A method for preparing a SiC-C porous composite negative electrode material and a formation method for a lithium battery containing the material

Through the preparation of SiC-C porous composite anode materials and the formation method of twice injecting electrolyte, the problem of insufficient cycle life in lithium battery production has been solved, and a lithium battery with high capacity, good conductivity and long cycle life has been realized, inhibiting the The volume of SiC expands and controls the thickness of the SEI film, improving the cycle performance of the battery.

CN115394975BActive Publication Date: 2024-10-25HU ZHOU YAO NING GU TAI DIAN CHI YAN JIU YUAN YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210878995.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-25
Publication Date
2024-10-25
Estimated Expiration
2042-07-25

AI Technical Summary

Technical Problem

It is difficult to achieve low-cost, high-efficiency and long cycle life lithium battery manufacturing in existing lithium battery production. The existing technology requires major modifications to the equipment and has little production modifiability, and the poor matching between the separator and the electrolyte leads to insufficient cycle life.

Method used

Using the preparation method of SiC-C porous composite anode material, by continuously changing the SiC and C content of the core layer and shell layer, combined with the two-time injection of electrolyte and two-time formation method, a material with high capacity, good conductivity and Lithium batteries with long cycle life suppress the volume expansion of SiC and control the SEI film thickness.

Benefits of technology

It achieves the high capacity, good conductivity and long cycle life of lithium batteries, avoids the volume expansion of SiC from destroying the anode structure, extends the cycle life, and promotes delithiation and lithium insertion through appropriate SEI film thickness, improving the battery cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003763518670000111
    Figure BDA0003763518670000111
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium batteries, and discloses a method for preparing a SiC-C porous composite negative electrode material and a formation method for a lithium battery containing the material. On the one hand, the present invention provides a SiC-C porous composite negative electrode material, including a core layer and a shell layer, in which the content of SiC is more than the content of C in the core layer, and in the shell layer, the content of C is more than the content of SiC, the content of SiC decreases transitionally from the core layer to the shell layer, and the content of C increases transitionally from the core layer to the shell layer. The lithium battery with the material as the negative electrode can well inhibit the expansion of the negative electrode, and has excellent performances of high capacity, good conductivity and long cycle life. At the same time, the volume expansion of SiC is further improved by showing continuous changes in the content of SiC and C. On the other hand, a formation method comprising two injections of electrolyte and two formations is provided, so that the SEI film obtained by the formation is generated at a suitable thickness, which promotes the de-lithiation and lithium insertion, and cooperates with the negative electrode containing the SiC-C porous composite negative electrode material provided by the present invention, which greatly prolongs the cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a method for preparing a SiC-C porous composite negative electrode material and a formation method for a lithium battery containing the material. Background Art

[0002] Lithium batteries have the advantages of high energy density and high safety. They are an indispensable component of the new energy industry chain in recent years, and the preparation of lithium batteries with excellent performance has become the goal of lithium battery industry professionals. With the development and progress of society, more lithium battery application scenarios have been opened up, such as industrial energy storage, household energy storage, or base station energy storage, and energy storage scenarios all require lithium batteries to have a long cycle life or an ultra-long calendar life. In the production and manufacturing process of lithium-ion batteries, due to the complex composition and system of the slurry, it is challenging for lithium battery manufacturers to develop lithium batteries with a long cycle life.

[0003] In the existing technology, the development of long cycle life lithium batteries is often achieved by replenishing lithium or improving the membrane interface. However, the existing production lines of such methods cannot manufacture lithium batteries at low cost and high efficiency, and the existing production equipment needs to be significantly modified.

[0004] For example, a Chinese patent with application publication number CN 112350026 A and application publication date February 9, 2021 provides a diaphragm and a lithium battery using the diaphragm to optimize the cycle life of the battery, but it has the following shortcomings: (1) The coatings on both sides of the diaphragm need to be different, but the existing process has not been able to achieve this well, and the existing equipment needs to be modified, and its production cost is relatively high; (2) The diaphragm needs to be matched with the electrolyte slurry to achieve a longer cycle life performance. Replacing the electrolyte cannot achieve long cycle life performance, and the production modifiability is low.

[0005] Therefore, developing long cycle life lithium batteries to meet people's production and life needs remains the goal of people in the lithium battery industry. Summary of the invention

[0006] In order to solve the above-mentioned technical problems of developing lithium batteries with long cycle life, the present invention provides a method for preparing a SiC-C porous composite negative electrode material and a formation method for a lithium battery containing the material. On the one hand, the present invention provides a method for preparing a SiC-C porous composite negative electrode material, and a lithium battery containing the prepared SiC-C porous composite negative electrode material has excellent performances of high capacity, good conductivity and long cycle life, and the volume expansion of SiC is further improved by setting the continuous change of the SiC and C contents. On the other hand, a formation method comprising two injections of electrolyte and two formations is provided, so that the SEI film obtained by the formation is generated at a suitable thickness, which promotes the delithiation and insertion of lithium, and cooperates with the negative electrode containing the SiC-C porous composite negative electrode material provided by the present invention, which greatly prolongs the cycle life.

[0007] The specific technical scheme of the present invention is:

[0008] On the one hand, the present invention provides a method for preparing a SiC-C porous composite negative electrode material. The prepared SiC-C porous composite negative electrode material includes a core layer and a shell layer. The core layer and the shell layer materials include SiC and C. In the core layer, the content of SiC is greater than that of C, and in the shell layer, the content of SiC is less than that of C; the content of SiC decreases gradually from the center of the core layer to the shell layer, while the content of C increases gradually toward the shell layer. At the same time, the number of pores in the core layer is greater than that in the shell layer.

