Preparation method of isohexitol-based polycarbonate copolymer

Through the optimization of diol ester exchange and gradient reaction conditions, combined with metal catalyst, the problems of low reaction activity and poor toughness in the preparation of isosorbate polycarbonate are solved, and high molecular weight, high heat resistance, high strength and high biological performance are achieved. The content of isohexitol-based polycarbonate copolymer is suitable for a variety of high-performance applications.

CN118994555AActive Publication Date: 2024-11-22DONGHUA UNIV

Patent Information

Application Number
CN202410371602.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-11-22
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

The existing isosorbate-based polycarbonate has problems such as low reactive activity, large melt viscosity, and poor toughness during the preparation process, making it difficult to prepare materials with high molecular weight, high heat resistance, high strength and high biological content.

Method used

The transesterification reaction, pre-polycondensation reaction and final polycondensation reaction of diol A1 and diol A2 are adopted. By controlling the molar ratio and gradient heating and pressure reduction conditions, metal catalysts are combined to improve molecular weight and toughness while maintaining high biological content.

Benefits of technology

It has achieved high molecular weight, high heat resistance, high strength, high toughness and high biological content of isohexitol-based polycarbonate copolymer, and is suitable for engineering plastics and films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004765704840000052
    Figure BDA0004765704840000052
  • Figure BDA0004765704840000061
    Figure BDA0004765704840000061
Patent Text Reader

Abstract

The invention relates to a preparation method of an isohexitol-based polycarbonate copolymer, which comprises the following steps: sequentially carrying out transesterification, pre-polycondensation reaction and final polycondensation reaction on dihydric alcohol and diester carbonate under the action of a catalyst to obtain the isohexitol-based polycarbonate copolymer, the dihydric alcohol comprises dihydric alcohol A1 and dihydric alcohol A2, or further comprises dihydric alcohol A3; the dihydric alcohol A1 is isohexitol; the molecular structural formula of the dihydric alcohol A2 contains a cyclic ether structure and two primary hydroxyl groups, and the primary hydroxyl groups are connected with the cyclic ether structure through a methylene group; the dihydric alcohol A3 is a dihydroxy compound; during the pre-polycondensation reaction, firstly, the temperature is gradually increased to 180-200 DEG C within 5-15 min, then the pressure is gradually reduced to 45-55 kPa within 5 min, and finally gradient temperature rise and gradient pressure reduction are performed. The copolymer prepared by the invention has high molecular weight, high heat resistance, high strength, high toughness and transparency, and is wide in application field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polycarbonate preparation, and relates to a method for preparing an isohexitol-based polycarbonate copolymer. Background Art

[0002] Polycarbonate (PC) has become one of the five fastest-growing engineering plastics due to its excellent thermal, mechanical and optical properties, and can be widely used in automotive parts, electronics / electrical, film / sheet, appliances / household goods and optical media. The most representative of these is bisphenol A polycarbonate (BPA-PC). However, bisphenol A (BPA), one of the main raw materials for bisphenol A polycarbonate, has chronic toxicity and can interfere with human endocrine. Studies have shown that bisphenol A in plastic products can penetrate into food and beverages and enter the human body, causing harm to human health, especially infants. Many countries have introduced policies to ban plastic products such as BPA bottles. BPA comes from non-renewable petroleum-based resources. In response to the call for green chemistry and sustainable development, it is of great significance to find green monomers that can replace bisphenol A and greener and safer processes.

[0003] Unlike petroleum-based resources, bio-based resources come from renewable green resources, such as sugar, starch, cellulose, vegetable oil, etc. Replacing traditional petroleum-based resources with bio-based resources can reduce oil consumption and achieve carbon dioxide emissions. In recent years, polymers based on green and renewable bio-based resources have become a research hotspot. Among them, carbohydrates have attracted widespread attention due to their wide sources, low prices, easy availability, and stereochemical diversity. Isohexides (1,4:3,6-dianhydrohexitol, isohexides) are a class of carbohydrate-derived diols with high rigidity, chirality, hydrophilicity, and low toxicity. They have broad development prospects in the preparation of new bio-based and biodegradable polymer materials. Among them, isosorbide (IS) has been industrialized on a large scale and is considered to be a monomer with great potential to replace bisphenol A.

[0004] The literature "Macromolecules, 2006, 39 (26): 9064-70; Journal of Industrial and Engineering Chemistry, 2016, 37, 42-6; Green Chemistry, 2020, 22 (8): 2488-97." points out that isosorbide-based polycarbonate (PIC) can be successfully prepared by reacting isosorbide with diphosgene / triphosgene or diphenyl carbonate (DPC) / dimethyl carbonate (DMC). Compared with BPA-PC, PIC has higher elastic modulus and tensile strength, and has better transparency and UV resistance. However, the preparation and application of PIC still have the following problems:

[0005] (1) The reactivity of the two secondary hydroxyl groups of isosorbide is low, and the different conformations of the two hydroxyl groups lead to differences in reactivity, making it difficult to prepare high molecular weight polycarbonate;

[0006] (2) PIC has a high melt viscosity, which makes it difficult to stir in the later stage of melt polymerization and polycondensation, and small molecules are difficult to remove, so it is impossible to prepare high molecular weight polycarbonate, and the later processing will be subject to certain restrictions;

[0007] (3) Due to the high rigidity of isosorbide, PIC is brittle, and its toughness and processability are poor, which will lead to certain limitations in industrial applications. Therefore, in order to obtain high-performance isosorbide-based polycarbonate, the above problems must be solved.

