Double-sided interconnected airtight packaging structure and preparation method thereof
By constructing metal frame and micro-column structures on ceramic packaging substrates, combined with laser local brazing technology, the problem that the packaging structure in the existing technology cannot meet the requirements of high integration density and airtightness is solved, and PoP stacked packaging and printing are realized High-efficiency air-seal packaging for double-sided interconnection of circuit boards.
Patent Information
- Application Number
- CN202210813168.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-07-12
AI Technical Summary
The prior art is difficult to meet the requirements of high integration density and airtightness when realizing double-sided interconnection of PoP stacked packaging and printed circuit boards, especially when using BGA technology.
Using a double-sided interconnected air-seal packaging structure, the air-seal packaging is formed through a ceramic packaging substrate and a metal frame. It combines metal micro-pillars and coaxial micro-band radio frequency transmission structure to ensure the air-tightness of the packaging and electrical signal transmission, and Local laser brazing is performed in high-purity inert gas environment to form sealed solder balls to enhance the airtightness of the packaging.
The requirements for double-sided integration of PoP stacked packaging and printed circuit boards are realized, which improves the integration density and packaging flexibility, while ensuring the airtightness of the packaging structure and the stability of the electrical signal, avoiding welding risks.
Smart Images

Figure CN115377050B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of microelectronic packaging, and in particular to a double-sided interconnected hermetic packaging structure and a preparation method thereof. Background Art
[0002] Miniaturization, multi-function and high performance are important directions for the development of electronic systems. Three-dimensional integration technology based on system-level packaging (SiP) is an important way to achieve miniaturization and multi-function of electronic systems. This technology emphasizes the use of adapter plates and packaging substrates to achieve chip stacking in three dimensions, integrating multiple chips, devices and passive components in one package to achieve a higher overall integration density. The use of package stacking technology (PoP, Package on Package) to stack packages with different functions in three dimensions can further improve the integration density of electronic systems. In PoP technology, it is usually necessary to achieve interconnection on both sides of the package to meet the needs of vertical transmission of electrical signals after three-dimensional integration.
[0003] In the plastic encapsulation structure, TMV (Through Molding Via) technology is usually used, that is, a hole is vertically punched on the plastic encapsulation material of the bottom plastic encapsulation module to the pad of the substrate, and then the TMV hole is metallized, and interconnected with the top module through BGA (Ball Grid Array) solder balls to achieve PoP stacked packaging. The above technology is used in the existing technology to achieve PoP stacked packaging. However, the plastic encapsulation structure cannot meet the needs of high-reliability applications due to its non-airtightness.
[0004] In silicon-based packaging structures, TSV (Through Silicon Via) technology is usually used, that is, by opening a cavity in the silicon adapter, combining TSV, metal micro-bumps or metal micro-pads, and using wafer-level bonding technology to achieve PoP stacked packaging. However, this technology is costly and not suitable for large-size packaging; ceramic and metal packaging processes are highly flexible and have high integration density and airtightness. They are the most widely used high-reliability packaging processes. The industry has conducted extensive research on this process. However, how to achieve double-sided interconnection based on BGA while meeting high integration density and airtight packaging, there are still some technical difficulties that need to be overcome. Summary of the invention
[0005] The present invention aims to provide a double-sided interconnected hermetic packaging structure and a preparation method thereof, so as to solve the problems in the prior art that the packaging structure cannot meet the requirements of PoP stacking packaging, cannot meet the requirements of double-sided interconnection with a printed circuit board, and cannot ensure the packaging airtightness requirements while improving the integration density.
[0006] The solution adopted by the present invention to solve the technical problem is:
[0007] A double-sided interconnected hermetic packaging structure comprises a first packaging substrate and a second packaging substrate;
[0008] The first packaging substrate and the second packaging substrate are both ceramic packaging substrates, the first packaging substrate and the second packaging substrate are parallel to each other, and both sides of the first packaging substrate and the second packaging substrate have a plurality of pads;
[0009] A metal frame is provided between the pads of the first packaging substrate and the second packaging substrate, and two ends of the metal frame are fixedly connected to the corresponding pads of the first packaging substrate and the second packaging substrate, respectively, and the first packaging substrate, the metal frame and the second packaging substrate together constitute an airtight packaging structure;
[0010] Part of the metal frame is hollowed out to form a semi-cylindrical cavity, and coaxial metal micro-columns are arranged in the semi-cylindrical cavity, and both ends of the metal micro-columns are fixedly connected to corresponding pads of the first packaging substrate and the second packaging substrate respectively;
[0011] The interconnection area between the first packaging substrate and the second packaging substrate and the metal micro-column is provided with a coaxial-to-microstrip radio frequency transmission structure;
[0012] A plurality of bare chips are arranged inside the airtight packaging structure, and the plurality of bare chips are respectively fixed on corresponding pads on the inner surfaces of the first packaging substrate and the second packaging substrate;
[0013] The solder pads on the outer surfaces of the first packaging substrate and the second packaging substrate are respectively fixedly connected with a first solder ball and a second solder ball.
