Alkali soluble resin, protective layer composition, protective layer, laminate and method for forming photoresist pattern
By using alkali-soluble resins and hydrophobic resin compositions of specific structural units in immersion lithography technology, a protective layer with high receding contact angle and water resistance is formed, which solves the problem of refractive index matching and water resistance of the protective layer in immersion lithography technology. and alkali solubility issues, achieving efficient photoresist pattern formation.
Patent Information
- Application Number
- CN202210585560.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-26
- Filing Date
- 2022-05-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-05-26
AI Technical Summary
In immersion lithography technology, the protective layer needs to have a refractive index that matches water and photoresist, a high receding contact angle, good water resistance and alkali solubility to prevent lens contamination and damage while ensuring exposure rate and development The process went smoothly.
Using alkali-soluble resin containing specific structural units, combined with a protective layer composition of hydrophobic resin and solvent, through a specific molar ratio and structural design, a protective layer with high receding contact angle, good water resistance and alkali solubility is formed to ensure its Effectiveness in immersion lithography.
It realizes the effective use of protective layer in immersion lithography technology, ensures the relative movement rate between water and photoresist, protects the lens group, and can be peeled off smoothly during the development process, improving exposure efficiency and pattern fineness. .
Smart Images

Figure CN115403696B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an alkali-soluble resin, a protective layer composition, a protective layer, a laminate and a method for forming a photoresist (photoresist, photoresist) pattern, and in particular to an alkali-soluble resin, a protective layer composition, a protective layer, a laminate (laminated body, stacked body) and a method for forming a photoresist pattern used in immersion lithography (immersion lithography, Immersion Lithography) technology. Background Art
[0002] In the past, the semiconductor manufacturing process mainly used dry development technology, with air as the medium between the lens group and the wafer, to form the pattern on the mask on the wafer. However, with the development of semiconductor manufacturing processes, from 0.13 micron, 90 nanometers to 65 nanometer processes, not only is it difficult to make breakthroughs in the technology of 157 nanometer dry exposure machines, but the requirements for the material of the lens group and the transparency of the photoresist are also getting higher and higher.
[0003] In view of the limitations of dry development technology, the semiconductor industry proposed an immersion lithography technology in 2002. It uses water with a refractive index of 1.44 as the medium between the mirror group and the wafer to shorten the 193-nanometer wavelength of light to 134-nanometer wavelength, thereby forming a finer pattern on the wafer.
[0004] In immersion lithography, the photoacid and quencher in the photoresist will dissolve in water, thus causing contamination or damage to the mirror. In response to this, the semiconductor industry has developed a method of forming a protective layer on the surface of the photoresist, thereby isolating the water from the photoresist with the protective layer, thereby preventing the photoacid and quencher in the photoresist from dissolving in water and causing contamination or damage to the mirror.
[0005] However, during the exposure process of immersion lithography, in addition to considering that the refractive index of the protective layer must be able to match that of water and photoresist, it is also necessary to consider that water and the wafer will have relative movement. Therefore, the protective layer must have a high receding contact angle for water to ensure the relative movement rate between water and the wafer, thereby increasing the exposure rate. In addition, the protective layer also needs to have sufficient water resistance to ensure that the structure of the protective layer itself will not be corroded by water. Furthermore, the protective layer must have sufficient alkali solubility to ensure that the protective layer can be peeled off after the subsequent development process.
[0006] Therefore, under the premise that the refractive index of the protective layer can match that of water and the photoresist, how to improve the receding contact angle, water resistance, and alkali solubility of the protective layer for water is a problem that technicians in this field want to solve. Summary of the invention
[0007] In view of this, the present invention provides an alkali-soluble resin, a protective layer composition comprising the alkali-soluble resin, a protective layer formed by the protective layer composition, a laminate, and a method for forming a photoresist pattern, wherein the protective layer has a high receding contact angle, good water resistance, and good alkali solubility, provided that the refractive index of the protective layer can match that of water and the photoresist.
[0008] The present invention provides an alkali-soluble resin (A) comprising a structural unit (a1) represented by the following formula (1), a structural unit (a2) represented by the following formula (2), and a structural unit (a3) represented by the following formula (3).
[0009]
[0010] In formula (1), R 1 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, R 2 is a fluorinated alkyl group having 1 to 10 carbon atoms, and * indicates a bonding position.
[0011]
[0012] In formula (2), R 3 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, Y 1 is an alkylene group having 1 to 10 carbon atoms, a cycloalkylene group having 5 to 10 carbon atoms, or an arylene group, and * indicates a bonding position. 1 When it is an alkylene group having 2 to 10 carbon atoms or a cycloalkylene group having 5 to 10 carbon atoms, one or more of the -CH2- groups may be replaced by -O- or replace.
[0013]
[0014] In formula (3), R 4 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, Y 2 is an alkylene group having 2 to 8 carbon atoms, and * indicates a bonding position. 2 In which one or more -CH2- can be replaced by -O- or replace.
[0015] In one embodiment of the present invention, the molar ratio of the structural unit (a1) represented by formula (1), the structural unit (a2) represented by formula (2), and the structural unit (a3) represented by formula (3) is 10-50:50-90:1-20.
[0016] In one embodiment of the present invention, R of formula (1) 2 In the embodiment, the fluorinated alkyl group having 1 to 10 carbon atoms contains 3 or more fluorine atoms.
[0017] The present invention provides a protective layer composition, comprising: the above-mentioned alkali-soluble resin (A), a hydrophobic resin (B), and a solvent (C).
[0018] In one embodiment of the present invention, the hydrophobic resin (B) includes a structural unit (b1) represented by the following formula (4) and a structural unit (b2) represented by the following formula (5).
[0019]
[0020] In formula (4), R 5 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, R 6 is an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group, and * indicates a bonding position. 6 When it is an alkyl group having 2 to 10 carbon atoms or a cycloalkyl group having 5 to 10 carbon atoms, one or more of the -CH2- groups may be replaced by -O- or replace.
[0021]
[0022] In formula (5), R 7 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, R 8 is a fluorinated alkyl group having 1 to 10 carbon atoms, and * indicates a bonding position.
[0023] In one embodiment of the present invention, the molar ratio between the structural unit (b1) represented by formula (4) and the structural unit (b2) represented by formula (5) is 10-50:50-90.
[0024] In one embodiment of the present invention, in formula (4), R 6 It is an alkyl group having 1 to 10 carbon atoms.
[0025] In one embodiment of the present invention, the solvent (C) includes an alcohol solvent (C1) and an ether solvent (C2).
[0026] In one embodiment of the present invention, the alcohol solvent (C1) is at least one selected from the group consisting of alcohols having 4 to 6 carbon atoms.
[0027] In one embodiment of the present invention, the ether solvent (C2) is at least one selected from the group consisting of ethers having 8 to 12 carbon atoms.
[0028] In one embodiment of the present invention, the weight ratio between the alcohol solvent (C1) and the ether solvent (C2) is 1-50:50-99.
[0029] In one embodiment of the present invention, the weight ratio (B / A) between the hydrophobic resin (B) and the alkali-soluble resin (A) is greater than 0.1 and less than 0.43.
[0030] The present invention provides a protective layer formed by the protective layer composition.
[0031] In one embodiment of the present invention, under the premise that the thickness of the protective layer is 50 nm, the protective layer is completely dissolved after being immersed in a 2.38 mass % aqueous solution of tetramethylammonium hydroxide for 1 second.
[0032] In one embodiment of the present invention, the protective layer has a receding contact angle with respect to water of 69.5 degrees or more.
[0033] In one embodiment of the present invention, the refractive index of the protective layer for light having a wavelength of 193 nm is 1.54 to 1.55.
[0034] The invention provides a laminated body, comprising: a substrate, a photoresist layer, and the above-mentioned protective layer, wherein the photoresist layer is located between the substrate and the protective layer.