[0009] The SiC-C porous composite negative electrode material prepared by the preparation method of the present invention has a core layer main material of SiC with high capacity and excellent cycle performance, and a shell layer main material of C with excellent conductivity, so that the SiC-C porous composite negative electrode material of the present invention has high capacity, good conductivity and excellent performance of long cycle life when used as a negative electrode of a lithium battery. However, SiC has the defect of volume expansion during the battery charging and discharging process. The present invention improves its preparation method and utilizes the mutual coordination between heating, heat preservation and cooling to reduce the interfacial tension between SiC and C materials contained in the prepared SiC-C porous composite negative electrode material, so that SiC and C are better integrated into a whole, thereby improving the compaction density of the SiC-C porous composite negative electrode material, effectively inhibiting the volume expansion of SiC and increasing the unit capacity of the negative electrode. At the same time, since SiC is mainly distributed in the core layer, more holes are set in the core layer, which can reserve space for the volume expansion of SiC, so that when SiC expands, the original material structure of the negative electrode will not be destroyed, and the destruction-reconstruction process of the SEI film is reduced, which plays a role in extending the cycle life. C is mainly distributed in the shell layer, and its excellent conductivity is used to improve the rate of lithium removal and lithium insertion of lithium batteries. Preferably, the content of SiC decreases gradually from the center of the core layer to the shell layer, while the content of C increases gradually toward the shell layer. The continuous change of SiC and C content further improves the inhibitory effect on the volume expansion of SiC.

[0010] The specific preparation method of the SiC-C porous composite negative electrode material comprises the following steps:

[0011] (1) Under an inert gas atmosphere, 60 to 70 parts by weight of carbon powder with a particle size of 1 to 3 μm, 240 to 300 parts by weight of silicon powder and 0.5 to 0.8 parts by weight of nickel are mixed uniformly, and then the temperature is raised to 1000 to 1100° C., kept at this temperature for 1 to 2 hours, and then cooled. The obtained solid is ball-milled to obtain a mixed powder with a particle size of 1 to 5 μm.

[0012] In step (1), the compatibility of the interface of the raw materials can be promoted by heating and heat preservation, and the particle size of the raw materials can be made uniform by ball milling, thereby increasing the contact area between the raw materials and providing conditions for the next step of composite reaction.

[0013] (2) Under an inert gas atmosphere, the mixed powder obtained in step (1) is heated to 1300-1450° C., kept warm for 3-4 h, then cooled to 700-900° C., kept warm for 1-2 h, and then cooled and ball-milled in sequence to obtain a mixture containing SiC with a particle size of 0.1-0.3 μm.

[0014] In step (2), the temperature is raised to 1300-1450°C, C reacts with Si, and the reaction is fully achieved by heat preservation once. The mixture obtained by this step includes SiC and a small amount of Si. The temperature is lowered to 700-900°C for secondary heat preservation, which can improve the density of the material and make SiC and Si more compatible. At the same time, the mixture has a finer particle size and a larger specific surface area, which provides conditions for obtaining a core layer with a larger number of pores.

[0015] (3) The mixture obtained in step (2) is heated to 1250-1350° C. and then heat-insulated for three times. At the beginning of the three heat-insulations, 60-70 parts by weight of carbon powder with a particle size of 0.5-0.8 μm is purged onto the surface of the mixture by inert gas. After three heat-insulations for 1-2 hours, a semi-finished product is obtained.

[0016] In step (3), the temperature is raised to 1250-1350°C and kept warm three times to allow the remaining small amount of Si to fully react with the purged C. Using an inert gas as a carrier gas, at the beginning of the three insulations, carbon powder with a particle size of 0.5-0.8 μm is brought into the reaction system, and the newly generated SiC is attached to the surface of the mixture together with the purged C by gas purging. As the reaction proceeds, the remaining small amount of Si is completely reacted. At this time, the purged C is attached to the surface of the mixture. At the same time, since the particle size of the purged carbon powder is relatively large, the number of shell pores accumulated on the newly generated surface is relatively small compared to the core layer. Until the target weight portion of carbon powder with a particle size of 0.5-0.8 μm is purged and mixed, a semi-finished product is finally obtained. In the semi-finished product, the content of SiC decreases transitionally from the center of the core layer to the shell layer, while the content of C increases transitionally toward the shell layer.

[0017] (4) Under reduced pressure, the semi-finished product obtained in step (3) is cooled to 800-900° C. and hot-pressed for 40-50 min, and then cooled to room temperature to obtain a SiC-C porous composite negative electrode material.

[0018] In step (4), a reduced pressure environment is used to fully expel the gas in the pores of the SiC-C porous composite negative electrode material, and hot pressing is used to further increase the density of SiC and C.

[0019] Preferably, the inert gas is argon or helium.

[0020] More preferably, the vacuum degree of the reduced pressure in step (4) is 0 to -20 kPa, and the pressure of the hot pressing is 90 to 120 MPa.

[0021] The above-mentioned SiC-C porous composite negative electrode material is applied to the negative electrode of lithium battery. While SiC is used to increase the battery capacity and prolong the cycle life, it can also effectively inhibit its volume expansion.

[0022] On the other hand, the present invention provides a formation method for a lithium battery containing a SiC-C porous composite negative electrode material. The method further improves the cycle life of the lithium battery by injecting the electrolyte twice and forming twice in combination with the negative electrode containing the SiC-C porous composite negative electrode material.

