Degradable foaming slipper material and preparation method thereof

Through a combination of materials such as citric acid esterified starch and maleic anhydride-modified polylactic acid, combined with specific processing, the problems of uneven cells and low foaming ratio in biodegradable foam plastics have been solved, and high mechanical strength and recovery have been achieved. Elastic, degradable foam slipper material reduces costs and improves the performance of traditional materials.

CN118725418APending Publication Date: 2024-10-01ANHUI TOPS SHOES CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410946730.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing biodegradable foams have problems with uneven cell sizes and low foaming rates during the foaming process. In particular, the thermodynamic incompatibility of PBAT/PLA blend materials leads to a decrease in melt strength and cell nucleation. Uneven.

Method used

Citrate esterified starch, maleic anhydride-modified polylactic acid, polybutylene adipate-terephthalate, cellulose nanofibers and other materials are used to prepare citrate esterified starch through infrared radiation, combined with hydrophobic additives , cross-linking agent, antioxidant, lubricant, foaming agent and plasticizer, and through blending, stirring, granulation and internal mixing processes, a degradable foam slipper material with uniform cells and high foaming ratio is prepared.

Benefits of technology

The cell size is uniform, the foaming ratio is increased, the material has good mechanical strength and resilience, the cost is reduced by 30%, and there is no obvious plastic taste, which significantly improves the performance of traditional foaming materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of foaming slippers, in particular to a degradable foaming slipper material and a preparation method thereof.The degradable foaming slipper material is prepared from, by weight, 40-55 parts of citric acid esterified starch; 10 to 20 parts of maleic anhydride modified polylactic acid; 5 to 15 parts of poly (butylene adipate-co-terephthalate); 3 to 10 parts of cellulose nanofiber; 0.3-1 part of a hydrophobic auxiliary agent; 3-5 parts of a cross-linking agent; 0.3 to 1 part of an antioxidant; 0.5-2 parts of a lubricant; 2-4 parts of a foaming agent; and 0.1-0.5 part of a plasticizer. According to the degradable foaming slipper material and the preparation method thereof, the degradable foaming slipper material is degradable, high in bio-based content and good in mechanical strength, the foaming slipper material is good in rebound resilience, the starch is adopted as a base material, the cost can be remarkably reduced, the modified starch prepared through a chemical reaction of citric acid and the starch can be used for preparing the degradable foaming slipper material, and the cost is reduced. The modification can improve the solubility and expansibility of the starch, the coloring is stable and uniform, and no obvious plastic taste exists.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of foam slippers, and in particular to a degradable foam slipper material and a preparation method thereof. Background Art

[0002] For more than half a century, petroleum-based non-degradable plastics have been widely used in daily life and in industrial and agricultural fields, but have also caused large-scale "white pollution", greenhouse gas emissions and consumption of petrochemical energy. In particular, disposable products such as plastic packaging shopping bags, plastic lunch boxes, foam products, etc. are widely used and then discarded in natural environments such as oceans, farmlands and lakes, seriously endangering human physical and mental health and becoming a global public hazard.

[0003] In order to solve the problem of "white pollution", there are currently two main research directions, one is the recycling and reuse of waste plastics, and the other is the research on biodegradable plastics.

[0004] Biodegradable plastics refer to products whose performance can meet the use requirements during the use and storage period, and can be completely degraded into carbon dioxide and water under natural environment (water, oxygen, heat and microorganisms, etc.) conditions after use and disposal. Most biodegradable plastics begin to become thinner, lose weight, and lose strength after being exposed to the natural environment for 3-6 months, and gradually break into pieces, and then gradually begin to degrade. In fact, biodegradable materials are an important way to solve "white pollution", achieve energy conservation and carbon reduction, and achieve sustainable development. Therefore, biodegradable foam materials have attracted widespread attention due to their biodegradability. The rapid development of biodegradable materials based on renewable resources has become an inevitable trend.

[0005] At present, the research and application of biodegradable foam plastics by scholars at home and abroad are mainly focused on polymers such as polylactic acid (PLA), polybutylene adipate / terephthalate (PBAT), polybutylene succinate (PBS) and starch. Among them, PBAT, PLA or PBAT / PLA blended alloy materials are mainly used for foaming. The performance of their products can reach or approach the performance standards of PE, EVA and PET foam products, and can completely replace petroleum-based non-degradable plastic products.