[0035] The present invention provides a method for forming a photoresist pattern, comprising: forming a photoresist layer on a substrate; forming the protective layer on the photoresist layer; exposing the photoresist layer and the protective layer; and developing the photoresist layer and the protective layer to form a photoresist pattern on the substrate.
[0036] Based on the above, the present invention provides an alkali-soluble resin, a protective layer composition of an alkali-soluble resin comprising specific structural units (for example, a structural unit (a1) having a fluorinated alkyl group, a structural unit (a2) containing α-trifluoromethyl alcohol, and a structural unit (a3) containing a long carbon chain carboxyl group), a protective layer formed by the protective layer composition, a laminate, and a method for forming a photoresist pattern, wherein, on the premise that the refractive index of the protective layer can match that of water and the photoresist, the protective layer has a high receding contact angle, good water resistance, and good alkali solubility, and is therefore suitable for immersion lithography technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figures 1 to 4 It is a schematic flow chart of a method for forming a photoresist pattern according to one embodiment of the present invention. DETAILED DESCRIPTION
[0038] The following are the terms used in this manual:
[0039] In this specification, "(meth)acrylic acid" means "acrylic acid" and / or "methacrylic acid".
[0040] In the present specification, "alkyl" may be a substituted or unsubstituted straight or branched chain alkyl group, such as, but not limited to, methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl or pentyl.
[0041] In the present specification, "alkylene" may be a substituted or unsubstituted straight or branched alkyl group. Examples of alkylene include, but are not limited to, methylene, ethylene, propylene, isopropylene, n-butylene, sec-butylene, tert-butylene, or pentylene.
[0042] In the present specification, "cycloalkyl" may be substituted or unsubstituted cycloalkyl. Examples of cycloalkyl include, but are not limited to, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, or cyclodecyl.
[0043] In the present specification, "cycloalkylene" may be substituted or unsubstituted cycloalkylene. Examples of cycloalkylene include, but are not limited to, cyclopentylene, cyclohexylene, cycloheptylene, cyclooctylene, cyclononylene, or cyclodecylene.
[0044] In the present specification, "aryl" is a substituted or unsubstituted monovalent group having at least one aromatic ring. Examples of aryl are, but not limited to, phenyl, 1-naphthyl, or 2-naphthyl.
[0045] In the present specification, "arylene" is a substituted or unsubstituted divalent group having at least one aromatic ring. Examples of arylene include, but are not limited to, phenylene or naphthalene.
[0046] In this specification, a "structural unit" refers to one or more units present in a polymer.
[0047] <Alkali-soluble resin (A)>
[0048] The present embodiment provides an alkali-soluble resin (A), including a structural unit (a1) represented by the following formula (1) (also referred to as a "structural unit (a1) having a fluorinated alkyl group" in the present specification), a structural unit (a2) represented by the following formula (2) (also referred to as a "structural unit (a2) containing α-trifluoromethyl alcohol" in the present specification), and a structural unit (a3) represented by the following formula (3) (also referred to as a "structural unit (a3) containing a long carbon chain carboxyl group" in the present specification).
[0049] [Structural unit (a1) represented by formula (1)]
[0050] The structural unit (a1) shown in formula (1) has a fluorinated alkyl group, wherein by introducing fluorine atoms into the structural unit, the refractive index of the resin layer or protective layer formed by the alkali-soluble resin (A) can be reduced, and the hydrophobicity and water resistance can be improved. It is worth noting that hydrophobicity is related to the contact angle with water, so the introduction of fluorine atoms into the structural unit can also increase the contact angle of the alkali-soluble resin (A) with water and the receding contact angle with water. In contrast, if the structural unit does not introduce fluorine atoms, there will be a phenomenon of too high a refractive index and too low a receding contact angle, which is not conducive to the use of the alkali-soluble resin (A) as a component of the protective layer.
[0051] Specifically, the structural unit (a1) represented by formula (1) is as follows:
[0052]
[0053] In formula (1),
[0054] R 1 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, preferably a hydrogen atom or a methyl group;
[0055] R 2 is a fluorinated alkyl group having 1 to 10 carbon atoms, preferably a fluorinated alkyl group having 5 to 10 carbon atoms;
[0056] *Indicates the bonding position.
[0057] When R 2 When the fluorinated alkyl group has 5 to 10 carbon atoms, the hydrophobicity and water resistance of the alkali-soluble resin (A) can be further increased.
[0058] R in formula (1) 2 In the embodiment, the fluorinated alkyl group having 1 to 10 carbon atoms may contain more than 1 fluorine atom, preferably more than 3 fluorine atoms, and more preferably more than 8 fluorine atoms. When the fluorinated alkyl group having 1 to 10 carbon atoms contains more than 3 fluorine atoms, the refractive index of the resin layer or protective layer formed by the alkali-soluble resin (A) can be further reduced, and the hydrophobicity and water resistance can be improved.
[0059] The structural unit (a1) represented by the formula (1) is, for example, a structural unit (a1-1) represented by the following formula (1-1).
[0060]
[0061] In formula (1),
[0062] R' is a fluorine atom or a trifluoromethyl group, preferably a fluorine atom;
[0063] R" is a hydrogen atom or a fluorine atom;
[0064] r is an integer from 0 to 3, preferably 1 or 2;
[0065] s is an integer from 0 to 7, preferably an integer from 3 to 7;
[0066] *Indicates the bonding position.
[0067] Specific examples of the structural unit (a1-1) represented by formula (1-1) include the structural unit represented by the following formula (1-1-1) to the structural unit represented by the following formula (1-1-23), or a combination thereof. Specific examples of the structural unit (a1-1) represented by formula (1-1) preferably include the structural unit represented by the following formula (1-1-5).
[0068]
[0069]
[0070]
[0071] [Structural unit (a2) represented by formula (2)]
[0072] The structural unit (a2) shown in formula (2) contains α-trifluoromethyl alcohol, wherein the refractive index of the alkali-soluble resin (A) can be reduced by introducing a fluorine atom into the structural unit. It is worth noting that the hydrogen of the -OH group in α-trifluoromethyl alcohol is acidic, so that the alkali-soluble resin (A) can be made alkali-soluble and have an appropriate development rate.
[0073] Specifically, the structural unit (a2) represented by formula (2) is as follows:
[0074]
[0075] In formula (2),
[0076] R 3 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, preferably a hydrogen atom or a methyl group;
[0077] Y 1 is an alkylene group having 1 to 10 carbon atoms, a cycloalkylene group having 5 to 10 carbon atoms, or an arylene group, preferably an alkylene group having 3 to 10 carbon atoms;
[0078] * indicates the bond position,
[0079] When Y 1 When it is an alkylene group having 2 to 10 carbon atoms or a cycloalkylene group having 5 to 10 carbon atoms, one or more of the -CH2- groups may be replaced by -O- or replace.
[0080] When Y 1When the alkylene group has 3 to 10 carbon atoms, the hydrophobicity and water resistance of the alkali-soluble resin (A) can be further increased.
[0081] Specific examples of the structural unit (a2) shown in formula (2) include the structural unit shown in formula (2-1-1) to the structural unit shown in formula (2-1-16), the structural unit shown in formula (2-2-1) to the structural unit shown in formula (2-2-5), and the structural unit shown in formula (2-3), or a combination thereof. Specific examples of the structural unit (a2) shown in formula (2) preferably include the structural unit shown in the following formula (2-1-3), the structural unit shown in the following formula (2-1-5), or a combination thereof.