[0023] Since the volume expansion of negative electrode materials in the long term will cause the SEI film to be destroyed, making lithium removal and lithium insertion hindered, the traditional method is to add excessive film-forming additives to prepare for the later repair of the damaged SEI film. However, adding too much film-forming additives often leads to an excessively thick SEI film, which in turn leads to the adverse consequence of increased resistance to lithium removal and lithium insertion. The method of the present invention controls the generated SEI film to a suitable thickness by injecting the electrolyte twice and forming it twice, and can reserve part of the film-forming additives for the repair of the SEI film in the later stage. The first injection is 70% to 90% of the total mass of the electrolyte contained in the lithium battery, and VC accounting for 2% to 4% of the total mass of the electrolyte is injected. At this time, the role of VC in the first formation is mainly to participate in the formation of the SEI film on the surface of the negative electrode. The second injection is 10% to 30% of the total mass of the electrolyte contained in the lithium battery, and 0.6% to 2% of the total mass of the electrolyte is injected. At a potential of 2.0 to 2.4V, VC does not participate in film formation, so the second injection of VC does not form a film during the secondary formation, avoiding the increase in impedance during lithium removal and lithium insertion caused by excessive SEI film thickness. The injected VC is used to repair and rebuild the SEI film that is damaged when SiC expands in the negative electrode in the later stage. At the same time, VC when it does not form a film can promote the migration of lithium and promote the cycle performance of the battery.

[0024] The above-mentioned lithium battery formation method specifically comprises the following steps:

[0025] (a) After sealing the three sides of the battery core pack, the battery core pack is dried under reduced pressure at 85-105° C. for 8-48 hours to obtain a battery ready for primary injection.

[0026] (b) Inject electrolyte A into the battery to be filled once, seal it with an air bag, and then let it stand until the electrolyte soaks the inside of the battery cell, then perform a formation, and then let it stand at 35-45°C for 48-60h to obtain a battery to be filled twice.

[0027] (c) Puncture a through hole in the airbag bag of the battery to be refilled with liquid, and then place it in an environment with a vacuum degree of no more than -95 kPa and let it stand for 15 to 30 seconds. Then, inject electrolyte B through the through hole and seal it. After secondary formation, evacuation, and edge sealing, a soft-pack lithium battery is obtained.

[0028] Preferably, in step (b), the electrolyte A accounts for 70% to 90% of the total mass of the electrolyte of the lithium battery, and the VC contained in the electrolyte A accounts for 2% to 4% of the total mass of the electrolyte of the lithium battery.

[0029] Preferably, in step (c), the electrolyte B accounts for 10% to 30% of the total mass of the electrolyte contained in the lithium battery, and the VC contained in the electrolyte B accounts for 0.6% to 2% of the total mass of the electrolyte of the lithium battery.

[0030] Specifically, the one-step formation method in step (b) comprises: charging at a rate of 0.02 to 0.05 C for 5 to 10 hours at a temperature of 42 to 48° C. and a clamping force of 0.3 to 0.6 MPa, to a charge level of 20% to 25% SOC.

[0031] Specifically, the secondary formation method in step (c) includes: charging to a capacity of 70% to 90% SOC at a rate of 0.1 to 0.3C under the conditions of a temperature of 42 to 48°C and a clamping force of 0.3 to 0.6MPa.

[0032] Preferably, in step (c), the vacuum degree is -110 to -95 kPa.

[0033] Compared with the prior art, the present invention has the following technical effects:

[0034] (1) The present invention provides a SiC-C porous composite negative electrode material. A lithium-ion battery containing a negative electrode prepared from the material has excellent properties of high capacity, good conductivity and long cycle life.

[0035] (2) The present invention further improves the effect of suppressing the volume expansion of SiC by setting the continuous change of SiC and C content.

[0036] (3) The present invention provides a formation method comprising two injections of electrolyte and two formations, thereby avoiding the problem of too thick SEI film obtained by formation due to the direct addition of too much film-forming additive to reserve for later SEI film repair, so that the SEI film obtained by formation is generated at an appropriate thickness, thereby promoting lithium removal and lithium insertion and extending the cycle life. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with the embodiments.

[0038] Example 1

[0039] The raw materials of the SiC-C porous composite negative electrode material include the following components in parts by weight: 100 parts of carbon powder with a particle size of 1 to 3 μm, 60 parts of carbon powder with a particle size of 0.5 to 0.8 μm, 240 parts of silicon powder, and 0.5 parts of nickel;

[0040] Preparation of SiC-C porous composite negative electrode material:

[0041] (1) In an argon atmosphere, carbon powder, silicon powder and nickel with a particle size of 1 to 3 μm are mixed uniformly, and then the temperature is raised to 1000° C., kept at this temperature for 1 hour and then cooled, and the obtained solid is ball-milled to obtain a mixed powder with a particle size of 1 to 5 μm;

[0042] (2) In an argon atmosphere, the mixed powder obtained in step (1) was heated to 1300° C., kept warm for 4 h, then cooled to 700° C. and kept warm for 1 h, and then cooled and ball-milled in sequence to obtain a mixture containing SiC with a particle size of 0.1 to 0.3 μm;

[0043] (3) heating the mixture obtained in step (2) to 1250° C. and then performing three heat preservation steps, and at the beginning of the three heat preservation steps, argon gas is used to purge carbon powder with a particle size of 0.5 to 0.8 μm onto the surface of the mixture, and after three heat preservation steps of 1 hour, a semi-finished product is obtained;

[0044] (4) Under a reduced pressure environment with a vacuum degree of 0 kPa, the semi-finished product obtained in step (3) is cooled to 800°C, hot-pressed at a pressure of 90 MPa for 50 minutes, and cooled to room temperature to obtain a SiC-C porous composite negative electrode material. The obtained SiC-C porous composite negative electrode material includes a core layer and a shell layer, the number of pores in the core layer is greater than that in the shell layer, the content of SiC decreases gradually from the core layer to the shell layer, and the content of C increases gradually from the core layer to the shell layer. In the core layer, the content of SiC is greater than that of C; in the shell layer, the content of SiC is less than that of C.