[0008] To solve problem (1), the document "Green Chemistry, 2021, 23, 973." discloses a series of highly active imidazolyl ionic liquid catalysts composed of halogen anions, and the weight-average molecular weight of the PIC synthesized by the catalyst can reach 98,700 g / mol. To further solve problems (2) and (3), copolymerization of isosorbide with flexible monomers is an effective solution. Patent CN111138650A discloses a high molecular weight and high flexibility bio-based polycarbonate copolymer and a preparation method thereof. The patent successfully improves the flexibility of PIC by copolymerizing with an aliphatic diol containing an ether bond, and the elongation at break can be as high as 176%. However, the glass transition temperature of the high molecular weight and high flexibility bio-based polycarbonate copolymer finally prepared is only 78-105°C, which does not meet the requirements of high heat-resistant applications, and its mechanical strength is not mentioned. The paper "Polymer, 2019, 179, 121685" prepares a series of high heat-resistant (T g:157.8-173.5℃), high strength (fiber tensile strength 83-185MPa), high molecular weight (weight average molecular weight: 73,000-103,000g / mol) copolycarbonates, but their elongation at break is <10%. The paper "Modern Chemical Industry, 2018, 38(08):130-134." A series of copolycarbonates were prepared by copolymerizing IS with linear diols. With the increase of carbon chain length and the decrease of IS content, the elongation at break of the copolycarbonate increased from 7.5% to 575.2%, but its tensile strength decreased from 84.6MPa to 22.2MPa. In the paper "Polymer, 2017, 116, 153-159", a series of copolycarbonates based on IS and 1,4-cyclohexane dimethanol (trans-cyclohexane-1,4-dimethanol, CHDM) were synthesized with high strength (68-69MPa) and certain toughness (elongation at break of 50%-100%), but their bio-based content was reduced. In summary, it is still challenging to obtain isosorbide-based polycarbonates with high molecular weight, high heat resistance, high strength, good toughness and high bio-content. Summary of the invention

[0009] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for preparing an isohexidet-based polycarbonate copolymer. The prepared isohexidet-based polycarbonate copolymer has high molecular weight, high heat resistance, high strength, high toughness, and high biocontent, and can be applied to electronic devices, automotive parts, packaging materials, medical devices and other fields in the form of engineering plastics or films.

[0010] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0011] A method for preparing an isohexitol-based polycarbonate copolymer comprises subjecting a diol and a carbonic acid diester to, under the action of a catalyst, an ester exchange reaction, a preliminary polycondensation reaction, and a final polycondensation reaction in sequence to obtain an isohexitol-based polycarbonate copolymer;

[0012] The diol includes diol A1 and diol A2, or further includes diol A3;

[0013] Diol A1 is isohexitol;

[0014] The molecular structure of diol A2 contains a cyclic ether structure and two primary hydroxyl groups, and the primary hydroxyl group and the cyclic ether structure are connected by a methylene group;

[0015] Diol A3 is a dihydroxy compound;

[0016] The molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.6-0.8:0.1-0.4:0-0.2:1-1.1;

[0017] During the pre-polycondensation reaction, the temperature is first gradually increased to 180-200°C within 5-15 minutes, and then the pressure is gradually reduced to 45-55kPa within 5 minutes. Finally, gradient temperature increase and gradient pressure reduction are performed, that is, each temperature increase of 10°C is maintained for 10-20 minutes, and the pressure is reduced by 3-15kPa at the same time. The total time for gradient temperature increase and gradient pressure reduction is 0.5-1h, and the termination conditions of gradient temperature increase and gradient pressure reduction are: temperature is 210-230°C, and pressure is 15-30kPa.

[0018] The isohexitol-based polycarbonate copolymer of the present invention has high molecular weight, high heat resistance, high strength, high toughness, and high biocontent. The specific reasons are as follows:

[0019] The diol includes diol A1 and diol A2, or further includes diol A3, wherein diol A1 is the main imparter of rigidity, and diol A2 is the main imparter of toughness, and has a rigid-flexible structure, which imparts toughness to the isohexide alcohol-based polycarbonate copolymer while maintaining a certain rigidity, thereby avoiding a substantial decrease in the glass transition temperature, and diol A3 is a further regulator of rigidity and toughness, wherein diol A1 and diol A2 are both bio-based monomers;

[0020] The present invention controls the molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester to be 0.6-0.8:0.1-0.4:0-0.2:1-1.1, so that the proportion of diol A1 in the diol is 60%-80%, thereby ensuring the high heat resistance and high strength of the isohexide alcohol-based polycarbonate copolymer, the proportion of diol A2 is 10%-40%, thereby ensuring that the toughness of the isohexide alcohol-based polycarbonate copolymer is improved while ensuring that the heat resistance and strength of the isohexide alcohol-based polycarbonate copolymer will not be greatly reduced, the proportion of diol A3 is 0-20%, thereby further regulating the rigidity and toughness of the isohexide alcohol-based polycarbonate copolymer; in addition, the total proportion of diol A1 and diol A2 in the diol is relatively high, thereby ensuring the high biocontent of the isohexide alcohol-based polycarbonate copolymer;

[0021] The molecular structure of the diol A2 controlled by the present invention contains a cyclic ether structure, so it has a certain structural rigidity. At the same time, the molecular structure also contains two primary hydroxyl groups, and the primary hydroxyl group is connected to the cyclic ether structure through a methylene group, so it has a certain flexibility. The diol A2 is a bio-based rigid and flexible diol monomer, which can effectively improve the melt viscosity and improve the processability; the primary hydroxyl group has a higher reactivity than the secondary hydroxyl group, which can make up for the lack of reactivity of the diol A1 and increase the molecular weight. In addition, the cyclic ether structure may form a hydrogen bond with the hydroxyl group of the diol A1, and play a self-catalytic role in the polymerization process, thereby increasing the molecular weight. Compared with the low molecular weight isohexitol-based polycarbonate copolymer, the increase in molecular weight is also conducive to the improvement of strength;

[0022] The temperature and pressure control of the pre-polycondensation reaction is particularly important. When the temperature is too high, side reactions such as yellowing and thermal degradation are prone to occur. When the temperature is too low, the reaction activity is low and the reaction cannot be fully reacted. When the pressure is too high, the byproduct phenol is difficult to remove and the reaction is difficult to proceed in the forward direction. When the pressure is too low, it will cause violent boiling, and part of the melt will be extracted, resulting in the loss of reactants, hindering the reaction, and even causing pipeline blockage. Therefore, the present invention adopts a method of gradient temperature increase and pressure reduction, controls the temperature and pressure within a suitable range, can effectively remove phenol, and avoids the removal of oligomers, and can effectively promote the reaction, thereby obtaining a high molecular weight isohexitol-based polycarbonate copolymer.