[0082]
[0083]
[0084]
[0085] [Structural unit (a3) represented by formula (3)]
[0086] The structural unit (a3) shown in formula (3) contains a long carbon chain carboxyl group. By introducing the long carbon chain carboxyl group into the structural unit, the alkali solubility of the alkali-soluble resin (A) can be improved and the developing rate can be appropriately obtained. In contrast, if the structural units containing carboxyl groups in the alkali-soluble resin (A) are all structural units derived from (meth)acrylic acid, the receding contact angle of the protective layer formed by the alkali-soluble resin (A) will decrease due to the excessive hydrophilicity of the carboxyl group.
[0087] Specifically, the structural unit (a3) represented by formula (3) is as follows:
[0088]
[0089] In formula (3),
[0090] R 4 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, preferably a hydrogen atom or a methyl group;
[0091] Y 2 is an alkylene group having 2 to 8 carbon atoms, preferably an alkylene group having 5 to 8 carbon atoms;
[0092] * indicates the bond position,
[0093] Among them, 2 In which one or more -CH2- can be replaced by -O- or Substitution, preferably one of the -CH2- replace.
[0094] When Y2 When the alkylene group has 5 to 8 carbon atoms, the hydrophobicity, water resistance and receding contact angle can be further improved while the alkali-soluble resin (A) has appropriate alkali solubility and development rate.
[0095] The structural unit (a3) represented by formula (3) is, for example, a structural unit (a3-1) represented by formula (3-1), a structural unit (a3-2) represented by formula (3-2), a structural unit (a3-3) represented by formula (3-3), a structural unit (a3-4) represented by formula (3-4), or a combination thereof. Specific examples of the structural unit (a3) represented by formula (3) are described in detail below, wherein the specific example of the structural unit (a3) represented by formula (3) preferably includes a structural unit represented by the following formula (3-3-5).
[0096]
[0097] In formula (3-1),
[0098] R 4 is a hydrogen atom or a methyl group;
[0099] Y 3 is an alkylene group having 2 to 8 carbon atoms;
[0100] *Indicates the bonding position.
[0101] Specific examples of the structural unit represented by the formula (3-1) include the structural unit represented by the formula (3-1-1) to the structural unit represented by the formula (3-1-7).
[0102]
[0103]
[0104] In formula (3-2),
[0105] R 4 is a hydrogen atom or a methyl group;
[0106] Y 4 is an alkylene group having 1 to 3 carbon atoms;
[0107] Y 5 is an alkylene group having 1 to 4 carbon atoms;
[0108] m is 1 or 2,
[0109] *Indicates the bonding position.
[0110] Specific examples of the structural unit represented by the formula (3-2) include the structural unit represented by the formula (3-2-1) to the structural unit represented by the formula (3-2-6).
[0111]
[0112]
[0113] In formula (3-3),
[0114] R 4 is a hydrogen atom or a methyl group;
[0115] Y 6 is an alkylene group having 1 to 5 carbon atoms;
[0116] Y 7 is an alkylene group having 1 to 4 carbon atoms;
[0117] *Indicates the bonding position.
[0118] Specific examples of the structural unit represented by the formula (3-3) include the structural unit represented by the formula (3-3-1) to the structural unit represented by the formula (3-3-14).
[0119]
[0120]
[0121]
[0122] In formula (3-4),
[0123] R 4 is a hydrogen atom or a methyl group;
[0124] Y 8 is an alkylene group having 1 to 5 carbon atoms;
[0125] Y 9 is an alkylene group having 1 to 4 carbon atoms;
[0126] *Indicates the bonding position.
[0127] Specific examples of the structural unit represented by the formula (3-4) include the structural unit represented by the formula (3-4-1) to the structural unit represented by the formula (3-4-2).
[0128]
[0129] In one embodiment, the molar ratio of the structural unit (a1) represented by formula (1), the structural unit (a2) represented by formula (2), and the structural unit (a3) represented by formula (3) can be 10-50:50-90:1-20, preferably 20-40:50-70:1-10. When the molar ratio of the structural unit (a1) represented by formula (1), the structural unit (a2) represented by formula (2), and the structural unit (a3) represented by formula (3) is within the above range, the resin layer formed by the alkali-soluble resin (A) or the protective layer described later can achieve a better balance in refractive index, alkali developability, and development rate. However, if it is desired to obtain a receding contact angle that meets the requirements of the protective layer as a photoresist, it is still necessary to use it in combination with the hydrophobic resin (B) described later.
[0130] In addition, without affecting the effectiveness of the present embodiment, the structural units constituting the alkali-soluble resin (A) may further include other structural units in addition to the structural unit (a1) represented by formula (1), the structural unit (a2) represented by formula (2), and the structural unit (a3) represented by formula (3).
[0131] The alkali-soluble resin (A) may be a random copolymer or a block copolymer.
[0132] The weight average molecular weight of the alkali soluble resin (A) is 2,000 to 30,000. When the weight average molecular weight of the alkali soluble resin (A) is within the above range, the resin layer or the protective layer formed by the alkali soluble resin (A) can have good water resistance and alkali solubility.
[0133] When the thickness of the resin layer formed by the alkali-soluble resin (A) is 50 nm, the resin layer is completely dissolved after being immersed in a 2.38 mass % aqueous solution of tetramethylammonium hydroxide for 1 second. That is, the alkali-soluble resin (A) has good alkali solubility.
[0134] [Synthesis of alkali-soluble resin (A)]
[0135] The alkali-soluble resin (A) can be polymerized from a first monomer mixture including a monomer derived from a structural unit (a1) represented by formula (1), a monomer derived from a structural unit (a2) represented by formula (2), and a monomer derived from a structural unit (a3) represented by formula (3). The polymerization method is not particularly limited, and an appropriate polymerization method can be selected according to the requirements. The polymerization method is, for example, a solution polymerization method.
[0136] The monomer from which the structural unit (a1) represented by the formula (1) is derived is, for example, a monomer represented by the formula (I).
[0137]
[0138] R in formula (I) 1 , R 2 With R in formula (1) 1 , R 2 The same, no further elaboration is given here.
[0139] Specific examples of the monomer represented by formula (I) include monomers derived from the structural unit represented by the above formula (1-1-1) to the structural unit represented by the above formula (1-1-9), which are not further described here.
[0140] The monomer from which the structural unit (a2) represented by the formula (2) is derived is, for example, a monomer represented by the formula (II).
[0141]
[0142] R in formula (II) 3 , Y 1 With R in formula (2) 3 , Y 1 The same, no further elaboration is given here.
[0143] Specific examples of the monomer represented by formula (II) include monomers derived from the structural unit represented by the above formula (2-1-1) to the structural unit represented by the above formula (2-1-16), the structural unit represented by the above formula (2-2-1) to the structural unit represented by the above formula (2-2-5), and the structural unit represented by the above formula (2-3), which are not further described here.
[0144] The monomer from which the structural unit (a3) represented by the formula (3) is derived is, for example, a monomer represented by the formula (III).
[0145]
[0146] R in formula (III) 4 , Y 2 With R in formula (3) 4 , Y 2 The same, no further elaboration is given here.
[0147] Specific examples of the monomer represented by formula (III) include those derived from the structural unit represented by the above formula (3-1-1) to the structural unit represented by the above formula (3-1-7), the structural unit represented by the above formula (3-2-1) to the structural unit represented by the above formula (3-2-6), the structural unit represented by the above formula (3-3-1) to the structural unit represented by the above formula (3-3-14), and the structural unit represented by the above formula (3-4-1) to the structural unit represented by the above formula (3-4-2), which are not further described here.
[0148] In addition, without affecting the efficacy of the present embodiment, the first monomer mixture may further include other monomers besides the monomer represented by formula (I), the monomer represented by formula (II), and the monomer represented by formula (III).
[0149] The mixture constituting the alkali-soluble resin (A) may include a solvent. The type of the solvent is not particularly limited as long as it does not react with the monomer and can dissolve the monomer. Specific examples of the solvent include acetone, methyl isobutyl ketone, 2-heptanone, cyclohexanone, or a combination thereof. Specific examples of the solvent preferably include cyclohexanone.