[0014] The double-sided interconnected airtight packaging structure disclosed in the present embodiment arranges the first solder ball and the second solder ball on the front and back sides of the ceramic packaging substrate, so that the packaging structure can meet the requirements of PoP stacking packaging and the requirements of double-sided integration with the printed circuit board, thereby improving the integration density and enhancing the flexibility of packaging use; the first packaging substrate, the above-mentioned metal frame and the above-mentioned second packaging substrate together form an airtight packaging structure, thereby ensuring the airtightness of the packaging structure.
[0015] Optionally, the thermal expansion coefficient of the metal frame is the same as or similar to the thermal expansion coefficients of the first packaging substrate and the second packaging substrate, that is, the difference in thermal expansion coefficients between the two does not exceed 5 ppm / °C.
[0016] With such arrangement, the same or similar thermal expansion coefficients can facilitate welding the two ends of the metal frame to the inner surfaces of the first packaging substrate and the second packaging substrate, respectively.
[0017] Optionally: the above-mentioned metal microcolumns are all located in the above-mentioned airtight packaging structure, and one end of the above-mentioned metal microcolumns is welded to a corresponding pad on the inner surface of the above-mentioned first packaging substrate, and the other end of the above-mentioned metal microcolumns is welded to a corresponding pad on the inner surface of the above-mentioned second packaging substrate.
[0018] With such arrangement, the connection of electrical signals can be easily achieved through the plurality of the above-mentioned pads.
[0019] Optionally, the height of the metal micro-column is higher than the height of the metal surrounding frame, and the height difference between the metal micro-column and the metal surrounding frame is between 10 μm and 50 μm.
[0020] In this way, by adjusting the relative height between the metal microcolumn and the metal frame, the height of the metal microcolumn is slightly higher than the metal frame, and the welding process between the metal microcolumn and the second packaging substrate and the welding process between the metal frame and the second packaging substrate are separated, thereby ensuring the welding strength between the metal microcolumn and the second packaging substrate; and avoiding the risk of electrical signal disconnection caused by insufficient solder or electrical signal short circuit caused by excessive solder overflow when the metal microcolumn and the metal frame are welded at the same height at the same time.
[0021] Optionally: a first sealing surface is provided between one end of the metal frame and the corresponding pad of the first packaging substrate, and one end of the metal frame is welded to the corresponding pad of the first packaging substrate through the first sealing surface;
[0022] A second sealing surface is provided between the other end of the metal frame and the corresponding pad of the second packaging substrate, and the other end of the metal frame is welded to the corresponding pad of the second packaging substrate through the second sealing surface.
[0023] The arrangement is such that the first sealing surface and the second sealing surface enable the first packaging substrate, the metal surrounding frame and the second packaging substrate to jointly form an airtight packaging structure.
[0024] In one implementation of this embodiment: a method for preparing a double-sided interconnected hermetic packaging structure is also provided, the method comprising the following steps:
[0025] S1: providing the first packaging substrate, the metal frame and the metal micro-column, and welding one end of the metal frame and the metal micro-column to the inner surface of the first packaging substrate, wherein the welding surface between the one end of the metal frame and the inner surface of the first packaging substrate is the first sealing surface;
[0026] S2: providing the second packaging substrate and the bare chip, and integrating the bare chip on corresponding pads on the inner surfaces of the first packaging substrate and the second packaging substrate;
[0027] S3: welding the second packaging substrate obtained in step S2 to the metal micro-columns on the surface of the first packaging substrate;
[0028] S4: using a laser ball implantation process to sequentially inject a plurality of sealing solder balls between the second packaging substrate and the metal frame, wherein the distance between each sealing solder ball is between 10 μm and 50 μm;
[0029] S5: placing the packaging structure consisting of the first packaging substrate, the metal frame and the second packaging substrate obtained in step S4 in a glove box filled with high-purity inert gas, and using a laser local brazing process to melt the sealing solder balls in step S4 to obtain the second sealing surface, thereby obtaining a hermetic packaging structure;
[0030] S6: providing the first solder ball and the second solder ball, and using a laser ball implantation process to implant the first solder ball and the second solder ball respectively on corresponding solder pads on the outer surfaces of the first packaging substrate and the second packaging substrate in the airtight packaging structure to obtain a double-sided interconnected airtight packaging structure.