[0023] As the preferred technical solution:

[0024] The preparation method of the isohexitol-based polycarbonate copolymer as described above, wherein the thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer is ≥345°C, the tensile strength is 65-85MPa, the elongation at break is 60%-110%, T g ≥110℃, number average molecular weight is 3×10 4 -13×10 4 g / mol.

[0025] In the method for preparing an isohexide-based polycarbonate copolymer as described above, the diol A1 is one or more of isosorbide, isomannide and isoidide.

[0026] In the preparation method of the isohexide alcohol-based polycarbonate copolymer described above, the diol A2 is IIDML (isoidose-2,5-dimethanol, )、IMDML(isomannose-2,5-dimethanol, )、ISDML(isosorbide-2,5-dimethanol, ), tetrahydrofuran dimethanol Furandiol Galx-OH(2,3:4,5-di-O-Methylene-galactitol, ), Manx-OH(2,3:4,5-di-O-Methylene-D-mannitol, ), BCD(4,4′-Bicyclohexanone Glycerol Diketal, ), CHD(1,4-Cyclohexanedione Glycerol Diketa, ), CaG(Camphorquinone Diketal Glycerol, ) and CM diol (2,4:3,5-di-O-camphor-D-mannitol, )

[0027] In the preparation method of the isohexide alcohol-based polycarbonate copolymer as described above, the diol A3 is one or more of CHDM, CBDO, ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol and 1,6-hexanediol.

[0028] In the preparation method of the isohexide alcohol-based polycarbonate copolymer as described above, the carbonate diester is one or more of diphenyl carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, dibutyl carbonate, dipentyl carbonate and dioctyl carbonate.

[0029] In the preparation method of an isohexide alcohol-based polycarbonate copolymer as described above, the catalyst is a metal catalyst, preferably an alkali metal catalyst, which has high catalytic activity for the carbonate exchange process and can promote the growth of molecular weight; the alkali metal catalyst is one or more of acetylacetone alkali metal compounds, alkali metal carbonates, alkali metal hydroxides and alkali metal chlorides; the acetylacetone alkali metal compounds are one or more of lithium acetylacetonate and lanthanum acetylacetonate; the alkali metal carbonates are one or more of lithium carbonate, sodium carbonate, potassium carbonate, rubidium carbonate and cesium carbonate; the alkali metal hydroxides are one or more of lithium hydroxide, sodium hydroxide and potassium hydroxide; the alkali metal chlorides are one or more of lithium chloride, sodium chloride and potassium chloride; the catalyst selected in the present invention has good catalytic activity for the carbonate exchange process, reduces the yellowing side reaction, and is conducive to further improving the molecular weight of the isohexide alcohol-based polycarbonate copolymer.

[0030] In the above-mentioned method for preparing an isohexitol-based polycarbonate copolymer, the molar amount of the catalyst is 1×10 of the total molar amount of the diol. -5 -5×10 -4 .

[0031] In the preparation method of the isohexide alcohol-based polycarbonate copolymer as described above, the ester exchange reaction is carried out under the protection of nitrogen or inert gas, the temperature of the ester exchange reaction is 120-160°C, the pressure is 0.1MPa, and the time is 1.5-4h; the temperature of the final polycondensation reaction is 230-250°C, the pressure is below 150Pa, and the time is 0.5-2h.

[0032] The preparation method of the isohexitol-based polycarbonate copolymer as described above, the structural formula of the isohexitol-based polycarbonate copolymer is as follows:

[0033]

[0034] In the formula, x, y, and z are the numbers of repeating units in the isohexide alcohol-based polycarbonate copolymer, which may be the same or different, and z may be 0.

[0035] Beneficial effects:

[0036] (1) A method for preparing an isohexide alcohol-based polycarbonate copolymer of the present invention, wherein the introduced diol A2 has two primary hydroxyl groups and has higher reactivity than the secondary hydroxyl groups of isohexide alcohol in melt polymerization, wherein the ether bonds of some diols A2, such as IIDML, IMDML or ISDML, can form intermolecular hydrogen bonds with the hydroxyl groups of isohexide alcohol, thereby activating the secondary hydroxyl groups of isohexide alcohol, and a high molecular weight isohexide alcohol-based polycarbonate copolymer can be obtained.

[0037] (2) The preparation method of the present invention effectively avoids the yellowing side reaction caused by the high-temperature pre-polycondensation reaction by using mild pre-polycondensation reaction conditions and catalyst screening, and can obtain a copolymer with good color.

[0038] (3) The diol A2 introduced in the present invention is a green bio-based monomer, which maintains a high bio-based content of the copolymer. At the same time, the preparation process is green and environmentally friendly, and the total reaction time does not exceed 6 hours. In addition, the copolymer prepared by the present invention also has good transparency, and the transmittance can reach 87%-92%.