[0006] However, PBAT, PLA or PBAT / PLA blended foaming materials often have disadvantages such as low cell density, large cells and uneven distribution. Especially in the foaming process of PBAT / PLA blended materials, due to the thermodynamic incompatibility between PBAT and PLA, there is less entanglement between the segments of different materials, resulting in a decrease in melt strength. Inorganic nucleating agents are often added to control the nucleation of the cells, but inorganic nucleating agents are often particles with uneven particle sizes, so they are also prone to uneven cell sizes and low foaming ratios. Summary of the invention

[0007] Based on this, the present invention proposes a degradable foam slipper material and a preparation method thereof, which solves the current problems of uneven pore size and low foaming ratio.

[0008] According to a first aspect of the present invention, a biodegradable foam slipper material is provided, comprising the following material components by weight:

[0009] 40-55 parts of citric acid esterified starch;

[0010] Maleic anhydride modified polylactic acid 10-20 parts;

[0011] Polybutylene adipate-terephthalate 5-15 parts;

[0012] 3-10 parts of cellulose nanofibers;

[0013] 0.3-1 part of hydrophobic additive;

[0014] 3-5 parts of cross-linking agent;

[0015] Antioxidant 0.3-1 part;

[0016] Lubricant 0.5-2 parts;

[0017] 2-4 parts of foaming agent;

[0018] Plasticizer 0.1-0.5 parts.

[0019] According to an embodiment of the present invention, the hydrophobic auxiliary agent is two or more of a silane coupling agent, a titanate coupling agent, dodecylbenzene sulfonyl, peanut oil, an aluminate coupling agent, an aluminum-titanium composite coupling agent and stearic acid.

[0020] According to an embodiment of the present invention, the antioxidant includes one or more of an ammonia antioxidant, a phenolic antioxidant, a phosphite antioxidant and a sulfur-containing antioxidant.

[0021] According to an embodiment of the present invention, the lubricant is zinc stearate.

[0022] According to an embodiment of the present invention, the foaming agent includes an azo foaming agent and / or a sulfonylhydrazide foaming agent.

[0023] According to an embodiment of the present invention, the plasticizer is selected from one or more of aliphatic dibasic acid esters, phthalates, polybenzoates, benzoates, polyol esters, chlorinated hydrocarbons, epoxies, citrates and polyester plasticizers.

[0024] According to an embodiment of the present invention, the cross-linking agent is selected from one or more of benzoyl peroxide, di-tert-butyl peroxide and dicumyl peroxide.

[0025] According to a second aspect of the present invention, there is provided a method for preparing the above-mentioned degradable foam slipper material, comprising the following steps:

[0026] preparing citric acid esterified starch;

[0027] Blending citrate-esterified starch, maleic anhydride-modified polylactic acid and polybutylene adipate terephthalate to form a uniform slurry;

[0028] Adjust the temperature to 85-95°C, add the hydrophobic additive, and stir at 1000-1500 rpm for 6-12 minutes;

[0029] Add the crosslinking agent, antioxidant, lubricant and plasticizer into a high-speed mixer, stir at 75-90°C and 500-1000 rpm for 10-30 minutes to obtain a mixture;

[0030] The mixed material is added into a twin-screw granulator, and the zone temperature is set, wherein the temperature of the first section and the rear section are both set to 130° C.-160° C., the temperature of the middle section is set to 160° C.-165° C., and the temperature of the rear section is set to 145° C.-150° C., and granulation is performed to obtain granules;

[0031] The granulated material and the foaming agent are added into an internal mixer, and are internally kneaded at 115-125° C. After the internal kneading is completed, the material is cooled to obtain a degradable foamed slipper material.

[0032] According to an embodiment of the present invention, the preparation of citric acid esterified starch comprises:

[0033] Adding citric acid to starch solution and reacting by infrared radiation to obtain the citric acid esterified starch;

[0034] Among them, the infrared radiation illumination is 2474W / m 2 , infrared radiation time 7.1min, pH value 2.96, mass ratio of citric acid to starch 1:2.

