Solid state battery and method for manufacturing solid state battery

By staggering concave and convex portions on the end face of the bipolar electrode plate to form a thin solid electrolyte layer, the problems of high stacking duty cycle and increased resistivity caused by sheet-like electrolyte layers are solved, thereby improving battery performance and simplifying manufacturing steps.

CN115395070BActive Publication Date: 2024-11-05HONDA MOTOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210564993.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-05-25
Filing Date
2022-05-23
Publication Date
2024-11-05
Estimated Expiration
2042-05-23

AI Technical Summary

Technical Problem

In existing solid-state batteries, the thickness requirement of the sheet-like solid electrolyte layer leads to a high stacking duty cycle and increased resistivity, which affects battery performance.

Method used

A structure with alternating recesses and convexities on the end faces of bipolar electrode plates is adopted to form a thin solid electrolyte layer. Solid electrolyte is coated on the recesses to ensure insulation between the electrode plates and simplify the manufacturing process.

Benefits of technology

This reduces the stacking duty cycle and resistivity of the solid electrolyte, simplifies the manufacturing process, and improves battery performance and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115395070B_ABST
    Figure CN115395070B_ABST
Patent Text Reader

Abstract

The problem to be solved by the present invention is to provide a solid battery with a bipolar electrode plate, which can reduce the stacking space factor of the solid electrolyte and reduce the resistivity. In order to solve the above problems, a solid battery includes a stacked body formed by stacking a positive electrode plate, one or more bipolar electrode plates and a negative electrode plate, and a solid electrolyte layer is formed on the stacking surface of the bipolar electrode plate. Preferably, a solid electrolyte layer is formed on at least a portion of the end surface of the bipolar electrode plate, the bipolar electrode plate is a plurality of bipolar electrode plates, and a concave portion formed with a solid electrolyte and a convex portion without a solid electrolyte layer are formed on the end surface of the bipolar electrode plate, and the concave portions and the convex portions are alternately arranged between adjacent bipolar electrode plates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solid battery and a method for manufacturing a solid battery Background Art

[0002] Conventionally, lithium-ion secondary batteries have been widely used as secondary batteries with high energy density. A lithium-ion secondary battery has a structure in which a separator is interposed between a positive electrode and a negative electrode and a liquid electrolyte is filled therein.

[0003] The electrolyte of a lithium-ion secondary battery is usually a flammable organic solvent, and sometimes the safety of the electrolyte, especially to heat, becomes a problem. Therefore, a solid battery using an inorganic solid electrolyte instead of an organic liquid electrolyte is proposed. For example, a technology involving a solid battery having a stack is proposed, wherein the stack has a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer (see Patent Document 1).

[0004] In a solid battery using bipolar electrode plates, a structure in which a solid electrolyte layer is stacked between the bipolar electrode plates is also adopted.

[0005] [Prior Technical Literature]

[0006] (Patent Document)

[0007] Patent Document 1: Japanese Patent Application Publication No. 2010-205479 Summary of the invention

[0008] [Problems to be solved by the invention]

[0009] The solid battery described in Patent Document 1 has a press-formed sheet-shaped solid electrolyte layer disposed between each electrode layer. The sheet-shaped solid electrolyte layer needs to be about several tens of microns thick because of the required strength. Therefore, there is room for improvement in terms of the increased stacking space factor of the solid electrolyte and the increased resistivity due to the increased distance between the electrodes.

[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a solid battery including a bipolar electrode plate, which can reduce the stacking space factor of the solid electrolyte and reduce the resistivity.

[0011] [Technical means to solve the problem]

[0012] (1) The present invention relates to a solid battery including a stacked body formed by stacking a positive electrode plate, one or more bipolar electrode plates, and a negative electrode plate, wherein a solid electrolyte layer is formed on the stacked surfaces of the bipolar electrode plates.

[0013] According to the invention of (1), it is possible to provide a solid battery having a bipolar electrode plate, which can reduce the stacking space factor of the solid electrolyte and reduce the resistivity.

[0014] (2) The solid battery according to (1), wherein a solid electrolyte layer is formed on at least a portion of an end surface of the bipolar electrode plate.

[0015] According to the invention of (2), insulation between the end surfaces of the bipolar electrode plates can be ensured.

