A kind of ABS composite material and its preparation method and application
By using silica and tetrafluoroethylene and olefin copolymers as flame retardant synergists in ABS composites, combining bromine and antimony flame retardants, the high cost and low efficiency of flame retardants in the prior art are solved. The problem is that efficient flame retardant effect and mechanical performance improvement have been achieved, meeting the application needs of high flame retardant levels.
Patent Information
- Application Number
- CN202211219419.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-09-30
AI Technical Summary
In the existing ABS flame retardant modification technology, halogen and antimony flame retardants have high cost and material performance are affected, and the halogen-free flame retardant efficiency is limited, making it difficult to meet the application needs of high flame retardant levels.
Silica and tetrafluoroethylene and olefin copolymer are used as flame retardant synergists, combined with bromine and antimony flame retardants, and through specific ratios and particle size optimization, the amount of flame retardant is reduced, and the flame retardant effect is improved. Mechanical properties.
It has achieved a significant reduction in the cost of ABS composite materials, while maintaining excellent flame retardant and mechanical properties, meeting the application needs of high flame retardant levels.
Smart Images

Figure GDA0004836813310000061 
Figure GDA0004836813310000071 
Figure GDA0004836813310000072
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of engineering plastics, in particular to an ABS composite material and a preparation method and application thereof. Background Art
[0002] ABS is one of the most widely used engineering plastics. It is composed of three units: acrylonitrile, butadiene and styrene, which give it excellent performance. Acrylonitrile gives ABS resin chemical stability, oil resistance, certain rigidity and hardness; butadiene can improve toughness, impact resistance and cold resistance; styrene has good dielectric properties and good processability; therefore, ABS has excellent comprehensive physical and mechanical properties, excellent low-temperature impact resistance, dimensional stability and good mechanical processing. However, ABS is a flammable material and cannot be used in industries and fields with high safety regulations. ABS needs to be flame-retardant modified.
[0003] At present, there are two main types of flame retardant modification technologies for ABS. One is halogen-antimony compound flame retardant, which uses bromine and chlorine to match antimony oxide for flame retardant modification. The technology is mature and has the highest market share. However, due to the limited resources of halogen compounds and antimony compounds, the price is currently expensive. At the same time, due to the need to fill a large amount of flame retardants, the material performance is affected to a certain extent; the other is halogen-free flame retardant, and the flame retardant system is mainly phosphate compounds. However, due to the limited flame retardant efficiency, the main commercial products are still low flame retardant grades such as V-2, and the product application is limited. At present, there is a strong interest in reducing the content of flame retardant ABS at home and abroad. Patent CN113429734A shows that a triazine or triamine derivative can replace part of the conventional brominated flame retardant at a certain number of additions. However, due to the high number of substitutes added, the overall content of flame retardant components has not been effectively reduced, the material cost reduction is limited, and the material performance has not been effectively improved. Summary of the invention
[0004] Based on this, the purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and provide an ABS composite material and a preparation method and application thereof.
[0005] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: an ABS composite material, comprising the following components in parts by weight: 80-82 parts of ABS resin, 10-13 parts of bromine-based flame retardant, 1-3 parts of antimony-based flame retardant, 4-10 parts of flame retardant synergist, and 0.5-1.5 parts of processing aid; wherein the flame retardant synergist comprises flame retardant synergist A and flame retardant synergist B, flame retardant synergist A is silicon dioxide, and flame retardant synergist B is a copolymer of tetrafluoroethylene and olefin.
[0006] The present invention provides an ABS composite material, which innovatively adopts a flame retardant synergist A and a flame retardant synergist B to effectively and synergistically improve the flame retardant effect, while reducing the amount of high-priced bromine-based and antimony-based flame retardants added in the ABS composite material, thereby maintaining excellent flame retardant properties while achieving a significant reduction in cost and maintaining mechanical properties.
[0007] The flame retardant synergist A selected in the present invention is silicon dioxide, which can cooperate with the halogen-antimony system during the combustion process to improve the strength of the carbide, thereby enhancing the barrier effect on the combustible gas; the flame retardant synergist B is a copolymer of tetrafluoroethylene and olefin, and the hydrogen fluoride generated by the combustion reacts with silicon dioxide to generate water, which plays a flame retardant role, thereby reducing the addition amount of the halogen flame retardant.