[0150] The mixture constituting the alkali-soluble resin (A) may include a polymerization initiator. The type of the polymerization initiator is not particularly limited as long as it does not react with the monomer and is soluble in the solvent monomer. Specific examples of the polymerization initiator include cumene hydroperoxide (CHP), diisopropylbenzenehydroperoxide, di-t-butyl peroxide, lauroyl peroxide, benzoyl peroxide, t-butyl peroxyisopropyl carbonate ... The polymerization initiator may be organic peroxides such as tert-amylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, etc.; azo compounds such as 2,2'-azobis(isobutyronitrile), 1,1'-azobis(cyclohexanecarbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), dimethyl 2,2'-azobis(2-methyl propionate), etc. The polymerization initiator is preferably tert-butyl peroxy-2-ethylhexanoate. The amount of the polymerization initiator used is not particularly limited, and may be 0.1 to 15 parts by weight, preferably 0.5 to 10 parts by weight, relative to 100 parts by weight of all monomers in the mixture.
[0151] When the alkali-soluble resin (A) is synthesized by solution polymerization, the polymerization temperature may be 40°C to 150°C, preferably 60°C to 130°C.
[0152] When the alkali-soluble resin (A) is synthesized by solution polymerization, the polymerization time may be 1 to 12 hours, preferably 2 to 6 hours.
[0153] In one embodiment, the synthesis of the alkali-soluble resin (A) may be performed under a nitrogen environment.
[0154] <Protective Layer Composition>
[0155] This embodiment provides a protective layer composition, including: an alkali-soluble resin (A), a hydrophobic resin (B), and a solvent (C). In addition, if necessary, the protective layer composition may further include other additives (D). The components of the protective layer composition will be described in detail below.
[0156] Alkali soluble resin (A)
[0157] The alkali-soluble resin (A) has been described above and will not be described again here.
[0158] Hydrophobic resin (B)
[0159] The hydrophobic resin (B) includes a structural unit (b1) represented by the following formula (4) (also referred to as a "structural unit (b1) not containing fluorine atoms" in the present specification) and a structural unit (b2) represented by the following formula (5) (also referred to as a "structural unit (b2) containing fluorine atoms" in the present specification).
[0160] [Structural unit (b1) represented by formula (4)]
[0161] The structural unit (b1) shown in formula (4) is related to the solubility of the hydrophobic resin (B) in the solvent (C). Specifically, the structural unit (b1) shown in formula (4) has a carbon chain, and therefore has good compatibility with the solvent (C) having a long carbon chain described later, so that the hydrophobic resin (B) can be smoothly dissolved in the solvent (C).
[0162] Specifically, the structural unit (b1) represented by formula (4) is as follows:
[0163]
[0164] In formula (4),
[0165] R 5 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, preferably a hydrogen atom or a methyl group;
[0166] R 6is an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group, preferably an alkyl group having 1 to 10 carbon atoms or a cycloalkyl group having 5 to 10 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms;
[0167] * indicates the bond position,
[0168] When R 6 When it is an alkyl group having 2 to 10 carbon atoms or a cycloalkyl group having 5 to 10 carbon atoms, one or more of the -CH2- groups may be replaced by -O- or replace.
[0169] In one embodiment, in formula (4), R 6 is an alkyl group having 1 to 10 carbon atoms. 6 When it is an alkyl group with a carbon number of 1 to 10, the structural unit (b1) shown in formula (4) has a carbon chain and therefore has good compatibility with the solvent (C) having a long carbon chain described later (especially the alcohol solvent (C1)), so that the hydrophobic resin (B) can be smoothly dissolved in the solvent (C).
[0170] In one embodiment, in formula (4), R 6 is an alkyl group having 5 to 10 carbon atoms. 6 When it is an alkyl group with a carbon number of 5 to 10, the structural unit (b1) shown in formula (4) has a long carbon chain, and therefore has better compatibility with the solvent (C) with a long carbon chain described later (especially the alcohol solvent (C1)), so that the hydrophobic resin (B) can be more smoothly dissolved in the solvent (C).
[0171] In one embodiment, in formula (4), R 6 is a cycloalkyl group having 5 to 10 carbon atoms. 6 When it is a cycloalkyl group having 5 to 10 carbon atoms, the receding contact angle of the resin layer or protective layer formed of the hydrophobic resin (B) can be further increased.
[0172] Specific examples of the structural unit represented by formula (4) include the structural unit represented by the following formula (4-4-1) to the structural unit represented by the following formula (4-4-34), the structural unit represented by the following formula (4-2-1) to the structural unit represented by the following formula (4-2-14), the structural unit represented by the following formula (4-3-1) to the structural unit represented by the following formula (4-3-2), or a combination thereof. Specific examples of the structural unit represented by formula (4) preferably include the structural unit represented by the following formula (4-1-29), the structural unit represented by formula (4-2-7), or a combination thereof.
[0173]
[0174]
[0175]
[0176]
[0177] [Structural unit (b2) represented by formula (5)]
[0178] The structural unit (b2) shown in formula (5) contains fluorine atoms, wherein by introducing fluorine atoms into the structural unit, the refractive index of the hydrophobic resin (B) can be reduced, and the hydrophobicity and water resistance can be improved. It is worth noting that hydrophobicity is related to the contact angle with water, so the introduction of fluorine atoms into the structural unit can also increase the contact angle with water and the receding contact angle with water of the hydrophobic resin (B). In contrast, if the structural unit does not introduce fluorine atoms, there will be a phenomenon of too high a refractive index and too low a receding contact angle, which is not conducive to the use of the hydrophobic resin (B) as a component of the protective layer.
[0179]
[0180] In formula (5),
[0181] R 7 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, preferably a hydrogen atom or a methyl group;
[0182] R 8 is a fluorinated alkyl group having 1 to 10 carbon atoms, preferably a fluorinated alkyl group having 5 to 10 carbon atoms,
[0183] *Indicates the bonding position.
[0184] When R 8 When the fluorinated alkyl group has 5 to 10 carbon atoms, the hydrophobicity and water resistance of the hydrophobic resin (B) can be further increased.
[0185] R in formula (5) 8 In the embodiment, the fluorinated alkyl group having 1 to 10 carbon atoms may contain more than 1 fluorine atom, preferably more than 3 fluorine atoms, and more preferably more than 8 fluorine atoms. When the fluorinated alkyl group having 1 to 10 carbon atoms contains more than 3 fluorine atoms, the refractive index of the resin layer or protective layer formed by the hydrophobic resin (B) can be further reduced, and the hydrophobicity and water resistance can be improved.
[0186] The specific example of the structural unit (b2) shown in formula (5) is the same as the specific example of the structural unit (a1) shown in formula (1). Furthermore, the structural unit (b2) shown in formula (5) is, for example, the structural unit shown in formula (1-1), and the specific example of the structural unit (a1) shown in formula (1-1) includes the structural unit shown in formula (1-1-1) to the structural unit shown in formula (1-1-9). The structural unit shown in formula (1-1) and the structural unit shown in formula (1-1-1) to the structural unit shown in formula (1-1-9) have been described in the previous text and are not repeated here. The specific example of the structural unit (b2) shown in formula (5) preferably includes the structural unit shown in the following formula (1-1-5).
[0187] In one embodiment, the molar ratio of the structural unit (b1) represented by formula (4) to the structural unit (b2) represented by formula (5) can be 10-50:50-90, preferably 20-30:70-80. When the molar ratio of the structural unit (b1) represented by formula (4) to the structural unit (b2) represented by formula (5) is within the above range, the resin layer formed by the hydrophobic resin or the protective layer described later can achieve a better balance in solubility, refractive index and receding contact angle. However, if the alkali solubility and development rate required for the protective layer as a photoresist are to be obtained, it is still necessary to use it in combination with the aforementioned alkali-soluble resin (A).
