by processing biomass such as soybean oil or castor oil as raw materials. The bio-based content of the bio-based polyester polyols is as high as 65-100%. Therefore, the bio-based polyurethane grindstone coating provided by the present invention meets the national carbon neutrality standards and has the advantages of emission reduction, environmental protection and low cost.
[0124] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A bio-based polyurethane grinding stone coating, characterized in that: It includes component A and component B; The A component includes the following components in percentage by weight: Bio-based polyester polyol 60-80%, defoamer 4-5%, pigment 4-5%, quartz powder 7-18%, coarse aggregate 5-12%; The B component is a curing agent, and the curing agent is a modified polyisocyanate.
2. The bio-based polyurethane grinding stone coating according to claim 1, characterized in that: The mass ratio of component A to component B is (5-6):
1.
3. The bio-based polyurethane grinding stone coating according to claim 1 or 2, characterized in that: The bio-based polyester polyol is Savimo castor oil modified polyol.
4. The bio-based polyurethane grinding stone coating according to claim 1, characterized in that: The mesh number of the quartz powder is 300-400 meshes; the average particle size of the coarse aggregate is 5-8 mm; the defoamer is an organosilicon defoamer; the coarse aggregate includes one or more of marble chips, glass, mine quartz, amethyst, turquoise, white marble, white crystal, colored glass, agate and shells.
5. Use of the bio-based polyurethane terrazzo coating according to any one of claims 1 to 4 in the preparation of polyurethane terrazzo floors.
6. A method for preparing a bio-based polyurethane terrazzo floor, characterized in that: The following steps are involved: Applying the terrazzo primer on the surface of the foundation to obtain a primer-treated foundation; Mix component A and component B of the bio-based polyurethane terrazzo coating according to any one of claims 1 to 4 to obtain a terrazzo mixture; apply the terrazzo mixture on the foundation surface treated with the primer to obtain a bio-based polyurethane terrazzo surface layer, thereby obtaining the bio-based polyurethane terrazzo floor.
7. The preparation method according to claim 6, characterized in that: The thickness of the bio-based polyurethane grindstone surface layer is 8 to 10 mm.
8. The preparation method according to claim 6 or 7, characterized in that: After obtaining the primer-treated foundation and before coating the grindstone mixture, the method further comprises: preparing an elastic polyurethane leveling cushion layer on the primer-treated foundation surface, wherein the thickness of the elastic polyurethane leveling cushion layer is 3-5 mm.
9. The preparation method according to claim 6 or 7, characterized in that: After obtaining the bio-based polyurethane terrazzo surface layer, the method further comprises using a covering material to seal the bio-based polyurethane terrazzo surface layer to obtain a covering layer, thereby obtaining the bio-based polyurethane terrazzo floor.
10. The bio-based polyurethane terrazzo floor prepared by the preparation method according to any one of claims 6 to 9.
Citation Information
Patent Citations
Renewable elastic polyurethane millstone material and application thereof
CN113549389A
Solvent-free polyurethane gravity flow self-leveling floor material and preparing method
CN101270259A
Rigid solvent-free polyurethane self-leveling floor coating and preparation method thereof
CN107384179A
Solvent-free polyurethane floating color sand self-leveling floor material and preparation method thereof
CN117701139A
Floor coating
EP4386031A1
Cited By
Prefabricated pressure-resistant stretch-proof polyurethane plastic floor material and preparation method thereof