[0008] Preferably, the weight ratio of the flame retardant synergist A to the flame retardant synergist B is: flame retardant synergist A: flame retardant synergist B = (3-5): (1-2).
[0009] After a lot of experimental research, the inventors of the present application found that when the weight ratio of flame retardant synergist A and flame retardant synergist B adopts the above-mentioned specific weight ratio, the prepared ABS composite material has the best flame retardant effect and further improves the mechanical properties of the ABS composite material.
[0010] Preferably, the flame retardant synergist B is at least one of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), and tetrafluoroethylene-ethylene copolymer (ETFE).
[0011] Preferably, the particle size D50 of the silicon dioxide is 5-12 μm.
[0012] The flame retardant synergist A of the present invention is selected as silicon dioxide with a particle size D50 of 5-12 μm, which further improves the mechanical properties of the ABS composite material.
[0013] Preferably, the processing aid is at least one of an anti-dripping agent, an antioxidant, and a lubricant. Further preferably, the anti-dripping agent is at least one of SAN-coated polytetrafluoroethylene micropowder, acrylate-coated polytetrafluoroethylene micropowder, and siloxane-coated polytetrafluoroethylene micropowder; the antioxidant is a hindered phenol antioxidant and / or a phosphite antioxidant; and the lubricant is at least one of amides, stearates, esters, and silicones.
[0014] Preferably, the ABS composite material is at least one of the following (a)-(c):
[0015] (a) the weight percentage of butadiene in the ABS resin is 22-29%;
[0016] (b) the brominated flame retardant is at least one of brominated triazine, brominated epoxy, and tetrabromobisphenol A;
[0017] (c) The antimony-based flame retardant is at least one of antimony oxide and antimonate.
[0018] In addition, the present invention provides a method for preparing the ABS composite material, comprising the following steps:
[0019] (1) Weigh various raw materials according to the ratio;
[0020] (2) adding various raw materials in step (1) into a mixer and mixing them uniformly to obtain a mixed material;
[0021] (3) adding the mixture obtained in step (2) into a twin-screw extruder for melt extrusion and granulation to obtain the ABS composite material.
[0022] Preferably, in step (2), the mixing time is 2-10 min, and the mixing speed is 800-1200 r / min; in step (3), the temperature of each section of the twin-screw extruder is 160-210° C., and the screw speed of the twin-screw extruder is 400-600 r / min.
[0023] Furthermore, the present invention provides application of the ABS composite material in the field of electrical appliances.
[0024] Preferably, the present invention provides applications of the ABS composite material in the fields of household appliances, electronic appliances, etc.
[0025] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention provides an ABS composite material, which ingeniously uses flame retardant synergist A and flame retardant synergist B to efficiently and synergistically improve the flame retardant effect, while reducing the amount of high-priced bromine-based and antimony-based flame retardants added in the ABS composite material, and still maintains excellent flame retardant properties under the premise of significantly reducing costs. The present invention further improves the mechanical properties of the ABS composite material while maintaining the best flame retardant effect of the prepared ABS composite material by selecting the specific ratio of flame retardant synergist A and flame retardant synergist B and the specific particle size D50 of flame retardant synergist A. DETAILED DESCRIPTION
[0026] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0027] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified. The anti-dripping agent, antioxidant, and lubricant used in all the examples and comparative examples of the present invention are exactly the same;
[0028] The raw materials used in the embodiments and comparative examples are described below, but are not limited to these materials:
[0029] ABS resin-1: the weight percentage of butadiene is 29%, ABS PA-747S, Chi Mei, Taiwan, China;
[0030] ABS resin-2: the weight percentage of butadiene is 22%, ABSD-120A, Guoqiao, Taiwan, China;
[0031] ABS resin-3: butadiene weight percentage is 16%, ABS GP-22, INEOS Styrolution;
[0032] Brominated flame retardant-1: tetrabromobisphenol A, FR-1524, commercially available;
[0033] Brominated flame retardant-2: brominated triazine, FR-245, commercially available;
[0034] Antimony flame retardant-1: antimony trioxide, commercially available;
[0035] Antimony flame retardant-2: sodium antimonate, commercially available;
[0036] Flame retardant synergist A-silicon dioxide:
[0037] Silica-1, HS-3386 (particle size D50 is 5 μm), Weifang Hengshuo Nanomaterials Co., Ltd.;
[0038] Silica-2, H-102 (particle size D50 is 7 μm), Zhuzhou Xinglong New Materials Co., Ltd.;
[0039] Silica-3, H-103, (particle size D50 is 12 μm), Zhuzhou Xinglong New Materials Co., Ltd.;
[0040] Silica-4, TS-720 (particle size D50 is 4.3 μm), Cabot, USA;
[0041] Silica-5, HS-3325 (particle size D50 is 45 μm), Weifang Hengshuo Nanomaterials Co., Ltd.;
[0042] Flame retardant synergist B-tetrafluoroethylene and olefin copolymer:
[0043] Tetrafluoroethylene and olefin copolymer-1: tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), AP-202, Daikin Fluorochemical (China) Co., Ltd.;
[0044] Tetrafluoroethylene and olefin copolymer-2: tetrafluoroethylene-hexafluoropropylene copolymer (FEP), NP-3180, Daikin Fluorochemical (China) Co., Ltd.;
[0045] Tetrafluoroethylene and olefin copolymer-3: tetrafluoroethylene-ethylene copolymer (ETFE), EP-506, Daikin Fluorochemical (China) Co., Ltd.;
[0046] Polytetrafluoroethylene-4: Polytetrafluoroethylene (PTFE), F-106, Daikin Fluorochemical (China) Co., Ltd.;
[0047] Processing aids:
[0048] Anti-dripping agent: acrylate coated polytetrafluoroethylene powder, commercially available;
[0049] Antioxidants: antioxidant 1-THANOX 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and antioxidant 2-THANOX168 (tris(2,4-di-tert-butylphenyl) phosphite), commercially available;
[0050] Lubricant: Pentaerythritol stearate lubricant, commercially available;
[0051] Examples 1-12 and Comparative Examples 1-6
[0052] The components and weight proportions of the ABS composite materials of the embodiments and comparative examples are shown in Table 1, wherein:
[0053] The preparation method of the ABS composite material of Examples 1-12 and Comparative Examples 1-6 comprises the following steps:
[0054] (1) Weigh various raw materials according to the ratio;
[0055] (2) adding various raw materials in step (1) into a mixer and mixing them uniformly to obtain a mixed material; the mixing time is 5 minutes and the mixing speed is 1000 r / min;
[0056] (3) adding the mixture obtained in step (2) into a twin-screw extruder for melt extrusion granulation, wherein the temperature of each section of the twin-screw extruder is 160-210° C. and the screw speed of the twin-screw extruder is 400-600 r / min, to obtain the ABS composite material.
[0057] The processing aid is composed of an anti-dripping agent, a pentaerythritol stearate lubricant, and an antioxidant in a mass ratio of 2:1:1, and the antioxidant is composed of a primary antioxidant THANOX 1010 and an auxiliary antioxidant THANOX 168 in a mass ratio of 3:2;
[0058] Table 1
[0059]
[0060] Table 2
[0061]
[0062] Performance Testing
[0063] The ABS composite materials prepared in the examples and comparative examples were dried in a blast oven at 80°C for 4 hours and then injection molded into standard specimens using a plastic injection molding machine at an injection molding temperature of 200-210°C. The injection molded specimens were placed at a relative humidity of 50% and 23°C for at least 24 hours before performance testing.
[0064] (1) Test the flame retardancy of 1.6 mm standard specimens according to UL94-2009 standard;
[0065] (2) Izod notched impact strength: The specimens were injection molded into rod-shaped specimens (notch type A) that meet the requirements of ISO 180-2019 Izod notched impact strength test and subjected to Izod notched impact strength test at 25°C.