[0016] (3) A solid battery according to (1) or (2), wherein the bipolar electrode plates are a plurality of bipolar electrode plates, and recesses with solid electrolyte layers and protrusions without solid electrolyte layers are formed on end faces of the bipolar electrode plates, and the recesses and protrusions are alternately arranged between adjacent bipolar electrode plates.

[0017] According to the invention of (3), even when a thin solid electrolyte layer is formed on the electrode plates instead of a sheet-like solid electrolyte layer, insulation between the electrode plates can be ensured.

[0018] (4) A solid battery according to (3), wherein, in the bipolar electrode plate arranged adjacent to the positive electrode plate or the negative electrode plate, the recess is arranged at a position corresponding to an electrode tab extending from the positive electrode plate or the negative electrode plate, and is wider than the width of the electrode tab.

[0019] According to the invention of (4), since it is possible to ensure insulation between the end face of the bipolar electrode plate and the electrode tab extending from the positive plate or the negative plate, and to form a stack without forming a solid electrolyte layer on the positive plate and the negative plate, the manufacturing steps of the solid battery can be simplified.

[0020] (5) The solid battery according to any one of (1) to (4), wherein a solid electrolyte layer is formed on a stacked surface of the positive electrode plate and the negative electrode plate.

[0021] According to the invention of (5), a laminated body can be constructed which can ensure insulation between the positive electrode plate and the negative electrode plate and the end surface of the bipolar electrode plate.

[0022] (6) The solid battery according to any one of (1) to (5), wherein the bipolar electrode plate is a plurality of bipolar electrode plates, and shapes of adjacent bipolar electrode plates are mirror images of each other.

[0023] According to the invention of (6), the shape of the bipolar electrode plate can be set to a shape suitable for ensuring insulation between the end surfaces of the bipolar electrode plate.

[0024] (7) In addition, the present invention also relates to a method for manufacturing a solid battery, comprising steps for manufacturing a bipolar electrode plate, wherein the steps for manufacturing the bipolar electrode plate sequentially include: an electrode material coating step, coating a positive electrode material on the surface of one side of a collector plate, and coating a negative electrode material on the surface of the other side; a perforating step, forming a hole portion on a portion of the collector plate coated with the electrode material; a solid electrolyte coating step, coating a solid electrolyte on the collector plate coated with the electrode material; and a cutting step, cutting the collector plate coated with the electrode material with a cutting line including the hole portion, thereby cutting the collector plate in a manner that a recess can be formed at the end edge of the collector plate.

[0025] According to the invention of (7), a bipolar electrode plate having a solid electrolyte layer formed on at least a portion of its end surface can be efficiently manufactured, and the manufacturing cost of a solid battery can be reduced.

[0026] (8) A method for manufacturing a solid battery according to (7), wherein, in the step of manufacturing the bipolar electrode plate, the punching step is a step of forming the hole portions in a manner that adjacent rows of the hole portions are staggered with each other, thereby manufacturing the bipolar electrode plates of two shapes that are mirror images of each other.

[0027] According to the invention of (8), since the bipolar electrode plates of two shapes that are mirror images of each other can be manufactured from a single sheet-like current collector plate, the manufacturing cost of the solid battery can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a diagram schematically showing a laminated body according to the first embodiment of the present invention.

[0029] Figure 2A It is along Figure 1 Cross-section diagram along line AA.

[0030] Figure 2B It is along Figure 1 Cross-sectional view of line BB.

[0031] Figure 2C It is along Figure 1 Cross-sectional view of the CC line.

[0032] Figure 2D It is along Figure 1 Cross-sectional view of the DD line.

[0033] Figure 3 This is a diagram schematically showing a bipolar electrode plate according to a first embodiment of the present invention.

[0034] Figure 4 This is a diagram schematically showing a bipolar electrode plate according to a first embodiment of the present invention.

[0035] Figure 5 This is a diagram schematically showing a laminated body according to a second embodiment of the present invention.

[0036] Fig. 6A It is along Figure 5 Cross-section diagram along line AA.

[0037] Figure 6B It is along Figure 5 Cross-sectional view of line BB.

[0038] Figure 6C It is along Figure 5 Cross-sectional view of the CC line.

[0039] Fig.6D It is along Figure 5 Cross-sectional view of the DD line.