[0039] (4) The present invention solves the problems of low molecular weight, high melt viscosity, difficult processing, poor toughness, and inability of PIC copolymers to have heat resistance, strength, toughness, and bio-based content by regulating the polymer structure and the polymerization process. The prepared isohexide alcohol-based polycarbonate copolymer has high molecular weight, high heat resistance, high strength, high toughness, and transparency, and can be used in electronic devices, automotive parts, packaging materials, medical devices, and other fields. DETAILED DESCRIPTION

[0040] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0041] The structural formula of isohexide-based polycarbonate copolymer is as follows:

[0042]

[0043] In the formula, x, y, and z are the numbers of repeating units in the isohexide alcohol-based polycarbonate copolymer, which may be the same or different, and z may be 0.

[0044] The following is the test method of the relevant performance in the embodiment:

[0045] Thermal weight loss 5wt% temperature: The thermal weight loss 5wt% temperature was determined by a thermogravimetric analyzer (TGA, manufactured by NETZSCH Instrument Manufacturing Co., Ltd., Germany, model TG 209F1); 1-5 mg of sample was weighed and placed in a crucible, and under nitrogen protection, the temperature was raised from 30°C to 600°C at a heating rate of 10°C / min.

[0046] Tensile strength: The tensile strength of the isohexide alcohol-based polycarbonate copolymer prepared in the example was tested using GB / T1040-2006 standard.

[0047] Elongation at break: The elongation at break of the isohexitol-based polycarbonate copolymer prepared in the example was tested using GB / T1040-2006 standard.

[0048] T g The glass transition temperature (T) was measured by differential scanning calorimetry (DSC, manufactured by TA Corporation, USA, model Q20). g ; Weigh 5-10 mg of sample and place it in an aluminum crucible. Under nitrogen protection, heat the temperature from 25°C to 260°C at a rate of 10°C / min and keep it warm for 3 minutes; then cool it down to 25°C at a rate of 10°C / min, keep it warm for 3 minutes, and then heat it to 260°C at a rate of 10°C / min.

[0049] Number average molecular weight: The number average molecular weight of the isohexide-based polycarbonate copolymer prepared in the examples was measured by gel permeation chromatography (GPC).

[0050] Example 1

[0051] A method for preparing an isohexitol-based polycarbonate copolymer, comprising the following steps:

[0052] (1) Preparation of raw materials;

[0053] Diol A1: isosorbide;

[0054] Diol A2: IIDML;

[0055] Diol A3: CHDM;

[0056] Carbonate diester: diphenyl carbonate;

[0057] Catalyst: lithium acetylacetonate;

[0058] (2) preparing isohexide alcohol-based polycarbonate copolymers;

[0059] The diols (diol A1, diol A2, diol A3) and carbonic acid diester are sequentially subjected to ester exchange reaction, preliminary polycondensation reaction and final polycondensation reaction under the action of a catalyst to obtain an isohexide alcohol-based polycarbonate copolymer; wherein the molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.6:0.3:0.1:1, and the molar amount of the catalyst is 5×10 of the total molar amount of the diols. -4 ;

[0060] The transesterification reaction was carried out under the protection of nitrogen or inert gas, the temperature of the transesterification reaction was 130°C, the pressure was 0.1MPa, and the time was 3h;

[0061] During the pre-polycondensation reaction, the temperature is first gradually increased to 180°C within 10 minutes, and then the pressure is gradually reduced to 45 kPa within 5 minutes. Finally, the temperature is gradually increased and the pressure is gradually reduced, that is, the temperature is increased by 10°C for 15 minutes, and the pressure is reduced by 3-8 kPa. The total time for the gradient temperature increase and the gradient pressure reduction is 60 minutes. The termination conditions of the gradient temperature increase and the gradient pressure reduction are: the temperature is 220°C and the pressure is 25 kPa.

[0062] The final polycondensation reaction was carried out at a temperature of 240°C, a pressure of 100 Pa, and a time of 50 min.

[0063] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained was 353°C, the tensile strength was 85MPa, the elongation at break was 92%, and the T g The temperature is 119℃ and the number average molecular weight is 13×10 4 g / mol.

[0064] Comparative Example 1

[0065] A method for preparing an isohexide alcohol-based polycarbonate copolymer is basically the same as Example 1, except that during the pre-polycondensation reaction, the temperature is first gradually increased to 180°C within 10 minutes, then the pressure is gradually reduced to 45 kPa within 5 minutes, and finally the temperature is gradually increased to 220°C within 60 minutes, while the pressure is gradually reduced to 25 kPa.

[0066] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained was 345°C, the tensile strength was 78MPa, the elongation at break was 87%, and the T g The temperature is 117℃ and the number average molecular weight is 2.8×10 4 g / mol.

[0067] By comparing Example 10 with Comparative Example 1, it can be seen that since gradient temperature increase and gradient pressure reduction are not used in the pre-condensation reaction in Comparative Example 1, the molecular weight will decrease. This is because the temperature is increased too quickly and the pressure is too low, which will make the reaction insufficient, and oligomers may be extracted, which may cause violent boiling and hinder the growth of molecular weight.

[0068] Example 2

[0069] A method for preparing an isohexide alcohol-based polycarbonate copolymer is basically the same as that of Example 1, except that the diol A2 prepared in step (1) is IMDML.

[0070] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 350°C, the tensile strength is 78MPa, the elongation at break is 89%, and the T g The temperature is 115℃ and the number average molecular weight is 7×10 4 g / mol.

[0071] Example 3

[0072] A method for preparing an isohexide alcohol-based polycarbonate copolymer is basically the same as that of Example 1, except that the diol A2 prepared in step (1) is ISDML.

[0073] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 348°C, the tensile strength is 82MPa, the elongation at break is 90%, and the T g The temperature is 116℃ and the number average molecular weight is 9×10 4 g / mol.