[0066] (3) Flexural strength: according to ISO 178-2019 method, test speed 2 mm / min;
[0067] The test results are shown in Table 3 and Table 4;
[0068] Table 3
[0069]
[0070]
[0071] Table 4
[0072]
[0073] The present invention provides an ABS composite material, which innovatively adopts a flame retardant synergist A and a flame retardant synergist B to effectively and synergistically improve the flame retardant effect, while reducing the amount of high-priced bromine-based and antimony-based flame retardants added in the ABS composite material, thereby maintaining excellent flame retardant properties while achieving a significant reduction in cost and maintaining mechanical properties.
[0074] It can be seen from the above table that the ABS composite materials prepared in the embodiments of the present invention all meet the requirements of flame retardancy (1.6 mm) of V-0 and Izod beam notched impact strength ≥ 15 KJ / m 2 , bending strength ≥60MPa.
[0075] From the comparison between Examples 3-6 and Example 1, it can be seen that the flame retardant synergist A is selected as silicon dioxide with a particle size D50 of 5-12 μm, which further improves the mechanical properties of the ABS composite material.
[0076] From the comparison between Examples 7-8, Example 1 and Comparative Example 1, it can be seen that when the flame retardant synergist B is a copolymer of tetrafluoroethylene and olefin, the flame retardant property and the mechanical property are better.
[0077] From the comparison between Example 1 and Comparative Examples 2-3, it can be seen that when the flame retardant synergist is 4-10 parts, the flame retardant properties and mechanical properties of the prepared ABS composite material are better.
[0078] By comparing Examples 9-12 with Example 1, it can be seen that when the weight ratio of flame retardant synergist A to flame retardant synergist B is: flame retardant synergist A: flame retardant synergist B = (3-5): (1-2), the prepared ABS composite material has better flame retardant properties and mechanical properties.
[0079] From the comparison between Example 1 and Comparative Examples 4-6, it can be seen that the flame retardant synergist of the present invention has a synergistic effect. Without any one of them, the flame retardant effect is poor and the Izod notched impact strength decreases significantly.
[0080] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. An ABS composite material, characterized in that: The invention comprises the following components in parts by weight: 80-82 parts of ABS resin, 10-13 parts of brominated flame retardant, 1-3 parts of antimony flame retardant, 4-10 parts of flame retardant synergist, and 0.5-1.5 parts of processing aid; The flame retardant synergist comprises a flame retardant synergist A and a flame retardant synergist B, the flame retardant synergist A is silicon dioxide, and the flame retardant synergist B is a copolymer of tetrafluoroethylene and olefin.
2. The ABS composite material according to claim 1, characterized in that: The weight ratio of the flame retardant synergist A to the flame retardant synergist B is: flame retardant synergist A: flame retardant synergist B = (3-5): (1-2).
3. The ABS composite material according to claim 1, characterized in that: The flame retardant synergist B is at least one of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and tetrafluoroethylene-ethylene copolymer.
4. The ABS composite material according to claim 1, characterized in that: The particle size D50 of the silicon dioxide is 5-12 μm.
5. The ABS composite material according to claim 1, characterized in that: The processing aid is at least one of an anti-drip agent, an antioxidant, and a lubricant.
6. The ABS composite material according to claim 1, characterized in that: At least one of the following (a)-(c): (a) the weight percentage of butadiene in the ABS resin is 22-29%; (b) the brominated flame retardant is at least one of brominated triazine, brominated epoxy, and tetrabromobisphenol A; (c) The antimony-based flame retardant is at least one of antimony oxide and antimonate.
7. A method for preparing the ABS composite material according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Weigh various raw materials according to the ratio; (2) adding various raw materials in step (1) into a mixer and mixing them uniformly to obtain a mixed material; (3) adding the mixture obtained in step (2) into a twin-screw extruder for melt extrusion and granulation to obtain the ABS composite material.
8. The method for preparing the ABS composite material according to claim 7, characterized in that: In the step (2), the mixing time is 2-10 min, and the mixing speed is 800-1200 r / min; in the step (3), the temperature of each section of the twin-screw extruder is 160-210° C., and the screw speed of the twin-screw extruder is 400-600 r / min.
9. Use of the ABS composite material according to any one of claims 1 to 6 in the field of electrical appliances.