[0188] In addition, without affecting the efficacy of the present embodiment, the structural units constituting the hydrophobic resin (B) may further include other structural units in addition to the structural unit (b1) represented by formula (4) and the structural unit (b2) represented by formula (5).
[0189] In one embodiment, the weight average molecular weight of the hydrophobic resin (B) is 2,000 to 3,0000. When the weight average molecular weight of the hydrophobic resin (B) is within the above range, the resin layer or the protective layer formed by the hydrophobic resin (B) can have good water resistance and alkali solubility.
[0190] In one embodiment, the weight ratio (B / A) of the hydrophobic resin (B) to the alkali-soluble resin (A) is greater than 0.1 and less than 0.43. When the weight ratio (B / A) of the hydrophobic resin (B) to the alkali-soluble resin (A) is within the above range, the protective layer can achieve a better balance between the receding contact angle and the alkali solubility, provided that the refractive index of the protective layer can match that of water and the photoresist.
[0191] On the premise that the thickness of the resin layer formed of the hydrophobic resin (B) is 50 nm, the receding contact angle of the resin layer with respect to water is 69.5 degrees or more.
[0192] [Synthesis of hydrophobic resin (B)]
[0193] The hydrophobic resin (B) can be polymerized from a second monomer mixture including a monomer derived from the structural unit (b1) shown in formula (4) and a monomer derived from the structural unit (b2) shown in formula (5). The polymerization method is not particularly limited, and an appropriate polymerization method can be selected according to the requirements. The polymerization method is, for example, a solution polymerization method.
[0194] The monomer from which the structural unit (b1) represented by the formula (4) is derived is, for example, a monomer represented by the formula (IV).
[0195]
[0196] R in formula (IV) 5 , R 6 With R in formula (4) 5 , R 6 The same, no further elaboration is given here.
[0197] Specific examples of the monomer represented by formula (IV) include monomers derived from the structural unit represented by the above formula (4-4-1) to the structural unit represented by the above formula (4-4-34), the structural unit represented by the above formula (4-2-1) to the structural unit represented by the above formula (4-2-14), and the structural unit represented by the above formula (4-3-1) to the structural unit represented by the above formula (4-3-2), which are not further described here.
[0198] The monomer from which the structural unit (b2) represented by the formula (5) is derived is, for example, a monomer represented by the formula (V).
[0199]
[0200] R in formula (V) 7 , R 8 With R in formula (5) 7 , R 8 The same, no further elaboration is given here.
[0201] Since the specific example of the structural unit (b2) shown in formula (5) is the same as the specific example of the structural unit (a1) shown in formula (1), the specific example of the monomer shown in formula (V) includes monomers derived from the structural unit shown in the above (1-1-1) to the structural unit shown in the above formula (1-1-9), which will not be further described here.
[0202] In addition, without affecting the efficacy of the present embodiment, the second monomer mixture may further include other monomers besides the monomer represented by formula (IV) and the monomer represented by formula (V).
[0203] The mixture constituting the hydrophobic resin (B) may include a solvent. The type of solvent is not particularly limited as long as it does not react with the monomer and can dissolve the monomer. Specific examples of the solvent include propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, or a combination thereof. Specific examples of the solvent preferably include propylene glycol monomethyl ether.
[0204] The mixture constituting the hydrophobic resin (B) may include a polymerization initiator. The type of the polymerization initiator is not particularly limited, as long as it can be non-reactive with the monomer and can be dissolved in the solvent monomer. The specific example of the polymerization initiator of the hydrophobic resin (B) may be the same as the specific example of the polymerization initiator of the alkali-soluble resin (A), and will not be described in detail here.
[0205] When the hydrophobic resin (B) is synthesized by solution polymerization, the polymerization temperature may be 40°C to 150°C, preferably 60°C to 130°C.
[0206] When the hydrophobic resin (B) is synthesized by solution polymerization, the polymerization time may be 1 to 12 hours, preferably 2 to 6 hours.
[0207] In addition, the synthesis of the hydrophobic resin (B) can be performed under a nitrogen atmosphere.
[0208] Solvent (C)
[0209] The solvent (C) includes an alcohol solvent (C1) and an ether solvent (C2).
[0210] The alcohol solvent (C1) is at least one selected from the group consisting of alcohols having 4 to 6 carbon atoms.
[0211] Specific examples of alcohol solvents (C1) include 1-butanol, 2-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-1-butanol, 1-hexanol, 2-hexanol, 2-methyl-1-pentanol, 3-methyl-1-pentanol, 2-ethyl-1-butanol, or a combination thereof. Specific examples of alcohol solvents (C1) preferably include 2-methyl-1-butanol.
[0212] The alcohol solvent (C1) has a long carbon chain and therefore has good compatibility with the structural unit represented by formula (4) in the hydrophobic resin (B), so that the hydrophobic resin (B) can be smoothly dissolved in the solvent (C).
[0213] The ether solvent (C2) is at least one selected from the group consisting of ethers having 8 to 12 carbon atoms.
[0214] Specific examples of the ether solvent (C2) include di-n-butyl ether, diisobutyl ether, diisoamyl ether, di-n-amyl ether, methylcyclopentyl ether, methylcyclohexyl ether, di-sec-butyl ether, di-sec-amyl ether, di-tert-amyl ether, di-n-hexyl ether or a combination thereof. Specific examples of the ether solvent (C2) preferably include di-n-butyl ether.
[0215] The ether solvent (C2) is stable in nature, so the protective layer formed by the protective layer composition will not interact with the photoresist layer, and the protective layer can fully exert its function of protecting the photoresist layer.
[0216] The weight ratio of the alcohol solvent (C1) to the ether solvent (C2) may be 1-50:50-99, preferably 5-15:85-95.
[0217] It is worth noting that in this embodiment, a dual solvent system is used, with an ether solvent (C2) as the main solvent and an alcohol solvent (C1) as the secondary solvent, so that the solvent (C) exhibits excellent solubility for the alkali-soluble resin (A) and the hydrophobic resin (B). In particular, when the weight ratio between the alcohol solvent (C1) and the ether solvent (C2) is within the above range, the alkali-soluble resin (A) and the hydrophobic resin (B) can be more smoothly dissolved in the solvent (C), and the protective layer formed by the protective layer composition will not interact with the photoresist layer, further exerting the function of the protective layer to protect the photoresist layer.
[0218] In one embodiment, from the viewpoint of the solubility of the alkali-soluble resin (A) and the hydrophobic resin (B) in the solvent (C) and the coating property of the protective layer composition on the photoresist layer, the weight ratio ((A+B) / C) between the sum of the hydrophobic resin (B) and the alkali-soluble resin (A) and the solvent (C) may be 0.01 to 0.06, preferably 0.02 to 0.04, and more preferably 0.025 to 0.035.
[0219] Additives (D)
[0220] In addition to the above components, the protective layer composition may contain additives (D) such as surfactants as needed without affecting the effects of the present embodiment.
[0221] <Preparation of Protective Layer Composition>
[0222] There is no particular limitation on the method for preparing the protective layer composition. For example, an alkali-soluble resin (A), a hydrophobic resin (B), and a solvent (C) are placed in a stirrer and stirred to uniformly mix them into a solution state. An additive (D) may also be added if necessary. After uniform mixing, a protective layer composition in a solution state can be obtained.
[0223] <Protective layer>
[0224] This embodiment provides a protective layer formed from the protective layer composition.
[0225] In one embodiment, when the thickness of the protective layer is 50 nm, the protective layer is completely dissolved after being immersed in a 2.38 mass % aqueous solution of tetramethylammonium hydroxide for 1 second. That is, the protective layer of this embodiment has good alkali solubility.