[0074] Example 4

[0075] A method for preparing an isohexitol-based polycarbonate copolymer, comprising the following steps:

[0076] (1) Preparation of raw materials;

[0077] Diol A1: isomannide;

[0078] Diol A2: tetrahydrofuran dimethanol;

[0079] Diol A3: 1,3-propylene glycol;

[0080] Carbonate diester: dipropyl carbonate;

[0081] Catalyst: lithium carbonate;

[0082] (2) preparing isohexide alcohol-based polycarbonate copolymers;

[0083] The diols (diol A1, diol A2, diol A3) and carbonic acid diester are sequentially subjected to ester exchange reaction, preliminary polycondensation reaction and final polycondensation reaction under the action of a catalyst to obtain an isohexide alcohol-based polycarbonate copolymer; wherein the molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.7:0.2:0.1:1.1, and the molar amount of the catalyst is 4×10 of the total molar amount of the diols. -4 ;

[0084] The transesterification reaction was carried out under the protection of nitrogen or inert gas, the temperature of the transesterification reaction was 140°C, the pressure was 0.1MPa, and the time was 2.5h;

[0085] During the pre-polycondensation reaction, the temperature is first gradually increased to 190°C within 10 minutes, and then the pressure is gradually reduced to 50 kPa within 5 minutes. Finally, the temperature is gradually increased and the pressure is gradually reduced, that is, the temperature is increased by 10°C for 15 minutes, and the pressure is reduced by 5-10 kPa. The total time for the gradient temperature increase and the gradient pressure reduction is 45 minutes. The termination conditions of the gradient temperature increase and the gradient pressure reduction are: the temperature is 220°C and the pressure is 25 kPa.

[0086] The final polycondensation reaction temperature was 235°C, the pressure was 150 Pa, and the time was 80 min.

[0087] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 348°C, the tensile strength is 68MPa, the elongation at break is 85%, and the T g The temperature is 112℃ and the number average molecular weight is 6×10 4 g / mol.

[0088] Example 5

[0089] A method for preparing an isohexide alcohol-based polycarbonate copolymer is basically the same as that of Example 4, except that the diol A2 prepared in step (1) is furan dimethanol.

[0090] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 350°C, the tensile strength is 70MPa, the elongation at break is 82%, and the T g The temperature is 117℃ and the number average molecular weight is 3×10 4 g / mol.

[0091] Example 6

[0092] A method for preparing an isohexitol-based polycarbonate copolymer, comprising the following steps:

[0093] (1) Preparation of raw materials;

[0094] Diol A1: isoidiol;

[0095] Diol A2: Galx-OH;

[0096] Diol A3: 1,5-pentanediol;

[0097] Carbonate diester: diamyl carbonate;

[0098] Catalyst: potassium carbonate;

[0099] (2) preparing isohexide alcohol-based polycarbonate copolymers;

[0100] The diols (diol A1, diol A2, diol A3) and carbonic acid diester are sequentially subjected to ester exchange reaction, preliminary polycondensation reaction and final polycondensation reaction under the action of a catalyst to obtain an isohexide alcohol-based polycarbonate copolymer; wherein the molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.7:0.25:0.05:1.1, and the molar amount of the catalyst is 5×10 of the total molar amount of the diols. -4 ;

[0101] The transesterification reaction was carried out under the protection of nitrogen or inert gas, the temperature of the transesterification reaction was 160°C, the pressure was 0.1MPa, and the time was 1.5h;

[0102] During the pre-polycondensation reaction, the temperature is first gradually increased to 200°C within 8 minutes, and then the pressure is gradually reduced to 55 kPa within 5 minutes. Finally, the temperature is gradually increased and the pressure is gradually reduced, that is, the temperature is increased by 10°C for 15 minutes, and the pressure is reduced by 5-10 kPa. The total time for the gradient temperature increase and the gradient pressure reduction is 45 minutes. The termination conditions of the gradient temperature increase and the gradient pressure reduction are: the temperature is 230°C and the pressure is 20 kPa.

[0103] The final polycondensation reaction temperature was 250°C, the pressure was 90 Pa, and the time was 1 h.

[0104] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained was 362°C, the tensile strength was 68MPa, the elongation at break was 97%, and the T g The temperature is 113℃ and the number average molecular weight is 6×10 4 g / mol.

[0105] Example 7

[0106] A method for preparing an isohexitol-based polycarbonate copolymer, comprising the following steps:

[0107] (1) Preparation of raw materials;

[0108] Diol A1: isoidiol;

[0109] Diol A2: Manx-OH;

[0110] Diol A3: 1,4-butanediol;

[0111] Carbonate diester: dioctyl carbonate;

[0112] Catalyst: rubidium carbonate;

[0113] (2) preparing isohexide alcohol-based polycarbonate copolymers;

[0114] The diols (diol A1, diol A2, diol A3) and carbonic acid diester are sequentially subjected to ester exchange reaction, preliminary polycondensation reaction and final polycondensation reaction under the action of a catalyst to obtain an isohexide alcohol-based polycarbonate copolymer; wherein the molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.7:0.2:0.1:1, and the molar amount of the catalyst is 2×10 of the total molar amount of the diols. -4 ;

[0115] The transesterification reaction was carried out under the protection of nitrogen or inert gas, the temperature of the transesterification reaction was 160°C, the pressure was 0.1MPa, and the time was 1.5h;

[0116] During the pre-polycondensation reaction, the temperature is first gradually increased to 200°C within 8 minutes, and then the pressure is gradually reduced to 55 kPa within 5 minutes. Finally, the temperature is gradually increased and the pressure is gradually reduced, that is, the temperature is increased by 10°C for 15 minutes, and the pressure is reduced by 5-10 kPa. The total time for the gradient temperature increase and the gradient pressure reduction is 45 minutes. The termination conditions of the gradient temperature increase and the gradient pressure reduction are: the temperature is 230°C and the pressure is 20 kPa.

[0117] The final polycondensation reaction temperature is 250°C, the pressure is 120 Pa, and the time is 1 h.