[0031] Optionally: in the above step S1, the welding process may adopt vacuum reflow welding or vacuum eutectic welding process, and the above first sealing surface is an airtight sealing surface.
[0032] This arrangement ensures the airtightness of the packaging structure.
[0033] Optionally: in the above step S3, the welding process may adopt reflow welding or eutectic welding process.
[0034] Such arrangement is used to realize electrical interconnection between the first packaging substrate and the second packaging substrate.
[0035] Optionally: in the above step S4, the size of the sealing solder ball is 50 μm to 300 μm, the material of the sealing solder ball is a high-temperature solder such as gold-tin, and the above laser ball implantation process is a local heating process.
[0036] With such an arrangement, the airtightness of the packaging structure is ensured by first laser ball implantation and then laser local brazing and sealing in a glove box, while at the same time ensuring that the atmosphere in the packaging structure is a high-purity inert gas. Compared with overall heating, the present invention ensures that the pressure of the atmosphere in the package is one atmosphere, thereby solving the problem of difficult airtight packaging of a double-sided interconnect structure.
[0037] Optionally: in the above step S6, the sizes of the above first solder ball and the above second solder ball are 100μm to 1000μm, and the materials of the above first solder ball and the above second solder ball are medium and low temperature solders such as tin-lead, tin-silver, tin-silver-copper, etc.
[0038] In summary, the double-sided interconnected hermetic packaging structure and the preparation method thereof disclosed in the present invention have the following beneficial effects:
[0039] (1) By arranging a plurality of the above-mentioned sealing solder balls on the outer side surfaces of the above-mentioned first packaging substrate and the above-mentioned second packaging substrate, the packaging structure can meet the requirements of PoP stacking packaging and the requirements of double-sided integration with a printed circuit board, thereby improving the integration density and enhancing the flexibility of packaging.
[0040] (2) By adjusting the relative height between the metal microcolumn and the metal frame so that the height of the metal microcolumn is slightly higher than the metal frame, and separating the welding process between the metal microcolumn and the second packaging substrate and the welding process between the metal frame and the second packaging substrate, the welding strength between the metal microcolumn and the second packaging substrate is ensured; and the risk of electrical signal disconnection due to insufficient solder or electrical signal short circuit due to excessive solder overflow when the metal microcolumn and the metal frame are welded at the same height and at the same time is avoided.
[0041] (3) The process of first laser ball implantation and then laser local brazing and sealing in a glove box ensures the airtightness of the packaging structure, while ensuring that the atmosphere in the packaging structure is a high-purity inert gas. Compared with overall heating, the present invention ensures that the pressure of the atmosphere in the package is one atmosphere, thus solving the problem of airtight packaging of double-sided interconnection structures. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0043] Figure 1 : A schematic cross-sectional view of a double-sided interconnected airtight packaging structure according to an embodiment of the present invention is shown;
[0044] Figure 2 Schematic diagram of the layout of the metal frame and the metal micro-columns in an embodiment of the present invention is shown in FIG.
[0045] Figure 3 A schematic diagram of the sealing solder ball injection process in an embodiment of the present invention is shown in FIG.
[0046] Figure 4 A schematic diagram of the laser local brazing process in an embodiment of the present invention is shown in FIG.
[0047] Figure 5 Detailed description of the process flow of the method for preparing the double-sided interconnected hermetic packaging structure according to the embodiment of the present invention is shown in FIG.