[0035] It can be seen from the above technical solutions that the degradable foam slipper material and the preparation method thereof provided by the present invention have the following beneficial effects:

[0036] The biodegradable foam slipper material and the preparation method thereof provided by the present invention are biodegradable, have a high biobased content, and have good mechanical strength. The foam slipper material has good resilience, and uses starch as a base material, which can significantly reduce costs. The modified starch is prepared by chemically reacting citric acid with starch using starch as a base material. This modification can improve the solubility and swelling power of the starch. The citric acid esterified starch has some unique functional properties, such as low sedimentation, ideal viscosity, shear resistance and high resistant starch content, stable and uniform coloring, and no obvious plastic taste. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0038] According to a first aspect of the present invention, a biodegradable foam slipper material is provided, comprising the following material components by weight:

[0039] 40-55 parts of citric acid esterified starch;

[0040] Maleic anhydride modified polylactic acid 10-20 parts;

[0041] Polybutylene adipate-terephthalate 5-15 parts;

[0042] 3-10 parts of cellulose nanofibers;

[0043] 0.3-1 part of hydrophobic additive;

[0044] 3-5 parts of cross-linking agent;

[0045] Antioxidant 0.3-1 part;

[0046] Lubricant 0.5-2 parts;

[0047] 2-4 parts of foaming agent;

[0048] Plasticizer 0.1-0.5 parts.

[0049] Citrate starch is a modified starch prepared by chemically reacting citric acid with starch. This modification can improve the solubility and swelling power of starch. Citrate starch has some unique functional properties, such as low sedimentation, ideal viscosity, shear resistance and high resistant starch content.

[0050] Cellulose nanofibers (CNF) have been widely studied for reinforcing materials due to their excellent mechanical properties, high specific surface area and renewability. Cellulose nanofibers can improve the mechanical properties and environmental adaptability of materials.

[0051] Maleic anhydride (MAH) modified polylactic acid is obtained by chemically reacting maleic anhydride with polylactic acid (PLA) to improve certain properties of PLA, such as toughness, hydrophilicity, and mechanical properties.

[0052] The present invention selects cellulose nanofibers as the main raw material to replace traditional plant fibers, modifies the fibers, and adds the fibers to the formulation system to significantly improve the tensile strength and the compressive strength.

[0053] According to an embodiment of the present invention, the hydrophobic auxiliary agent is two or more of a silane coupling agent, a titanate coupling agent, dodecylbenzenesulfonyl, peanut oil, an aluminate coupling agent, an aluminum-titanium composite coupling agent and stearic acid.

[0054] The degradable foam slipper material and the preparation method thereof provided by the present invention are degradable, have a high bio-based content, and have good mechanical strength. The foam slipper material has good resilience and uses starch as a base material, which can significantly reduce costs. Compared with traditional EVA foam materials, the cost can be reduced by 30%. Using starch as a base material, the coloring is stable and uniform, and there is no obvious plastic smell.

[0055] According to an embodiment of the present invention, the antioxidant includes one or more of an ammonia antioxidant, a phenolic antioxidant, a phosphite antioxidant and a sulfur-containing antioxidant.

[0056] According to an embodiment of the present invention, the lubricant is zinc stearate.

[0057] According to an embodiment of the present invention, the foaming agent includes an azo foaming agent and / or a sulfonylhydrazide foaming agent.

[0058] According to an embodiment of the present invention, the plasticizer is selected from one or more of aliphatic dibasic acid esters, phthalic acid esters, polybenzoic acid esters, benzoic acid esters, polyol esters, chlorinated hydrocarbons, epoxies, citrates and polyester plasticizers.

[0059] According to an embodiment of the present invention, the cross-linking agent is selected from one or more of benzoyl peroxide, di-tert-butyl peroxide and dicumyl peroxide.

[0060] According to a second aspect of the present invention, there is provided a method for preparing the above-mentioned degradable foam slipper material, comprising the following steps:

[0061] preparing citric acid esterified starch;

[0062] Blending citrate-esterified starch, maleic anhydride-modified polylactic acid and polybutylene adipate terephthalate to form a uniform slurry;

[0063] Adjust the temperature to 85-95°C, add the hydrophobic additive, and stir at 1000-1500 rpm for 6-12 minutes;

[0064] Add the crosslinking agent, antioxidant, lubricant and plasticizer into a high-speed mixer, stir at 75-90°C and 500-1000 rpm for 10-30 minutes to obtain a mixture;

[0065] The mixed material is added into a twin-screw granulator, and the zone temperature is set, wherein the temperature of the first section and the rear section are both set to 130°C-160°C, the temperature of the middle section is set to 160°C-165°C, and the temperature of the rear section is set to 145-150°C, and granulation is performed to obtain granules;

[0066] The granulated material and the foaming agent are added into an internal mixer, and are internally kneaded at 115-125° C. After the internal kneading is completed, the material is cooled to obtain a biodegradable foamed slipper material.