[0226] In one embodiment, the receding contact angle of the protective layer to water is 69.5 degrees or more. In another embodiment, the receding contact angle of the protective layer to water is 72 degrees or more, 76 degrees or more, or 78 degrees or more. That is, the protective layer of this embodiment has a high receding contact angle.
[0227] In one embodiment, the refractive index of the protective layer for light with a wavelength of 193 nm is 1.54 to 1.55. That is, the refractive index of the protective layer of this embodiment can match that of water and photoresist.
[0228] <Laminate and method for forming photoresist pattern>
[0229] This embodiment provides a method for forming a photoresist pattern, comprising: step (i): forming a photoresist layer on a substrate; step (ii): forming a protective layer on the photoresist layer; step (iii): exposing the photoresist layer and the protective layer; and step (iv): developing the photoresist layer and the protective layer to form a photoresist pattern on the substrate. Figure 1 to Figure 4 Detailed description of each step:
[0230] Step (i)
[0231] like Figure 1 As shown, a photoresist layer 120 is formed on the substrate 110 , wherein the method for forming the photoresist layer 120 is not particularly limited, for example, a coating method such as a spin coating method, a spray coating method, or a roller coating method.
[0232] The substrate 110 is not particularly limited, and may be, for example, a glass substrate, a silicon wafer substrate, a ceramic substrate, or a quartz substrate.
[0233] The photoresist layer 120 is not particularly limited, and can be, for example, a photoresist containing a photoacid and a quencher. In addition, the photoresist layer 120 can be a positive photoresist or a negative photoresist.
[0234] Step (ii)
[0235] like Figure 2As shown, the protective layer 130 is formed on the photoresist layer 120. Thus, a stacked body 100 including the substrate 110, the photoresist layer 120, and the protective layer 130 can be formed, wherein the photoresist layer 120 is located between the substrate 110 and the protective layer 130.
[0236] The method of forming the protective layer 130 is not particularly limited, for example, after coating by a coating method such as a spin coating method, a spray coating method, or a roller coating method, baking is performed. The baking method is not particularly limited, for example, the laminate 100 is placed on a heating plate. The heating temperature is 60° C. to 120° C. The heating time is 30 seconds to 120 seconds.
[0237] The protective layer 130 is formed of the protective layer composition described above. The protective layer 130 is coated on the photoresist layer 120 to prevent water, which is used as an immersion medium in immersion lithography, from penetrating into the photoresist layer and to prevent the photoacid and quencher in the photoresist from dissolving in water and causing contamination or damage to the mirror assembly. In addition, in order to reduce the surface tension of water and increase the surface activity, aliphatic alcohols such as methanol, ethanol, or isopropanol may also be added to the water.
[0238] The thickness of the protective layer 130 is not particularly limited, but in terms of developability and light transmittance, the thickness is 10 nm to 150 nm.
[0239] The protection layer 130 is preferably not mixed with the photoresist layer 120 and covers the photoresist layer 120 .
[0240] Step (iii)
[0241] like Figure 3 As shown, the photoresist layer 120 and the protective layer 130 on the substrate 110 are exposed. Specifically, the light L emitted by the light source 300 passes through the photomask 200 with a pattern and water (not shown) as an immersion medium to expose the photoresist layer 120 and the protective layer 130.
[0242] The wavelength of exposure may be far ultraviolet light of 250 nm or shorter, more preferably 220 nm or shorter, such as KrF excimer laser (248 nm), ArF excimer laser (193 nm), F2 excimer laser (157 nm), or X-rays.
[0243] The exposure dose may be 1 mJ / cm2 to 100 mJ / cm2.
[0244] Step (iv)
[0245] like Figure 4 As shown, the photoresist layer 120 and the protective layer 130 are developed to form a photoresist pattern 120 a on the substrate 110 .
[0246] The photoresist layer 120 may be a positive photoresist or a negative photoresist. When the photoresist layer 120 is a positive photoresist, after the photoresist layer 120 is exposed, the exposed portion of the photoresist layer 120 and the protective layer 130 will be dissolved in the developer during development, so that the unexposed photoresist pattern 120a is left after development. When the photoresist layer 120 is a negative photoresist, after the photoresist layer 120 is exposed, the unexposed portion of the photoresist layer 120 and the protective layer 130 will be dissolved in the developer during development, so that the exposed photoresist pattern 120a is left after development.
[0247] The developer is, for example, an inorganic alkaline aqueous solution. Specific examples of the alkali contained in the developer include sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate or amine; aliphatic primary amines such as ethylamine or n-propylamine; aliphatic secondary amines such as diethylamine or n-propylamine; aliphatic tertiary amines such as trimethylamine, diethylaminomethyl, dimethylethylamine or triethylamine; tertiary aliphatic cyclic acids such as pyrrole, piperidine, N-methylpiperidine, N-methyl 1,8-diazabicyclo[5.4.0]-7-undecene or 1,5-diazabicyclo[4.3.0]-5-nonene; aromatic tertiary amines such as pyridine, methylpyrimidine, dimethylpyridine or quinoline; quaternary ammonium salt alkaline compounds such as aqueous solutions of tetramethylammonium hydroxide or tetraethylammonium hydroxide.
[0248] The alkali concentration of the developer may be 0.1% by mass to 20% by mass.
[0249] The pH of the developer may be from 10.0 to 15.0.
[0250] In one embodiment, the developer is a 2.38 mass % aqueous solution of tetramethylammonium hydroxide.
[0251] After step (iv), a cleaning step may be further performed. Specifically, pure water and / or supercritical fluid may be used to remove the developer adhering to the substrate 110 and the photoresist pattern 120a.
[0252] The following experimental examples are given to describe the present invention in more detail. Although the following experimental examples are described, the materials used, their amounts and ratios, processing details, and processing procedures, etc., may be appropriately changed without exceeding the scope of the present invention. Therefore, the present invention should not be interpreted restrictively based on the experimental examples described below.
[0253] Example
[0254] <Synthesis of Alkali-Soluble Resin (A)>
[0255] Hereinafter, Synthesis Example A-1 of the alkali-soluble resin (A) and Comparative Synthesis Examples A'-1 and A'-2 of the resin (A') as a comparative example will be described.
[0256] [Synthesis Example A-1]
[0257] 2.34 g of octafluoropentyl methacrylate, 4.35 g of 1,1,1-trifluoro-2-trifluoromethyl-2-hydroxy-4-pentyl methacrylate, 4.01 g of 1,1,1-trifluoro-2-trifluoromethyl-2-hydroxy-5-pentyl methacrylate, and 0.63 g of mono[2-[(2-methyl-acryloyl)oxy]ethyl]succinate were dissolved in 19 ml of cyclohexanone, and 0.67 g of tert-butyl peroxy 2-ethylhexanoate was added as a polymerization initiator. Then, the mixed solution was stirred at 90° C. for 4 hours in a nitrogen atmosphere for reaction. Then, the reaction solution was poured into 36 g of n-hexane while being vigorously stirred. After the polymer was precipitated, the upper solvent was removed, and finally vacuum dried to obtain a white alkali-soluble resin (A-1).
[0258] The structural units contained in the alkali-soluble resin (A-1) and their molar ratios are as follows:
[0259]
[0260] The weight average molecular weight, refractive index, receding contact angle, water resistance, and alkali solubility of the alkali-soluble resin (A-1) were evaluated by the following evaluation methods and are shown in Table 1.