[0048] Icons: 1-first packaging substrate, 2-second packaging substrate, 3-solder pad, 4-metal frame, 5-airtight packaging structure, 6-semi-cylindrical cavity, 7-metal micro-column, 8-coaxial to microstrip RF transmission structure, 9-bare chip, 10-first solder ball, 11-second solder ball, 12-first sealing surface, 13-second sealing surface, 14-sealing solder ball. DETAILED DESCRIPTION
[0049] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0050] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] Example 1
[0052] See also Figure 1 , Figure 2 , Figure 3 and Figure 4 , this embodiment discloses a double-sided interconnected hermetic packaging structure, including a first packaging substrate 1 and a second packaging substrate 2;
[0053] The first packaging substrate 1 and the second packaging substrate 2 are both ceramic packaging substrates, the first packaging substrate 1 and the second packaging substrate 2 are parallel to each other, and both sides of the first packaging substrate 1 and the second packaging substrate 2 have a plurality of pads 3;
[0054] A metal frame 4 is provided between the pads 3 of the first packaging substrate 1 and the second packaging substrate 2, and two ends of the metal frame 4 are fixedly connected to the corresponding pads 3 of the first packaging substrate 1 and the second packaging substrate 2, respectively. The first packaging substrate 1, the metal frame 4 and the second packaging substrate 2 together form a hermetic packaging structure 5;
[0055] Part of the metal frame 4 is hollowed out to form a semi-cylindrical cavity 6, and coaxial metal micro-columns 7 are provided in the semi-cylindrical cavity 6. Both ends of the metal micro-columns 7 are fixedly connected to corresponding pads 3 of the first packaging substrate 1 and the second packaging substrate 2 respectively;
[0056] A coaxial-to-microstrip radio frequency transmission structure 8 is provided in the interconnection area between the first packaging substrate 1 and the second packaging substrate 2 and the metal microcolumn 7;
[0057] A plurality of bare chips 9 are arranged inside the airtight packaging structure 5, and the plurality of bare chips 9 are respectively fixed on corresponding pads 3 on the inner surfaces of the first packaging substrate 1 and the second packaging substrate 2;
[0058] The pads 3 on the outer surfaces of the first packaging substrate 1 and the second packaging substrate 2 are fixedly connected with the first solder ball 10 and the second solder ball 11 respectively.
[0059] The double-sided interconnected airtight packaging structure disclosed in the present embodiment arranges the first solder ball 10 and the second solder ball 11 on the front and back sides of the ceramic packaging substrate, so that the packaging structure can meet the requirements of PoP stacking packaging and the requirements of double-sided integration with the printed circuit board, thereby improving the integration density and enhancing the flexibility of packaging use; the first packaging substrate 1, the metal frame 4 and the second packaging substrate 2 together form an airtight packaging structure 5, which ensures the airtightness of the packaging structure.
[0060] See also Figure 1 , Figure 2 , Figure 3 and Figure 4 The thermal expansion coefficient of the metal frame 4 is the same as or similar to the thermal expansion coefficients of the first packaging substrate 1 and the second packaging substrate 2, that is, the difference in thermal expansion coefficients between the two does not exceed 5ppm / ℃. The same or similar thermal expansion coefficients can facilitate the welding of the two ends of the metal frame 4 on the inner surfaces of the first packaging substrate 1 and the second packaging substrate 2 respectively.
[0061] The metal microcolumns 7 are all located in the airtight packaging structure 5, and one end of the metal microcolumn 7 is welded to the corresponding pad 3 on the inner surface of the first packaging substrate 1, and the other end of the metal microcolumn 7 is welded to the corresponding pad 3 on the inner surface of the second packaging substrate 2. Through several pads 3, it is convenient to realize the connection of electrical signals.
[0062] The height of the metal microcolumn 7 is higher than the height of the metal frame 4, and the height difference between the metal microcolumn 7 and the metal frame 4 is between 10μm and 50μm. By adjusting the relative height of the metal microcolumn 7 and the metal frame 4, the height of the metal microcolumn 7 is slightly higher than the metal frame 4, and the welding process of the metal microcolumn 7 and the second packaging substrate 2 is separated from the welding process of the metal frame 4 and the second packaging substrate 2, thereby ensuring the welding strength of the metal microcolumn 7 and the second packaging substrate 2; avoiding the risk of electrical signal disconnection caused by insufficient solder or electrical signal short circuit caused by excessive solder overflow when the metal microcolumn 7 and the metal frame 4 are welded at the same height at the same time.