[0118] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained was 371°C, the tensile strength was 81MPa, the elongation at break was 90%, and the T g The temperature is 126℃ and the number average molecular weight is 4×10 4 g / mol.

[0119] Example 8

[0120] A method for preparing an isohexitol-based polycarbonate copolymer, comprising the following steps:

[0121] (1) Preparation of raw materials;

[0122] Diol A1: isomannide;

[0123] Diol A2: BCD;

[0124] Diol A3: 1,6-hexanediol;

[0125] Carbonate diester: diethyl carbonate;

[0126] Catalyst: lithium hydroxide;

[0127] (2) preparing isohexide alcohol-based polycarbonate copolymers;

[0128] The diols (diol A1, diol A2, diol A3) and carbonic acid diester are sequentially subjected to ester exchange reaction, preliminary polycondensation reaction and final polycondensation reaction under the action of a catalyst to obtain an isohexide alcohol-based polycarbonate copolymer; wherein the molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.8:0.1:0.1:1, and the molar amount of the catalyst is 3×10 of the total molar amount of the diols. -4 ;

[0129] The transesterification reaction was carried out under the protection of nitrogen or inert gas, the temperature of the transesterification reaction was 150°C, the pressure was 0.1MPa, and the time was 1.5h;

[0130] During the pre-polycondensation reaction, the temperature is first gradually increased to 200°C within 10 minutes, and then the pressure is gradually reduced to 50 kPa within 5 minutes. Finally, the temperature is gradually increased and the pressure is gradually reduced. That is, the temperature is increased by 10°C for 20 minutes, and the pressure is reduced by 10-15 kPa. The total time for the gradient temperature increase and the gradient pressure reduction is 60 minutes. The termination conditions of the gradient temperature increase and the gradient pressure reduction are: the temperature is 230°C and the pressure is 15 kPa.

[0131] The final polycondensation reaction temperature was 240°C, the pressure was 130 Pa, and the time was 1 h.

[0132] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 345°C, the tensile strength is 80MPa, the elongation at break is 79%, and the T g The temperature is 121℃ and the number average molecular weight is 5×10 4 g / mol.

[0133] Example 9

[0134] A method for preparing an isohexide alcohol-based polycarbonate copolymer is basically the same as that of Example 8, except that the diol A2 prepared in step (1) is CHD.

[0135] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 355°C, the tensile strength is 70MPa, the elongation at break is 93%, and the T g The temperature is 110℃ and the number average molecular weight is 3×10 4 g / mol.

[0136] Example 10

[0137] A method for preparing an isohexitol-based polycarbonate copolymer, comprising the following steps:

[0138] (1) Preparation of raw materials;

[0139] Diol A1: isosorbide;

[0140] Diol A2: CaG;

[0141] Diol A3: CBDO;

[0142] Carbonate diester: dimethyl carbonate;

[0143] Catalyst: lithium chloride;

[0144] (2) preparing isohexide alcohol-based polycarbonate copolymers;

[0145] The diols (diol A1, diol A2, diol A3) and carbonic acid diester are sequentially subjected to ester exchange reaction, preliminary polycondensation reaction and final polycondensation reaction under the action of a catalyst to obtain an isohexide alcohol-based polycarbonate copolymer; wherein the molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.6:0.3:0.1:1, and the molar amount of the catalyst is 1×10 of the total molar amount of the diols. -5 ;

[0146] The transesterification reaction was carried out under the protection of nitrogen or inert gas, the temperature of the transesterification reaction was 160°C, the pressure was 0.1MPa, and the time was 1.5h;

[0147] During the pre-polycondensation reaction, the temperature is first gradually increased to 190°C within 5 minutes, and then the pressure is gradually reduced to 47 kPa within 5 minutes. Finally, the temperature is gradually increased and the pressure is gradually reduced, that is, the temperature is increased by 10°C for 10 minutes, and the pressure is reduced by 6-12 kPa. The total time for the gradient temperature increase and the gradient pressure reduction is 30 minutes. The termination conditions of the gradient temperature increase and the gradient pressure reduction are: the temperature is 220°C and the pressure is 20 kPa.

[0148] The final polycondensation reaction temperature was 230°C, the pressure was 80 Pa, and the time was 2 h.

[0149] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 350°C, the tensile strength is 82MPa, the elongation at break is 60%, and the T g The temperature is 127℃ and the number average molecular weight is 4×10 4 g / mol.

[0150] Comparative Example 2

[0151] A method for preparing an isohexide alcohol-based polycarbonate copolymer is basically the same as Example 10, except that the molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.4:0.5:0.1:1.

[0152] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 340°C, the tensile strength is 52MPa, the elongation at break is 95%, and the T g is 99°C, and the number average molecular weight is 4×10 4 g / mol.

[0153] By comparing Example 10 with Comparative Example 2, it can be seen that since the proportion of diol A2 in Comparative Example 2 is greater than the proportion of diol A1, the heat resistance and strength of the obtained isohexide alcohol-based polycarbonate copolymer will be reduced. This is because diol A1 is the main rigidity provider, and A2 is a monomer with a rigid and flexible structure and is also the main provider of toughness. If the proportion of diol A1 is too low, the obtained copolymer will not have sufficient rigidity to provide high heat resistance and high strength properties.

[0154] Comparative Example 3

[0155] A method for preparing an isohexide alcohol-based polycarbonate copolymer is basically the same as Example 10, except that the molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.85:0.05:0.1:1.

[0156] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 349°C, the tensile strength is 68MPa, the elongation at break is 30%, and the T gAt 150°C, the number average molecular weight is 2.9×10 4 g / mol.