[0040] Figure 7 This is a diagram schematically showing a bipolar electrode plate according to a second embodiment of the present invention.

[0041] Figure 8 This is a diagram schematically showing a bipolar electrode plate according to a second embodiment of the present invention.

[0042] Fig. 9 The diagram shows the steps of manufacturing the bipolar electrode plate according to the first embodiment of the present invention.

[0043] Fig.10 The diagram shows the steps of manufacturing the solid battery electrode according to the first embodiment of the present invention.

[0044] Fig.11 It is a diagram showing the manufacturing steps of the bipolar electrode plate according to the second embodiment of the present invention.

[0045] Fig.12 1 is a flow chart showing the steps of manufacturing the solid state battery according to the first embodiment of the present invention.

[0046] Fig.13 1 is a flow chart showing steps for manufacturing a solid battery according to a second embodiment of the present invention. DETAILED DESCRIPTION

[0047] 《First Implementation Mode》

[0048] <Solid State Battery>

[0049] The solid battery of this embodiment includes a stacked body formed by stacking a positive electrode plate, a bipolar electrode plate, and a negative electrode plate. The stacked body is housed in an outer casing, and the positive electrode plate and the negative electrode plate are electrically connected to the positive electrode and the negative electrode, respectively.

[0050] [Laminated body]

[0051] like Figure 1 and Figure 2A to Figure 2D As shown, the laminate 1 of this embodiment has a structure in which positive electrode plates 20 and negative electrode plates 30 are arranged at both ends of the laminate, and two types of bipolar electrode plates 50 a and 50 b are alternately laminated between the positive electrode plates 20 and the negative electrode plates 30 .

[0052] (Positive plate)

[0053] like Figure 2A to Figure 2D As shown, the positive electrode plate 20 has: a positive electrode collector plate 21; a positive electrode active material layer 22, which includes a positive electrode active material formed on the positive electrode collector plate 21; a solid electrolyte layer 40, which includes a solid electrolyte formed on the positive electrode active material layer 22; and a positive electrode tab 211, which is formed by extending from the positive electrode collector plate 21.

[0054] The positive electrode current collector plate 21 is not particularly limited, and is made of a known current collecting material that can be used for a positive electrode of a solid battery, for example, aluminum, aluminum alloy, stainless steel, nickel, iron, titanium, or the like.

[0055] The positive electrode active material constituting the positive electrode active material layer 22 is not particularly limited, and a known material that can store and release a charge transfer medium such as lithium ions can be appropriately selected. For example, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, Li-Mn spinel substituted with a different element, lithium metal phosphate, lithium sulfide, sulfur, etc. can be listed. Specifically, LiCoO2, Li(Ni 5 / 10 Co 2 / 10 Mn 3 / 10 )O2、Li(Ni 6 / 10 Co 2 / 10 Mn 2 / 10 )O2、 Li(Ni 8 / 10 Co 1 / 10 Mn 1 / 10 )O2、Li(Ni 0.8 Co 0.15 Al 0.05 )O2、Li(Ni 1 / 6 Co 4 / 6 Mn 1 / 6 )O2、 Li(Ni 1 / 3 Co 1 / 3 Mn 1 / 3 )O2, LiCoO4, LiMn2O4, LiNiO2, LiFePO4, etc. In addition to the positive electrode active material, the positive electrode active material layer 22 may further contain a conductive auxiliary agent and a binder, etc.

[0056] (Negative plate)

[0057] like Figure 2A to Figure 2DAs shown, the negative electrode plate 30 includes: a negative electrode collector plate 31; a negative electrode active material layer 32, which includes a negative electrode active material formed on the negative electrode collector plate 31; a solid electrolyte layer 40, which includes a solid electrolyte formed on the negative electrode active material layer 32; and a negative electrode tab 311, which is formed by extending from the negative electrode collector plate 31.

[0058] The negative electrode active material constituting the negative electrode active material layer 32 is not particularly limited, and a known material that can store and release a charge transfer medium such as lithium ions can be appropriately selected. For example, lithium transition metal oxides such as lithium titanate, transition metal oxides such as TiO2, Nb2O3 and WO3, Si, SiO, metal sulfides, metal nitrides, and carbon materials such as artificial graphite, natural graphite, graphite, soft carbon and hard carbon, as well as metal lithium, metal indium and lithium alloys can be listed. In addition to the negative electrode active material, the negative electrode active material layer 32 can also arbitrarily contain a conductive aid and a binder.