[0045] The obtained SiC-C porous composite negative electrode material is prepared into a lithium battery negative electrode, stacked with a positive electrode, assembled into a battery core pack, and then formed:

[0046] (a) The battery core package is sealed on three sides with aluminum-plastic film and then dried under reduced pressure at 85° C. for 48 h to obtain a battery ready for primary injection.

[0047] (b) Inject electrolyte A into the battery to be injected once, where electrolyte A accounts for 70% of the total mass of the electrolyte of the lithium battery, and VC contained in electrolyte A accounts for 2% of the total mass of the electrolyte of the lithium battery. Then seal it with an airbag bag, and then let it stand until electrolyte A soaks into the inside of the battery cell, and then perform a primary formation. The primary formation is specifically: charge at a rate of 0.02C for 10 hours at a temperature of 42°C and a clamping force of 0.3MPa, and charge 20% SOC. After the primary formation is completed, place it in a 35°C environment and let it stand for 60 hours to obtain a battery to be injected twice.

[0048] (c) Puncture a through hole in the airbag bag of the battery to be refilled with liquid, and then place it in a vacuum environment of -95kPa for 15s, then inject electrolyte B through the through hole and seal it. The electrolyte B accounts for 30% of the total mass of the electrolyte contained in the lithium battery, and the VC contained in the electrolyte B accounts for 2% of the total mass of the electrolyte contained in the lithium battery. Then perform secondary formation, which is specifically: charge to 70% SOC at a rate of 0.1C under the conditions of a temperature of 42°C and a clamping force of 0.3MPa. After the secondary formation is completed, evacuation and edge sealing are performed in sequence to finally obtain a soft-pack lithium battery.

[0049] Example 2

[0050] The raw materials of the SiC-C porous composite negative electrode material include the following components in parts by weight: 100 parts of carbon powder with a particle size of 1 to 3 μm, 70 parts of carbon powder with a particle size of 0.5 to 0.8 μm, 300 parts of silicon powder, and 0.8 parts of nickel;

[0051] Preparation of SiC-C porous composite negative electrode material:

[0052] (1) In a helium atmosphere, carbon powder, silicon powder and nickel with a particle size of 1 to 3 μm are mixed uniformly, and then the temperature is raised to 1100° C., kept at this temperature for 1.5 hours and then cooled, and the obtained solid is ball-milled to obtain a mixed powder with a particle size of 1 to 5 μm;

[0053] (2) In a helium atmosphere, the mixed powder obtained in step (1) was heated to 1450° C., kept warm for 3 h, then cooled to 900° C. and kept warm for 2 h, and then cooled and ball-milled in sequence to obtain a mixture containing SiC with a particle size of 0.1 to 0.3 μm;

[0054] (3) heating the mixture obtained in step (2) to 1350° C. and then performing three heat preservation operations. At the beginning of the three heat preservation operations, helium is used to blow carbon powder with a particle size of 0.5 to 0.8 μm onto the surface of the mixture. After three heat preservation operations for 1 hour, a semi-finished product is obtained.

[0055] (4) Under a reduced pressure environment with a vacuum degree of -20 kPa, the semi-finished product obtained in step (3) is cooled to 900°C, hot-pressed at a pressure of 120 MPa for 40 minutes, and cooled to room temperature to obtain a SiC-C porous composite negative electrode material. The obtained SiC-C porous composite negative electrode material includes a core layer and a shell layer, the number of pores in the core layer is greater than that in the shell layer, the content of SiC decreases gradually from the core layer to the shell layer, and the content of C increases gradually from the core layer to the shell layer. In the core layer, the content of SiC is greater than that of C; in the shell layer, the content of SiC is less than that of C.

[0056] The obtained SiC-C porous composite negative electrode material is prepared into a lithium battery negative electrode, stacked with a positive electrode, assembled into a battery core pack, and then formed:

[0057] (a) The battery core package was sealed on three sides with aluminum-plastic film and then dried under reduced pressure at 105° C. for 8 h to obtain a battery ready for single injection.

[0058] (b) Inject electrolyte A into the battery to be injected once, where electrolyte A accounts for 90% of the total mass of the electrolyte of the lithium battery, and VC contained in electrolyte A accounts for 4% of the total mass of the electrolyte of the lithium battery. Then seal it with an airbag bag, and then let it stand until electrolyte A soaks into the inside of the battery cell, and then perform a primary formation. The primary formation is specifically: charge at a rate of 0.05C for 5 hours at a temperature of 48°C and a clamping force of 0.6MPa, and charge 25% SOC. After the primary formation is completed, place it in a 45°C environment and let it stand for 48 hours to obtain a battery to be injected twice.