[0157] By comparing Example 10 with Comparative Example 3, it can be seen that since the proportion of diol A1 in Comparative Example 3 is too large and the proportion of diol A2 is too small, the molecular weight of the obtained copolymer will be reduced, the toughness will be poor, and the material will become brittle. This is because diol A1 is the main rigidity provider and A2 is the main toughness imparter. When the proportion of diol A1 is too large, the obtained copolymer will be too rigid and the toughness will be poor. Moreover, since diol A1 is a secondary alcohol and its reaction activity is lower than that of a primary alcohol, when the content of diol A1 is too high, the molecular weight of the polymer will also decrease.

[0158] Embodiment 11

[0159] A method for preparing an isohexide alcohol-based polycarbonate copolymer is basically the same as Example 10, except that: diol A3 is not prepared in step (1); and the molar ratio of diol A1, diol A2 and carbonic acid diester in step (2) is 0.6:0.4:1.

[0160] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 345°C, the tensile strength is 75MPa, the elongation at break is 80%, and the T g The temperature is 125℃ and the number average molecular weight is 4.5×10 4 g / mol.

[0161] Example 12

[0162] A method for preparing an isohexitol-based polycarbonate copolymer, comprising the following steps:

[0163] (1) Preparation of raw materials;

[0164] Diol A1: isoidiol;

[0165] Diol A2: CM diol;

[0166] Diol A3: ethylene glycol;

[0167] Carbonate diester: dibutyl carbonate;

[0168] Catalyst: sodium chloride;

[0169] (2) preparing isohexide alcohol-based polycarbonate copolymers;

[0170] The diols (diol A1, diol A2, diol A3) and carbonic acid diester are sequentially subjected to ester exchange reaction, preliminary polycondensation reaction and final polycondensation reaction under the action of a catalyst to obtain an isohexide alcohol-based polycarbonate copolymer; wherein the molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.7:0.2:0.1:1, and the molar amount of the catalyst is 5×10 of the total molar amount of the diols. -4 ;

[0171] The transesterification reaction was carried out under the protection of nitrogen or inert gas, the temperature of the transesterification reaction was 120°C, the pressure was 0.1MPa, and the time was 4h;

[0172] During the pre-polycondensation reaction, the temperature is first gradually increased to 180°C within 15 minutes, and then the pressure is gradually reduced to 45 kPa within 5 minutes. Finally, the temperature is gradually increased and the pressure is gradually reduced, that is, the temperature is increased by 10°C for 20 minutes, and the pressure is reduced by 3-7 kPa. The total time for the gradient temperature increase and the gradient pressure reduction is 60 minutes. The termination conditions of the gradient temperature increase and the gradient pressure reduction are: the temperature is 210°C and the pressure is 30 kPa.

[0173] The final polycondensation reaction temperature was 250°C, the pressure was 90 Pa, and the time was 0.5 h.

[0174] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 345°C, the tensile strength is 65MPa, the elongation at break is 76%, and the T g At 120°C, the number average molecular weight is 5×10 4 g / mol.

[0175] Example 13

[0176] A method for preparing an isohexide alcohol-based polycarbonate copolymer is basically the same as Example 12, except that: diol A3 is not prepared; and the molar ratio of diol A1, diol A2 and carbonic acid diester in step (2) is 0.7:0.3:1.

[0177] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 470°C, the tensile strength is 71MPa, the elongation at break is 80%, and the T g The temperature is 127℃ and the number average molecular weight is 3×10 4 g / mol.

[0178] Embodiment 14

[0179] A method for preparing an isohexitol-based polycarbonate copolymer, comprising the following steps:

[0180] (1) Preparation of raw materials;

[0181] Diol A1: a mixture of isosorbide and isomannide in a mass ratio of 13:1;

[0182] Diol A2: a mixture of IIDML and tetrahydrofuran dimethanol in a mass ratio of 1:1;

[0183] Carbonate diester: a mixture of diethyl carbonate and dibutyl carbonate in a mass ratio of 1:1;

[0184] Catalyst: potassium hydroxide;

[0185] (2) preparing isohexide alcohol-based polycarbonate copolymers;

[0186] The diols (diol A1, diol A2) and carbonic acid diester are sequentially subjected to ester exchange reaction, preliminary polycondensation reaction and final polycondensation reaction under the action of a catalyst to obtain an isohexide alcohol-based polycarbonate copolymer; wherein the molar ratio of diol A1, diol A2 and carbonic acid diester is 0.6:0.4:1.1, and the molar amount of the catalyst is 4×10 of the total molar amount of the diols. -4 ;

[0187] The transesterification reaction was carried out under the protection of nitrogen or inert gas, the temperature of the transesterification reaction was 130°C, the pressure was 0.1MPa, and the time was 3h;

[0188] During the pre-polycondensation reaction, the temperature is first gradually increased to 190°C within 15 minutes, and then the pressure is gradually reduced to 50 kPa within 5 minutes. Finally, the temperature is gradually increased and the pressure is gradually reduced, that is, the temperature is increased by 10°C for 20 minutes, and the pressure is reduced by 5-15 kPa. The total time for the gradient temperature increase and the gradient pressure reduction is 60 minutes. The termination conditions of the gradient temperature increase and the gradient pressure reduction are: the temperature is 220°C and the pressure is 25 kPa.

[0189] The final polycondensation reaction was carried out at a temperature of 240°C, a pressure of 100 Pa, and a time of 80 min.

[0190] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 350°C, the tensile strength is 72MPa, the elongation at break is 110%, and the T g The temperature is 115℃ and the number average molecular weight is 9×10 4 g / mol.