[0059] (Bipolar electrode plate)

[0060] like Figure 2A to Figure 2D As shown, bipolar electrode plates 50a and 50b are electrode plates in which a positive electrode active material layer 22 as a positive electrode of a polarizable electrode is formed on one surface of a collector plate 51, and a negative electrode active material layer 32 as a negative electrode of a polarizable electrode is formed on the other surface. The structure of the positive electrode active material layer 22 and the negative electrode active material layer 32 can adopt the same structure as described above. A solid electrolyte layer 40 containing a solid electrolyte is formed on the positive electrode active material layer 22 and the negative electrode active material layer 32. The collector plate 51 is not particularly limited, and for example, stainless steel foil can be cited.

[0061] The solid electrolyte layer 40 is a layer having a thickness of about several μm formed on the positive electrode active material layer 22 and the negative electrode active material layer 32 of the positive electrode plate 20, the negative electrode plate 30, and the bipolar electrode plates 50a and 50b, and is a layer containing at least a solid or gel electrolyte, that is, a solid electrolyte material. Charge transfer between the positive electrode active material and the negative electrode active material can be performed via the above-mentioned solid electrolyte material. The solid electrolyte material contained in the solid electrolyte layer 40 is not particularly limited, and for example, a sulfide solid electrolyte material, an oxide solid electrolyte material, a nitride solid electrolyte material, a halide solid electrolyte material, etc. can be used.

[0062] A solid electrolyte layer 40 is formed on the positive electrode active material layer 22 and the negative electrode active material layer 32, so that the thickness of the solid electrolyte layer 40 can reach about several micrometers, thereby reducing the stacking space factor of the solid electrolyte and reducing the resistivity. In addition, by utilizing the structure of the bipolar electrode described below, the solid battery of this embodiment has a thin solid electrolyte layer, while ensuring insulation between electrodes, and simplifying the manufacturing steps and structure.

[0063] The bipolar electrode plates 50a and 50b are constructed as follows: Figure 3 , Figure 4 shown. Figure 3 , Figure 4 The bipolar electrode plates 50a and 50b are observed from the stacking surface side where the positive electrode active material layer 22 is formed. The bipolar electrode plates 50a and 50b have a shape in which convex portions 51a and concave portions 52a are alternately formed on the end surfaces and are mirror images of each other. The solid electrolyte layer 40 is not formed on the end surface of the convex portion 51a, but is formed on the end surface of the concave portion 52a. Figure 2A to Figure 2D As shown, in the stacked body 1, the bipolar electrode plates 50a and 50b are alternately stacked. The number of stacked bipolar electrode plates 50a and 50b is not particularly limited, as long as the bipolar electrode plates 50a and 50b are alternately stacked. In the case of stacking only the bipolar electrode plates, ensuring the insulation between the end faces becomes a problem, but by alternately stacking the bipolar electrode plates 50a and 50b having the above-mentioned structure, the insulation between the bipolar electrode plates 50a and 50b can be ensured.

[0064] like Figure 1 As shown in FIG. 1 , the convex portions 51a and the concave portions 52a of the bipolar electrode plates 50a and 50b are arranged to be staggered when viewed from the stacking direction. Moreover, the width of the concave portion 52a is wider than that of the convex portion 51a. Figure 1 , Figure 2A and Figure 2D As shown, the insulation distance L1a can be ensured between the convex portions 51a of the bipolar electrode plates 50a and 50b when viewed from the stacking direction, and the insulation distance L1b can be ensured when viewed from the stacking cross section. The width of the concave portion 52a is not particularly limited, but can be wider than the width T1 of the positive electrode tab 211 and the negative electrode tab 311, for example, and the width of the convex portion 51a can be narrower than the width T1, for example.