[0067] According to an embodiment of the present invention, preparing citrate esterified starch comprises:

[0068] Adding citric acid into starch solution and reacting by infrared radiation to obtain citric acid esterified starch;

[0069] Among them, the infrared radiation illumination is 2474W / m 2 , infrared radiation time 7.1min, pH value 2.96, mass ratio of citric acid to starch 1:2.

[0070] The technical solution of the present invention is described in detail below through preferred embodiments. It should be noted that the specific embodiments below are only used for illustration and are not used to limit the present invention.

[0071] A method for preparing the above-mentioned degradable foam slipper material is provided, comprising the following steps:

[0072] Citric acid was added to the starch solution and reacted by infrared radiation to obtain citric acid esterified starch; the infrared radiation illumination was 2474W / m 2 , infrared radiation time 7.1min, pH value 2.96, mass ratio of citric acid to starch 1:2;

[0073] Blending citrate-esterified starch, maleic anhydride-modified polylactic acid and polybutylene adipate terephthalate to form a uniform slurry;

[0074] Adjust the temperature to 85-95°C, add the hydrophobic additive, and stir at 1000-1500 rpm for 6-12 minutes;

[0075] Add the crosslinking agent, antioxidant, lubricant and plasticizer into a high-speed mixer, stir at 75-90°C and 500-1000 rpm for 10-30 minutes to obtain a mixture;

[0076] The mixed material is added into a twin-screw granulator, and the zone temperature is set, wherein the temperature of the first section and the rear section are both set to 130°C-160°C, the temperature of the middle section is set to 160°C-165°C, and the temperature of the rear section is set to 145-150°C, and granulation is performed to obtain granules;

[0077] The granulated material and the foaming agent are added into an internal mixer, and are internally kneaded at 115-125° C. After the internal kneading is completed, the material is cooled to obtain a biodegradable foamed slipper material.

[0078] Embodiment 1:

[0079] Provided is a degradable foam slipper material, comprising the following components:

[0080] 40 parts of citric acid esterified starch;

[0081] Maleic anhydride modified polylactic acid 20 parts;

[0082] Polybutylene adipate-terephthalate 15 parts;

[0083] 3 parts of cellulose nanofibers;

[0084] 0.3 parts of a mixture of a silane coupling agent and a titanate coupling agent;

[0085] 3 parts of benzoyl peroxide;

[0086] 0.3 parts of sulfur-containing antioxidant;

[0087] 0.5 parts of zinc stearate;

[0088] 2 parts of sulfonylhydrazide foaming agent;

[0089] Polyol esters 0.1 parts.

[0090] Embodiment 2:

[0091] 55 parts of citric acid esterified starch;

[0092] Maleic anhydride modified polylactic acid 10 parts;

[0093] Polybutylene adipate-terephthalate 5 parts;

[0094] 5 parts of cellulose nanofibers;

[0095] 1 part of dodecylbenzenesulfonyl and peanut oil;

[0096] 5 parts of di-tert-butyl peroxide;

[0097] 1 part of phosphite antioxidant;

[0098] 2 parts of zinc stearate;

[0099] 3 parts of azo foaming agent;

[0100] 0.5 parts of benzoic acid esters.

[0101] Embodiment 3:

[0102] 50 parts of citric acid esterified starch;

[0103] Maleic anhydride modified polylactic acid 15 parts;

[0104] 10 parts of polybutylene adipate-terephthalate;

[0105] 8 parts of cellulose nanofibers;

[0106] 0.8 parts of aluminate coupling agent and aluminum-titanium composite coupling agent; 4 parts of dicumyl peroxide;

[0107] 0.5 parts of phenolic antioxidant;

[0108] 1 part of zinc stearate;

[0109] 2 parts of azo foaming agent;

[0110] 2 parts of sulfonylhydrazide foaming agent;

[0111] Chlorinated hydrocarbons 0.2 parts.

[0112] Embodiment 4:

[0113] 45 parts of citric acid esterified starch;

[0114] Maleic anhydride modified polylactic acid 12 parts;

[0115] Polybutylene adipate-terephthalate 8 parts;

[0116] 10 parts of cellulose nanofibers;

[0117] Peanut oil and stearic acid 0.5 parts;

[0118] 4 parts of benzoyl peroxide;

[0119] 0.3 parts of ammonia antioxidant;

[0120] 1 part of zinc stearate;

[0121] 4 parts of sulfonylhydrazide foaming agent;

[0122] 0.5 parts of benzene polyesters.