[0191] Embodiment 15

[0192] A method for preparing an isohexitol-based polycarbonate copolymer, comprising the following steps:

[0193] (1) Preparation of raw materials;

[0194] Diol A1: a mixture of isoidol and isomannide in a mass ratio of 1:1;

[0195] Diol A2: a mixture of IIDML and tetrahydrofuran dimethanol in a mass ratio of 1:1;

[0196] Diol A3: a mixture of CHDM and ethylene glycol in a mass ratio of 1:2;

[0197] Carbonate diester: a mixture of diethyl carbonate and dibutyl carbonate in a mass ratio of 1:1;

[0198] Catalyst: potassium hydroxide;

[0199] (2) preparing isohexide alcohol-based polycarbonate copolymers;

[0200] The diols (diol A1, diol A2, diol A3) and carbonic acid diester are sequentially subjected to ester exchange reaction, preliminary polycondensation reaction and final polycondensation reaction under the action of a catalyst to obtain an isohexide alcohol-based polycarbonate copolymer; wherein the molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.6:0.2:0.2:1.1, and the molar amount of the catalyst is 4×10 of the total molar amount of the diols. -4 ;

[0201] The transesterification reaction was carried out under the protection of nitrogen or inert gas, the temperature of the transesterification reaction was 130°C, the pressure was 0.1MPa, and the time was 3h;

[0202] During the pre-polycondensation reaction, the temperature is first gradually increased to 190°C within 15 minutes, and then the pressure is gradually reduced to 50 kPa within 5 minutes. Finally, the temperature is gradually increased and the pressure is gradually reduced, that is, the temperature is increased by 10°C for 20 minutes, and the pressure is reduced by 5-15 kPa. The total time for the gradient temperature increase and the gradient pressure reduction is 60 minutes. The termination conditions of the gradient temperature increase and the gradient pressure reduction are: the temperature is 220°C and the pressure is 25 kPa.

[0203] The final polycondensation reaction was carried out at a temperature of 240°C, a pressure of 100 Pa, and a time of 80 min.

[0204] The thermal weight loss 5wt% temperature of the isohexitol-based polycarbonate copolymer finally obtained is 345°C, the tensile strength is 70MPa, the elongation at break is 103%, and the T g The temperature is 113℃ and the number average molecular weight is 8×10 4 g / mol.

Claims

1. A method for preparing an isohexitol-based polycarbonate copolymer, characterized in that: The diol and the carbonic acid diester are sequentially subjected to an ester exchange reaction, a preliminary polycondensation reaction, and a final polycondensation reaction under the action of a catalyst to obtain an isohexitol-based polycarbonate copolymer; The diol includes diol A1 and diol A2, or further includes diol A3; Diol A1 is isohexitol; The molecular structure of diol A2 contains a cyclic ether structure and two primary hydroxyl groups, and the primary hydroxyl group and the cyclic ether structure are connected by a methylene group; Diol A3 is a dihydroxy compound; The molar ratio of diol A1, diol A2, diol A3 and carbonic acid diester is 0.6-0.8:0.1-0.4:0-0.2:1-1.1; During the pre-polycondensation reaction, the temperature is first gradually increased to 180-200°C within 5-15 minutes, and then the pressure is gradually reduced to 45-55kPa within 5 minutes. Finally, gradient temperature increase and gradient pressure reduction are performed, that is, each temperature increase of 10°C is maintained for 10-20 minutes, and the pressure is reduced by 3-15kPa at the same time. The total time for gradient temperature increase and gradient pressure reduction is 0.5-1h, and the termination conditions of gradient temperature increase and gradient pressure reduction are: temperature is 210-230°C, and pressure is 15-30kPa.

2. The method for preparing an isohexide alcohol-based polycarbonate copolymer according to claim 1, characterized in that: The thermal weight loss 5wt% temperature of isohexitol-based polycarbonate copolymer is ≥345°C, the tensile strength is 65-85MPa, the elongation at break is 60%-110%, T g ≥110℃, number average molecular weight is 3×10 4 -13×10 4 g / mol.

3. The method for preparing an isohexide alcohol-based polycarbonate copolymer according to claim 1, characterized in that: The diol A1 is one or more of isosorbide, isomannide and isoidide.

4. The method for preparing an isohexide alcohol-based polycarbonate copolymer according to claim 1, characterized in that: The diol A2 is one or more of IIDML, IMDML, ISDML, tetrahydrofuran dimethanol, furan dimethanol, Galx-OH, Manx-OH, BCD, CHD, CaG and CM diol.

5. The method for preparing an isohexide alcohol-based polycarbonate copolymer according to claim 1, characterized in that: The diol A3 is one or more of CHDM, CBDO, ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol.

6. The method for preparing an isohexide alcohol-based polycarbonate copolymer according to claim 1, characterized in that: The carbonic acid diester is one or more of diphenyl carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, dibutyl carbonate, dipentyl carbonate and dioctyl carbonate.

7. The method for preparing an isohexide alcohol-based polycarbonate copolymer according to claim 1, characterized in that: The catalyst is a metal catalyst.

8. The method for preparing an isohexide alcohol-based polycarbonate copolymer according to claim 1, characterized in that: The molar amount of catalyst is 1×10 of the total molar amount of diol. -5 -5×10 -4 .

9. The method for preparing an isohexide alcohol-based polycarbonate copolymer according to claim 1, characterized in that: The transesterification reaction is carried out under the protection of nitrogen or inert gas, the temperature of the transesterification reaction is 120-160°C, the pressure is 0.1MPa, and the time is 1.5-4h; the temperature of the final polycondensation reaction is 230-250°C, the pressure is below 150Pa, and the time is 0.5-2h.

Citation Information

Patent Citations

  • High-molecular-weight high-flexibility bio-based polycarbonate copolymer and preparation method thereof

    CN111138650A

  • Preparation method of isosorbide copolyester

    CN109134834A

  • Bio-based polycarbonate compound and preparation method thereof

    CN111925513A

  • Isosorbide polycarbonate and preparation method thereof

    CN114957640A

  • Bio-based heat-resistant copolyester as well as preparation method and application thereof

    CN117510811A

Cited By