[0065] The end surfaces of the bipolar electrode plates 50a and 50b are formed with convex portions 51a or concave portions 52a. Thus, insulation is ensured between the concave portions 52a and the end surfaces of the positive electrode plate 20 and the negative electrode plate 30. Figure 2A , Figure 2C and Figure 2DAs shown, from the stacked cross section, insulation distances L2a and L2b can be ensured between the end surfaces of the positive electrode plate 20 and the negative electrode plate 30 where the positive electrode tab 211 and the negative electrode tab 311 are not arranged and the protrusion 51a. The insulation distance L2a is ensured by arranging the protrusion 51a on the outer peripheral side of the end surfaces of the positive electrode plate 20 and the negative electrode plate 30.

[0066] In this embodiment, the bipolar electrode plate 50a is disposed adjacent to the positive electrode plate 20 and the negative electrode plate 30. Figure 2A and Figure 2C As shown, the positive electrode tab 211 and the negative electrode tab 311 are provided with a solid electrolyte layer 40 having a certain length along the extension direction of the tab on the stacking surface. Figure 1 As shown, the insulation distance L3a can be ensured between the positive electrode tab 211 and the negative electrode tab 311 and the convex portion 51a of the bipolar electrode plate 50a when viewed from the stacking direction. Figure 2A As shown in FIG. 1 , from the stacked cross section, an insulation distance L3b can be ensured between the positive electrode tab 211 and the convex portion 51a of the bipolar electrode plate 50b. Figure 2C As shown, an insulation distance L3c can be ensured between the negative electrode tab 311 and the protrusion 51a of the bipolar electrode plate 50a when viewed from the stacked cross section.

[0067] <Method for manufacturing solid state battery>

[0068] like Fig.12 As shown, the method for manufacturing a solid battery of the present embodiment includes a positive electrode plate manufacturing step S1 , a bipolar electrode plate manufacturing step S2 , a negative electrode plate manufacturing step S3 , a stacking step S4 , and a pressurizing step S5 .

[0069] like Fig.12 As shown, the positive electrode plate manufacturing step S1 sequentially includes: a positive electrode material coating step S11, a drying step S12, a solid electrolyte coating step S13, a drying step S14 and a cutting step S15.

[0070] like Fig.10 As shown, the positive electrode material coating step S11 is a step of forming a positive electrode active material layer 22 on both sides of the sheet-like positive electrode collector plate 21. The method for forming the positive electrode active material layer 22 is not particularly limited. For example, it can be listed as: preparing a positive electrode composite material containing a positive electrode active material, and coating the positive electrode composite material on the positive electrode collector. There is no particular limitation on the coating (coating) method. For example, it can be listed as a scraper method, spraying, screen printing, etc. The drying step S12 is a step of drying the coated positive electrode composite, and the drying method is not particularly limited.

[0071] like Fig.10As shown, the solid electrolyte coating step S13 is a step of forming a solid electrolyte layer 40 on both sides of the sheet-like positive electrode collector plate 21 having a positive electrode active material layer 22 formed on both sides. The method of forming the solid electrolyte layer 40 is not particularly limited, and the same as the positive electrode material coating step S11, a method of coating the solid electrolyte by a doctor blade method, spraying, screen printing, etc. can be cited. The drying step S14 is a step of drying the coated solid electrolyte layer 40, and the drying method is not particularly limited.

[0072] The cutting step S15 is a step of cutting the sheet-like positive electrode current collector plate 21 into a predetermined size to form a positive electrode tab 211 .

[0073] like Fig.12 As shown, the bipolar electrode plate manufacturing step S2 sequentially includes: a positive / negative electrode material coating step S21, a drying step S22, a perforating step S23, a solid electrolyte coating step S24, a drying step S25 and a cutting step S26.

[0074] like Fig. 9 As shown, the positive / negative electrode material coating step S21 is a step of forming a positive electrode active material layer 22 on one surface of the sheet-like current collector plate 51 and a negative electrode active material layer 32 on the other surface. As a specific method, the same steps as the positive electrode material coating step S11 and the negative electrode material coating step S31 can be adopted. The drying step S22 is a step of drying the coated positive electrode composite material and negative electrode composite material, and the drying method is not particularly limited.

[0075] The perforation step S23 is a step of forming holes in the sheet-like current collector plate 51 on which the positive electrode active material layer 22 and the negative electrode active material layer 32 are formed respectively. There is no particular limitation on the method of forming the holes, and a conventionally known method such as a perforation processing method using a punching die or a laser processing method can be used. Fig. 9 As shown, the punching step S23 is preferably a step of forming holes in a manner that adjacent rows of holes are staggered. Thus, bipolar electrode plates 50a and 50b having two shapes that are mirror images of each other can be manufactured from a sheet-like current collector plate 51.