[0261] It is worth noting that the refractive index, receding contact angle, water resistance, and alkali solubility of the resin need to be evaluated in the form of a "film". Specifically, 100 parts by weight of the resin, 323 parts by weight of 2-methyl-1-butanol, and 2910 parts by weight of di-n-butyl ether were mixed with a mechanical stirrer, and the resin was applied to a silicon substrate by spin coating to form a coating film. The silicon substrate and the coating film were then placed on a hot plate and baked at 80°C for 60 seconds to form a film (film thickness 50nm). Next, the refractive index, receding contact angle, water resistance, and alkali solubility were evaluated using the film.
[0262] [Comparative Synthesis Example A'-1]
[0263] 2.47 g of octafluoropentyl methacrylate, 4.48 g of 1,1,1-trifluoro-2-trifluoromethyl-2-hydroxy-4-pentyl methacrylate, 3.99 g of 1,1,1-trifluoro-2-trifluoromethyl-2-hydroxy-5-pentyl methacrylate, and 0.35 g of methacrylic acid were dissolved in 19 ml of cyclohexanone, and 0.71 g of tert-butyl peroxy 2-ethylhexanoate was added as a polymerization initiator. Then, the mixed solution was stirred at 90° C. for 4 hours in a nitrogen environment for reaction. Then, the reaction solution was poured into 36 g of n-hexane while being vigorously stirred. After the polymer was precipitated, the upper solvent was removed, and finally vacuum dried to obtain a white resin (A'-1).
[0264] The structural units contained in the resin (A'-1) and their molar ratios are as follows:
[0265]
[0266] The weight average molecular weight, refractive index, receding contact angle, water resistance, and alkali solubility of the resin (A′-1) were evaluated by the evaluation methods described below and are shown in Table 1.
[0267] [Comparative Synthesis Example A'-2]
[0268] 2.30 g of octafluoropentyl methacrylate, 4.74 g of 1,1,1-trifluoro-2-trifluoromethyl-2-hydroxy-4-pentyl methacrylate, and 4.29 g of 1,1,1-trifluoro-2-trifluoromethyl-2-hydroxy-5-pentyl methacrylate were dissolved in 19 ml of cyclohexanone, and 0.66 g of tert-butyl peroxy 2-ethylhexanoate was added as a polymerization initiator. Then, the mixed solution was stirred at 90° C. for 4 hours in a nitrogen environment for reaction. Then, the reaction solution was poured into 36 g of n-hexane while being vigorously stirred. After the polymer was precipitated, the upper solvent was removed, and finally vacuum dried to obtain a white resin (A'-2).
[0269] The structural units contained in the resin (A'-2) and their molar ratios are as follows:
[0270]
[0271] The weight average molecular weight, refractive index, receding contact angle, water resistance, and alkali solubility of the resin (A'-2) were evaluated by the evaluation methods described below and are shown in Table 1.
[0272] Table 1
[0273]
[0274] <Preparation of Hydrophobic Resin (B)>
[0275] Synthesis Examples B-1 and B-2 of the hydrophobic resin (B) are described below.
[0276] [Synthesis Example B-1]
[0277] 8.79 g of octafluoropentyl methacrylate and 2.49 g of 2-ethylhexyl methacrylate were dissolved in 19.56 ml of propylene glycol monomethyl ether, and 0.72 g of tert-butyl peroxy 2-ethylhexanoate was added thereto as a polymerization initiator. Then, the mixed solution was stirred at 90° C. for 4 hours in a nitrogen environment to react. Then, the reaction solution was poured into 36 g of n-hexane while being vigorously stirred. After the polymer was precipitated, the upper solvent was removed, and finally vacuum dried to obtain a white hydrophobic resin (B-1).
[0278] The structural units contained in the hydrophobic resin (B-1) and their molar ratios are as follows:
[0279]
[0280] Table 2 shows the weight average molecular weight, refractive index, receding contact angle, water resistance, and alkali solubility of the hydrophobic resin (B-1).
[0281] [Synthesis Example B-2]
[0282] 8.59 g of octafluoropentyl methacrylate and 2.70 g of tricyclo[5.2.1.0 2,6 ] decyl ester was dissolved in 19.56 ml of propylene glycol monomethyl ether, and 0.71 g of tert-butyl peroxy 2-ethylhexanoate was added thereto as a polymerization initiator. Then, the mixed solution was stirred at 90° C. for 4 hours in a nitrogen environment to react. Then, the reaction solution was poured into 36 g of n-hexane while being vigorously stirred. After the polymer was precipitated, the upper solvent was removed, and finally vacuum dried to obtain a white hydrophobic resin (B-2).
[0283] The structural units contained in the hydrophobic resin (B-2) and their molar ratios are as follows:
[0284]
[0285] Table 2 shows the weight average molecular weight, refractive index, receding contact angle, water resistance, and alkali solubility of the hydrophobic resin (B-2).
[0286] Table 2
[0287] Synthesis Example B-1 Synthesis Example B-2 Resin name Hydrophobic resin (B-1) Hydrophobic resin (B-2) Weight average molecular weight 11,000 10,000 Refractive Index 1.54 1.54 Receding contact angle 81 84 Water resistance ○ ○ Alkali soluble × ×
[0288] <Preparation of Composition and Evaluation Results>
[0289] Next, Experimental Examples 1 to 4 and Comparative Examples 1 to 5 regarding the composition and the film will be described.
[0290] [Experimental Example 1]
[0291] a. Preparation of the composition
[0292] The composition of Experimental Example 1 was obtained by mixing 90 parts by weight of an alkali-soluble resin (A-1), 10 parts by weight of a hydrophobic resin (B-1), 323 parts by weight of 2-methyl-1-butanol, and 2910 parts by weight of di-n-butyl ether using a mechanical stirrer.
[0293] b. Membrane Preparation
[0294] The composition of Experimental Example 1 was applied to a silicon substrate by spin coating to form a coating film, and then the silicon substrate together with the coating film was placed on a hot plate and baked at 80° C. for 60 seconds to form the film of Experimental Example 1 (film thickness 50 nm).
[0295] [Experimental Examples 2 to 4 and Comparative Examples 1 to 5]
[0296] The compositions and films of Experimental Examples 2 to 4 and Comparative Examples 1 to 5 were prepared in the same manner as Experimental Example 1, except that the types of components and their amounts used in the compositions were changed (as shown in Tables 3 and 4). The prepared compositions and films were evaluated using the evaluation methods described below, and the results are shown in Tables 3 and 4.
[0297] Table 3
[0298]
[0299] Table 4
[0300]
[0301] [Evaluation method]
[0302] 1. Weight average molecular weight
[0303] Using a gel permeation chromatograph (GPC) (model 1515 (autosampler), 2707 (GPC pump) + 2414 (refractive index (RI) detector), manufactured by Waters Corporation), at a column temperature of 40°C, tetrahydrofuran (THF) (stabilized with 2,6-dibutyl hydroxytoluene (BHT), purchased from Duksan) was used as the eluting liquid, and the weight average molecular weight of the resin was obtained by converting the time it took to pass through polystyrene.
[0304] 2. Refractive index
[0305] The refractive index of the film with respect to light of a wavelength of 193 nm was measured using an ellipsometer (Model M2000DI, manufactured by JA Woollam Co., Ltd.).
[0306] 3. Receding contact angle
[0307] Using a contact angle meter (model DSA100, manufactured by KRUSS Co., Ltd.), water was injected into the needle at room temperature and pressure, and the position of the needle was slightly adjusted to an initial position where a water droplet could be formed on the film of the silicon substrate. Subsequently, water was discharged from the needle to form a 25 μL water droplet on the film of the silicon substrate, the needle was temporarily withdrawn from the water droplet, and the needle was pulled down again at the initial position and arranged in the water droplet. Next, at a speed of 10 μL / min, the water droplet was attracted by the needle within 90 seconds and the contact angle was measured once per second (a total of 90 times). In this way, the average value of the contact angle between 20 seconds after the point at which the measured value of the contact angle stabilized was calculated as the receding contact angle (°).