[0059] (c) Puncture a through hole in the airbag bag of the battery to be refilled with liquid, and then place it in a vacuum environment of -80kPa for 25s, then inject electrolyte B through the through hole and seal it. The electrolyte B accounts for 10% of the total mass of the electrolyte contained in the lithium battery, and the VC contained in the electrolyte B accounts for 1.5% of the total mass of the electrolyte contained in the lithium battery. Then perform secondary formation, which is specifically: charge to 90% SOC at a rate of 0.3C under the conditions of a temperature of 48°C and a clamping force of 0.6MPa. After the secondary formation is completed, evacuation and edge sealing are performed in sequence to finally obtain a soft-pack lithium battery.

[0060] Example 3

[0061] The raw materials of the SiC-C porous composite negative electrode material include the following components in parts by weight: 100 parts of carbon powder with a particle size of 1 to 3 μm, 65 parts of carbon powder with a particle size of 0.5 to 0.8 μm, 280 parts of silicon powder, and 0.6 parts of nickel;

[0062] Preparation of SiC-C porous composite negative electrode material:

[0063] (1) In an argon atmosphere, carbon powder, silicon powder and nickel with a particle size of 1 to 3 μm are mixed uniformly, and then the temperature is raised to 1050° C., kept at this temperature for 2 hours and then cooled, and the obtained solid is ball-milled to obtain a mixed powder with a particle size of 1 to 5 μm;

[0064] (2) In an argon atmosphere, the mixed powder obtained in step (1) was heated to 1400° C., kept warm for 3.5 h, then cooled to 800° C. and kept warm for 1.5 h, and then cooled and ball-milled in sequence to obtain a mixture containing SiC with a particle size of 0.1 to 0.3 μm;

[0065] (3) heating the mixture obtained in step (2) to 1300° C. and then performing three heat preservation cycles. At the beginning of the three heat preservation cycles, argon gas is blown onto the surface of the mixture to add carbon powder with a particle size of 0.5 to 0.8 μm. After three heat preservation cycles of 1.5 h, a semi-finished product is obtained.

[0066] (4) Under a reduced pressure environment with a vacuum degree of -10 kPa, the semi-finished product obtained in step (3) is cooled to 850°C, hot-pressed at a pressure of 100 MPa for 45 minutes, and cooled to room temperature to obtain a SiC-C porous composite negative electrode material. The obtained SiC-C porous composite negative electrode material includes a core layer and a shell layer, the number of pores in the core layer is greater than that in the shell layer, the content of SiC decreases gradually from the core layer to the shell layer, and the content of C increases gradually from the core layer to the shell layer. In the core layer, the content of SiC is greater than that of C; in the shell layer, the content of SiC is less than that of C.

[0067] The obtained SiC-C porous composite negative electrode material is prepared into a lithium battery negative electrode, stacked with a positive electrode, assembled into a battery core pack, and then formed:

[0068] (a) The battery core package is sealed on three sides with aluminum-plastic film and then dried under reduced pressure at 955°C for 24 hours to obtain a battery ready for single injection.

[0069] (b) Inject electrolyte A into the battery to be injected once, where electrolyte A accounts for 80% of the total mass of the electrolyte of the lithium battery, and VC contained in electrolyte A accounts for 3% of the total mass of the electrolyte of the lithium battery. Then seal it with an airbag bag, and then let it stand until electrolyte A soaks into the inside of the battery cell, and then perform a primary formation. The primary formation is specifically: charging at a rate of 0.04C for 7 hours at a temperature of 45°C and a clamping force of 0.5MPa, and charging a charge of 22% SOC. After the primary formation is completed, place it in a 40°C environment and let it stand for 55 hours to obtain a battery to be injected twice.

[0070] (c) Puncture a through hole in the airbag bag of the battery to be refilled with liquid, and then place it in a vacuum environment of -75kPa for 30s, then inject electrolyte B through the through hole and seal it. The electrolyte B accounts for 20% of the total mass of the electrolyte contained in the lithium battery, and the VC contained in the electrolyte B accounts for 2% of the total mass of the electrolyte contained in the lithium battery. Then perform secondary formation, which is specifically: charge to 80% SOC at a rate of 0.2C under the conditions of a temperature of 45°C and a clamping force of 0.5MPa. After the secondary formation is completed, evacuation and edge sealing are performed in sequence to finally obtain a soft-pack lithium battery.

[0071] Comparative Example 1 (The difference from Example 1 is that the negative electrode material is prepared by directly mixing the raw materials and then sintering them.) The raw materials of the negative electrode material include the following components in parts by weight: 100 parts of carbon powder with a particle size of 1 to 3 μm, 60 parts of carbon powder with a particle size of 0.5 to 0.8 μm, 240 parts of silicon powder, and 0.5 parts of nickel;

[0072] Preparation of negative electrode materials:

[0073] (1) Under an argon atmosphere, all the raw materials are mixed evenly, then heated to 1000°C, kept at this temperature for 1 hour, and then cooled, and the obtained solid is ball-milled to obtain a mixed powder with a particle size of 1 to 5 μm;

[0074] (2) In an argon atmosphere, the mixed powder obtained in step (1) was heated to 1300° C., kept warm for 4 h, then cooled to 700° C. and kept warm for 1 h, and then cooled and ball-milled in sequence to obtain a mixture containing SiC with a particle size of 0.1 to 0.3 μm;

[0075] (3) heating the mixture obtained in step (2) to 1250° C. and then performing three 1-hour heat preservation steps to obtain a semi-finished product;

[0076] (4) Under a reduced pressure environment with a vacuum degree of 0 kPa, the semi-finished product obtained in step (3) is cooled to 800° C., hot-pressed at a pressure of 90 MPa for 50 min, and cooled to room temperature to obtain a negative electrode material.