[0076] like Fig. 9As shown, the solid electrolyte coating step S24 is a step of forming a positive electrode active material layer 22 and a negative electrode active material layer 32 on both sides, and forming a solid electrolyte layer 40 on both sides of a sheet-like collector plate 51 having a hole portion. The method of forming the solid electrolyte layer 40 is not particularly limited, and the same as the positive electrode material coating step S11, the method of coating the solid electrolyte using a doctor blade method, spraying, screen printing, etc. can be listed. The solid electrolyte is coated on the collector plate 51 having a hole portion, thereby, the solid electrolyte wraps the end surface of the hole portion, and the solid electrolyte layer 40 can also be formed on the end surface of the hole portion. The drying step S25 is a step of drying the coated solid electrolyte layer 40, and the drying method is not particularly limited.

[0077] The cutting step S26 is a step of cutting the sheet-like current collector plate 51 along the cutting lines including the holes formed in the punching step S23 to form bipolar electrode plates 50a and 50b having protrusions 51a and recesses 52a formed on the end surfaces.

[0078] According to the bipolar electrode plate manufacturing step S2 having the above steps, it is possible to manufacture bipolar electrode plates 50a and 50b, on which convex portions 51a and concave portions 52a are formed on the end faces and on which solid electrolyte layers 40 are formed on the end faces of the concave portions 52a. That is, before cutting the sheet-like current collector plate 51, a solid electrolyte may be applied to the end faces of the holes to manufacture bipolar electrode plates 50a and 50b on which solid electrolyte layers 40 are formed on at least a portion of the end portions, and therefore, this is preferred from the viewpoint of the production efficiency of the bipolar electrode plates 50a and 50b.

[0079] like Fig.12 As shown, the negative electrode plate manufacturing step S3 sequentially includes: a negative electrode material coating step S31, a drying step S32, a solid electrolyte coating step S33, a drying step S34 and a cutting step S35. The negative electrode plate manufacturing step S3 is the same as the positive electrode plate manufacturing step S1 except that the negative electrode active material layer 32 is formed on both sides of the sheet-like negative electrode collector plate 31 in the negative electrode material coating step S31.

[0080] The stacking step S4 is a step of stacking the positive electrode plate 20 manufactured by the positive electrode plate manufacturing step S1, the bipolar electrode plates 50a and 50b manufactured by the bipolar electrode plate manufacturing step S2, and the negative electrode plate 30 manufactured by the negative electrode plate manufacturing step S3. In the stacking step S4, the bipolar electrode plates 50a and 50b are stacked alternately, and the positive electrode plate 20 and the negative electrode plate 30 are arranged at both ends of the stack.

[0081] The pressurizing step S5 is a step of sandwiching and pressurizing the stacked positive electrode plate 20 , bipolar electrode plates 50 a and 50 b , and negative electrode plate 30 by a press machine or the like to integrate them.

[0082] Hereinafter, another embodiment of the present invention will be described. The description of the same structure as the structure described above may be omitted.

[0083] Second Implementation Method

[0084] [Laminated body]

[0085] Figure 5 1 is a diagram showing an overview of a stacked body 1a of a solid battery according to a second embodiment. Figure 5 and Figure 6A to Figure 6D As shown, the stacked body 1a has a structure in which positive electrode plates 20a and negative electrode plates 30a are arranged at both ends of the stack, and two types of bipolar electrode plates 50c and 50d are alternately arranged between the positive electrode plates 20a and the negative electrode plates 30a.

[0086] In this embodiment, if Figure 6A to Figure 6D As shown, the solid electrolyte layer 40 is not formed on the stacked surface of the positive electrode plate 20a and the negative electrode plate 30a. Therefore, the solid electrolyte is not formed on the surface of the positive electrode tab 211 and the negative electrode tab 311. Therefore, the manufacturing steps of the stacked body 1a can be simplified. On the other hand, in the stacked body 1a, it is necessary to ensure the insulation between the positive electrode tab 211 and the negative electrode tab 311 and the adjacent bipolar electrode plate.