[0063] A first sealing surface 12 is provided between one end of the metal frame 4 and the corresponding pad 3 of the first packaging substrate 1, and one end of the metal frame 4 is welded to the corresponding pad 3 of the first packaging substrate 1 through the first sealing surface 12; a second sealing surface 13 is provided between the other end of the metal frame 4 and the corresponding pad 3 of the second packaging substrate 2, and the other end of the metal frame 4 is welded to the corresponding pad 3 of the second packaging substrate 2 through the second sealing surface 13: the first sealing surface 12 and the second sealing surface 13 make the first packaging substrate 1, the metal frame 4 and the second packaging substrate 2 together form an airtight packaging structure 5.
[0064] Example 2
[0065] See also Figure 1 , Figure 2 , Figure 3 , Figure 4 and Figure 5 This embodiment specifically discloses the preparation method of embodiment 1, which specifically includes the following steps:
[0066] S1: providing a first packaging substrate 1, a metal frame 4 and a metal micro-column 7, and welding one end of the metal frame 4 and the metal micro-column 7 to the inner surface of the first packaging substrate 1, wherein the welding surface between one end of the metal frame 4 and the inner surface of the first packaging substrate 1 is a first sealing surface 12;
[0067] In step S1, the welding process may adopt vacuum reflow welding or vacuum eutectic welding process, and the first sealing surface 12 is a hermetic sealing surface, so as to ensure the airtightness of the packaging structure;
[0068] Further, the welding process is a gold-germanium welding process;
[0069] S2: providing a second packaging substrate 2 and a bare chip 9, and integrating the bare chip 9 on corresponding pads 3 on the inner surfaces of the first packaging substrate 1 and the second packaging substrate 2;
[0070] S3: welding the second packaging substrate 2 obtained in step S2 to the metal micro-pillars 7 on the surface of the first packaging substrate 1 to achieve electrical interconnection between the first packaging substrate 1 and the second packaging substrate 2;
[0071] In step S3, the welding process may adopt reflow welding or eutectic welding process;
[0072] Further, the welding process is a gold-germanium welding process;
[0073] S4: using a laser ball implantation process to sequentially inject a plurality of sealing solder balls 14 between the second package substrate 2 and the metal frame 4, wherein the distance between each sealing solder ball 14 is between 10 μm and 50 μm;
[0074] In step S4, the size of the sealing solder ball 14 is 50 μm to 300 μm, and the material of the sealing solder ball 14 is a high-temperature solder such as gold tin. The laser ball implantation process is a local heating process. The process of laser ball implantation first and then laser local brazing and sealing in a glove box ensures the airtightness of the packaging structure, and at the same time ensures that the atmosphere in the packaging structure is a high-purity inert gas. Compared with overall heating, the present invention ensures that the pressure of the atmosphere in the package is one atmosphere, which solves the problem of difficult airtight packaging of a double-sided interconnect structure.
[0075] S5: placing the packaging structure consisting of the first packaging substrate 1, the metal frame 4 and the second packaging substrate 2 obtained in step S4 in a glove box filled with high-purity inert gas, and using a laser local brazing process to melt the sealing solder balls 14 in step S4 to obtain a second sealing surface 13, thereby obtaining a hermetic packaging structure 5;
[0076] S6: providing a first solder ball 10 and a second solder ball 11, and using a laser ball implantation process to implant the first solder ball 10 and the second solder ball 11 respectively on corresponding solder pads 3 on the outer surfaces of the first packaging substrate 1 and the second packaging substrate 2 in the airtight packaging structure 5, so as to obtain a double-sided interconnected airtight packaging structure 5;
[0077] In step S6 , the sizes of the first solder ball 10 and the second solder ball 11 are 100 μm to 1000 μm, and the materials of the first solder ball 10 and the second solder ball 11 are medium- and low-temperature solders such as tin-lead, tin-silver, or tin-silver-copper.