[0123] Experimental example:

[0124] For Examples 1-4, the tensile strength was tested according to GB / T6344-1996, and the compressive strength was tested according to GB / T6669-2001. The test results are as follows.

[0125] Table 1. Performance test table of Examples 1-4

[0126] Tensile strength / MPa Compression strength / MPa Example 1 32.4 4.2 Example 2 33.2 4.3 Example 3 31.6 4.1 Example 4 31.5 3.9

[0127] It can be seen from the contents in Table 1 that Examples 1-4 have relatively good properties in all tests. The degradable foam slipper material and the preparation method thereof provided by the present invention are degradable, have a high bio-based content, and have good mechanical strength. The foam slipper material has good resilience, and using starch as a base material can significantly reduce costs. The modified starch prepared by chemically reacting citric acid with starch using starch as a base material can improve the solubility and swelling power of the starch. The citric acid esterified starch has some unique functional properties, such as low sedimentation, ideal viscosity, shear resistance and high resistant starch content, stable and uniform coloring, and no obvious plastic taste.

[0128] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A degradable foam slipper material, characterized in that: According to weight fraction, it includes the following material components: 40-55 parts of citric acid esterified starch; Maleic anhydride modified polylactic acid 10-20 parts; Polybutylene adipate-terephthalate 5-15 parts; 3-10 parts of cellulose nanofibers; 0.3-1 part of hydrophobic additive; 3-5 parts of cross-linking agent; Antioxidant 0.3-1 part; Lubricant 0.5-2 parts; 2-4 parts of foaming agent; Plasticizer 0.1-0.5 parts.

2. The biodegradable foam slipper material according to claim 1, characterized in that: The hydrophobic auxiliary agent is two or more of silane coupling agent, titanate coupling agent, dodecylbenzene sulfonyl, peanut oil, aluminate coupling agent, aluminum-titanium composite coupling agent and stearic acid.

3. The biodegradable foam slipper material according to claim 1, characterized in that: The antioxidant includes one or more of an ammonia antioxidant, a phenolic antioxidant, a phosphite antioxidant and a sulfur-containing antioxidant.

4. The biodegradable foam slipper material according to claim 1, characterized in that: The lubricant is zinc stearate.

5. The biodegradable foam slipper material according to claim 1, characterized in that: The foaming agent includes an azo foaming agent and / or a sulfonylhydrazide foaming agent.

6. The biodegradable foam slipper material according to claim 1, characterized in that: The plasticizer is selected from one or more of aliphatic dibasic acid esters, phthalic acid esters, polybenzoic acid esters, benzoic acid esters, polyol esters, chlorinated hydrocarbons, epoxies, citrates and polyester plasticizers.

7. The biodegradable foam slipper material according to claim 1, characterized in that: The cross-linking agent is selected from one or more of benzoyl peroxide, di-tert-butyl peroxide and dicumyl peroxide.

8. A method for preparing the degradable foam slipper material according to any one of claims 1 to 7, characterized in that: The steps include: preparing citric acid esterified starch; Blending citrate-esterified starch, maleic anhydride-modified polylactic acid and polybutylene adipate terephthalate to form a uniform slurry; Adjust the temperature to 85-95°C, add the hydrophobic additive, and stir at 1000-1500 rpm for 6-12 minutes; Add the crosslinking agent, antioxidant, lubricant and plasticizer into a high-speed mixer, stir at 75-90°C and 500-1000 rpm for 10-30 minutes to obtain a mixture; The mixed material is added into a twin-screw granulator, and the zone temperature is set, wherein the temperature of the first section and the rear section are both set to 130° C.-160° C., the temperature of the middle section is set to 160° C.-165° C., and the temperature of the rear section is set to 145° C.-150° C., and granulation is performed to obtain granules; The granulated material and the foaming agent are added into an internal mixer, and are internally kneaded at 115-125° C. After the internal kneading is completed, the material is cooled to obtain a degradable foamed slipper material.

9. The method for preparing a degradable foam slipper material according to claim 8, characterized in that: The preparation of citric acid esterified starch comprises: Adding citric acid to starch solution and reacting by infrared radiation to obtain the citric acid esterified starch; Among them, the infrared radiation illumination is 2474W / m 2 , infrared radiation time 7.1min, pH value 2.96, mass ratio of citric acid to starch 1:2.

Citation Information

Cited By

  • Preparation process of degradable environment-friendly shoe material

    CN119286068A