[0087] The bipolar electrode plates 50c and 50d are constructed as follows: Figure 7 , Figure 8 shown. Figure 7 , Figure 8 The bipolar electrode plates 50c and 50d are respectively viewed from the stacking surface side where the positive electrode active material layer 22 is formed. The bipolar electrode plates 50c and 50d have a shape in which convex portions 51b and concave portions 52b are alternately formed on the end surface and are mirror images of each other. The solid electrolyte layer 40 is not formed on the convex portion 51b, but is formed on the concave portion 52b. Figure 6A to Figure 6D As shown, in the stacked body 1a, bipolar electrode plates 50c and 50d are alternately stacked.

[0088] In the present embodiment, the bipolar electrode plate disposed adjacent to the positive electrode plate 20a is the bipolar electrode plate 50c, and the bipolar electrode plate disposed adjacent to the negative electrode plate 30a is the bipolar electrode plate 50d. Therefore, the number of stacked bipolar electrode plates in the present embodiment is an even number.

[0089] like Figure 5 and Figure 7 As shown in FIG. 1 , the concave portion 52b formed on the end surface of the bipolar electrode plate 50c is arranged at a position corresponding to the positive electrode tab 211 having a width T1. Figure 5and Figure 7 As shown, the recessed portion 52b formed on the end surface of the bipolar electrode plate 50d is arranged at a position corresponding to the negative electrode tab 311 having a width T1. The recessed portion 52b is a recessed portion wider than the width of the positive electrode tab 211 and the negative electrode tab 311, and a solid electrolyte layer 40 is formed on the end surface. Thus, the insulation between the positive electrode tab 211 and the adjacent bipolar electrode plate 50c and the insulation between the negative electrode tab 311 and the adjacent bipolar electrode plate 50d can be ensured.

[0090] like Figure 5 , Fig. 6A and Fig.6D As shown, an insulation distance L1c can be ensured between the convex portions 51a of the bipolar electrode plates 50c and 50d when viewed from the stacking direction, and an insulation distance L1b can be ensured when viewed from the stacking cross section.

[0091] like Fig. 6A and Fig.6D As shown, insulation distances L2a and L2b can be ensured between the end surfaces of the positive electrode plate 20 and the negative electrode plate 30 where the positive electrode tab 211 and the negative electrode tab 311 are not arranged and the protrusion 51a when viewed from the stacked cross section.

[0092] like Figure 5 As shown in FIG. 1 , an insulation distance L3d can be ensured between the positive electrode tab 211 and the convex portion 51a of the bipolar electrode plate 50c when viewed from the stacking direction. The same is true for the negative electrode tab 311 and the convex portion 51a of the bipolar electrode plate 50d. Fig. 6A As shown in FIG. 1 , from the stacked cross section, an insulation distance L3b can be ensured between the positive electrode tab 211 and the convex portion 51a of the bipolar electrode plate 50d. Figure 6C As shown, from the stacked cross section, the insulation distance L3c can be ensured between the negative electrode tab 311 and the convex portion 51a of the bipolar electrode plate 50c. That is, at the positions corresponding to the positive electrode tab 211 and the negative electrode tab 311 of the bipolar electrode plate adjacent to the positive electrode plate 20a and the negative electrode plate 30a, a concave portion 52b having a solid electrolyte 40 formed on the end surface is provided. Thus, even if the positive electrode plate 20a and the negative electrode plate 30a do not have the solid electrolyte layer 40, the insulation distances L3b, L3c and L3d can be ensured between the convex portions 51a of each bipolar electrode plate.

[0093] <Method for manufacturing solid state battery>

[0094] like Fig.13 As shown, the method for manufacturing a solid battery of this embodiment includes a positive electrode plate manufacturing step S1a, a bipolar electrode plate manufacturing step S2a, a negative electrode plate manufacturing step S3a, a stacking step S4, and a pressurizing step S5.

[0095] The positive electrode plate manufacturing step S1a and the negative electrode plate manufacturing step S3a are the same steps as the positive electrode plate manufacturing step S1 and the negative electrode plate manufacturing step S3 except that the solid electrolyte coating steps S13 and S33 and the drying steps S14 and S34 are not included.