[0308] 4. Water resistance
[0309] The membrane was immersed in ultrapure water for 5 minutes and the dissolution state was observed.
[0310] The evaluation criteria for water resistance are as follows:
[0311] ○: completely insoluble;
[0312] △: partially dissolved;
[0313] ×: Completely dissolved.
[0314] 5. Alkali Solubility
[0315] The film was immersed in a 2.38 mass % aqueous solution of tetramethylammonium hydroxide for 1 second, and the dissolution state was observed.
[0316] The evaluation criteria for alkali solubility are as follows:
[0317] ○: completely dissolved;
[0318] △: partially dissolved;
[0319] ×: Not dissolved at all.
[0320] [Evaluation results]
[0321] According to Tables 3 and 4, compared with the composition not containing the alkali-soluble resin (A) (Comparative Examples 1 to 5), the film formed by the composition containing the alkali-soluble resin (A) (Experimental Examples 1 to 4) can have a high receding contact angle, good water resistance, and good alkali solubility under the premise that the refractive index can match that of water and the photoresist.
[0322] Furthermore, although Comparative Example 1 contains resin (A'-1), which has good alkali solubility, resin (A'-1) contains structural units derived from (meth) acrylic acid, so the receding contact angle is low due to the excessive hydrophilicity of the carboxyl group. Comparative Examples 2 and 3 containing resin (A'-1) increase the proportion of hydrophobic resin (B), but the proportion of resin (A'-1) decreases, resulting in poor alkali solubility. Comparative Examples 4 and 5 contain resin (A'-2), but resin (A'-2) does not contain structural units having carboxyl groups, so the alkali solubility is poor.
[0323] Furthermore, it can be seen from Experimental Example 3, Comparative Example 2 and Comparative Example 5 that, under the premise that the proportion of the hydrophobic resin (B) is the same, the alkali-soluble resin (A-1) has a structural unit (a3) containing a long carbon chain carboxyl group (Experimental Example 3), and therefore has good alkali solubility.
[0324] Furthermore, it can be seen from Experimental Examples 2 and 4 that when the hydrophobic resin (B) contains a cycloalkyl structural unit (Experimental Example 4), the formed film has a higher receding contact angle than when the hydrophobic resin (B) does not contain a cycloalkyl structural unit (Experimental Example 2).
[0325] On the other hand, it can be seen from Experimental Examples 1 to 3 that, as the proportion of the hydrophobic resin (B) increases, the receding contact angle of the formed film increases.
[0326] In summary, the present invention provides an alkali-soluble resin, a protective layer composition of an alkali-soluble resin comprising specific structural units (e.g., a structural unit (a1) having a fluorinated alkyl group, a structural unit (a2) containing α-trifluoromethyl alcohol, and a structural unit (a3) containing a long carbon chain carboxyl group), a protective layer formed by the protective layer composition, a laminate, and a method for forming a photoresist pattern, wherein, on the premise that the refractive index of the protective layer can match that of water and the photoresist, the protective layer has a high receding contact angle, good water resistance, and good alkali solubility, and is therefore suitable for immersion lithography technology.
[0327] Although the present invention has been disclosed as above by way of embodiments, it is not intended to limit the present invention. Any person having ordinary knowledge in the technical field may make some changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the scope of the appended claims.
[0328]
Explanation of symbols
[0329] 100: Laminated body
[0330] 110:Substrate
[0331] 120: Photoresist layer
[0332] 120a: Photoresist pattern
[0333] 130: Protective layer
[0334] 200: Photomask
[0335] 300: Light source
[0336] L: Light
Claims
1. An alkali-soluble resin (A), comprising a structural unit (a1) represented by the following formula (1), a structural unit (a2) represented by the following formula (2), and a structural unit (a3) represented by the following formula (3), In formula (1), R 1 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, R 2 is a fluorinated straight-chain alkyl group or a fluorinated branched-chain alkyl group having 1 to 10 carbon atoms, * indicates a bonding position, In formula (2), R 3 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, Y 1 is an alkylene group having 1 to 10 carbon atoms, a cycloalkylene group having 5 to 10 carbon atoms, or an arylene group, and * indicates a bonding position. 1 When it is an alkylene group having 2 to 10 carbon atoms or a cycloalkylene group having 5 to 10 carbon atoms, one or more of the -CH2- groups may be replaced by -O- or replace, In formula (3), R 4 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, Y 2 is an unsubstituted alkylene group having 2 to 8 carbon atoms, and * indicates a bonding position. 2 In which one or more -CH2- can be replaced by -O- or replace, The molar ratio of the structural unit (a1) represented by the formula (1), the structural unit (a2) represented by the formula (2), and the structural unit (a3) represented by the formula (3) is 10-50:50-90:1-20.
2. The alkali-soluble resin (A) according to claim 1, wherein R 2 The fluorine-containing straight-chain alkyl group or fluorine-containing branched-chain alkyl group having 1 to 10 carbon atoms contains 3 or more fluorine atoms.
3. A protective layer composition comprising: The alkali-soluble resin (A) according to claim 1 or 2; a hydrophobic resin (B); and Solvent (C), The hydrophobic resin (B) comprises a structural unit (b1) represented by the following formula (4) and a structural unit (b2) represented by the following formula (5), In formula (4), R 5 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, R 6 is an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group, and * indicates a bonding position. 6 When it is an alkyl group having 2 to 10 carbon atoms or a cycloalkyl group having 5 to 10 carbon atoms, one or more of the -CH2- groups may be replaced by -O- or replace, In formula (5), R 7 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group, R 8 is a fluorinated alkyl group having 1 to 10 carbon atoms, and * indicates a bonding position. 4 . The protective layer composition according to claim 3 , wherein the molar ratio between the structural unit (b1) represented by the formula (4) and the structural unit (b2) represented by the formula (5) is 10-50:50-90.
5. The protective layer composition according to claim 3, wherein in formula (4), R 6 It is an alkyl group having 1 to 10 carbon atoms. 6 . The protective layer composition according to claim 3 , wherein the solvent (C) comprises an alcohol solvent (C1) and an ether solvent (C2). 7 . The protective layer composition according to claim 6 , wherein the alcohol solvent (C1) is at least one selected from the group consisting of alcohols having 4 to 6 carbon atoms. 8 . The protective layer composition according to claim 6 , wherein the ether solvent (C2) is at least one selected from the group consisting of ethers having a carbon number of 8 to 12. 9 . The protective layer composition according to claim 6 , wherein the weight ratio between the alcohol solvent (C1) and the ether solvent (C2) is 1-50:50-99. 10 . The protective layer composition according to claim 3 , wherein a weight ratio (B / A) between the hydrophobic resin (B) and the alkali-soluble resin (A) is greater than 0.1 and less than 0.
43. 11 . A protective layer formed from the protective layer composition according to claim 3 . 12 . The protective layer according to claim 11 , wherein, under the premise that the thickness of the protective layer is 50 nm, the protective layer is completely dissolved after being immersed in a 2.38 mass % aqueous solution of tetramethylammonium hydroxide for 1 second. 13 . The protective layer according to claim 11 , wherein a receding contact angle of the protective layer to water is 69.5 degrees or more. 14 . The protective layer according to claim 11 , wherein the refractive index of the protective layer with respect to light having a wavelength of 193 nm is 1.54 to 1.
55.
15. A laminate comprising: substrate; a photoresist layer; as well as The protective layer according to any one of claims 11 to 14, The photoresist layer is located between the substrate and the protective layer.
16. A method for forming a photoresist pattern, comprising: forming a photoresist layer on a substrate; forming a protective layer according to any one of claims 11 to 14 on the photoresist layer; exposing the photoresist layer and the protective layer; and The photoresist layer and the protective layer are developed to form a photoresist pattern on the substrate.