[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A double-sided interconnected airtight packaging structure, characterized in that: including a first packaging substrate and a second packaging substrate; The first packaging substrate and the second packaging substrate are both ceramic packaging substrates, the first packaging substrate and the second packaging substrate are parallel to each other, and both sides of the first packaging substrate and the second packaging substrate have a plurality of pads; A metal frame is provided between the pads of the first packaging substrate and the second packaging substrate, and two ends of the metal frame are fixedly connected to the corresponding pads of the first packaging substrate and the second packaging substrate, respectively, and the first packaging substrate, the metal frame and the second packaging substrate together constitute an airtight packaging structure; Part of the metal frame is hollowed out to form a semi-cylindrical cavity, each of the semi-cylindrical cavities is provided with a coaxial metal micro-column, and both ends of the metal micro-column are respectively fixedly connected to corresponding pads of the first packaging substrate and the second packaging substrate; The first packaging substrate and the second packaging substrate are provided with a coaxial-to-microstrip radio frequency transmission structure in the interconnection area with the metal micro-column; A plurality of bare chips are arranged inside the hermetic packaging structure, and the bare chips are respectively fixed on corresponding pads on the inner surfaces of the first packaging substrate and the second packaging substrate; The solder pads on the outer surfaces of the first packaging substrate and the second packaging substrate are respectively fixedly connected with a first solder ball and a second solder ball.
2. A double-sided interconnected airtight packaging structure according to claim 1, characterized in that: The thermal expansion coefficient of the metal frame is similar to the thermal expansion coefficients of the first packaging substrate and the second packaging substrate.
3. The double-sided interconnected airtight packaging structure according to claim 1, characterized in that: The metal microcolumns are all located in the airtight packaging structure, and one end of the metal microcolumns is welded to a corresponding pad on the inner surface of the first packaging substrate, and the other end of the metal microcolumns is welded to a corresponding pad on the inner surface of the second packaging substrate.
4. The double-sided interconnected airtight packaging structure according to claim 1, characterized in that: The height of the metal micro-column is higher than the height of the metal surrounding frame, and the height difference between the metal micro-column and the metal surrounding frame is between 10 μm and 50 μm.
5. The double-sided interconnected airtight packaging structure according to claim 1, characterized in that: A first sealing surface is provided between one end of the metal frame and the corresponding pad of the first packaging substrate, and one end of the metal frame is welded to the corresponding pad of the first packaging substrate through the first sealing surface; A second welding surface is provided between the other end of the metal frame and the corresponding welding pad of the second packaging substrate, and the other end of the metal frame is welded to the corresponding welding pad of the second packaging substrate through the second welding surface.
6. A method for preparing a double-sided interconnected hermetic packaging structure according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: S1: providing the first packaging substrate, the metal frame and the metal micro-column, and welding one end of the metal frame and the metal micro-column to the inner surface of the first packaging substrate, wherein the welding surface between one end of the metal frame and the inner surface of the first packaging substrate is the first sealing surface; S2: providing the second packaging substrate and the bare chip, and integrating the bare chip on corresponding pads on the inner surfaces of the first packaging substrate and the second packaging substrate; S3: welding the second packaging substrate obtained in step S2 to the metal micro-columns on the surface of the first packaging substrate; S4: using a laser ball implantation process to sequentially inject a plurality of sealing solder balls between the second packaging substrate and the metal frame, wherein the distance between each sealing solder ball is between 10 μm and 50 μm; S5: placing the packaging structure consisting of the first packaging substrate, the metal frame and the second packaging substrate obtained in step S4 in a glove box filled with high-purity inert gas, and using a laser local brazing process to melt the sealing solder balls in step S4 to obtain the second sealing surface, thereby obtaining a hermetic packaging structure; S6: providing the first solder ball and the second solder ball, and using a laser ball implantation process to implant the first solder ball and the second solder ball respectively on corresponding solder pads on the outer surfaces of the first packaging substrate and the second packaging substrate in the hermetic packaging structure to obtain a double-sided interconnected hermetic packaging structure.
7. The method for preparing a double-sided interconnected hermetic packaging structure according to claim 6, characterized in that: In the step S1, the welding process adopts a vacuum reflow welding process or a vacuum eutectic welding process, and the first sealing surface is a hermetic sealing surface.
8. The method for preparing a double-sided interconnected hermetic packaging structure according to claim 6, characterized in that: In step S3, the welding process adopts a reflow welding process or a eutectic welding process.
9. The method for preparing a double-sided interconnected hermetic packaging structure according to claim 6, characterized in that: In the step S4, the size of the sealing solder ball is 50 μm to 300 μm, the material of the sealing solder ball is gold-tin high-temperature solder, and the laser ball implantation process is a local heating process.
10. The method for preparing a double-sided interconnected hermetic packaging structure according to claim 6, characterized in that: In the step S6, the sizes of the first solder ball and the second solder ball are 100 μm to 1000 μm, and the materials of the first solder ball and the second solder ball are both medium-low temperature solder.