[0096] like Fig.13 As shown, the bipolar electrode plate manufacturing step S2a sequentially includes: a positive / negative electrode material coating step S21, a drying step S22, a perforation step S23, a solid electrolyte coating step S24, a drying step S25, and a cutting step S26. The steps of the bipolar electrode plate manufacturing step S2a are the same as the bipolar electrode plate manufacturing step S2 except for the perforation step S23a.

[0097] like Fig.11 As shown, the perforation step S23a is a step of forming a hole portion on the sheet-like collector plate 51 on which the positive electrode active material layer 22 and the negative electrode active material layer 32 are formed respectively. As a method for forming the hole portion, the same method as the first embodiment can be adopted. Fig.11 As shown, the punching step S23a is the same as the punching step S23, and is preferably a step of forming holes in a manner that holes in adjacent rows are staggered. Thus, two bipolar electrode plates 50c and 50d of mirror-image relationship can be manufactured from a sheet-like current collector plate 51.

[0098] The punching step S23a forms holes in the collector plate 51 so that two rows of bipolar electrode plates can be manufactured from one sheet of collector plate 51 along the sheet moving direction. The two rows of bipolar electrode plates are manufactured so that adjacent bipolar electrode plates are mirror images of each other.

[0099] The preferred embodiments of the present invention have been described above, but the present invention is not limited to the above-described embodiments, and embodiments that have been appropriately modified are also within the scope of the present invention. Fig. 9 The punching step S23 of the bipolar electrode plate manufacturing step S2 of the solid battery manufacturing method of the first embodiment is described, and the method of manufacturing the solid battery of the first embodiment is described. Fig.11 The punching step S23a of the bipolar electrode plate manufacturing step S2a of the solid battery manufacturing method of the second embodiment has been described. However, the present invention is not limited to the above. Fig. 9 The perforation steps shown and Fig.11 The perforating steps shown can be applied to any one of the perforating step S23 and the perforating step S23a, respectively.

[0100] Reference numerals

[0101] 1. 1a, 1b laminate

[0102] 20, 20a, 20b positive plate

[0103] 211 positive electrode tab (electrode tab)

[0104] 30, 30a, 30b negative plate

[0105] 311 negative electrode tab (electrode tab)

[0106] 40Solid electrolyte layer

[0107] 50a, 50b, 50c, 50d bipolar electrode plates

[0108] 51a, 51b convex parts

[0109] 52a, 52b recessed parts

Claims

1. A solid battery comprising a stacked body formed by stacking a positive electrode plate, a plurality of bipolar electrode plates and a negative electrode plate, A solid electrolyte layer is formed on the stacked surface of the bipolar electrode plates. The end surface of the bipolar electrode plate viewed from the stacking surface side has concave portions where the solid electrolyte layer is formed and convex portions where the solid electrolyte layer is not formed alternately formed. The shapes of the adjacent bipolar electrode plates are mirror images of each other. The concave portions and the convex portions are alternately arranged between the adjacent bipolar electrode plates.

2. The solid battery according to claim 1, wherein: A solid electrolyte layer is formed on at least a portion of an end surface of the bipolar electrode plate.

3. The solid battery according to claim 1, wherein: In the bipolar electrode plate disposed adjacent to the positive electrode plate or the negative electrode plate, the recess is disposed at a position corresponding to an electrode tab extending from the positive electrode plate or the negative electrode plate and is wider than a width of the electrode tab.

4. The solid battery according to claim 1, wherein: A solid electrolyte layer is formed on the stacked surface of the positive electrode plate and the negative electrode plate.

5. A method for manufacturing a solid battery, comprising the steps of manufacturing a bipolar electrode plate, The manufacturing steps of the bipolar electrode plate are as follows: An electrode material coating step of coating a positive electrode material on one surface of the collector plate and coating a negative electrode material on the other surface of the collector plate; A perforating step of forming a hole in a portion of the collector plate coated with the electrode material; a solid electrolyte coating step, coating a solid electrolyte on the aforementioned collector plate coated with the electrode material; and, a cutting step of cutting the collector plate coated with the electrode material along a cutting line including the hole, thereby cutting the collector plate in a manner that a recessed portion is formed at an end edge of the collector plate, In the manufacturing steps of the bipolar electrode plate, the punching step is a step of forming the holes in adjacent rows in a staggered manner, thereby manufacturing the bipolar electrode plates in two shapes that are mirror images of each other.