[0077] The obtained negative electrode material is prepared into a negative electrode for a lithium battery, which is stacked with a positive electrode to assemble a battery core pack and start the formation process:

[0078] (a) The battery core package is sealed on three sides with aluminum-plastic film and then dried under reduced pressure at 85° C. for 48 h to obtain a battery ready for primary injection.

[0079] (b) Inject electrolyte A into the battery to be injected once, where electrolyte A accounts for 70% of the total mass of the electrolyte of the lithium battery, and VC contained in electrolyte A accounts for 2% of the total mass of the electrolyte of the lithium battery. Then seal it with an airbag bag, and then let it stand until electrolyte A soaks into the inside of the battery cell, and then perform a primary formation. The primary formation is specifically: charge at a rate of 0.02C for 10 hours at a temperature of 42°C and a clamping force of 0.3MPa, and charge 20% SOC. After the primary formation is completed, place it in a 35°C environment and let it stand for 60 hours to obtain a battery to be injected twice.

[0080] (c) Puncture a through hole in the airbag bag of the battery to be refilled with liquid, and then place it in a vacuum environment of -95kPa for 15s, then inject electrolyte B through the through hole and seal it. The electrolyte B accounts for 30% of the total mass of the electrolyte contained in the lithium battery, and the VC contained in the electrolyte B accounts for 2% of the total mass of the electrolyte contained in the lithium battery. Then perform secondary formation, which is specifically: charge to 70% SOC at a rate of 0.1C under the conditions of a temperature of 42°C and a clamping force of 0.3MPa. After the secondary formation is completed, evacuation and edge sealing are performed in sequence to finally obtain a soft-pack lithium battery.

[0081] Comparative Example 2 (The difference from Example 1 is that the contents of SiC and C in the negative electrode material do not change in a gradient.)

[0082] The raw materials of the negative electrode material include the following components in parts by weight: 100 parts of carbon powder with a particle size of 1 to 3 μm, 60 parts of carbon powder with a particle size of 0.5 to 0.8 μm, 230 parts of silicon powder, and 0.5 parts of nickel;

[0083] Preparation of negative electrode materials:

[0084] (1) In an argon atmosphere, carbon powder, silicon powder and nickel with a particle size of 1 to 3 μm are mixed uniformly, and then the temperature is raised to 1000° C., kept at this temperature for 1 hour and then cooled, and the obtained solid is ball-milled to obtain a mixed powder with a particle size of 1 to 5 μm;

[0085] (2) In an argon atmosphere, the mixed powder obtained in step (1) was heated to 1300° C., kept warm for 4 h, then cooled to 700° C. and kept warm for 1 h, and then cooled and ball-milled in sequence to obtain a mixture containing SiC with a particle size of 0.1 to 0.3 μm;

[0086] (3) heating the mixture obtained in step (2) to 1250° C. and then performing three heat preservation steps, and at the beginning of the three heat preservation steps, argon gas is used to purge carbon powder with a particle size of 0.5 to 0.8 μm onto the surface of the mixture, and after three heat preservation steps of 1 hour, a semi-finished product is obtained;

[0087] (4) Under a reduced pressure environment with a vacuum degree of 0 kPa, the semi-finished product obtained in step (3) is cooled to 800°C, hot-pressed at a pressure of 90 MPa for 50 min, and cooled to room temperature to obtain a negative electrode material. The obtained negative electrode material includes a core layer and a shell layer, wherein the main material of the core layer is SiC, containing a very small amount of C; and the main material of the shell layer is C.

[0088] The obtained negative electrode material is prepared into a negative electrode for a lithium battery, which is stacked with a positive electrode to assemble a battery core pack and start the formation process:

[0089] (a) The battery core package is sealed on three sides with aluminum-plastic film and then dried under reduced pressure at 85° C. for 48 h to obtain a battery ready for primary injection.

[0090] (b) Inject electrolyte A into the battery to be injected once, where electrolyte A accounts for 70% of the total mass of the electrolyte of the lithium battery, and VC contained in electrolyte A accounts for 2% of the total mass of the electrolyte of the lithium battery. Then seal it with an airbag bag, and then let it stand until electrolyte A soaks into the inside of the battery cell, and then perform a primary formation. The primary formation is specifically: charge at a rate of 0.02C for 10 hours at a temperature of 42°C and a clamping force of 0.3MPa, and charge 20% SOC. After the primary formation is completed, place it in a 35°C environment and let it stand for 60 hours to obtain a battery to be injected twice.

[0091] (c) Puncture a through hole in the airbag bag of the battery to be refilled with liquid, and then place it in a vacuum environment of -95kPa for 15s, then inject electrolyte B through the through hole and seal it. The electrolyte B accounts for 30% of the total mass of the electrolyte contained in the lithium battery, and the VC contained in the electrolyte B accounts for 2% of the total mass of the electrolyte contained in the lithium battery. Then perform secondary formation, which is specifically: charge to 70% SOC at a rate of 0.1C under the conditions of a temperature of 42°C and a clamping force of 0.3MPa. After the secondary formation is completed, evacuation and edge sealing are performed in sequence to finally obtain a soft-pack lithium battery.

[0092] Comparative Example 3 (The difference from Example 1 is that the lithium battery is prepared by a common formation method.)

[0093] The raw materials of the negative electrode material include the following components in parts by weight: 100 parts of carbon powder with a particle size of 1 to 3 μm, 60 parts of carbon powder with a particle size of 0.5 to 0.8 μm, 240 parts of silicon powder, and 0.5 parts of nickel;

[0094] Preparation of negative electrode materials:

[0095] (1) In an argon atmosphere, carbon powder, silicon powder and nickel with a particle size of 1 to 3 μm are mixed uniformly, and then the temperature is raised to 1000° C., kept at this temperature for 1 hour and then cooled, and the obtained solid is ball-milled to obtain a mixed powder with a particle size of 1 to 5 μm;

[0096] (2) In an argon atmosphere, the mixed powder obtained in step (1) was heated to 1300° C., kept warm for 4 h, then cooled to 700° C. and kept warm for 1 h, and then cooled and ball-milled in sequence to obtain a mixture containing SiC with a particle size of 0.1 to 0.3 μm;

[0097] (3) heating the mixture obtained in step (2) to 1250° C. and then performing three heat preservation steps, and at the beginning of the three heat preservation steps, argon gas is used to purge carbon powder with a particle size of 0.5 to 0.8 μm onto the surface of the mixture, and after three heat preservation steps of 1 hour, a semi-finished product is obtained;

[0098] (4) Under a reduced pressure environment with a vacuum degree of 0 kPa, the semi-finished product obtained in step (3) is cooled to 800°C, hot-pressed at a pressure of 90 MPa for 50 min, and cooled to room temperature to obtain an AAAAA porous negative electrode material. The obtained negative electrode material includes a core layer and a shell layer, the core layer has more pores than the shell layer; in the core layer, the content of SiC is more than the content of C; in the shell layer, the content of SiC is less than the content of C.

[0099] The obtained negative electrode material is prepared into a negative electrode of a lithium battery, which is stacked with a positive electrode to assemble a battery core pack, and then directly injected with electrolyte, wherein the mass proportion of VC in the electrolyte is 4%. The formation is started as follows:

[0100] Under the conditions of a temperature of 45°C and a clamping force of 0.3MPa, after charging to 30% SOC at a rate of 0.03C, the current was converted to 0.2C and charged to 80% SOC, and then evacuation and sealing were performed in sequence to finally obtain a soft-pack lithium battery.

[0101] Comparative Example 4 (The difference from Example 1 is that the lithium battery is prepared by a common formation method, and the mass proportion of VC in the electrolyte is increased.)

[0102] The raw materials of the negative electrode material include the following components in parts by weight: 100 parts of carbon powder with a particle size of 1 to 3 μm, 60 parts of carbon powder with a particle size of 0.5 to 0.8 μm, 240 parts of silicon powder, and 0.5 parts of nickel;

[0103] Preparation of negative electrode materials:

[0104] (1) In an argon atmosphere, carbon powder, silicon powder and nickel with a particle size of 1 to 3 μm are mixed uniformly, and then the temperature is raised to 1000° C., kept at this temperature for 1 hour and then cooled, and the obtained solid is ball-milled to obtain a mixed powder with a particle size of 1 to 5 μm;

[0105] (2) In an argon atmosphere, the mixed powder obtained in step (1) was heated to 1300° C., kept warm for 4 h, then cooled to 700° C. and kept warm for 1 h, and then cooled and ball-milled in sequence to obtain a mixture containing SiC with a particle size of 0.1 to 0.3 μm;

[0106] (3) heating the mixture obtained in step (2) to 1250° C. and then performing three heat preservation steps, and at the beginning of the three heat preservation steps, argon gas is used to purge carbon powder with a particle size of 0.5 to 0.8 μm onto the surface of the mixture, and after three heat preservation steps of 1 hour, a semi-finished product is obtained;

[0107] (4) In a reduced pressure environment with a vacuum degree of 0 kPa, the semi-finished product obtained in step (3) is cooled to 800° C., hot-pressed at a pressure of 90 MPa for 50 min, and cooled to room temperature to obtain a negative electrode material. The obtained negative electrode material includes a core layer and a shell layer, the core layer has more pores than the shell layer; in the core layer, the content of SiC is more than the content of C; in the shell layer, the content of SiC is less than the content of C.

[0108] The obtained negative electrode material is prepared into a negative electrode of a lithium battery, which is stacked with a positive electrode to assemble a battery core pack, and then directly injected with electrolyte, wherein the mass proportion of VC in the electrolyte is 5%. The formation is started as follows:

[0109] Under the conditions of a temperature of 45°C and a clamping force of 0.3MPa, after charging to 30% SOC at a rate of 0.03C, the current was converted to 0.2C and charged to 80% SOC, and then evacuation and sealing were performed in sequence to finally obtain a soft-pack lithium battery.

[0110] Performance Testing

[0111] The lithium batteries prepared in the above Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to performance tests, and the test results are shown in Table 1. The normal temperature cycle performance test method is: at 30°C, "1C full charge to 3.6V, stand for 10min, then 1C discharge to 2.5V, then stand for 10min" is repeated once, and the number of times the last capacity retention rate is above 80% is recorded.

[0112] Table 1

[0113]

[0114] Data Analysis and Conclusion:

[0115] (1) The preparation of the negative electrode material of Comparative Example 1 is to directly mix the raw materials and then sinter them. Compared with Example 1, the DC internal resistance of Comparative Example 1 increases, indicating that the present invention adopts a method of multiple heating, cooling, and heat preservation, and at the same time, the content of SiC and C is continuously changed, which can effectively reduce the DC internal resistance of the lithium battery. The comparison between Example 1 and Comparative Example 1 shows the excellent performance of the lithium battery with a long cycle life containing the SiC-C porous composite negative electrode material prepared by the present invention.

[0116] (2) The contents of SiC and C in the negative electrode material of Comparative Example 2 change discontinuously. Compared with Example 1, the DC internal resistance of Comparative Example 2 increases, indicating that the contents of SiC and C change continuously, which can effectively reduce the DC internal resistance of the lithium battery. At the same time, the cycle life of the lithium battery is also improved.

[0117] (3) Compared with Example 1, the DC internal resistance of the lithium battery prepared by the ordinary formation method of direct one-time formation in Comparative Example 3 is greatly increased, indicating that the lithium battery containing the SiC-C porous composite negative electrode material can effectively reduce the DC internal resistance and improve the cycle performance of the lithium battery by the formation method of twice injecting electrolyte and twice forming. Compared with Comparative Example 4, increasing the mass proportion of VC in the electrolyte not only fails to improve the performance of the lithium battery, but also leads to an increase in the DC internal resistance, indicating that the traditional method of improving the performance of lithium batteries by increasing the amount of VC has certain defects, and the amount of VC increased should be within a certain limit to achieve the purpose of improving the performance of lithium batteries.

[0118] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0119] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a SiC-C porous composite negative electrode material, characterized in that: The following steps are involved: (1) In an inert gas atmosphere, 60-70 parts by weight of carbon powder with a particle size of 1-3 μm, 240-300 parts by weight of silicon powder and 0.5-0.8 parts by weight of nickel are mixed uniformly, and then the temperature is raised to 1000-1100°C, kept at this temperature for 1-2 hours and then cooled, and the obtained solid is ball-milled to obtain a mixed powder with a particle size of 1-5 μm; (2) In an inert gas atmosphere, the mixed powder obtained in step (1) is heated to 1300-1450° C., kept warm for 3-4 h, then cooled to 700-900° C., kept warm for 1-2 h, and then cooled and ball-milled to obtain a mixture containing SiC with a particle size of 0.1-0.3 μm; (3) The mixture obtained in step (2) is heated to 1250-1350° C. and then heat-insulated for three times. At the beginning of the three heat-insulations, 60-70 parts by weight of carbon powder with a particle size of 0.5-0.8 μm is purged onto the surface of the mixture by inert gas. After the three heat-insulations for 1-2 hours, a semi-finished product is obtained. (4) Under reduced pressure, the semi-finished product obtained in step (3) is cooled to 800-900° C. and hot-pressed for 40-50 min, and then cooled to room temperature to obtain a SiC-C porous composite negative electrode material; The SiC-C porous composite negative electrode material includes a core layer and a shell layer; the number of pores in the core layer is greater than that in the shell layer; the content of SiC decreases transitionally from the core layer to the shell layer, and the content of C increases transitionally from the core layer to the shell layer; in the core layer, the content of SiC is greater than that of C; in the shell layer, the content of SiC is less than that of C.

2. The method for preparing a SiC-C porous composite negative electrode material according to claim 1, characterized in that: The inert gas is argon or helium.

3. The method for preparing a SiC-C porous composite negative electrode material according to claim 1, characterized in that: In step (4), the vacuum degree of the reduced pressure environment is 0 ~ -20 kPa.

4. The method for preparing a SiC-C porous composite negative electrode material according to claim 1, characterized in that: In step (4), the hot pressing pressure is 90-120 MPa.

5. Application of the SiC-C porous composite negative electrode material obtained by the preparation method as claimed in any one of claims 1 to 4 in the negative electrode of a lithium battery.

6. A formation method for a lithium battery containing a SiC-C porous composite negative electrode material obtained by the preparation method according to any one of claims 1 to 4, characterized in that: The following steps are involved: (a) After sealing the three sides of the battery core package, the battery core package is dried under reduced pressure at 85-105°C for 8-48 hours to obtain a battery ready for primary injection; (b) injecting electrolyte A into the battery to be filled once, sealing it with an air bag, and then leaving it to stand until the electrolyte soaks the inside of the battery cell, followed by a primary formation, and then leaving it in an environment of 35-45°C for 48-60 hours to obtain a battery to be filled twice; (c) A through hole is pierced in the airbag bag of the battery to be refilled with liquid, and then the bag is placed in a vacuum environment with a degree of vacuum not greater than -95 kPa for 15 to 30 seconds, and then electrolyte B is injected through the through hole and sealed. After secondary formation, air extraction, and edge sealing, a soft-pack lithium battery is obtained.

7. The chemical formation method according to claim 6, characterized in that: In step (b), the electrolyte A accounts for 70% to 90% of the total mass of the electrolyte of the lithium battery, and the VC contained in the electrolyte A accounts for 2% to 4% of the total mass of the electrolyte of the lithium battery.

8. The chemical formation method according to claim 6, characterized in that: In step (c), the electrolyte B accounts for 10% to 30% of the total mass of the electrolyte contained in the lithium battery, and the VC contained in the electrolyte B accounts for 0.6% to 2% of the total mass of the electrolyte contained in the lithium battery.

9. The chemical formation method according to claim 6, characterized in that: In step (b), the one-step formation method comprises: charging at a rate of 0.02-0.05C for 5-10h at a temperature of 42-48°C and a clamping force of 0.3-0.6MPa, and charging the battery to a charge level of 20%-25% SOC.

10. The chemical formation method according to claim 6, characterized in that: In step (c), the secondary formation method comprises: charging to a SOC of 70% to 90% at a rate of 0.1 to 0.3C under the conditions of a temperature of 42 to 48°C and a clamping force of 0.3 to 0.6MPa.